Resin composition

The resin composition, formed by chemically bonding thermoplastic resin with a carbonyl group-containing material using maleic anhydride, achieves high elastic modulus and shape recovery at high temperatures, addressing the plastic deformation issue in thermoplastic resins and enhancing their durability for industrial applications.

WO2024232195A1PCT designated stage expired Publication Date: 2024-11-14PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013712
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-10
Filing Date
2024-04-03
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Thermoplastic resin compositions deform plastically at high temperatures and fail to return to their original shape when force is removed, limiting their application in industrial parts that require durability and shape retention.

Method used

A resin composition is developed by chemically bonding a thermoplastic resin with a carbonyl group-containing material, using a maleic anhydride structure-containing additive to form a three-dimensional crosslinked structure through ring-opening reactions, enhancing the elastic modulus and allowing the resin to recover its shape upon force removal at high temperatures.

Benefits of technology

The resin composition exhibits high elastic modulus and shape recovery at high temperatures, overcoming the plastic deformation issue of conventional thermoplastic resins, making it suitable for industrial applications that require durability and shape retention.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013712_14112024_PF_FP_ABST
    Figure JP2024013712_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The resin composition contains a thermoplastic resin and a carbonyl group based on other than the thermoplastic resin, and the thermoplastic resin and the carbonyl group are chemically bonded.
Need to check novelty before this filing date? Find Prior Art

Description

resin composition

[0001] The present disclosure relates to a resin composition made from a thermoplastic resin and having a high elastic modulus at high temperatures.

[0002] Thermoplastic resins are generally widely used in general-purpose resin compositions due to their high productivity, which allows for rapid molding using methods such as injection molding, and their ease of recycling, which allows molded products to be remolded into any shape by remelting them. Thermoplastic resins with particularly excellent strength, such as polyamides, are widely used as so-called engineering plastics in industrial parts that require high durability, such as automotive interior parts. However, at high temperatures close to the upper limit of the heat resistance temperature range of the thermoplastic resins that make up the resin compositions, they deform when force is applied, and remain deformed even after the force is released, making it impossible to maintain their original shape, a problem known as plastic deformation.

[0003] As a means for imparting the characteristic of so-called elastic deformation, in which a resin composition deforms when a force is applied to it but returns to its original shape when the force is released, for example, Patent Document 1 discloses a resin composition that is flexible and can restore its original shape even if deformed, which is obtained by mixing a polyrotaxane, a thermosetting resin, and a curing agent.

[0004] Patent No. 6380942

[0005] However, when polyrotaxane, which imparts flexibility, is mixed into the resin composition, it is prone to deformation even at room temperature, which limits its application to industrial parts that must maintain their shape even when force is applied at room temperature.

[0006] The present disclosure has been made in view of the above points as a result of the inventors' diligent efforts, and aims to provide a resin composition that uses a thermoplastic resin as a raw material and has a high elastic modulus at high temperatures.

[0007] The resin composition according to the present disclosure is a resin composition that contains a thermoplastic resin and a carbonyl group based on a material other than the thermoplastic resin, and in which the thermoplastic resin and the carbonyl group are chemically bonded.

[0008] The resin composition according to the present disclosure is formed by blending a predetermined amount of a thermoplastic resin and a maleic anhydride structure-containing additive, powder-mixing the blend, and subjecting the powder-mixed mixture to hot melt stirring or hot melt kneading. Hot melt stirring or hot melt kneading causes ring-opening of the maleic anhydride structure in the maleic anhydride structure-containing compound, and the open ring sites bond to functional groups in the thermoplastic resin and other functional groups in the thermoplastic resin, thereby forming a three-dimensional crosslinked structure between the thermoplastic resins, resulting in a resin composition characterized by a high elastic modulus that allows the resin composition to recover its original shape when the force is released even if it is deformed by the application of force at high temperatures.

[0009] 1 is a diagram showing an AFM image of a resin composition according to Example 1. FIG. 1 is a diagram showing an example of an AFM-IR measurement spectrum at AFM-IR measurement point 1 in the AFM image of the resin composition according to Example 1. FIG. 1 is a diagram showing an example of an AFM-IR measurement spectrum at AFM-IR measurement point 2 in the AFM image of the resin composition according to Example 1. FIG. 1 is a diagram showing an AFM image of a resin composition according to Comparative Example 1. FIG. 4 is a diagram showing an example of an AFM-IR measurement spectrum at AFM-IR measurement point 1 in the AFM image of the resin composition according to Comparative Example 1. FIG. 4 is a diagram showing an example of an AFM-IR measurement spectrum at AFM-IR measurement point 2 in the AFM image of the resin composition according to Comparative Example 1. (a) is a bird's-eye view showing an example of a method for evaluating deformation and restoration at high temperatures in Examples 1 to 16 and Comparative Examples 1 to 3, and (b) is a side view of (a). Table 1 shows the weight parts of each raw material and the evaluation results in Examples 1 to 9. Table 2 shows the weight parts of each raw material and the evaluation results in Examples 10 to 16 and Comparative Examples 1 to 3.

[0010] The resin composition according to the first aspect of the present disclosure is a resin composition that contains a thermoplastic resin and a carbonyl group based on a material other than the thermoplastic resin, and the thermoplastic resin and the carbonyl group are chemically bonded to each other.

[0011] The resin composition according to the second aspect of the present disclosure may be, in the first aspect, one that deforms when a compressive or tensile force is applied at 180°C or higher and 260°C or lower, and then restores to its shape before the force was applied when the force is released.

[0012] In the resin composition according to a third aspect of the present disclosure, in the first or second aspect, the thermoplastic resin may have an amino group.

[0013] In the resin composition according to the fourth aspect of the present disclosure, in the third aspect, the thermoplastic resin may be polyamide.

[0014] The resin composition according to the fifth aspect of the present disclosure is a resin composition in any one of the first to fourth aspects described above, which contains an organic fibrous filler as a raw material and in which the thermoplastic resin and the organic fibrous filler are chemically bonded, and the chemical bond between the thermoplastic resin and the filler may include a carbonyl group based on a material other than the thermoplastic resin.

[0015] In the resin composition according to a sixth aspect of the present disclosure, in any one of the first to fifth aspects, the carbonyl group may be part of an ester bond.

[0016] In the resin composition according to a seventh aspect of the present disclosure, in the fifth or sixth aspect, the organic fibrous filler may be cellulose fiber.

[0017] The resin composition according to the eighth aspect of the present disclosure may be the same as the seventh aspect, wherein the weight content of the cellulose fiber in the entire resin composition is 30% by weight or more and 90% by weight or less.

[0018] Hereinafter, a resin composition according to an embodiment of the present disclosure will be described in detail with reference to the accompanying drawings.

[0019] (Embodiment 1) <Resin Composition> The resin composition according to embodiment 1 is a resin composition containing a thermoplastic resin and a carbonyl group based on a material other than the thermoplastic resin, in which the thermoplastic resin and the carbonyl group are chemically bonded. Specifically, the thermoplastic resin may be, for example, a resin having an amino group or a polyamide.

[0020] <Method for producing resin composition> An example of a method for producing a resin composition according to the present disclosure includes: (A) a step of powder-mixing a thermoplastic resin and a maleic anhydride structure-containing additive to obtain a powder mixture; and (B) a step of stirring and kneading the powder mixture while thermally melting it to obtain a resin composition.

[0021] <(A) Regarding the step of preparing a powder mixture> The step of preparing a powder mixture is a step of physically mixing a pellet-shaped thermoplastic resin with, for example, a powder of a maleic anhydride structure-containing material to prepare a physical mixture (powder mixture).

[0022] <(B) Regarding the step of preparing a resin composition> The step of preparing a resin composition is a manufacturing process in which the physical mixture (powder mixture) is kneaded while being heated using a device capable of hot melt mixing, such as a single-screw kneader, a twin-screw kneader, or a Banbury mixer. During the hot melt process, a chemical bond is formed between the resin and the maleic anhydride structure-containing substance by reaction of, for example, a terminal functional group or a part of the skeletal structure of the resin with an active site generated by ring-opening of the maleic anhydride structure. When multiple maleic anhydride structures are present in the maleic anhydride structure-containing substance, a maleic anhydride structure other than the maleic anhydride structure bonded to the resin reacts with another part of the resin, and the thermoplastic resin is chemically bonded via the carbonyl group derived from the maleic anhydride structure, forming a three-dimensional crosslinked structure between the thermoplastic resins.

[0023] The method for producing the resin composition will be described in detail below.

[0024] (1) Raw Materials <Thermoplastic Resin> Among the raw materials used in the method for producing a resin composition according to the present disclosure, the thermoplastic resin may be any resin that can be deformed by being heated and melted, and that can be mixed with not only organic fibrous fillers but also glass fillers, glass fibers, and other inorganic fillers. A mixture of multiple thermoplastic resins may also be used. Examples of thermoplastic resins include, but are not limited to, polyethylene, polyvinyl chloride, polypropylene, polystyrene, acrylonitrile-butadiene-styrene, acrylonitrile-styrene, polymethyl methacrylate, polybutylene terephthalate, polyethylene terephthalate, polyamide, polyoxymethylene, polyvinyl alcohol, polyphenylene ether, polycarbonate, polyphenylene sulfide, aromatic polyether ketone, and polyimide. In particular, thermoplastic resins with a softening temperature of 150°C or higher and 250°C or lower are preferred due to their ease of melting during production and thermal stability during use. Furthermore, it is preferable that the thermoplastic resin has reactivity with the chemically active site generated by ring-opening of maleic anhydride, and from this viewpoint, it is preferable that the thermoplastic resin has an amino group, a hydroxyl group, a carboxyl group, a thiol group, an ester structure, an amide structure, a urea structure, an amine structure, or a cyano structure. From the above viewpoints, polyamides and polyesters are particularly preferable as the thermoplastic resin in the present disclosure, and particularly preferable specific examples include polybutylene terephthalate, polyethylene terephthalate, and polyamides such as nylon 6 and nylon 66.

[0025] <Maleic anhydride structure-containing additive> The maleic anhydride structure-containing additive may be one containing at least one maleic anhydride structure per molecule. However, the maleic anhydride structure-containing additive is not limited to the above. The maleic anhydride structure undergoes ring-opening, and the ring-opened structure reacts with the thermoplastic resin, while another maleic anhydride structure contained in the same molecule as the molecule containing the maleic anhydride structure undergoes ring-opening, and the ring-opened structure reacts with another part of the thermoplastic resin. As a result, the thermoplastic resins are chemically bonded via the carbonyl group derived from the maleic anhydride structure, forming a three-dimensional crosslinked structure, and the elastic modulus of the resin composition at high temperatures is improved. Examples of maleic anhydride structure-containing compounds that function in this manner include maleic anhydride-styrene copolymer, maleic anhydride-vinyl acetate copolymer, maleic anhydride-vinyl benzoate copolymer, poly(ethylene-alt-maleic anhydride), polypropylene-graft-maleic anhydride, poly(isobutylene-alt-maleic anhydride), poly(methyl vinyl ether-alt-maleic anhydride), polystyrene-block-poly(ethylene-lan-butylene)-block-polystyrene-graft-maleic anhydride, (-)-2,3-bis[(2R,5R)-2,5-dimethylphosphorano]maleic anhydride, citraconic anhydride, and cyclobutane-1,2,3,4-tetracarboxylic dianhydride.

[0026] The amount of the maleic anhydride structure-containing material added can be 0.5 wt% or more and 7 wt% or less based on the total weight of the resin composition. If it is less than 0.5 wt%, the effect of improving the elastic modulus at high temperatures will not be sufficient. If it is more than 7 wt%, a large amount of maleic anhydride structure will be contained that does not form an open ring structure and does not react with part of the thermoplastic resin. This unreacted maleic anhydride structure becomes a non-functional foreign matter that can become the starting point for cracks, which is undesirable. Furthermore, from the viewpoint of ensuring that the maleic anhydride structure reacts with the thermoplastic resin in just the right amount, a content of 1.25 wt% or more and 5 wt% or less is even more preferable.

[0027] <Method for Producing Resin Composition> The resin composition according to the first embodiment can be produced by mixing specified amounts of a thermoplastic resin and a maleic acid structure-containing substance to form a mixture, hot-melt mixing the mixture, and then cooling the mixture. To mix the components, the respective components can be weighed into a container or bag and mixed manually using a spatula or a rod-shaped jig that can be used for stirring, or by using a rotary mixer such as a Henschel mixer to achieve a substantially uniform mixture. From the standpoint of facilitating the above-described mixing process, the thermoplastic resin and the maleic acid structure-containing substance are preferably in powder or pellet form. For hot-melt mixing, the substantially uniformly mixed powder mixture can be mixed using a single-screw mixer, twin-screw mixer, roll mixer, kneader, Banbury mixer, or the like, or a combination of these. After hot-melt mixing, the mixture can be cooled to a temperature at which pulverization is possible, resulting in the resin composition according to the present disclosure. Furthermore, other additives such as pigments and flame retardants can be added to the mixture to be mixed in the hot-melt mixer, as appropriate, depending on the intended use.

[0028] When the resin composition produced in this manner is molded and applied to, for example, industrial parts, the crosslinking reaction between the thermoplastic resins results in an excellent molded product that can elastically deform and restore its shape at high temperatures, even though conventional resin molded products would undergo plastic deformation when force is applied.

[0029] (Embodiment 2) <Resin Composition> The resin composition according to embodiment 2 includes an organic fibrous filler and a thermoplastic resin, and is a resin composition in which the thermoplastic resin and the organic fibrous filler are chemically bonded. The chemical bond between the thermoplastic resin and the organic fibrous filler includes a carbonyl group based on a material other than the thermoplastic resin. Specifically, the carbonyl group is, for example, part of an ester bond. The organic fibrous filler is, for example, cellulose fiber. The weight content of the cellulose fiber in the entire resin composition is, for example, 30% by weight or more and 90% by weight or less. The thermoplastic resin may be the same as that in embodiment 1, and may be, for example, one having an amino group or polyamide.

[0030] <Method for producing resin composition> An example of a method for producing a resin composition according to the present disclosure includes: (A) a step of powder-mixing a thermoplastic resin, an organic fibrous filler, and a maleic anhydride structure-containing additive to obtain a powder mixture; and (B) a step of stirring and kneading the powder mixture while thermally melting it to obtain a resin composition.

[0031] Another example of the method for producing a resin composition according to the present disclosure includes: (A0) a step of powder-mixing an organic fibrous filler and an epoxy group-containing alkoxysilane to produce an epoxy group-modified organic fibrous filler; (A1) a step of powder-mixing a thermoplastic resin, the epoxy group-modified organic fibrous filler, and a maleic anhydride structure-containing additive to prepare a powder mixture; and (B) a step of stirring and kneading the powder mixture while heat-melting it to prepare a resin composition.

[0032] <Regarding (A) and (A1) the step of preparing a powder mixture> The step of preparing a powder mixture is a step of physically mixing a pellet-shaped thermoplastic resin, an organic fibrous filler, and, for example, a powdered maleic anhydride structure-containing material to prepare a physical mixture (powder mixture).

[0033] <(B) Step of Producing a Resin Composition> The step of producing a resin composition is a production process in which the physical mixture (powder mixture) is kneaded under heating using an apparatus capable of hot melt mixing, such as a single-screw kneader, a twin-screw kneader, a Banbury mixer, etc. In the hot melt process, the resin and the maleic anhydride structure-containing substance are bonded together by reaction between, for example, a terminal functional group or a part of the skeletal structure of the resin and an active site generated by ring-opening of the maleic anhydride structure, and a chemical bond is formed between the organic fibrous filler and the maleic anhydride structure by reaction between a hydroxyl group present on the surface of the organic fibrous filler and an active site generated by ring-opening of the maleic anhydride structure-containing substance. When a plurality of maleic anhydride structures are present in the maleic anhydride structure-containing material, a maleic anhydride structure other than the maleic anhydride structure bonded to the resin reacts with the organic fibrous filler, and the organic fibrous filler and the thermoplastic resin are chemically bonded via the carbonyl group in the ester bond derived from the maleic anhydride structure, thereby forming a three-dimensional crosslinked structure between the organic fibrous filler and the thermoplastic resin. Furthermore, as in the first embodiment, a maleic anhydride structure other than the maleic anhydride structure bonded to the resin reacts with another part of the resin, and a chemical bond of the thermoplastic resin is also formed via the carbonyl group derived from the maleic anhydride structure, thereby forming a three-dimensional crosslinked structure between the thermoplastic resins.

[0034] The method for producing the resin composition will be described in detail below.

[0035] (1) Raw Materials <Thermoplastic Resin> Of the raw materials used in the method for producing a resin composition according to the second embodiment, the thermoplastic resin may be the same as that used in the first embodiment.

[0036] <Organic fibrous filler> As the organic fibrous filler, those derived from known plant fibers can be used. Specifically, but not limited to, for example, cellulose, cellulose fiber, cellulose nanofiber, lignocellulose, lignocellulose fiber, lignocellulose nanofiber, pulp, rayon, acetate, cupra, cotton, hemp, jute fiber, etc. can be used. Among them, celluloses are preferably used from the viewpoint of having a stable surface structure and being easy to modify, and these plant fiber-derived fibrous fillers may be mixed.

[0037] The length of the fibrous filler can be, for example, 50 nm or more and 500 μm or less. If it is shorter than 50 nm, aggregation becomes severe, making dispersion difficult during hot melt mixing. If it is longer than 500 μm, the viscosity during hot melting becomes too high, making molding difficult. From the viewpoint of simultaneously suppressing aggregation and suppressing high viscosity, a length of 100 nm or more and 100 μm or less is more preferable.

[0038] The organic fibrous filler may be surface-modified in advance, and from the viewpoint of facilitating reaction with the maleic anhydride structure-containing additive, alkoxysilanes such as epoxy group-containing alkoxysilanes and amino group-containing alkoxysilanes can be used as surface modifiers.

[0039] As a surface modification method, for example, a method in which an organic fibrous filler is dispersed in a solvent such as water or alcohol to form a dispersion, a specified amount of the alkoxysilane is dropped into the dispersion while stirring, and the solvent is then volatilized while the dispersion is heated in a heating furnace, or a method in which the organic fibrous filler and the alkoxysilane are mixed and stirred in a known dry blending device such as a Henschel mixer, etc., can be used to perform surface modification.

[0040] The amount of alkoxysilanes used for surface modification is not limited, but can be, for example, 0.1% by weight to 2% by weight based on the weight of the organic fibrous filler. If it is less than 0.1% by weight, the amount of alkoxysilanes is too small, and the effect of the reaction with the maleic anhydride structure-containing additive due to surface modification is insufficient. If it is more than 2% by weight, agglomerates are formed due to the reaction between the alkoxysilanes, which may hinder uniform dispersion of the organic fibrous filler.

[0041] As described above, by using an organic fibrous filler whose surface is modified with epoxy groups or amino groups, the epoxy groups or amino groups are more likely to react with the ring-open structure of the maleic anhydride structure in the maleic anhydride structure-containing additive described below, and it is possible to form an even stronger three-dimensional crosslinked structure compared to when an organic fibrous filler that is not surface-modified is used.

[0042] <Maleic anhydride structure-containing additive> The maleic anhydride structure-containing additive may be the same as that in Embodiment 1. As in Embodiment 1, in addition to the formation of a three-dimensional crosslinked structure between thermoplastic resins, the maleic anhydride structure undergoes ring-opening, and the ring-opened structure reacts with the thermoplastic resin, while another maleic anhydride structure contained in the same molecule as the molecule containing the maleic anhydride structure undergoes ring-opening, and the ring-opened structure reacts with a hydroxyl group on the organic fibrous filler, thereby chemically bonding the thermoplastic resin and the organic fibrous filler, and the thermoplastic resin and the organic fibrous filler firmly adhere to each other to form a three-dimensional crosslinked structure, thereby improving the elastic modulus of the composite, i.e., the resin composition, at high temperatures.

[0043] The amount of the maleic anhydride structure-containing compound added depends on the blending ratio of the organic fibrous filler to the resin composition, but can be, for example, 0.5 wt % to 7 wt % based on the total weight of the resin composition. If it is less than 0.5 wt %, the effect of improving the elastic modulus at high temperatures described above is insufficient. If it is more than 7 wt %, a large amount of maleic anhydride structure is contained that does not form an open ring structure and does not react with the organic fibrous filler or part of the thermoplastic resin. This unreacted maleic anhydride structure becomes a non-functional foreign matter that can become the starting point for cracks, which is undesirable. Furthermore, from the viewpoint of ensuring that the maleic anhydride structure reacts appropriately with the organic fibrous filler and the thermoplastic resin, a content of 1.25 wt % to 5 wt % is even more preferable.

[0044] <Method for Producing Resin Composition> The resin composition according to the second embodiment can be produced by mixing specified amounts of a thermoplastic resin, an organic fibrous filler, and a maleic acid structure-containing substance to form a mixture, hot-melt mixing the mixture, and then cooling the mixture. To mix the components, the components can be weighed into a container or bag and mixed manually using a spatula or a rod-shaped jig that can be used for stirring, or by using a rotary mixer such as a Henschel mixer to achieve a substantially uniform mixture. From the standpoint of facilitating the above-described mixing process, the thermoplastic resin and the maleic acid structure-containing substance are preferably in powder or pellet form. For hot-melt mixing, the substantially uniformly mixed powder mixture can be mixed using a single-screw mixer, a twin-screw mixer, a roll mixer, a kneader, a Banbury mixer, or a combination of these. After hot-melt mixing, the mixture can be cooled to a temperature at which pulverization is possible, resulting in the resin composition according to the present disclosure. Furthermore, other additives such as pigments and flame retardants can be added to the mixture to be mixed in the hot-melt mixer, as appropriate, depending on the intended use.

[0045] When the resin composition produced in this manner is molded and applied to, for example, industrial parts, the incorporation of the organic fibrous filler results in a higher biomass content than conventional resin molded articles, contributing to a reduction in the burden on the environment. At the same time, the crosslinking reaction between the organic fibrous filler and the thermoplastic resin, and the crosslinking reaction between the thermoplastic resins, result in an excellent molded article that can elastically deform and restore its shape at high temperatures, where conventional resin molded articles would undergo plastic deformation when force is applied.

[0046] Examples 1 to 16 and Comparative Examples 1 to 3 will be specifically described below.

[0047] Example 1 Production of Resin Composition As a thermoplastic resin, 43.9 parts by weight of nylon 6, a type of polyamide, 55.0 parts by weight of cellulose fiber (Nippon Paper Industries Co., Ltd. (KC Flock (W-100G))) was prepared as an organic fibrous filler, and 1.1 parts by weight of polypropylene-graft-maleic anhydride was prepared as a maleic anhydride structure-containing additive. These were placed in a polyethylene container and manually stirred and mixed for 5 minutes using a spatula. The mixture was then sequentially fed into the hopper of a twin-screw kneader set at 260°C, and hot-melt mixed while being extruded at a rotation speed of 100 rpm. The molten mixture was recovered from the discharge outlet and used as a resin composition according to Example 1.

[0048] <Analysis of molecular structure of resin composition> AFM-IR measurement was performed to analyze the molecular structure of the resin composition. An observation spot was determined while observing a piece of the resin composition sliced ​​with a microtome for TEM observation using an optical microscope, and an AFM image and infrared absorption spectrum reflection measurement were performed at that spot to perform structural analysis in the nano region.

[0049] FIG. 1 shows an example of an AFM image of the resin composition according to Example 1. FIGS. 2 and 3 show examples of spectra obtained by AFM-IR measurement at AFM-IR measurement points 1 and 2 in the AFM image of the resin composition according to Example 1 shown in FIG. 1. First, in the AFM image, the boundary between the maleic anhydride structure-containing additive and the resin is unclear, revealing that the maleic anhydride structure-containing additive is chemically reacting. Furthermore, polyamide resin is impregnated between the cellulose fibers. Furthermore, FIGS. 2 and 3 show that peaks of carbonyl groups not derived from the raw material resin, polyamide, are observed in the resin phase. The inventors believe that these characteristics are formed by the following mechanism. Specifically, during the hot melt mixing process, the maleic anhydride structure in the polypropylene-graft-maleic anhydride undergoes ring-opening, resulting in a reaction with the hydroxyl groups on the surface of the cellulose fibers. Furthermore, the ring-opened structure of another maleic anhydride structure in the polypropylene-graft-maleic anhydride molecule having the maleic anhydride structure reacts with the amino group at the polymer chain end of the polyamide. This chemically bonds the cellulose fiber and polyamide, improving compatibility and allowing the polyamide resin to impregnate the spaces between the cellulose fibers. Furthermore, during the hot melt mixing process, the ring-opened structure of the maleic anhydride structure in the polypropylene-graft-maleic anhydride molecule reacts with the amino group at the polymer chain end of the polyamide. Furthermore, the ring-opened structure of another maleic anhydride structure in the polypropylene-graft-maleic anhydride molecule having the maleic anhydride structure reacts with the amino group at the polymer chain end of another polyamide. This chemically bonds the polyamides together, forming a three-dimensional crosslinked structure. The carbonyl groups not derived from polyamide, which were confirmed in the spectrum measured by AFM-IR, are due to ester bonds formed by the ring-opening structure of the additive containing a maleic anhydride structure, and indicate that the cellulose fiber and polyamide are chemically bonded to form a three-dimensional crosslinked structure, and that a three-dimensional crosslinked structure is also formed between the polyamides.

[0050] Example 2 This example was the same as Example 1, except that an epoxy surface-modified organic fibrous filler was used as the organic fibrous filler. The epoxy surface-modified organic fibrous filler was produced by the following method.

[0051] <Production of Surface-Modified Organic Fibrous Filler> In this Example 2, the organic fibrous filler was a surface-modified organic fibrous filler, and the surface modification was carried out with an epoxy group-containing alkoxysilane. (1) 1000 parts by weight of cellulose fiber (Nippon Paper Industries Co., Ltd. (KC Flock (W-100G)) was prepared as an organic fibrous filler, and 50 parts by weight of 3-glycidoxypropyltrimethoxysilane (Shin-Etsu Chemical Co., Ltd. KBM403) was prepared as an epoxy group-containing alkoxysilane. (2) The cellulose fiber was placed in a Henschel mixer, and 3-glycidoxypropyltrimethoxysilane was placed in a syringe. (3) While the cellulose fiber in the Henschel mixer was being stirred at a rotation speed of 1000 rpm, the needle of the syringe was inserted through a syringe hole provided in the lid of the Henschel mixer, and 3-glycidoxypropyltrimethoxysilane was injected into the mixer. (4) After the injection, rotation was continued for another 10 minutes, and after the rotation was stopped, the epoxy surface-modified cellulose fiber was recovered from the Henschel mixer.

[0052] Example 3 Example 3 was the same as Example 1, except that 98.9 parts by weight of nylon 6 was prepared as the thermoplastic resin, and no organic fibrous filler was prepared.

[0053] Example 4 Example 4 was the same as Example 2, except that 68.9 parts by weight of nylon 6 was prepared as the thermoplastic resin, and 30 parts by weight of epoxy surface-modified cellulose fiber was prepared as the organic fibrous filler.

[0054] Example 5 Example 5 was the same as Example 2, except that 8.9 parts by weight of nylon 6 was prepared as the thermoplastic resin, and 90.0 parts by weight of epoxy surface-modified cellulose fiber was prepared as the organic fibrous filler.

[0055] Example 6 Example 6 was the same as Example 2, except that 43.9 parts by weight of nylon 66, a type of polyamide, was prepared as the thermoplastic resin.

[0056] Example 7 Example 7 was the same as Example 2, except that 44.5 parts by weight of nylon 6 was prepared as the thermoplastic resin, and 0.5 parts by weight of polypropylene-graft-maleic anhydride was prepared as the maleic anhydride structure-containing additive.

[0057] Example 8 Example 8 was the same as Example 2, except that 38.0 parts by weight of nylon 6 was prepared as the thermoplastic resin, and 7.0 parts by weight of polypropylene-graft-maleic anhydride was prepared as the maleic anhydride structure-containing additive.

[0058] Example 9 This example was the same as Example 2, except that 43.75 parts by weight of nylon 6 was used as the thermoplastic resin, and 1.25 parts by weight of polypropylene-graft-maleic anhydride was used as the maleic anhydride structure-containing additive.

[0059] Example 10 The procedure was the same as Example 2, except that 40.0 parts by weight of nylon 6 was prepared as the thermoplastic resin, and 5.0 parts by weight of polypropylene-graft-maleic anhydride was prepared as the maleic anhydride structure-containing additive.

[0060] Example 11 The procedure was the same as Example 1, except that poly(isobutylene-alt-maleic anhydride) was used as the maleic anhydride structure-containing additive.

[0061] Example 12 This example was the same as Example 1, except that an amino-surface-modified cellulose fiber (KC Flock (W-100G) manufactured by Nippon Paper Industries Co., Ltd.) was used as the organic fibrous filler. The amino-surface-modified cellulose fiber was produced by the same method as the production of the surface-modified organic fibrous filler in Example 2, using 3-aminopropyltrimethoxysilane (KBM903 manufactured by Shin-Etsu Chemical Co., Ltd.) as the amino group-containing alkoxysilane.

[0062] Example 13 Example 13 was the same as Example 1, except that 73.9 parts by weight of nylon 6 was prepared as the thermoplastic resin, and 25.0 parts by weight of epoxy surface-modified cellulose fiber was prepared as the organic fibrous filler.

[0063] Example 14 Example 14 was the same as Example 1, except that 6.9 parts by weight of nylon 6 was prepared as the thermoplastic resin, and 92.0 parts by weight of epoxy surface-modified cellulose fiber was prepared as the organic fibrous filler.

[0064] Example 15 The same as Example 1 was carried out, except that 44.7 parts by weight of nylon 6 was prepared as the thermoplastic resin, and 0.3 parts by weight of polypropylene-graft-maleic anhydride was prepared as the maleic anhydride structure-containing additive.

[0065] Example 16 The same as Example 1 was carried out, except that 36.0 parts by weight of nylon 6 was prepared as the thermoplastic resin, and 9.0 parts by weight of polypropylene-graft-maleic anhydride was prepared as the maleic anhydride structure-containing additive.

[0066] Comparative Example 1 This comparative example was the same as Example 1, except that 45.0 parts by weight of nylon 6 was prepared as the thermoplastic resin, and 55.0 parts by weight of the cellulose fiber (Nippon Paper Industries Co., Ltd. (KC Flock (W-100G))) was prepared as the organic fibrous filler, and further, no maleic anhydride structure-containing additive was added.

[0067] The molecular structure of the resin composition was analyzed in the same manner as in Example 1.

[0068] FIG. 4 shows an example of an AFM image of a resin composition according to Comparative Example 1. FIGS. 5 and 6 show examples of spectra obtained by AFM-IR measurement at AFM-IR measurement points 1 and 2 in the AFM image of the resin composition according to Comparative Example 1 in FIG. 4 . That is, the boundary between the cellulose fiber and the resin is confirmed in FIG. 4 , and the AFM-IR measurement spectrum at that interface is shown in FIG. 5 . In Example 1, a broad peak specific to the carbonyl group derived from the ester bond, not derived from an amide, was observed at the boundary between the cellulose fiber and the resin, as described above. However, this is not observed in FIG. 5 . Furthermore, FIG. 6 shows the AFM-IR measurement spectrum of the interior of the resin in FIG. 4 . Even within the resin, the broad peak specific to the carbonyl group derived from the ester bond, not derived from an amide, as described above, is not observed. Therefore, it can be seen that in Comparative Example 1, a structure that directly bonds the resin and cellulose fiber, as observed in Example 1, and a three-dimensional crosslinked structure between the resins, were not formed.

[0069] Comparative Example 2 The same procedure as in Example 1 was repeated except that 55.0 parts by weight of epoxy surface-modified cellulose fiber was prepared as the organic fibrous filler, and no maleic anhydride structure-containing additive was added.

[0070] Comparative Example 3 The same as Example 1 was carried out except that 100.0 parts by weight of nylon 6 was prepared as the thermoplastic resin, no organic fibrous filler was prepared, and no maleic anhydride structure-containing additive was added.

[0071] <Molding of Resin Composition and Evaluation of Elastic Deformation> The resin composition according to the present disclosure can be injection molded. The resin composition was pulverized in a pulverizer to form pellets, and then the pellets were used to prepare dumbbell test pieces of the resin composition using an injection molding machine (180AD manufactured by The Japan Steel Works, Ltd.). The dumbbell test pieces were prepared under the following conditions: resin temperature 240°C, mold temperature 80°C, injection speed 60 mm / s, and holding pressure 100 MPa. The shape of the test piece was JIS K7139 dumbbell test piece type A for evaluating deformation and recovery. The test pieces of the resin composition obtained in this manner were evaluated by the following method.

[0072] (Evaluation of Deformation and Recovery at High Temperature) The obtained dumbbell test specimens were evaluated for deformation when heated and subjected to force, and for whether they returned to their original shape when the force was released. FIG. 7( a) is an overhead view showing an example of the evaluation method at high temperature, and FIG. 7( b) is a side view of FIG. 7( a). The obtained dumbbell test specimen 10 was placed on the heating plate 20 of a hot plate controlled at an arbitrary temperature by the heating plate control unit 40. After 10 minutes, compressive and tensile forces were applied to the obtained dumbbell test specimen in the long axis direction using a rod-shaped tool 30. The obtained dumbbell test specimen was evaluated for visually observable deformation. Furthermore, when deformation was observed, specimens that returned to their original shape when the force was released after deformation were evaluated as ○, those that returned particularly quickly as ⊚, those that only partially returned as △, and those that did not return at all were evaluated as ×.

[0073] The parts by weight of each raw material and the evaluation results in Examples 1 to 9 are shown in Table 1 of Figure 8. The parts by weight of each raw material and the evaluation results in Examples 10 to 16 and Comparative Examples 1 to 3 are shown in Table 2 of Figure 9.

[0074] A comparison between Example 1 and Comparative Example 1 reveals that the addition of a maleic anhydride structure-containing product results in a resin composition with a high elastic modulus at high temperatures, which means that the shape is restored even if the resin is deformed at high temperatures of 180° C. or higher and 260° C. or lower. It is also clear that at 80° C., a room temperature range where no deformation occurs even without the addition of a maleic anhydride structure-containing product, no deformation occurs even when the maleic anhydride structure-containing product is added.

[0075] Examples 1, 2, 12 and Comparative Example 2 show that when a substance containing a maleic anhydride structure is added, if the surface of the cellulose fiber is appropriately modified, the effect is even more pronounced, resulting in a resin composition with a higher elastic modulus at high temperatures.

[0076] A comparison between Example 3 and Comparative Example 3 reveals that even without adding an organic fibrous filler, the addition of a maleic anhydride structure-containing substance results in a resin composition with a high elastic modulus that restores its shape when the force is released even if it is deformed at high temperatures.

[0077] From the results of Examples 4, 5, 13, and 14, it can be seen that the amount of organic fibrous filler added is preferably 30% by weight or more and 90% by weight or less, and a resin composition having a particularly high elastic modulus at high temperatures is obtained.

[0078] From Examples 2 and 6, it can be seen that the resin to which the present disclosure can be applied is not limited to the type of polyamide, and that it is possible to improve the elastic modulus at high temperatures.

[0079] From Examples 7, 8, 9, 10, 15, and 16, it is clear that the amount of the maleic anhydride structure-containing substance to be added is preferably 0.5% by weight or more and 7% by weight or less, and particularly preferably 1.25% by weight or more and 5% by weight or less.

[0080] Examples 1 and 11 show that a plurality of types of maleic anhydride structure-containing materials can be used.

[0081] As described above, the resin composition according to the present disclosure has excellent elastic modulus at high temperatures and can be applied to various industrial products that can maintain their shape even in conditions involving temperature changes.

[0082] 10 Dumbbell test piece 20 Heating plate 30 Tool 40 Heating plate control unit

Claims

1. A resin composition comprising a thermoplastic resin and a carbonyl group based on a material other than the thermoplastic resin, wherein the thermoplastic resin and the carbonyl group are chemically bonded.

2. The resin composition according to claim 1, wherein the resin composition deforms when a compressive or tensile force is applied at a temperature of 180°C or higher and 260°C or lower, and then restores to its original shape when the force is released.

3. The resin composition according to claim 1 or 2, wherein the thermoplastic resin has an amino group.

4. The resin composition according to claim 3, wherein the thermoplastic resin is a polyamide.

5. A resin composition according to claim 1 or 2, which contains an organic fibrous filler, in which the thermoplastic resin and the organic fibrous filler are chemically bonded, and in which the chemical bond between the thermoplastic resin and the organic fibrous filler includes a carbonyl group based on a material other than the thermoplastic resin.

6. The resin composition according to claim 1 or 2, wherein the carbonyl group is part of an ester bond.

7. The resin composition according to claim 5, wherein the organic fibrous filler is cellulose fiber.

8. The resin composition according to claim 7, wherein the weight content of the cellulose fiber in the entire resin composition is 30% by weight or more and 90% by weight or less.

Citation Information

Patent Citations

  • Resin composition and film using the same

    JP6380942B2

  • Fiber-reinforced polyamide resin composition

    JP2021084999A

  • Resin composition and method for producing the same

    JP2022159126A

  • Sliding member

    WO2019098210A1