Rubber composition, vulcanized product, and vulcanized molded body

A rubber composition combining chloroprene and butyl rubber with specific additives enhances gas barrier, bending fatigue resistance, and heat resistance, addressing the limitations of conventional butyl rubber compositions in achieving these properties.

WO2024232223A1PCT designated stage expired Publication Date: 2024-11-14DENKA CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014998
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-08
Filing Date
2024-04-15
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Conventional rubber compositions face challenges in simultaneously improving gas barrier properties, flex fatigue resistance, and heat resistance in vulcanizates and vulcanized molded products, particularly when using butyl rubber, which struggles to maintain these properties while enhancing bending fatigue resistance.

Method used

A rubber composition combining chloroprene-based rubber and butyl-based rubber, with chloroprene rubber containing an unsaturated nitrile monomer unit, along with specific additives like thiourea compounds and sulfenamide compounds, is used to achieve improved gas barrier, bending fatigue resistance, and heat resistance.

Benefits of technology

The resulting vulcanizates and vulcanized molded products exhibit excellent gas barrier, bending fatigue resistance, and heat resistance, making them suitable for applications requiring these properties, such as tire inner liners, tubes, and curing bladders.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

Provided is a rubber composition that makes it possible to obtain a vulcanized product and a vulcanized molded body excellent in gas barrier property, bending fatigue resistance, and heat resistance. The present invention provides a rubber composition including a chloroprene-based rubber and a butyl-based rubber, the rubber composition containing 0.1-99 parts by mass of a chloroprene-based rubber with respect to 100 parts by mass of a rubber contained in the rubber composition, wherein the chloroprene-based rubber contains a chloroprene-based rubber containing an unsaturated nitrile monomer unit.
Need to check novelty before this filing date? Find Prior Art

Description

Rubber composition, vulcanizate, and vulcanized molded product

[0001] The present invention relates to a rubber composition, a vulcanizate, and a vulcanized molded article.

[0002] Taking advantage of their properties, rubber compositions are used in a wide range of fields, such as general industrial power transmission belts and conveyor belts, automotive air springs, vibration-isolating rubber, hoses, wipers, dipped products, sealing parts, adhesives, boots, rubber-coated fabrics, rubber rolls, etc. In recent years, the properties required of rubber parts have increased significantly.

[0003] Patent Document 1 discloses a rubber composition for tire vulcanization bladders, characterized by blending 1 to 20 parts by mass of an alkylphenol-formaldehyde condensate and 0.1 to 10 parts by mass of a citraconic imide compound with 100 parts by mass of a rubber component containing 90 parts by mass or more of a butyl-based rubber consisting of butyl rubber and / or halogenated butyl rubber. Patent Document 2 discloses a rubber composition for bladders, which contains a rubber component containing a butyl-based rubber and zinc oxide having an average primary particle size of 15 to 190 nm.

[0004] JP 2016-098294 A JP 2010-285225 A

[0005] However, it has been difficult to simultaneously improve gas barrier property, flex fatigue resistance, and heat resistance in vulcanizates and vulcanization molded articles obtained from conventional rubber compositions. The present invention has been made in view of these circumstances, and provides a rubber composition from which vulcanizates and vulcanization molded articles excellent in gas barrier property, flex fatigue resistance, and heat resistance can be obtained.

[0006] According to the present invention, there is provided a rubber composition containing a chloroprene-based rubber and a butyl-based rubber, wherein the rubber composition contains 0.1 to 99 parts by mass of the chloroprene-based rubber when the rubber contained in the rubber composition is taken as 100 parts by mass, and the chloroprene-based rubber contains a chloroprene-based rubber containing an unsaturated nitrile monomer unit.

[0007] It has been known that butyl-based rubber has excellent gas barrier properties and heat resistance. However, it has been difficult to improve flex fatigue resistance while maintaining gas barrier properties and heat resistance in vulcanizates and vulcanized molded articles obtained from rubber compositions containing butyl-based rubber. The present inventors have conducted extensive research and found that, in chloroprene-based rubber compositions containing butyl-based rubber and chloroprene-based rubber, it is possible to obtain vulcanizates and vulcanized molded articles having excellent gas barrier properties, flex fatigue resistance, and heat resistance by specifying the type and amount of chloroprene-based rubber, thereby completing the present invention.

[0008] Various embodiments of the present invention are exemplified below. The embodiments shown below can be combined with each other. [1] A rubber composition containing a chloroprene-based rubber and a butyl-based rubber, wherein the rubber composition contains 0.1 to 99 parts by mass of the chloroprene-based rubber per 100 parts by mass of rubber contained in the rubber composition, and the chloroprene-based rubber contains a chloroprene-based rubber containing an unsaturated nitrile monomer unit. [2] The rubber composition according to [1], wherein the rubber composition contains a thiourea-based compound, 3-methyl-thiazolidine-2-thione, and a thiadiazole-based compound in a total amount of 0.1 to 10.0 parts by mass per 100 parts by mass of rubber contained in the rubber composition. [3] The rubber composition according to [1] or [2], wherein the butyl-based rubber contains a halogenated butyl rubber. [4] The rubber composition according to any one of [1] to [3], wherein the rubber composition contains a total of 0.1 to 10.0 parts by mass of a thiuram compound, a thiazole compound, and a sulfenamide compound per 100 parts by mass of rubber contained in the rubber composition. [5] The rubber composition according to any one of [1] to [4], wherein the chloroprene-based rubber contains 1 to 25% by mass of unsaturated nitrile monomer units per 100 parts by mass of the chloroprene-based rubber. [6] The rubber composition according to any one of [1] to [5], wherein the rubber composition contains 1 to 30 parts by mass of compound A having at least one ester structure and a molecular weight of 300 to 1,000 per 100 parts by mass of rubber contained in the rubber composition. [7] A vulcanizate of the rubber composition according to any one of [1] to [6]. [8] A vulcanized molded article of the vulcanizate according to [7].

[0009] The rubber composition according to the present invention can provide a vulcanizate and a vulcanized molded article having excellent gas barrier properties, flex fatigue resistance, and heat resistance. The vulcanizate and the vulcanized molded article according to the present invention also have excellent gas barrier properties, flex fatigue resistance, and heat resistance. In addition to known applications (e.g., general industrial power transmission belts and conveyor belts, automotive air springs, anti-vibration rubber, hoses, wipers, immersion products, sealing parts, adhesives, boots, rubberized fabrics, and rubber rolls), the vulcanizate and the vulcanized molded article according to the present invention can be suitably used, taking advantage of their properties, as materials for, for example, tire innerliners, tubes, curing bladders, pharmaceutical rubber stoppers, electrical wire coatings, vibration-proofing materials, hoses, linings, capacitor packings, and gaskets. The vulcanizate and the vulcanized molded article according to one embodiment of the present invention can be suitably used for applications requiring particularly excellent gas barrier properties, flex fatigue resistance, and heat resistance, such as tire innerliners, tubes, and curing bladders.

[0010] 1. Rubber Composition The rubber composition according to the present invention is a rubber composition containing a chloroprene-based rubber and a butyl-based rubber, and the rubber composition contains 0.1 to 99 parts by mass of the chloroprene-based rubber relative to 100 parts by mass of the rubber contained in the rubber composition, and the chloroprene-based rubber contains a chloroprene-based rubber containing an unsaturated nitrile monomer unit.

[0011] 1.1 Chloroprene-Based Rubber The chloroprene-based rubber according to the present invention refers to a rubber containing a chloroprene-based polymer having chloroprene (2-chloro-1,3-butadiene) as a monomer unit (monomer unit = structural unit). Examples of the chloroprene-based polymer include a chloroprene homopolymer and a chloroprene copolymer (a copolymer of chloroprene and a monomer copolymerizable with chloroprene). The polymer structure of the chloroprene-based polymer is not particularly limited.

[0012] Commercially available 2-chloro-1,3-butadiene may contain a small amount of 1-chloro-1,3-butadiene as an impurity. 2-chloro-1,3-butadiene containing such a small amount of 1-chloro-1,3-butadiene can also be used as the chloroprene monomer of this embodiment.

[0013] The chloroprene-based rubber according to the present invention contains a chloroprene-based rubber containing an unsaturated nitrile monomer unit. The chloroprene-based rubber according to the present invention may contain one or more chloroprene-based rubbers. The chloroprene-based rubber according to one embodiment of the present invention may contain a chloroprene-based rubber containing one or more unsaturated nitrile monomer units. Furthermore, the chloroprene-based rubber according to one embodiment of the present invention may further contain a chloroprene-based rubber that does not contain one or more unsaturated nitrile monomer units.

[0014] The chloroprene-based rubber (the chloroprene-based rubber containing unsaturated nitrile monomer units and the chloroprene-based rubber not containing unsaturated nitrile monomer units) according to one embodiment of the present invention may also have monomer units derived from a monomer other than the chloroprene monomer and the unsaturated nitrile monomer. The monomer other than the chloroprene monomer and the unsaturated nitrile monomer is not particularly limited as long as it is copolymerizable with the chloroprene monomer, and examples thereof include esters of (meth)acrylic acid (methyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc.), hydroxyalkyl (meth)acrylates (2-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, etc.), 2,3-dichloro-1,3-butadiene, 1-chloro-1,3-butadiene, butadiene, isoprene, ethylene, styrene, sulfur, etc. For example, the chloroprene-based rubber according to one embodiment of the present invention may include 2,3-dichloro-1,3-butadiene monomer units.

[0015] In the chloroprene-based rubber containing unsaturated nitrile monomer units according to one embodiment of the present invention, the content of the unsaturated nitrile monomer units can be 1 to 25% by mass, preferably 1 to 20% by mass, and more preferably 5 to 20% by mass, based on 100% by mass of the chloroprene-based rubber containing unsaturated nitrile monomer units. The content of the unsaturated nitrile monomer units in the chloroprene-based rubber containing unsaturated nitrile monomer units according to one embodiment of the present invention is, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, or 25% by mass, or may be within a range between any two of the values ​​exemplified here. By controlling the content of the unsaturated nitrile monomer units in the rubber composition to be equal to or less than the above upper limit, the water resistance and cold resistance of a vulcanized molded article made from the rubber composition are further improved. Furthermore, by containing unsaturated nitrile monomer units, the oil resistance of a vulcanized molded article of the rubber composition is improved.

[0016] When the chloroprene-based rubber according to one embodiment of the present invention contains two or more chloroprene-based rubbers, the content based on the total amount of unsaturated nitrile monomer units contained in the two or more chloroprene-based rubbers, relative to 100% by mass of the total of the two or more chloroprene-based rubbers contained in the rubber composition, is preferably within the above-mentioned numerical range. That is, the chloroprene-based rubber according to one embodiment of the present invention preferably contains 1 to 25% by mass of unsaturated nitrile monomer units relative to 100% by mass of the chloroprene-based rubber, and the content of the unsaturated nitrile monomer units may be within a range between any two of the above-mentioned numerical values. Furthermore, the chloroprene-based rubber according to one embodiment of the present invention preferably contains 1 to 25% by mass of acrylonitrile monomer units relative to 100% by mass of the chloroprene-based rubber, and the content of the acrylonitrile monomer units may be within a range between any two of the above-mentioned numerical values.

[0017] Examples of unsaturated nitriles include acrylonitrile, methacrylonitrile, ethacrylonitrile, and phenylacrylonitrile. The unsaturated nitriles may be used alone or in combination of two or more. The unsaturated nitrile preferably contains acrylonitrile, from the viewpoint of easily obtaining excellent moldability and easily obtaining excellent breaking strength, breaking elongation, hardness, tear strength, and oil resistance in a vulcanized molded product.

[0018] The content of unsaturated nitrile monomer units in chloroprene-based rubber can be calculated from the content of nitrogen atoms in the chloroprene-based rubber. Specifically, the content of nitrogen atoms in 100 mg of chloroprene-based rubber can be measured using an elemental analyzer (Sumigraph 220F, manufactured by Sumika Chemical Analysis Center Co., Ltd.), and the content of structural units derived from unsaturated nitrile monomers can be calculated. Elemental analysis can be performed under the following conditions. For example, the electric furnace temperatures are set to 900°C for the reactor, 600°C for the reduction furnace, 70°C for the column, and 100°C for the detector, and oxygen is flowed at 0.2 mL / min as the combustion gas and 80 mL / min as the carrier gas. A calibration curve can be prepared using aspartic acid (10.52%), which has a known nitrogen content, as a standard substance.

[0019] The chloroprene-based rubber according to one embodiment of the present invention preferably contains 75 to 100 mass% of chloroprene monomer units, and more preferably 80 to 100 mass%, of the chloroprene-based rubber taken as 100 mass%. The content of the chloroprene monomer units in the chloroprene-based rubber may be, for example, 75, 80, 85, 90, 95, 99, or 100 mass%, or may be within a range between any two of the values ​​exemplified here. By setting the content of the chloroprene monomer units within the above numerical range, a rubber composition can be obtained that can give a molded product having an excellent balance of hardness, tensile strength, and cold resistance.

[0020] A chloroprene-based rubber according to one embodiment of the present invention may contain 0 to 20 mass% of monomer units other than chloroprene monomer units and unsaturated nitrile monomer units, when the chloroprene-based rubber is taken as 100 mass%. The content of monomer units other than chloroprene monomer units and unsaturated nitrile monomer units in the chloroprene-based rubber may be, for example, 0, 2, 4, 6, 8, 10, 12, 14, 16, 18, or 20 mass%, and may be within a range between any two of the values ​​exemplified here. By adjusting the copolymerization amount of the monomer other than the chloroprene monomer and the unsaturated nitrile monomer within the above range, the effects of copolymerizing these monomers can be achieved without impairing the properties of the resulting rubber composition.

[0021] When the rubber composition according to one embodiment of the present invention contains two or more types of chloroprene-based rubber, it is preferable that the content based on the total amount of each monomer unit contained in the two or more types of chloroprene-based rubber be within the above-mentioned numerical range, relative to 100 mass% in total of the two or more types of chloroprene-based rubber contained in the rubber composition.

[0022] The chloroprene polymer (e.g., chloroprene homopolymer or chloroprene copolymer) contained in the chloroprene rubber according to the present invention may be a sulfur-modified chloroprene polymer, a mercaptan-modified chloroprene polymer, a xanthogen-modified chloroprene polymer, a dithiocarbonate-based chloroprene polymer, a trithiocarbonate-based chloroprene polymer, a carbamate-based chloroprene polymer, or the like.

[0023] 1.2 Method for Producing Chloroprene-Based Rubber The method for producing the chloroprene-based rubber according to the present invention is not particularly limited, but the rubber can be obtained by a production method including an emulsion polymerization step in which raw material monomers containing a chloroprene monomer are emulsion-polymerized. In the emulsion polymerization step according to one embodiment of the present invention, raw material monomers containing a chloroprene monomer are emulsion-polymerized using an appropriate emulsifier, dispersant, catalyst, chain transfer agent, etc., and a polymerization terminator is added when the target final conversion rate is reached, thereby obtaining a latex containing a chloroprene-based polymer containing chloroprene monomer units. Next, unreacted monomers can be removed from the polymerization liquid obtained by the emulsion polymerization step. The method for this removal is not particularly limited, and examples include steam stripping. Thereafter, the pH is adjusted, and the resulting mixture is subjected to conventional processes such as freeze coagulation, water washing, and hot air drying, thereby obtaining a chloroprene-based rubber containing a chloroprene-based polymer.

[0024] The polymerization initiator used in emulsion polymerization is not particularly limited, and any known polymerization initiator generally used in emulsion polymerization of chloroprene can be used. Examples of the polymerization initiator include potassium persulfate, ammonium persulfate, sodium persulfate, hydrogen peroxide, and organic peroxides such as t-butyl hydroperoxide.

[0025] The emulsifier used in emulsion polymerization is not particularly limited, and any known emulsifier generally used in emulsion polymerization of chloroprene can be used. Examples of the emulsifier include alkali metal salts of saturated or unsaturated fatty acids having 6 to 22 carbon atoms, alkali metal salts of rosin acid or disproportionated rosin acid (e.g., potassium rosinate), and alkali metal salts of formalin condensates of β-naphthalenesulfonic acid (e.g., sodium salt).

[0026] The molecular weight modifier used in emulsion polymerization is not particularly limited, and any known molecular weight modifier commonly used in emulsion polymerization of chloroprene can be used, such as mercaptan compounds, xanthogen compounds, dithiocarbonate compounds, trithiocarbonate compounds, and carbamate compounds. Xanthogen compounds, dithiocarbonate compounds, trithiocarbonate compounds, and carbamate compounds are preferably used as molecular weight modifiers for the chloroprene rubber according to one embodiment of the present invention.

[0027] The polymerization temperature and the final conversion rate of the monomer are not particularly limited, but the polymerization temperature may be, for example, 0 to 50°C or 10 to 50°C. The polymerization may be carried out so that the final conversion rate of the monomer falls within the range of 40 to 95% by mass. In order to adjust the final conversion rate, a polymerization terminator that terminates the polymerization reaction may be added to terminate the polymerization when the desired conversion rate is reached.

[0028] The polymerization terminator is not particularly limited, and any known polymerization terminator generally used in emulsion polymerization of chloroprene can be used, such as phenothiazine (thiodiphenylamine), 4-t-butylcatechol, and 2,2-methylenebis-4-methyl-6-t-butylphenol.

[0029] The chloroprene rubber according to one embodiment of the present invention can be obtained, for example, by removing unreacted monomers by a steam stripping method, adjusting the pH of the latex, and then performing conventional steps such as freeze coagulation, water washing, and hot air drying.

[0030] Chloroprene rubbers are classified into mercaptan-modified, xanthogen-modified, sulfur-modified, dithiocarbonate-based, trithiocarbonate-based and carbamate-based types depending on the type of molecular weight modifier.

[0031] 1.3 Butyl-Based Rubber The rubber composition according to the present invention contains a butyl-based rubber. In the present invention, butyl-based rubber refers to a rubber containing a butyl-based polymer containing monomer units derived from isobutylene. That is, the butyl-based rubber contains isobutylene monomer units. Furthermore, the butyl-based rubber according to one embodiment of the present invention may contain isobutylene monomer units and isoprene monomer units, i.e., a copolymer obtained by copolymerizing raw monomers containing isobutylene and isoprene. The butyl-based rubber may contain 0.5 to 10 mol% of isoprene monomer units. The content of isoprene monomer units refers to the proportion (mol%) of isoprene monomer units when the sum of the number of moles of isobutylene monomer units, the number of moles of isoprene monomer units, and, if present, the number of moles of other monomer units contained in the butyl-based rubber is taken as 100 mol%.

[0032] The butyl-based rubber according to the present invention may contain one or more types of butyl-based rubber. The butyl-based rubber according to one embodiment of the present invention may contain one or more types selected from regular butyl rubber (non-halogenated butyl rubber) and halogenated butyl rubber. The butyl-based rubber according to one embodiment of the present invention may contain halogenated butyl rubber. The butyl-based rubber according to one embodiment of the present invention may be halogenated butyl rubber. Examples of halogenated butyl rubber include chlorinated butyl rubber and brominated butyl rubber. The halogenated butyl rubber may contain 0.1 to 5.0% by mass of halogen, preferably 0.5 to 3.0% by mass, of halogenated butyl rubber taken as 100% by mass. The halogen content of the halogenated butyl rubber may be, for example, 0.1, 0.2, 0.3, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0% by mass, and may be within a range between any two of the values ​​exemplified here.

[0033] The butyl rubber according to one embodiment of the present invention preferably contains 75 to 100 mass % of isobutylene monomer units, and more preferably 80 to 100 mass %, of the butyl rubber taken as 100 mass %. The content of chloroprene monomer units in the butyl rubber may be, for example, 75, 80, 85, 90, 95, 99, or 100 mass %, or may be within a range between any two of the values ​​exemplified here.

[0034] 1.4 Other Rubbers The rubber composition according to one embodiment of the present invention may contain rubbers other than chloroprene-based rubber and butyl-based rubber. Examples of other rubbers include natural rubber (NR), hydrogenated acrylonitrile butadiene rubber (H-NBR), acrylonitrile butadiene rubber (NBR), chlorosulfonated polyethylene (CSM), ethylene-propylene-diene rubber (EPDM), isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene rubber (SBR), epoxidized natural rubber (ENR), acrylonitrile butadiene rubber (NBR), styrene-isoprene-butadiene copolymer rubber (SIBR), epichlorohydrin rubber (CO), acrylic rubber (ACM), urethane rubber (U), silicone rubber (Q), fluororubber (FKM), and polysulfide rubber (T). The rubber composition according to one embodiment of the present invention may contain chloroprene-based rubber, butyl-based rubber, and natural rubber.

[0035] 1.5 Rubber Amount The rubber composition according to the present invention contains 0.1 to 99 parts by mass of chloroprene rubber, based on 100 parts by mass of the rubber contained in the rubber composition. According to the present invention, by including a chloroprene rubber containing a chloroprene rubber containing an unsaturated nitrile monomer unit, flex fatigue resistance is significantly improved even if the content is small. The content of the chloroprene rubber is preferably 0.1 to 90 parts by mass, more preferably 0.1 to 70 parts by mass, and even more preferably 0.3 to 50 parts by mass. The content of the chloroprene-based rubber is, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 99 parts by mass, and may be within a range between any two of the numerical values ​​exemplified here.

[0036] The rubber composition according to the present invention may contain 1 to 99.9 parts by mass of butyl rubber, preferably 10 to 99.9 parts by mass, more preferably 30 to 99.9 parts by mass, and even more preferably 50 to 99.9 parts by mass, of butyl rubber, based on 100 parts by mass of rubber contained in the rubber composition. The amount of butyl rubber is, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 96, 97, 98, 99, 99.5, or 99.9 parts by mass, and may be within a range between any two of the values ​​exemplified here.

[0037] The rubber composition according to the present invention may contain a total of 50 to 100 parts by mass, preferably 70 to 100 parts by mass, and more preferably 90 to 100 parts by mass of chloroprene-based rubber and butyl-based rubber per 100 parts by mass of rubber contained in the rubber composition. The total content of chloroprene-based rubber and butyl-based rubber may be, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 100 parts by mass, and may be within a range between any two of the values ​​exemplified here. The rubber composition according to the present invention may contain 0 to 50 parts by mass, 0 to 30 parts by mass, or 0 to 10 parts by mass of rubber other than chloroprene-based rubber and butyl-based rubber per 100 parts by mass of rubber contained in the rubber composition.

[0038] 1.6 Vulcanizing Agent and Vulcanization Accelerator The rubber composition according to the present invention may contain a vulcanizing agent. The rubber composition according to the present invention may also contain a vulcanization accelerator. The types of vulcanizing agent and vulcanization accelerator are not particularly limited as long as they do not impair the effects of the present invention. The vulcanizing agent and vulcanization accelerator preferably contribute to the vulcanization of butyl-based rubber and / or chloroprene-based rubber, and more preferably contribute to the vulcanization of butyl-based rubber and chloroprene-based rubber.

[0039] One or more vulcanizing agents can be freely selected and used. Examples of vulcanizing agents include sulfur. When the rubber composition according to one embodiment of the present invention contains regular butyl rubber as the butyl rubber, it preferably contains sulfur. The content of the vulcanizing agent can be 0 to 10.0 parts by mass, preferably 0 to 5.0 parts by mass, per 100 parts by mass of rubber contained in the rubber composition. For example, the content may be 0, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7, 8, 9, or 10.0 parts by mass, or may be within a range between any two of the values ​​exemplified here. The rubber composition according to the present invention may also be free of a vulcanizing agent.

[0040] The rubber composition according to one embodiment of the present invention may contain a vulcanization accelerator. The rubber composition according to one embodiment of the present invention may contain 0 to 10.0 parts by mass of the vulcanization accelerator per 100 parts by mass of the rubber contained in the rubber composition. The content of the vulcanization accelerator is, for example, 0, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, or 10.0 parts by mass, or may be within a range between any two of the values ​​exemplified here. Note that the rubber composition according to the present invention may not contain a vulcanization accelerator.

[0041] One or more vulcanization accelerators can be freely selected and used, and examples of the vulcanization accelerator include thiuram compounds, 3-methyl-thiazolidine-2-thione, thiadiazole compounds, dithiocarbamate compounds, thiourea compounds, guanidine compounds, xanthogenate compounds, thiazole compounds, and sulfenamide compounds.

[0042] A rubber composition according to one embodiment of the present invention preferably contains at least one selected from a thiourea-based compound, 3-methyl-thiazolidine-2-thione, and a thiadiazole-based compound. A rubber composition according to one embodiment of the present invention preferably contains at least a thiourea-based compound. A rubber composition according to one embodiment of the present invention preferably contains 0.1 to 10.0 parts by mass, and more preferably 0.3 to 5.0 parts by mass, of the thiourea-based compound, 3-methyl-thiazolidine-2-thione, and the thiadiazole-based compound in total per 100 parts by mass of rubber contained in the rubber composition. The total content of the thiourea compound, 3-methyl-thiazolidine-2-thione, and thiadiazole compound is, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, and may be within a range between any two of the values ​​exemplified herein. By containing one vulcanization accelerator selected from the group consisting of a thiourea compound, 3-methyl-thiazolidine-2-thione, and a thiadiazole compound, and particularly by containing these in a total content within the above-mentioned range, the vulcanization of the chloroprene rubber and the butyl rubber proceeds sufficiently, resulting in a rubber composition from which a vulcanizate and a vulcanized molded article having excellent gas barrier properties, flex fatigue resistance, and heat resistance can be obtained.

[0043] The thiourea compound may be a compound having a thiourea structure, such as a compound represented by the following formula:

[0044]

[0045] In the above formula, R 11 ~R 14can each independently represent hydrogen or an organic group, can represent hydrogen or a hydrocarbon group, and the hydrocarbon group can be an alkyl group or an aryl group. Examples of thiourea compounds include ethylene thiourea, diethyl thiourea (N,N'-diethyl thiourea), trimethyl thiourea, diphenyl thiourea (N,N'-diphenyl thiourea), 1,3-trimethylene-2-thiourea, etc.

[0046] 3-Methyl-thiazolidine-2-thione is represented by the following formula:

[0047]

[0048] An example of the thiadiazole compound is di(5-mercapto-1,3,4-thiadiazol-2-yl)disulfide, which is represented by the following formula:

[0049]

[0050] The rubber composition according to one embodiment of the present invention preferably contains one selected from the group consisting of thiuram compounds, thiazole compounds, and sulfenamide compounds. The rubber composition according to one embodiment of the present invention preferably contains 0.1 to 10.0 parts by mass, and more preferably 0.1 to 5.0 parts by mass, of the thiuram compounds, thiazole compounds, and sulfenamide compounds in total, per 100 parts by mass of rubber contained in the rubber composition. The total amount of the thiuram compounds, thiazole compounds, and sulfenamide compounds is 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, and may be within a range between any two of the values ​​exemplified herein. By including at least one vulcanization accelerator selected from thiuram compounds, thiazole compounds and sulfenamide compounds, particularly within the above-mentioned numerical range, the rubber composition can give vulcanizates and vulcanized molded articles having even better resistance to flex fatigue.

[0051] Thiuram compounds include compounds containing one or more structures represented by the following formula:

[0052]

[0053] In the above formula, R 21 , R 22 , R 23 , R 24 can each independently be an organic group, preferably a hydrocarbon group. The hydrocarbon group can be an alkyl group having 1 to 12 carbon atoms or a cycloalkyl group having 1 to 12 carbon atoms. 21 and R 22 , R 23 and R 24 may be linked to each other to form a cyclic structure (for example, a cycloalkyl group). n can be an integer of 1 or greater, and can be 1 to 4, preferably 1 or 2, and more preferably 2. Examples of thiuram compounds include tetramethylthiuram disulfide (TMTD), tetraethylthiuram disulfide, tetrabutylthiuram disulfide, tetrakis(2-ethylhexyl)thiuram disulfide, tetramethylthiuram monosulfide, and dipentamethylenethiuram tetrasulfide.

[0054] Examples of sulfenamide compounds include compounds having a sulfenamide structure. Examples of sulfenamide compounds include N-cyclohexyl-2-benzothiazolyl sulfenamide and N-oxydiethylene-2-benzothiazolyl sulfenamide. The sulfenamide compound may be a compound having a sulfenamide structure and a thiazole skeleton.

[0055] Examples of the thiazole compound include compounds having a thiazole skeleton (excluding the compounds listed as Compound A), and those having a benzothiazole skeleton are more preferred. Examples of the thiazole compound include 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, 2-mercaptobenzothiazole zinc salt, cyclohexylamine salt of 2-mercaptobenzothiazole, 2-(4'-morpholinodithio)benzothiazole, N-cyclohexylbenzothiazole-2-sulfenamide, N-cyclohexyl-2-benzothiazolyl sulfenamide, and N-oxydiethylene-2-benzothiazolyl sulfenamide. The thiazole compound may be a compound having a thiazole skeleton and a sulfenamide structure.

[0056] The rubber composition according to an embodiment of the present invention may contain vulcanization accelerators other than thiourea-based compounds, thiuram-based compounds, thiazole-based compounds, and sulfenamide-based compounds, such as dithiocarbamate-based compounds, guanidine-based compounds, xanthogenate-based compounds, and benzimidazole-based compounds.

[0057] Examples of dithiocarbamate compounds include sodium dibutyldithiocarbamate, zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc N-ethyl-N-phenyldithiocarbamate, zinc N-pentamethylenedithiocarbamate, copper dimethyldithiocarbamate, ferric dimethyldithiocarbamate, and tellurium diethyldithiocarbamate. Examples of guanidine compounds include 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, 1-o-tolylbiguanide, and di-o-tolylguanidine salt of dicatechol borate. Examples of xanthate compounds include zinc butylxanthate and zinc isopropylxanthate. Examples of benzimidazole compounds include compounds having a benzimidazole skeleton. Examples of the benzimidazole compounds include 2-mercaptobenzimidazole, 2-mercaptomethylbenzimidazole, and zinc salts of 2-mercaptomethylbenzimidazole.

[0058] A rubber composition according to one embodiment of the present invention preferably contains any one selected from thiourea compounds, 3-methyl-thiazolidine-2-thione, and thiadiazole compounds, and any one selected from thiuram compounds, thiazole compounds, and sulfenamide compounds, and it is more preferable that the total content of the thiourea compounds, 3-methyl-thiazolidine-2-thione, and thiadiazole compounds is within the above-mentioned numerical range, and that the total content of the thiuram compounds, thiazole compounds, and sulfenamide compounds is also within the above-mentioned numerical range.

[0059] 1.7 Metal Oxide The rubber composition according to one embodiment of the present invention may contain a metal oxide. The metal oxide can function as an acid acceptor and / or an acid acceptor. Examples of the metal oxide include zinc oxide, magnesium oxide, lead oxide, trimlead tetroxide, iron trioxide, titanium dioxide, and calcium oxide. The metal oxide preferably contains at least one of zinc oxide and magnesium oxide, and may contain zinc oxide and magnesium oxide.

[0060] The rubber composition according to one embodiment of the present invention may contain 0.1 to 15.0 parts by mass, and more preferably 0.5 to 10.0 parts by mass, of a metal oxide per 100 parts by mass of rubber contained in the rubber composition. The metal oxide content may be, for example, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0, 11.0, 12.0, 13.0, 14.0, or 15.0 parts by mass, or may be within a range between any two of the values ​​exemplified here.

[0061] A rubber composition according to one embodiment of the present invention may contain zinc oxide. Zinc oxide can function as an acid acceptor and / or an acid acceptor. The rubber composition according to one embodiment of the present invention may contain 0.1 to 10.0 parts by mass of zinc oxide, and more preferably 0.5 to 5.0 parts by mass, per 100 parts by mass of rubber contained in the rubber composition. The zinc oxide content may be, for example, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, or may be within a range between any two of the values ​​exemplified here.

[0062] The rubber composition according to one embodiment of the present invention may contain a metal oxide other than zinc oxide. The metal oxide other than zinc oxide can function as an acid acceptor. The rubber composition according to one embodiment of the present invention may contain 0.1 to 10.0 parts by mass, and more preferably 0.5 to 5.0 parts by mass, of the metal oxide other than zinc oxide per 100 parts by mass of rubber contained in the rubber composition. The content of the metal oxide other than zinc oxide is, for example, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, and may be within a range between any two of the values ​​exemplified here.

[0063] 1.8 Plasticizer The rubber composition according to one embodiment of the present invention may contain a plasticizer. The plasticizer is preferably compatible with chloroprene-based rubber and / or butyl-based rubber, and more preferably compatible with chloroprene-based rubber and butyl-based rubber. Examples of plasticizers include vegetable oils such as rapeseed oil, phthalate-based plasticizers, dioctyl sebacate (DOS), dibutyl sebacate (DBS), dioctyl adipate (DOA), ester-based plasticizers, ether-ester-based plasticizers, thioether-based plasticizers, aromatic oils, naphthenic oils, and paraffinic oils. These may be used alone or in combination of two or more.

[0064] A rubber composition according to one embodiment of the present invention may contain 0 to 50 parts by mass of a plasticizer relative to 100 parts by mass of rubber contained in the rubber composition. The amount of plasticizer may be, for example, 0, 5, 10, 15, 20, 25, 30, 35, 40, 45, or 50 parts by mass, or may be within a range between any two of the values ​​exemplified here.

[0065] The rubber composition according to one embodiment of the present invention preferably contains a compound A having at least one ester structure and a molecular weight of 300 to 1,000. Compound A can be used as a plasticizer. Compound A preferably contains DOS (dioctyl sebacate), DBS (dibutyl sebacate), DOA (bis(2-ethylhexyl) adipate), DOZ (bis(2-ethylhexyl) azelate), DINA (diisononyl adipate), DIDA (diisodecyl adipate), or DOP (bis(2-ethylhexyl) phthalate), and more preferably contains at least DOS (dioctyl sebacate). Compound A satisfying the above requirements has particularly excellent affinity with chloroprene-based rubber and butyl-based rubber, thereby further improving the properties of the resulting vulcanizate and vulcanized molded article. Compound A has at least one ester structure, and may have two or more. The molecular weight (weight average molecular weight) of compound A is 300 to 1000, and preferably 300 to 700. The molecular weight of compound A may be, for example, 300, 400, 500, 600, 700, 800, 900, or 1000, or may be within a range between any two of the numerical values ​​exemplified here.

[0066] A rubber composition according to one embodiment of the present invention may contain, per 100 parts by mass of rubber contained in the rubber composition, 1 to 30 parts by mass of compound A. The content of compound A may be, for example, 0, 5, 10, 15, 20, 25, or 30 parts by mass, or may be within a range between any two of the values ​​exemplified here.

[0067] 1.9 Filler The rubber composition according to one embodiment of the present invention may contain a filler. Examples of fillers include furnace carbon black such as SAF, ISAF, HAF, EPC, XCF, FEF, GPF, HMF, and SRF, modified carbon black such as hydrophilic carbon black, channel black, lamp black, thermal carbon such as FT and MT, acetylene black, ketjen black, silica, clay, talc, and calcium carbonate. The rubber composition according to one embodiment of the present invention may contain one or more fillers.

[0068] A rubber composition according to one embodiment of the present invention may contain a total of 20 to 90 parts by mass, preferably 35 to 80 parts by mass, of filler per 100 parts by mass of rubber contained in the rubber composition. The filler content may be, for example, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, or 90 parts by mass, or may be within a range between any two of the values ​​exemplified here. By containing the filler content within the above numerical range, the rubber composition according to one embodiment of the present invention can adjust the hardness of the vulcanizate and vulcanized molded article.

[0069] 1.10 Lubricants and Processing Aids The rubber composition according to the present invention may further contain a lubricant and / or a processing aid. Lubricants and processing aids are added primarily to improve processability, such as by making it easier for the rubber composition to be released from rolls, molding dies, extruder screws, etc. Examples of lubricants and processing aids include fatty acids such as stearic acid, paraffin-based processing aids such as polyethylene, fatty acid amides, petrolatum, and factice. The rubber composition according to one embodiment of the present invention may contain one or more types of lubricants and / or processing aids.

[0070] The rubber composition according to the present invention may contain a total of 0 to 15 parts by mass of lubricant and processing aid per 100 parts by mass of rubber contained in the rubber composition, and may also contain 1 to 10 parts by mass. The total content of lubricant and processing aid is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15 parts by mass, and may be within a range between any two of the values ​​exemplified here. The rubber composition according to the present invention may also be free of lubricant and / or processing aid.

[0071] 1.11 Others In addition to the above-mentioned components, the rubber composition according to the present invention may further contain components such as organic peroxides, silane coupling agents, co-crosslinking agents (e.g., maleimide-based compounds), stabilizers, flame retardants, and vulcanization retarders, as long as the effects of the present invention are not impaired. Examples of antioxidants and antioxidants include ozonants, phenolic antioxidants, amine-based antioxidants, acrylate-based antioxidants, waxes, and phosphorus-based antioxidants. Examples of amine-based antioxidants include 4,4'-bis(α,α-dimethylbenzyl)diphenylamine. The rubber composition according to the present invention may contain a total of 0.1 to 10 parts by mass of antioxidants and antioxidants per 100 parts by mass of rubber contained in the rubber composition.

[0072] 2. Method for Producing Rubber Composition A rubber composition according to one embodiment of the present invention can be obtained by kneading rubber and other necessary components at a temperature not higher than the vulcanization temperature. A method for producing a rubber composition according to one embodiment of the present invention can include a mixing step of mixing rubber and other necessary components at a temperature not higher than the vulcanization temperature. Examples of kneading devices include conventionally known kneading devices such as mixers, Banbury mixers, kneader mixers, and open rolls.

[0073] 3. Properties of Rubber Composition The rubber composition according to one embodiment of the present invention preferably has the following properties.

[0074] <Hardness of vulcanized molded article> In the rubber composition according to one embodiment of the present invention, the durometer hardness (Type A) of a vulcanized molded article of the rubber composition, as defined in JIS K 6253, can be 30 to 90, and preferably 40 to 80. The durometer hardness (Type A) of a vulcanized molded article of the rubber composition is, for example, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, or 90, and may be within a range between any two of the numerical values ​​exemplified here.

[0075] <Gas barrier properties of vulcanized molded article> The rubber composition according to one embodiment of the present invention preferably has an air permeability index, as defined in JIS K 6275-1:2022, of a vulcanized molded article of the rubber composition, of which the air permeability index is 160 or less, relative to an air permeability index of 100 for a vulcanized molded article of a rubber composition containing only butyl-based rubber as the rubber. The air permeability index, as defined in JIS K 6275-1:2022, of a vulcanized molded article of the rubber composition containing only butyl-based rubber as the rubber, relative to an air permeability index of 100, is, for example, 90, 100, 110, 120, 130, 140, 150, or 160, and may be within a range between any two of the values ​​exemplified here. <Heat resistance of vulcanized molded article> The rubber composition according to one embodiment of the present invention preferably has an elongation at break (EB), as measured in accordance with JIS K 6251, of a vulcanized molded article of the rubber composition. 0 The vulcanized molded body was heated at 150°C for 72 hours, and then the elongation at break (EB) was measured according to JIS K 6251. i The change in elongation at break, ΔEB, which is the difference between ΔEB and ΔEB, is preferably −65 to 0. ΔEB is, for example, −65, −60, −55, −50, −45, −40, −35, −30, −25, −20, −15, −10, −5, or 0, and may be within a range between any two of the numerical values ​​exemplified here.

[0076] <Oil Resistance of Vulcanized Molded Article> In the rubber composition according to one embodiment of the present invention, a vulcanized molded article of the rubber composition is immersed in a test oil (high-grade lubricating oil for automobiles, ASTM No. 3, IRM 903 oil) at 130°C for 72 hours, and the volume change rate ΔV before and after the immersion is preferably 0 to 340. The volume change rate ΔV is, for example, 0, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300, 310, 320, 330, or 340, and may be within a range between any two of the values ​​exemplified here.

[0077] <Flexural fatigue resistance of vulcanized molded article> The rubber composition according to one embodiment of the present invention preferably has a flexural fatigue test time of 1.5 million or more when a vulcanized molded article of the rubber composition is subjected to a de Mattia flexural fatigue test at room temperature under conditions of a stroke of 58 mm, a speed of 300±10 rpm, and according to JIS K 6260. The flexural fatigue test time when cracks occur is, for example, 1.5 million, 2 million, 2.5 million, 3 million, 3.5 million, 4 million, 4.5 million, 5 million, 5.5 million, 6 million, 6.5 million, 7 million, 7.5 million, 8 million, 8.5 million, 9 million, 9.5 million, or 10 million, and may be within a range between any two of the values ​​exemplified here.

[0078] <Dynamic Heat Buildup of Vulcanized Molded Article> When a constant strain flexometer test is carried out on a vulcanized molded article of the rubber composition according to JIS K 6265:2018 under conditions of 55°C, a strain of 0.175 inches, a load of 55 pounds, and a frequency of 1,800 vibrations per minute, the heat buildup measured is preferably 0 to 70°C. The heat buildup may be, for example, 0, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, or 70°C, and may be within a range between any two of the values ​​exemplified here.

[0079] The properties of the rubber composition can be values ​​obtained by forming a vulcanized molded product from the rubber composition under the conditions and by the method described in the Examples and measuring the properties by the method described in the Examples. The properties of the vulcanized molded product of the rubber composition can be controlled by adjusting the type and amount of the rubber composition. For example, the flex fatigue resistance of the vulcanized molded product can be adjusted by adjusting the amount of chloroprene-based rubber or the amount of unsaturated nitrile monomer units contained in the chloroprene-based rubber.

[0080] 4. Unvulcanized molded body, vulcanized product, and vulcanized molded body The unvulcanized molded body according to one embodiment of the present invention uses the rubber composition according to one embodiment of the present invention, and is a molded body (molded article) of the rubber composition (unvulcanized state) according to one embodiment of the present invention. A method for producing an unvulcanized molded body according to one embodiment of the present invention includes a step of molding the rubber composition (unvulcanized state) according to one embodiment of the present invention. The unvulcanized molded body according to one embodiment of the present invention is made of the rubber composition (unvulcanized state) according to one embodiment of the present invention.

[0081] A vulcanizate according to one embodiment of the present invention is a vulcanizate of the rubber composition according to one embodiment of the present invention. A method for producing a vulcanizate according to one embodiment of the present invention includes a step of vulcanizing the rubber composition according to one embodiment of the present invention.

[0082] A vulcanization molded article according to one embodiment of the present invention is a vulcanization molded article of a rubber composition according to one embodiment of the present invention. The vulcanization molded article according to one embodiment of the present invention uses a vulcanizate according to one embodiment of the present invention and is a molded article (molded product) of the vulcanizate according to one embodiment of the present invention. The vulcanization molded article according to one embodiment of the present invention is made of a vulcanizate according to one embodiment of the present invention.

[0083] The vulcanized molded article according to one embodiment of the present invention can be obtained by molding a vulcanizate obtained by vulcanizing the rubber composition (unvulcanized state) according to one embodiment of the present invention, and can also be obtained by vulcanizing a molded article obtained by molding the rubber composition (unvulcanized state) according to one embodiment of the present invention. The vulcanized molded article according to one embodiment of the present invention can be obtained by vulcanizing the rubber composition according to one embodiment of the present invention after molding or during molding. A method for producing a vulcanized molded article according to one embodiment of the present invention comprises a step of molding a vulcanized article according to one embodiment of the present invention, or a step of vulcanizing an unvulcanized molded article according to one embodiment of the present invention.

[0084] The vulcanized molded article according to one embodiment of the present invention preferably has the above-mentioned hardness, gas barrier properties, heat resistance, oil resistance, flex fatigue resistance, and / or dynamic heat buildup properties.

[0085] The unvulcanized molded article, vulcanized product, and vulcanized molded article according to this embodiment can be used as rubber parts in various industrial fields, such as buildings, structures, ships, railways, coal mines, and automobiles. They can be used for known applications, such as rubber parts for automobiles (e.g., automobile seals), hose materials, rubber molds, gaskets, rubber rolls, industrial cables, industrial conveyor belts, and sponges. The vulcanized product and vulcanized molded article according to this embodiment have excellent gas barrier properties, flex fatigue resistance, and heat resistance, and can therefore be used as various components in which these properties are particularly required. For example, the vulcanized product and vulcanized molded article according to one embodiment of the present invention can be suitably used as materials for tire innerliners, tubes, curing bladders, pharmaceutical rubber stoppers, electrical wire coatings, vibration-proofing materials, hoses, linings, capacitor packings, gaskets, and other applications requiring particularly excellent gas barrier properties, such as tire innerliners, tubes, and curing bladders.

[0086] (Automobile tire components, tire manufacturing components) Examples of automobile tire components and tire manufacturing components include tire innerliners, tubes, and curing bladders. A tire innerliner is a rubber sheet that replaces a tube and is attached to the inside of a tubeless tire. Attaching the innerliner prevents air leakage and maintains the tire's air pressure. A curing bladder is a jig used when molding a tire. During tire molding, a tire prototype is placed in a mold, and a bladder is inserted into the tire cavity. The bladder is inflated to press the tire against the mold, and the tire is molded and vulcanized by applying pressure and heat. The vulcanizate and vulcanized molded article obtained from the rubber composition according to the present invention have excellent gas barrier properties, flex fatigue resistance, and heat resistance. Therefore, it is possible to manufacture components such as tire innerliners, tubes, and curing bladders that are highly reliable and long-lasting and can withstand repeated deformation while maintaining the properties required for these applications, such as gas barrier properties and heat resistance.

[0087] (Automotive Rubber Components) Automotive rubber components include gaskets, oil seals, and packings, which are used in machinery and equipment to prevent leaks of liquids and gases and the intrusion of debris and foreign objects such as rainwater and dust. Specifically, there are gaskets used for fixed applications and oil seals and packings used for moving parts. Gaskets whose sealing parts are fixed with bolts or other fasteners are made of various materials depending on the purpose, as opposed to soft gaskets such as O-rings and rubber sheets. Packings are also used for rotating parts such as pump and motor shafts, moving parts of valves, reciprocating parts such as pistons, coupler connections, and water stop parts of water faucets. The rubber composition of the present invention can improve gas barrier properties, flex fatigue resistance, and heat resistance. This makes it possible to produce highly reliable, long-lasting automotive rubber components that can withstand repeated deformation while maintaining gas barrier properties and heat resistance, something that was difficult to achieve with conventional rubber compositions.

[0088] (Hose Material) A hose material is a flexible pipe, and specific examples include high- and low-pressure hoses for water supply, oil supply, air supply, steam supply, and hydraulic use. The rubber composition of the present invention can improve the gas barrier properties, flex fatigue resistance, and heat resistance of the hose material while maintaining the processability of the unvulcanized product. This makes it possible to produce, for example, a highly reliable, long-life hose material that can withstand repeated deformation while maintaining gas barrier properties and heat resistance, which was difficult to achieve with conventional rubber compositions.

[0089] (Rubber molded products) Examples of rubber molded products include vibration-isolating rubber, vibration-damping materials, and boots. Vibration-isolating rubber and vibration-damping materials are rubbers that prevent the transmission and spread of vibration. Specific examples include torsional dampers, engine mounts, and muffler hangers for automobiles and various other vehicles that absorb vibrations during engine operation to prevent noise. The rubber composition of the present invention can improve the gas barrier properties, flexural fatigue resistance, and heat resistance of vibration-isolating rubber and vibration-damping materials. This makes it possible to produce vibration-isolating rubber and vibration-damping materials that can be used for long periods of time even in harsh environments, something that was difficult to achieve with conventional rubber compositions. Boots are bellows-shaped components whose outer diameter gradually increases from one end to the other. Specific examples include boots for constant velocity joint covers, boots for ball joint covers (dust cover boots), and boots for rack and pinion gears that protect drive parts such as automotive drive systems. The rubber composition of the present invention can improve gas barrier properties, flexural fatigue resistance, and heat resistance. This makes it possible to produce boots that can be used for long periods of time even in harsh environments compared to conventional rubber compositions.

[0090] (Gaskets, etc.) Gaskets, oil seals, and packings are components in machines and equipment that prevent the leakage of liquids and gases and the intrusion of debris and foreign objects such as rainwater and dust into the interior. Specifically, there are gaskets used for fixed applications and oil seals and packings used for moving parts. Gaskets in which the sealing part is fixed with bolts or other fasteners are made of various materials depending on the purpose, as opposed to soft gaskets such as O-rings and rubber sheets. Packings are also used for rotating parts such as pump and motor shafts, moving parts of valves, reciprocating parts such as pistons, coupler connections, and water stop parts of water faucets. The rubber composition of the present invention can improve the gas barrier properties, flex fatigue resistance, and heat resistance of these components. This makes it possible to produce highly reliable, long-lasting seals that can withstand repeated deformation while maintaining gas barrier properties and heat resistance, something that was difficult to achieve with conventional rubber compositions.

[0091] (Rubber Roll) A rubber roll is manufactured by adhesively coating a metal core, such as an iron core, with rubber, and is generally manufactured by spirally winding a rubber sheet around a metal iron core. Rubber materials such as NBR, EPDM, and CR are used for rubber rolls depending on the required characteristics for various applications, such as papermaking, various metal manufacturing, film manufacturing, printing, general industrial use, agricultural machinery such as rice hullers, and food processing. CR has good mechanical strength that can withstand the friction of the objects being conveyed, and is therefore used in a wide range of rubber roll applications. Furthermore, rubber rolls that convey heavy objects have the problem of deformation under load, and improvements are needed. The rubber composition of the present invention can improve the gas barrier properties, flex fatigue resistance, and heat resistance of rubber rolls. This makes it possible to manufacture embossing rubber rolls that can be used for long periods of time even in harsh environments, something that has been difficult to achieve with conventional rubber compositions.

[0092] (Industrial Cable) Industrial cables are linear components for transmitting electricity or optical signals. They are made by coating a good conductor such as copper or a copper alloy, or an optical fiber, with an insulating coating layer, and a wide variety of industrial cables are manufactured depending on their structure and installation location. The rubber composition of the present invention can improve the gas barrier property, flex fatigue resistance, and heat resistance of industrial cables. This makes it possible to manufacture highly reliable, long-life industrial cables that can withstand repeated deformation while maintaining gas barrier property and heat resistance, which was difficult with conventional rubber compositions.

[0093] (Industrial Conveyor Belts) Industrial conveyor belts are available in rubber, resin, and metal, and are selected to suit a wide variety of uses. Among these, rubber conveyor belts are inexpensive and widely used, but when used in environments where there is a lot of friction and collision with the conveyed materials, they have been prone to damage due to deterioration. The rubber composition of the present invention can improve the gas barrier properties, flex fatigue resistance, and heat resistance of industrial conveyor belts. This makes it possible to produce industrial conveyor belts that can be used for long periods of time even in harsh environments, which has been difficult with conventional rubber compositions.

[0094] (Sponge) Sponges are porous materials with countless fine pores inside, and are specifically used in vibration-damping materials, sponge sealing parts, wetsuits, shoes, etc. The rubber composition of the present invention can improve the gas barrier properties, flex fatigue resistance, and heat resistance of the sponge. Furthermore, the use of chloroprene-based rubber can also improve the flame retardancy of the sponge. This makes it possible to produce sponges that can be used for long periods of time even in harsh environments, which was difficult with conventional rubber compositions, and sponges with excellent flame retardancy. Furthermore, the hardness of the resulting sponge can be appropriately adjusted by adjusting the content of the foaming agent, etc.

[0095] Methods for molding the rubber composition (unvulcanized state) and vulcanized product according to this embodiment include press molding, extrusion molding, calendar molding, etc. The temperature for vulcanizing the rubber composition may be appropriately set in accordance with the composition of the rubber composition, and may be 140 to 220°C or 160 to 190°C. The vulcanization time for vulcanizing the rubber composition may be appropriately set depending on the composition of the rubber composition, the shape of the unvulcanized molded product, etc.

[0096] The present invention will be described in more detail below based on examples, but the present invention should not be construed as being limited to these examples.

[0097] <Method for Producing Chloroprene Rubber (10% by Mass of Acrylonitrile (AN))> 24 parts by mass of chloroprene (monomer), 24 parts by mass of acrylonitrile (monomer), 0.5 parts by mass of diethylxanthogen disulfide, 200 parts by mass of pure water, 5.00 parts by mass of potassium rosinate (manufactured by Harima Chemicals Co., Ltd.), 0.40 parts by mass of sodium hydroxide, and 2.0 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (manufactured by Kao Corporation) were added to a 3 L polymerization vessel equipped with a heating / cooling jacket and a stirrer. Next, 0.1 parts by mass of potassium persulfate was added as a polymerization initiator, and emulsion polymerization was carried out in a nitrogen stream at a polymerization temperature of 40°C. The chloroprene was added in portions starting 20 seconds after the start of polymerization. The portion-by-portion addition flow rate was adjusted with a solenoid valve based on the change in the heat quantity of the refrigerant over the first 10 seconds of polymerization, and the flow rate was readjusted every 10 seconds thereafter, for continuous polymerization. When the polymerization rate relative to the total amount of chloroprene and acrylonitrile reached 50%, 0.02 parts by mass of phenothiazine as a polymerization terminator was added to terminate the polymerization. Thereafter, unreacted monomers in the reaction solution were removed under reduced pressure to obtain a chloroprene-based rubber latex containing a chloroprene-acrylonitrile copolymer.

[0098] The above-mentioned polymerization rate [%] of the chloroprene latex was calculated from the dry mass of the air-dried chloroprene latex. Specifically, it was calculated using the following formula (A). In the formula, "solid content concentration" refers to the concentration [% by mass] of the solid content obtained by heating 2 g of a sample of chloroprene latex at 130°C and removing volatile components such as the solvent (water), volatile chemicals, and raw materials. "Total charge amount" refers to the total amount [g] of raw materials, reagents, and solvent (water) charged into the polymerization vessel from the start of polymerization to a certain time. "Evaporation residue" refers to the mass [g] of chemicals and raw materials charged from the start of polymerization to a certain time that do not volatilize under conditions of 130°C and remain as solids together with the polymer. "Monomer charge amount" refers to the sum [g] of the amount of monomer initially charged into the polymerization vessel and the amount of monomer added in portions from the start of polymerization to a certain time. Note that "monomer" here refers to the total amount of chloroprene and acrylonitrile. Conversion rate = {[(total charge amount × solid content concentration / 100) - evaporation residue] / charge amount of monomer} × 100 (A)

[0099] The content of acrylonitrile monomer units contained in the chloroprene-based rubber was calculated from the content of nitrogen atoms in the chloroprene-acrylonitrile copolymer rubber. Specifically, the content of nitrogen atoms in 100 mg of chloroprene-based rubber A-2 was measured using an elemental analyzer (Sumigraph 220F, manufactured by Sumika Chemical Analysis Center, Ltd.), and the content of acrylonitrile monomer units was calculated.

[0100] The above elemental analysis was carried out as follows. The electric furnace temperatures were set to 900°C for the reactor, 600°C for the reduction furnace, 70°C for the column, and 100°C for the detector. Oxygen gas was flowed at 0.2 mL / min as the combustion gas, and helium gas was flowed at 80 mL / min as the carrier gas. A calibration curve was prepared using aspartic acid (10.52%), which has a known nitrogen content, as a standard substance. The chloroprene rubber obtained by the above production method had an acrylonitrile monomer unit content of 10.0% by mass (chloroprene rubber AN 10%).

[0101] <Method for producing chloroprene-based rubber> The amount of acrylonitrile monomer added in the polymerization step was changed to obtain chloroprene-based rubber AN 5%, in which the acrylonitrile monomer unit content in the chloroprene-based rubber was 5.0 mass%, and chloroprene-based rubber AN 20%, in which the acrylonitrile monomer unit content was 20.0 mass%.

[0102] <Preparation of Rubber Compositions> The components were mixed in the formulations shown in Tables 1 to 3 and kneaded with an 8-inch open roll to obtain rubber compositions of Examples and Comparative Examples.

[0103] The components used to obtain the rubber composition are as follows: (Chloroprene rubber) Acrylonitrile-containing chloroprene rubber: the above-mentioned chloroprene-acrylonitrile copolymer rubber (chloroprene rubber AN 5%, chloroprene rubber AN 10%, chloroprene rubber AN 20%) Unsaturated nitrile-free chloroprene rubber: "M-42" manufactured by Denka Co., Ltd.

[0104] (Butyl rubber) Halogenated butyl rubber CIIR1066: chlorinated butyl rubber, manufactured by ENEOS Material Corporation, CIIR1066, Cl 1.2 mass% BIIR2244: brominated butyl rubber, manufactured by ENEOS Material Corporation, BIIR2244, Br 2.0 mass% Non-halogenated butyl rubber RIIR268: regular butyl rubber, manufactured by ENEOS Material Corporation, RIIR 268, isoprene 1.7 mol%,

[0105] (Vulcanization accelerators) Thiourea compounds Accel 22S: ethylene thiourea manufactured by Kawaguchi Chemical Industry Co., Ltd. Noccela TMU: trimethylthiourea manufactured by Ouchi Shinko Chemical Industry Co., Ltd. 3-methyl-thiazolidine-2-thione: Rhenogran MTT-80 manufactured by Lanxess Thiazole compounds Noccela DM: di-2-benzothiazolyl disulfide manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Thiadiazole compounds MIXLAND+SD 75 GA F250: di(5-mercapto-1,3,4-thiadiazol-2-yl)disulfide manufactured by MLPC International Thiuram compounds Noccela TT: tetramethylthiuram disulfide manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Sulfenamide compounds Noccela CZ: N-cyclohexyl-2-benzothiazolylsulfenamide (vulcanizing agent), manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Sulfur: Fine sulfur 200 mesh (plasticizer), manufactured by Hosoi Chemical Industry Co., Ltd. DOS: Sanso Cizer DOS, di-2-ethylhexyl sebacate, molecular weight 427, manufactured by New Japan Chemical Co., Ltd.

[0106] Castor oil: No. 1 industrial castor oil, manufactured by Fukoku Oil Mills Co., Ltd.

[0107] (Filler) FEF: Carbon black, manufactured by Asahi Carbon Co., Ltd., Asahi #60UG

[0108] (Metal oxides) Kyowamag 150: Magnesium oxide manufactured by Kyowa Chemical Industry Co., Ltd. Zinc oxide type 2: Zinc oxide manufactured by Sakai Chemical Industry Co., Ltd.

[0109] (Lubricant) Stearic acid: Stearic acid 50S, manufactured by New Japan Chemical Co., Ltd.

[0110] (Anti-aging agent) Nocrac CD: 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.

[0111] <Hardness (Type A Durometer)> The obtained rubber composition was press-vulcanized at 170°C for 20 minutes in accordance with JIS K 6299 to produce a sheet-like vulcanized molded product having a thickness of 2 mm. The obtained sheet-like vulcanized molded product was measured for durometer hardness (Type A) as defined in JIS K 6253 using a GS-610 (manufactured by Teclock Corporation). The results are shown in Tables 1 to 3.

[0112] <Gas barrier properties> The obtained rubber composition was press-vulcanized at 170°C for 20 minutes in accordance with JIS K 6299 to produce a sheet-like vulcanized molded product having a thickness of 2 mm. The air permeability of the obtained sheet-like vulcanized molded product was measured at 25°C using an air permeability tester M-C1 (manufactured by Toyo Seiki Seisaku-sho, Ltd.). The air permeability (JIS K 6275-1:2022) was expressed as an index, with the air permeability of the vulcanized molded product of Comparative Example 4 set at 100. The smaller the index, the lower the air permeability and the better the gas barrier properties.

[0113] <Heat resistance (change in elongation at break after heating)> The obtained rubber composition was press-vulcanized at 170°C for 20 minutes in accordance with JIS K 6299 to produce a sheet-like vulcanized molded article having a thickness of 2 mm. The obtained sheet-like vulcanized molded article was molded into a dumbbell-shaped No. 3 test piece, and the elongation at break (EB) was measured in accordance with JIS K 6251. 0 Next, the vulcanized molded article was heated at 150°C for 72 hours, and then the elongation at break (EB) was measured again in accordance with JIS K 6251. i The change in elongation at break ΔEB before and after the heat resistance test was calculated from the elongation at break EB0 before heating and the elongation at break EBi after heating.

[0114] <Oil Resistance> The obtained rubber composition was press-vulcanized at 170°C for 20 minutes according to JIS K 6299 to produce a 2 mm thick sheet-like vulcanized molded product. A test piece measuring 25 mm in length and 20 mm in width was punched out from the sheet-like vulcanized molded product to obtain a test piece. The obtained test piece was immersed in a test oil (high-performance lubricating oil for automobiles, ASTM No. 3, IRM 903 oil) at 130°C for 72 hours. The volume change rate ΔV was calculated according to JIS K 6258.

[0115] <Flexural Fatigue Resistance> The obtained rubber composition was press-vulcanized at 170°C for 20 minutes to prepare a vulcanized molded article for a De Mattia flexural fatigue test. Using the obtained vulcanized molded article, a De Mattia flexural fatigue test was conducted based on JIS K 6260. The number of flexural tests (unit: 10,000 times) at which cracks occurred was measured under conditions of a stroke of 58 mm, a speed of 300±10 rpm, and room temperature, and flexural fatigue resistance was evaluated. Measurements were performed up to 5,000,000 times. The number of flexural tests at which cracks occurred was evaluated according to the following evaluation criteria.

[0116] <Dynamic Heat Buildup> The rubber composition was press-vulcanized at 170°C for 20 minutes to obtain a cylindrical vulcanized molded article having a diameter of 15 mm and a height of 25 mm. Heat buildup was evaluated by a constant strain flexometer test using a Goodrich Flexometer in accordance with JIS K 6265:2018. The constant strain flexometer test is a test method for evaluating fatigue properties due to heat buildup within a test specimen, such as vulcanized rubber, by applying a dynamic, repeated load. Specifically, a static initial load is applied to the test specimen under constant temperature conditions, and a constant amplitude sinusoidal vibration is then applied to measure the heat buildup and creep of the test specimen over time. The test was performed in accordance with JIS K 6265:2018 under conditions of 55°C, a strain of 0.175 inches, a load of 55 pounds, and a vibration frequency of 1,800 vibrations per minute, and heat buildup (°C) was measured.

[0117]

[0118]

[0119]

Claims

1. A rubber composition comprising a chloroprene-based rubber and a butyl-based rubber, the rubber composition containing 0.1 to 99 parts by mass of the chloroprene-based rubber per 100 parts by mass of rubber contained in the rubber composition, the chloroprene-based rubber containing an unsaturated nitrile monomer unit.

2. The rubber composition according to claim 1, wherein the rubber composition contains a thiourea compound, 3-methyl-thiazolidine-2-thione, and a thiadiazole compound in a total amount of 0.1 to 10.0 parts by mass per 100 parts by mass of rubber contained in the rubber composition.

3. The rubber composition according to claim 1 or 2, wherein the butyl-based rubber comprises a halogenated butyl rubber.

4. A rubber composition according to claim 1 or 2, wherein the rubber composition contains a thiuram compound, a thiazole compound, and a sulfenamide compound in a total amount of 0.1 to 10.0 parts by mass per 100 parts by mass of rubber contained in the rubber composition.

5. A rubber composition according to claim 1 or 2, wherein the chloroprene rubber contains 1 to 25 mass % of unsaturated nitrile monomer units relative to 100 mass % of the chloroprene rubber.

6. A rubber composition according to claim 1 or 2, wherein the rubber composition contains 1 to 30 parts by mass of compound A having at least one ester structure and having a molecular weight of 300 to 1,000 per 100 parts by mass of rubber contained in the rubber composition.

7. A vulcanizate of the rubber composition according to claim 1 or 2.

8. A vulcanized molded article made from the vulcanizate according to claim 7.

Citation Information

Patent Citations

  • Rubber composition for tire vulcanization bladder and tire vulcanization bladder using the same

    JP2016098294A

  • Rubber composition, vulcanizate, and molded article thereof

    JP2020015819A

  • Copolymer of chloroprene monomer and unsaturated nitrile compound, composition containing copolymer, vulcanization molded body of composition, and use of vulcanization molded body

    WO2020044899A1