Resin composition and carpet backing layer containing same

The resin composition, comprising polyvinyl chloride resin, fibers, and chlorinated polyolefin, addresses the issues of poor mechanical and low-temperature properties in recycled polyvinyl chloride resin, resulting in enhanced elongation and tear strength for carpet backing layers.

WO2024232230A1PCT designated stage expired Publication Date: 2024-11-14RESONAC CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015220
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-09
Filing Date
2024-04-17
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Recycled polyvinyl chloride resin compositions exhibit poor elongation at break, tear strength, and low-temperature properties, making them prone to cracking, especially when used in carpet backing layers.

Method used

A resin composition combining polyvinyl chloride resin, fibers, a plasticizer, and chlorinated polyolefin, with specific ratios and types of each component, is developed to enhance mechanical properties and maintain low-temperature performance.

Benefits of technology

The resin composition achieves excellent elongation at break and tear strength while maintaining low-temperature properties, reducing the likelihood of cracking and improving mechanical performance in carpet backing layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present disclosure relates to a resin composition containing: a resin material (X) which contains a thermoplastic resin (A) containing a polyvinyl chloride resin, fibers (B), and a plasticizer (C); and a chlorinated polyolefin (Y).
Need to check novelty before this filing date? Find Prior Art

Description

Resin composition and carpet backing layer containing same

[0001] FIELD OF THE DISCLOSURE The present disclosure relates to resin compositions and carpet backing layers comprising same.

[0002] Polyvinyl chloride resin is widely used due to its excellent chemical and mechanical stability, processability, and moldability. However, incineration of polyvinyl chloride resin is prone to generate hazardous substances. Furthermore, from the perspective of protecting the global environment, there is a strong demand for recycling used polyvinyl chloride resin. Against this background, various attempts have been made to recycle polyvinyl chloride resin. For example, Patent Document 1 discloses a method for producing a recycled and modified resin compound, in which composite thermoplastic resin waste is first pulverized to a particle size of 500 μm or less to obtain one or more recycled resin compounds, which are then granulated by stirring and mixing until the recycled resin compounds reach a semi-molten state.

[0003] WO 06 / 035820

[0004] Although the recycled modified resin compound produced by the manufacturing method described in Patent Document 1 has improved operational efficiency as a powder, compositions containing the recycled modified resin compound lack sufficient elongation at break, tear strength, low-temperature properties, etc., and are prone to breaking when bent and cracking in low-temperature environments. Furthermore, when fibers are mixed into the resin, for example, when recycling resins such as polyvinyl chloride resin from waste materials such as tile carpets, there is a problem that the elongation at break, tear strength, low-temperature properties, etc. are lower than those of the original resin due to the mixed fibers. Therefore, the present disclosure aims to provide a resin composition that has excellent elongation at break and tear strength and does not impair low-temperature properties.

[0005] As a result of extensive research to solve the above-mentioned problems, the present inventors have found that a resin composition containing a resin material (X) including a thermoplastic resin (A) containing a polyvinyl chloride resin, a fiber (B), and a plasticizer (C), and a chlorinated polyolefin (Y) has excellent elongation at break and tear strength, and does not impair low-temperature properties. Furthermore, the present inventors have found that a resin composition containing a thermoplastic resin (A) containing a polyvinyl chloride resin, a fiber (B), a plasticizer (C), and a chlorinated polyolefin (Y) has excellent elongation at break and tear strength, and does not impair low-temperature properties.

[0006] That is, the present invention relates to, for example, the following [1] to

[15] . [1] A resin composition comprising a resin material (X) including a thermoplastic resin (A) containing a polyvinyl chloride resin, a fiber (B), and a plasticizer (C), and a chlorinated polyolefin (Y). [2] The resin composition according to [1], which contains 1.0 part by mass or more and 80.0 parts by mass or less of the chlorinated polyolefin (Y) per 100 parts by mass of the resin material (X). [3] The resin composition according to [1] or [2], in which the fiber (B) is at least one selected from the group consisting of nylon fiber, polyester fiber, acrylic fiber, polypropylene fiber, glass fiber, and carbon fiber. [4] The resin composition according to any one of [1] to [3], which contains 0.1% by mass or more and 40.0% by mass or less of the fiber (B) per 100% by mass of the resin material (X). [5] The resin composition according to any one of [1] to [4], wherein the content of the plasticizer (C) in the resin material (X) is 20.0 parts by mass or more and 200.0 parts by mass or less per 100 parts by mass of the thermoplastic resin (A). [6] The resin composition according to any one of [1] to [5], wherein the resin material (X) further contains a filler which is at least one selected from the group consisting of calcium carbonate, talc, mica, clay, silicon dioxide, aluminum hydroxide, magnesium hydroxide, and carbon black. [7] The resin composition according to any one of [1] to [6], wherein the resin material (X) is a waste-derived material. [8] The resin composition according to any one of [1] to [7], wherein the chlorinated polyolefin (Y) is chlorinated polyethylene. [9] The resin composition according to any one of [1] to [8], wherein the melt flow rate of the chlorinated polyolefin (Y) at 180°C and 211.8 N is 150 g / 10 min or less.

[10] A carpet backing layer comprising the resin composition according to any one of [1] to [9].

[11] A resin composition comprising a thermoplastic resin (A) containing a polyvinyl chloride resin, a fiber (B), a plasticizer (C), and a chlorinated polyolefin (Y).

[12] The resin composition according to

[11] , wherein the chlorinated polyolefin (Y) is contained in the resin composition in an amount of 1.0 mass % or more and 45.0 mass % or less.

[13] The resin composition according to

[11] or

[12] , wherein the fiber (B) is at least one selected from the group consisting of nylon fiber, polyester fiber, acrylic fiber, polypropylene fiber, glass fiber, and carbon fiber.

[14] The resin composition according to any one of

[11] to

[13] , wherein the resin composition contains 0.01 mass% or more and 20.0 mass% or less of the fiber (B).

[15] The resin composition according to any one of

[11] to

[14] , wherein the resin composition contains 3.0 mass% or more and 80.0 mass% or less of a plasticizer (C).

[0007] According to the present disclosure, it is possible to provide a resin composition that is excellent in elongation at break and tear strength and does not impair low-temperature properties.

[0008] Fig. 1 is a photograph of the sheet produced in Example 4 observed under a microscope at a magnification of 70. Fig. 2 is a photograph of the sheet produced in Comparative Example 1 observed under a microscope at a magnification of 70.

[0009] Next, the present invention will be described in detail. A resin composition in one embodiment of the present invention comprises a resin material (X) containing a thermoplastic resin (A) containing a polyvinyl chloride resin, fibers (B), and a plasticizer (C), and a chlorinated polyolefin (Y). This resin composition is also referred to as a resin composition (Z-1). A resin composition in one embodiment of the present invention comprises a thermoplastic resin (A) containing a polyvinyl chloride resin, fibers (B), a plasticizer (C), and a chlorinated polyolefin (Y). This resin composition is also referred to as a resin composition (Z-2). Resin compositions (Z-1) and (Z-2) are collectively referred to as resin composition (Z).

[0010] <<Resin Material (X)>> The resin material (X) includes a thermoplastic resin (A) containing a polyvinyl chloride resin, fibers (B), and a plasticizer (C).

[0011] <Thermoplastic Resin (A)> The thermoplastic resin (A) includes a polyvinyl chloride resin. The polyvinyl chloride resin is a homopolymer or copolymer of vinyl chloride, and examples thereof include vinyl chloride homopolymer, vinyl chloride-vinyl acetate copolymer, vinyl chloride-ethylene copolymer, vinyl chloride-ethylene-vinyl acetate copolymer, and vinyl chloride graft copolymer obtained by graft polymerizing vinyl chloride onto an ethylene-propylene copolymer. The polyvinyl chloride resin can be used alone or in combination of two or more.

[0012] The thermoplastic resin other than the polyvinyl chloride resin contained in the thermoplastic resin (A) is not particularly limited, and examples thereof include polyethylene resin, ethylene-vinyl acetate resin copolymer, acrylic resin, etc. The other thermoplastic resins can be used singly or in combination of two or more.

[0013] The content of polyvinyl chloride resin contained in the thermoplastic resin (A) is not particularly limited, but the thermoplastic resin (A) preferably contains 50.0 mass % or more of polyvinyl chloride resin, more preferably 70.0 mass % or more, and even more preferably 100.0 mass % (i.e., the thermoplastic resin (A) consists solely of polyvinyl chloride resin).

[0014] In the resin composition (Z-1), the content of the thermoplastic resin (A) is preferably 5.0% by mass or more and 80.0% by mass or less, more preferably 10.0% by mass or more and 50.0% by mass or less, and even more preferably 15.0% by mass or more and 30.0% by mass or less, based on 100% by mass of the resin material (X). The resin composition (Z-1) contains the thermoplastic resin (A) preferably in an amount of 5.0 parts by mass or more and 80.0 parts by mass or less, more preferably 10.0 parts by mass or more and 50.0 parts by mass or less, and even more preferably 15.0 parts by mass or more and 30.0 parts by mass or less, relative to a total of 40 parts by mass of the thermoplastic resin (A) containing the polyvinyl chloride resin, the fiber (B), and the plasticizer (C).

[0015] <Fiber (B)> Fiber (B) is not particularly limited as long as it is a fiber that can be used with a polyvinyl chloride resin. Typically, it is a fiber that can exist as a fiber in the polyvinyl chloride resin and is incompatible with the polyvinyl chloride resin. Examples of such fibers include synthetic fibers such as nylon fibers including nylon 6 and / or nylon 66, polyester fibers, acrylic fibers, and polypropylene fibers; natural fibers such as hemp fibers, cotton fibers, and wool fibers; regenerated fibers such as cupra fibers, rayon fibers, and acetate fibers; and inorganic fibers such as glass fibers and carbon fibers. Fiber (B) can be used alone or in combination of two or more. Fiber (B) is preferably at least one selected from the group consisting of synthetic fibers, glass fibers, and carbon fibers, and more preferably at least one selected from the group consisting of nylon fibers, polyester fibers, acrylic fibers, polypropylene fibers, glass fibers, and carbon fibers.

[0016] The diameter and length of the fiber (B) are not particularly limited, but the length is preferably 100 times or more the diameter or width. The fiber (B) exists in the resin material (X) in a state where it is not mixed with the thermoplastic resin (A) and maintains the shape of the fiber. The fiber (B) also exists in the resin composition (Z) in a state where it is not mixed with the thermoplastic resin (A) and maintains the shape of the fiber.

[0017] When the resin material (X) is a waste-derived material, the fibers (B) are waste-derived fibers mixed into the thermoplastic resin (A). For example, when the resin material (X) is a material derived from tile carpet waste, the resin material (X) contains fibers derived from the tile carpet waste, particularly fibers derived from the surface pile layer and / or intermediate layer of the tile carpet. Tile carpets typically consist of a surface pile layer, at least one intermediate layer made of a nonwoven fabric, a woven fabric, and / or a reinforcing material, and a backing layer containing a thermoplastic resin (A) and a plasticizer (C). These layers are mechanically or chemically bonded together, and therefore, even if an attempt is made to separate only the backing layer from the tile carpet in order to recover the thermoplastic resin (A), it is inevitable that fibers derived from the surface pile layer and / or intermediate layer will be mixed into the thermoplastic resin (A). When the resin material (X) is a material derived from tile carpet waste, the fiber (B) is preferably at least one selected from the group consisting of nylon fiber and polypropylene fiber derived from the surface pile layer, and polyester fiber and glass fiber derived from the intermediate layer.

[0018] In the resin composition (Z-1), the content of the fiber (B) is preferably 0.1 to 40.0% by mass, more preferably 1.0 to 20.0% by mass, and even more preferably 2.0 to 7.0% by mass, based on 100% by mass of the resin material (X). The resin composition (Z-1) contains the fiber (B) in an amount of preferably 0.1 to 40.0 parts by mass, more preferably 1.0 to 20.0 parts by mass, and even more preferably 2.0 to 7.0 parts by mass, per 40 parts by mass of the thermoplastic resin (A) containing the polyvinyl chloride resin, the fiber (B), and the plasticizer (C). When the content of the fiber (B) is below the upper limit, the physical properties are easily improved sufficiently when the chlorinated polyolefin (Y) described below is added to the resin material (X), and the resulting resin composition (Z-1) is less likely to crack during use. When the content of the fiber (B) is equal to or greater than the lower limit, the effect of improving the mechanical properties when the chlorinated polyolefin (Y) is added to the resin material (X) tends to be large.

[0019] In the resin composition (Z-1), the content of the fiber (B) in the resin material (X) is preferably 10.0 parts by mass or more and 60.0 parts by mass or less, more preferably 20.0 parts by mass or more and 50.0 parts by mass or less, and even more preferably 30.0 parts by mass or more and 40.0 parts by mass or less, per 100 parts by mass of the thermoplastic resin (A). When the content of the fiber (B) is equal to or less than the upper limit, the physical properties are easily improved when the chlorinated polyolefin (Y) described below is added to the resin material (X), and cracks and the like are less likely to occur during use of the resulting resin composition (Z-1). When the content of the fiber (B) is equal to or more than the lower limit, the effect of improving the mechanical properties when the chlorinated polyolefin (Y) is added to the resin material (X) is easily increased.

[0020] <Plasticizer (C)> As the plasticizer (C), any plasticizer commonly used for polyvinyl chloride resins can be used without any particular limitation. Since the resin material (X) contains a polyvinyl chloride resin and a plasticizer (C), it is preferably a material that can be used as a soft polyvinyl chloride resin material.

[0021] Examples of the plasticizer (C) include phthalate ester-based plasticizers such as phthalate diesters such as dimethyl phthalate, diethyl phthalate, dibutyl phthalate, diheptyl phthalate, di-n-octyl phthalate, di-2-ethylhexyl phthalate (usually referred to as dioctyl phthalate, DOP), diisononyl phthalate (hereinafter also referred to as "DINP"), octyldecyl phthalate, diisodecyl phthalate, ditridecyl phthalate, butyl benzyl phthalate, and dicyclohexyl phthalate, and tetrahydrophthalate diesters such as di-n-octyl tetrahydrophthalate, di-2-ethylhexyl tetrahydrophthalate, and diisodecyl tetrahydrophthalate; aliphatic monobasic acid ester-based plasticizers such as butyl oleate and glycerin monooleate; aliphatic dibasic acid ester plasticizers such as dibutyl adipate, di-n-hexyl adipate, di-2-ethylhexyl adipate, diisononyl adipate, diisodecyl adipate, di-n-alkyl adipate, di(butoxyethoxyethyl) adipate diester, di-2-ethylhexyl azelate, di-n-hexyl azelate, dibutyl sebacate, and di-2-ethylhexyl sebacate; trimellitic acid ester plasticizers such as trialkyl trimellitates such as trioctyl trimellitate (hereinafter also referred to as "TOTM"), tris(2-ethylhexyl trimellitate), and trioctyl trimellitate; Examples of suitable plasticizers include polyester-based plasticizers such as propylene glycol adipate and 1,3-butylene glycol adipate, which are composed of polymers of dibasic acids such as adipic acid, zelaic acid, sebacic acid, and phthalic acid with glycols, glycerins, and monobasic acids; phosphate ester-based plasticizers such as triethyl phosphate, tributyl phosphate, tri-2-ethylhexyl phosphate, triphenyl phosphate, tricresyl phosphate, trichloroethyl phosphate, trisdichloropropyl phosphate, tributoxyethyl phosphate, tris(2-chloro-1-methylethyl) phosphate, octyldiphenyl phosphate, tris(isopropylphenyl phosphate), and cresyldiphenyl phosphate; and chlorinated paraffin-based plasticizers.Of these, the plasticizer (C) is preferably a phthalate ester plasticizer, more preferably di-2-ethylhexyl phthalate or diisononyl phthalate. The plasticizer (C) can be used alone or in combination of two or more.

[0022] The content of the plasticizer (C) is preferably 1.0% by mass or more and 40.0% by mass or less, more preferably 3.0% by mass or more and 30.0% by mass or less, and even more preferably 10.0% by mass or more and 20.0% by mass or less, based on 100% by mass of the resin material (X). The resin composition (Z-1) preferably contains 1.0 parts by mass or more and 40.0 parts by mass or less of the plasticizer (C), more preferably 3.0 parts by mass or more and 30.0 parts by mass or less, and even more preferably 10.0 parts by mass or more and 20.0 parts by mass or less, based on a total of 40 parts by mass of the thermoplastic resin (A) containing the polyvinyl chloride resin, the fiber (B), and the plasticizer (C). When the content of the plasticizer (C) is within the above range, the thermoplastic resin (A) is easily plasticized to an appropriate degree.

[0023] In the resin composition (Z-1), the content of the plasticizer (C) in the resin material (X) is preferably 20.0 parts by mass or more and 200.0 parts by mass or less, more preferably 40.0 parts by mass or more and 150.0 parts by mass or less, and even more preferably 50.0 parts by mass or more and 110.0 parts by mass or less, per 100 parts by mass of the thermoplastic resin (A). When the content of the plasticizer (C) is within the above range, the thermoplastic resin (A) is easily plasticized to an appropriate degree. Note that when the thermoplastic resin (A) is a polyvinyl chloride resin, a resin containing 20.0 parts by mass or more of the plasticizer (C) per 100 parts by mass of the thermoplastic resin (A) is generally referred to as a soft vinyl chloride resin.

[0024] <Other Components> In addition to the thermoplastic resin (A), the fiber (B), and the plasticizer (C), the resin material (X) may further contain other components such as a filler, a lubricant, a stabilizer for polyvinyl chloride resin, a pigment, a flame retardant, and an ultraviolet absorber.

[0025] Fillers are typically particulate substances and are blended to increase the amount of polyvinyl chloride resin and reduce costs. The filler is not particularly limited, and fillers commonly used in polyvinyl chloride resins can be used. In one embodiment of the present invention, the filler is a material different from the fiber (B). Examples of fillers include calcium carbonate, talc, mica, clay, silicon dioxide, aluminum hydroxide, magnesium hydroxide, and carbon black. These fillers can be used alone or in combination. The resin material (X) preferably further contains at least one filler selected from the group consisting of calcium carbonate, talc, mica, clay, silicon dioxide, aluminum hydroxide, magnesium hydroxide, and carbon black. The filler content is preferably 80.0% by mass or less, more preferably 60.0% by mass or less, based on 100% by mass of the resin material (X). The resin composition (Z-1) contains the filler in an amount of preferably 80.0 parts by mass or less, more preferably 60.0 parts by mass or less, relative to a total of 40 parts by mass of the thermoplastic resin (A) containing the polyvinyl chloride resin, the fiber (B), and the plasticizer (C).

[0026] Examples of the lubricant include fatty acid metal soap-based lubricants, ester compound-based lubricants, hydrocarbon-based lubricants, fatty acid-based lubricants, and higher alcohol-based lubricants.

[0027] Examples of the pigment include titanium oxide and organic pigments. Examples of the flame retardant include diantimony trioxide, halogen-based flame retardants, phosphorus-based flame retardants, and composite flame retardants. Examples of the ultraviolet absorber include benzotriazole-based ultraviolet absorbers.

[0028] The resin material (X) is not particularly limited as long as it contains a thermoplastic resin (A), fiber (B), and plasticizer (C). The resin material (X) can be used alone or in combination of two or more. The resin material (X) is preferably a material derived from waste. The waste may be a mixed resin waste containing a thermoplastic resin (A), fiber (B), plasticizer (C), and filler, or a laminate waste consisting of a layer of a mixed resin containing a thermoplastic resin (A), plasticizer (C), and filler and a layer of fiber. Examples of waste include the PVC (polyvinyl chloride resin) backing layer of tile carpets, long PVC floor sheets, multilayer vinyl floor tiles (PVC homogeneous style), PVC waterproof sheets for construction, the surface resin layer of PVC wallpaper, waterproof PVC sheets for civil engineering, PVC leather sheets for vehicle interiors, PVC covering materials for agriculture, and soundproof PVC sheets. The waste is preferably waste tile carpet that is disposed of, i.e., offcuts from tile carpet manufacturing or installation and used tile carpet from ordinary homes or offices, etc., and more preferably a backing layer containing polyvinyl chloride resin contained in the waste tile carpet.

[0029] The shape of the resin material (X) used as the raw material for resin composition (Z-1) is not particularly limited, but it is preferable that the resin material (X) be cut in advance by a known method, and the particle size after cutting is preferably 500 μm or less, more preferably 300 μm or less. By setting the particle size to 500 μm or less, it becomes easier to mix uniformly with chlorinated polyolefin during the production of resin composition (Z-1) described below. The particle size of resin material (X) is the 50% particle size (D50) in the volume-based cumulative particle size distribution measured using a laser diffraction / scattering particle size distribution analyzer (FRA, manufactured by Microtrac-Bell Co., Ltd.).

[0030] <<Chlorinated Polyolefin (Y)>> Chlorinated polyolefin (Y) is obtained by chlorinating a polyolefin. The type of polyolefin used as a raw material for the chlorinated polyolefin (Y) is not particularly limited, and examples include homopolymers of ethylene, homopolymers of α-olefins such as propylene, butene-1, pentene-1, hexene-1, octene-1, and 4-methylpentene-1, copolymers of ethylene and α-olefins, and copolymers of two or more types of α-olefins. The copolymers may be either random or block copolymers. These polyolefins may be used alone or in combination of two or more types. Among these, homopolymers of ethylene and copolymers of ethylene and propylene, i.e., polyethylene and ethylene-propylene copolymers, are preferred, with polyethylene being more preferred.

[0031] Here, an example of a physical property related to the molecular weight of the chlorinated polyolefin (Y) is the melt flow rate (MFR). The melt flow rate of the chlorinated polyolefin (Y) is preferably 150 g / 10 min or less, more preferably 0.01 g / 10 min to 150 g / 10 min, even more preferably 0.01 g / 10 min to 20 g / 10 min, and particularly preferably 0.01 g / 10 min to 10 g / 10 min. A melt flow rate of 20 g / 10 min or less of the chlorinated polyolefin (Y) is preferred because it is particularly excellent in cold resistance such as low-temperature impact brittleness temperature. On the other hand, in consideration of handleability such as moldability, the melt flow rate of the chlorinated polyolefin (Y) is preferably 0.01 g / 10 min or more. Usually, when a polyolefin having a high molecular weight and a low MFR is used as a raw material for the chlorinated polyolefin (Y), the MFR of the chlorinated polyolefin (Y) also becomes low. It is known that the larger the molecular weight of the chlorinated polyolefin (Y), the higher the filling property and cold resistance, and there is a tendency that various properties can be improved more significantly. The melt flow rate is a value measured in accordance with Method A of JIS K7210-1999 at a temperature of 180°C and a load of 211.8 N (21.6 kgf).

[0032] The chlorinated polyolefin (Y) can be obtained by chlorinating the polyolefin. The method for chlorinating the polyolefin is not particularly limited, and known methods can be used. Examples of known methods include an aqueous suspension method and a gas phase method, with the aqueous suspension method being preferred. Specifically, methods described in JP-A-54-124096 and JP-A-4-106109 can be used as the production method using the aqueous suspension method. Taking the production of chlorinated polyethylene from polyethylene as an example, an example of a method for producing chlorinated polyethylene using the aqueous suspension method includes a method in which chlorine is introduced into a suspension obtained by mixing polyethylene powder with water together with a surfactant and suspending the polyethylene powder in water, or into a solution obtained by dissolving polyethylene in a solvent, and the resulting mixture is chlorinated by heating or ultraviolet irradiation.

[0033] The chlorinated polyolefin (Y) is preferably a chlorinated polyethylene or a chlorinated ethylene-propylene copolymer, more preferably a chlorinated polyethylene, and even more preferably a chlorinated polyethylene produced using an aqueous suspension method.

[0034] Chlorinated polyethylene is characterized by being a rubbery elastomer with high fillability, cold resistance, and weather resistance. Fillability, also known as filler loading, refers to the ability of a resin to maintain tensile strength, elongation, toughness, impact strength, and the like even when it contains a high proportion of incompatible components. Resin material (X) contains a thermoplastic resin (A) containing polyvinyl chloride resin and a plasticizer (C), as well as fibers (B), and in some cases, a filler. As a result, resin material (X) tends to lose various physical properties, such as elongation at break, that are expected from a flexible polyvinyl chloride resin composition containing polyvinyl chloride resin and plasticizer (C). For these reasons, it is believed that adding chlorinated polyethylene with high fillability to resin material (X) can improve mechanical properties such as elongation at break and tear strength. In addition, the property of chlorinated polyethylene, which is a soft material similar to rubber, also contributes to improving the elongation at break of resin composition (Z-1). Elongation at break, tear strength, etc. are mechanical properties particularly necessary for the backing layer of a tile carpet, as they are less likely to break during installation, etc.

[0035] The chlorine content of the chlorinated polyolefin (Y) is preferably 5.0% by mass or more and 50.0% by mass or less, more preferably 20.0% by mass or more and 50.0% by mass or less, still more preferably 25.0% by mass or more and 45.0% by mass or less, and particularly preferably 30.0% by mass or more and 35.0% by mass or less. If the chlorine content of the chlorinated polyolefin (Y) is too small, the performance becomes similar to that of polyolefin, and if it is too large, the properties become similar to that of polyvinyl chloride. Therefore, when the chlorine content of the chlorinated polyolefin (Y) is within the above range, the above properties of the chlorinated polyolefin (Y) are easily exhibited.

[0036] The chlorinated polyolefin (Y) may be amorphous or crystalline. The chlorinated polyolefin (Y) is preferably amorphous because a resin composition (Z) having excellent low-temperature properties can be obtained. In the present invention, "amorphous" means that the heat of crystalline fusion measured by using a differential scanning calorimeter to raise the temperature of a measurement sample from room temperature at a heating rate of 10°C per minute is 2.0 J / g or less.

[0037] The specific gravity of the chlorinated polyolefin (Y) is preferably 1.05 or more and 1.30 or less. When the specific gravity of the chlorinated polyolefin (Y) is within the above range, a soft resin composition (Z) is likely to be obtained.

[0038] The content of the chlorinated polyolefin (Y) in the resin composition (Z-1) is preferably 1.0 part by mass or more and 80.0 parts by mass or less, more preferably 5.0 parts by mass or more and 40.0 parts by mass or less, even more preferably 10.0 parts by mass or more and 30.0 parts by mass or less, and particularly preferably 15.0 parts by mass or more and 30.0 parts by mass or less, per 100 parts by mass of the resin material (X). The resin composition (Z-1) preferably contains 1.0 part by mass or more and 80.0 parts by mass or less, more preferably 5.0 parts by mass or more and 40.0 parts by mass or less, even more preferably 10.0 parts by mass or more and 30.0 parts by mass or less, and particularly preferably 15.0 parts by mass or more and 30.0 parts by mass or less, of the chlorinated polyolefin (Y) per 40 parts by mass total of the thermoplastic resin (A) containing the polyvinyl chloride resin, the fiber (B), and the plasticizer (C). When the content of the chlorinated polyolefin (Y) is equal to or more than the lower limit, the effect of improving the properties of the resin material (X) is easily obtained. Furthermore, it is economically preferable if the content of the chlorinated polyolefin (Y) is equal to or less than the upper limit value.

[0039] The chlorinated polyolefin (Y) is preferably used in the form of powder or pellets so that it can be easily mixed uniformly with other components such as the resin material (X).

[0040] <<Resin Composition (Z-1)>> The method for producing the resin composition (Z-1) is not particularly limited, and the resin composition (Z-1) can be obtained by mixing the resin material (X) and the chlorinated polyolefin (Y). The mixing can be performed by a method commonly used for mixing resins, such as kneading using a mixing roll, a Banbury mixer, a kneader, an extrusion molding machine, or the like.

[0041] The resin composition (Z-1) may contain one or more third components consisting of components other than the resin material (X) and the chlorinated polyolefin (Y). For example, when the amount of plasticizer (C) in the resin material (X) is small and it is difficult to knead it with the chlorinated polyolefin (Y), the plasticizer (C) may be added as the third component. The resin composition (Z-1) may contain a stabilizer for chlorinated polyolefins as the third component to prevent deterioration of the chlorinated polyolefin (Y). Examples of stabilizers for chlorinated polyolefins include metal soaps, organotin compounds, inorganic acid salts, composite stabilizers, and hydrotalcite. The stabilizers for chlorinated polyolefins may be used alone or in combination of two or more. The amount of the stabilizer for chlorinated polyolefins added is preferably 1.0 part by mass or more to 20.0 parts by mass or less, more preferably 3.0 parts by mass or more to 15.0 parts by mass or less, per 100 parts by mass of the chlorinated polyolefin (Y).

[0042] The resin composition (Z-1) can be produced by mixing the components including the resin material (X) and the chlorinated polyolefin (Y) at 50°C or higher and 180°C or lower for about 1 minute or higher and 10 minutes or lower.

[0043] One embodiment of the present invention is a method for producing a resin composition (Z-1), which includes a step of mixing a resin material (X) with a chlorinated polyolefin (Y).

[0044] <<Resin Composition (Z-2)>> The thermoplastic resin (A), fiber (B), plasticizer (C), and chlorinated polyolefin (Y) in the resin composition (Z-2) are as described in the section for the resin composition (Z-1), except for the matters described below. In the resin composition (Z-2), the thermoplastic resin (A), fiber (B), and plasticizer (C) are preferably derived from waste, more preferably from tile carpet waste.

[0045] <Thermoplastic Resin (A)> When the thermoplastic resin (A) is derived from tile carpet waste, the thermoplastic resin (A) is preferably derived from a backing layer (lining layer).

[0046] In the resin composition (Z-2), the content of the thermoplastic resin (A) is preferably 5.0 parts by mass or more and 80.0 parts by mass or less, more preferably 10.0 parts by mass or more and 50.0 parts by mass or less, and even more preferably 15.0 parts by mass or more and 30.0 parts by mass or less, relative to a total of 40 parts by mass of the thermoplastic resin (A), the fiber (B), and the plasticizer (C).

[0047] In the resin composition (Z-2), the content of the thermoplastic resin (A) is preferably 2.0% by mass or more and 50.0% by mass or less, more preferably 5.0% by mass or more and 30.0% by mass or less, and even more preferably 10.0% by mass or more and 20.0% by mass or less, based on 100% by mass of the resin composition (Z-2).

[0048] <Fiber (B)> When the fiber (B) is derived from tile carpet waste, the fiber (B) is preferably at least one selected from the group consisting of nylon fiber, polypropylene fiber, polyester fiber derived from the intermediate layer, and glass fiber, and more preferably these fibers derived from the surface pile layer.

[0049] In the resin composition (Z-2), the content of the fiber (B) is preferably 0.1 parts by mass or more and 40.0 parts by mass or less, more preferably 1.0 parts by mass or more and 20.0 parts by mass or less, and even more preferably 2.0 parts by mass or more and 7.0 parts by mass or less, relative to 40 parts by mass of the total of the thermoplastic resin (A), the fiber (B), and the plasticizer (C). When the content of the fiber (B) is equal to or less than the upper limit, the physical properties are easily improved when the chlorinated polyolefin (Y) is added to the thermoplastic resin (A), the fiber (B), and the plasticizer (C), and cracks and the like are less likely to occur during use of the resulting resin composition (Z-2). When the content of the fiber (B) is equal to or more than the lower limit, the effect of improving the mechanical properties when the chlorinated polyolefin (Y) is added to the thermoplastic resin (A), the fiber (B), and the plasticizer (C) is easily increased.

[0050] In the resin composition (Z-2), the content of the fiber (B) is preferably 0.01% by mass or more and 20.0% by mass or less, more preferably 0.1% by mass or more and 15.0% by mass or less, and even more preferably 2.0% by mass or more and 10.0% by mass or less, based on 100% by mass of the resin composition (Z-2). When the content of the fiber (B) is equal to or less than the upper limit, the physical properties are easily improved when the chlorinated polyolefin (Y) is added to the thermoplastic resin (A), the fiber (B), and the plasticizer (C), and cracks and the like are less likely to occur during use of the resulting resin composition (Z-2). When the content of the fiber (B) is equal to or more than the lower limit, the effect of improving the mechanical properties when the chlorinated polyolefin (Y) is added to the thermoplastic resin (A), the fiber (B), and the plasticizer (C) is easily increased.

[0051] In the resin composition (Z-2), the content of the fiber (B) is preferably 10.0 parts by mass or more and 60.0 parts by mass or less, more preferably 20.0 parts by mass or more and 50.0 parts by mass or less, and even more preferably 30.0 parts by mass or more and 40.0 parts by mass or less, relative to 100 parts by mass of the thermoplastic resin (A). When the content of the fiber (B) is equal to or less than the upper limit, the physical properties are easily improved when the chlorinated polyolefin (Y) is added to the thermoplastic resin (A), the fiber (B), and the plasticizer (C), and cracks and the like are less likely to occur during use of the resulting resin composition (Z-2). When the content of the fiber (B) is equal to or more than the lower limit, the effect of improving the mechanical properties when the chlorinated polyolefin (Y) is added to the thermoplastic resin (A), the fiber (B), and the plasticizer (C) is easily increased.

[0052] <Plasticizer (C)> When the plasticizer (C) is derived from tile carpet waste, the plasticizer (C) is preferably derived from the backing layer (lining layer).

[0053] In the resin composition (Z-2), the content of the plasticizer (C) is preferably 20.0 parts by mass or more and 200.0 parts by mass or less, more preferably 40.0 parts by mass or more and 150.0 parts by mass or less, and even more preferably 50.0 parts by mass or more and 110.0 parts by mass or less, relative to a total of 40 parts by mass of the thermoplastic resin (A), the fiber (B), and the plasticizer (C). When the content of the plasticizer (C) is within the above range, the thermoplastic resin (A) is easily plasticized to an appropriate degree.

[0054] In the resin composition (Z-2), the content of the plasticizer (C) is preferably 3.0% by mass or more and 80.0% by mass or less, more preferably 8.0% by mass or more and 40.0% by mass or less, and even more preferably 10.0% by mass or more and 20.0% by mass or less, based on 100% by mass of the resin composition (Z-2). When the content of the plasticizer (C) is within the above range, the thermoplastic resin (A) is easily plasticized to an appropriate degree.

[0055] <Chlorinated Polyolefin (Y)> In the resin composition (Z-2), the content of the chlorinated polyolefin (Y) is preferably 1.0 part by mass or more and 80.0 parts by mass or less, more preferably 5.0 parts by mass or more and 40.0 parts by mass or less, even more preferably 10.0 parts by mass or more and 30.0 parts by mass or less, and particularly preferably 15.0 parts by mass or more and 30.0 parts by mass or less, relative to 40 parts by mass of the total of the thermoplastic resin (A), the fiber (B), and the plasticizer (C). When the content of the chlorinated polyolefin (Y) is equal to or more than the lower limit, the effect of improving the properties when the chlorinated polyolefin (Y) is added to the thermoplastic resin (A), the fiber (B), and the plasticizer (C) is easily obtained. Furthermore, it is economically preferable if the content of the chlorinated polyolefin (Y) is equal to or less than the upper limit.

[0056] In the resin composition (Z-2), the content of the chlorinated polyolefin (Y) is preferably 1.0 mass% or more and 45.0 mass% or less, more preferably 1.5 mass% or more and 40.0 mass% or less, even more preferably 4.0 mass% or more and 30.0 mass% or less, and particularly preferably 5.0 mass% or more and 15.0 mass% or less, based on 100 mass% of the resin composition (Z-2). When the content of the chlorinated polyolefin (Y) is equal to or more than the lower limit, the effect of improving the properties when the chlorinated polyolefin (Y) is added to the thermoplastic resin (A), the fiber (B), and the plasticizer (C) is easily obtained. Furthermore, it is economically preferable for the content of the chlorinated polyolefin (Y) to be equal to or less than the upper limit.

[0057] Chlorinated polyethylene is characterized by being a rubbery elastomer with high fillability, cold resistance, and weather resistance. Fillability, also known as filler loading, refers to the ability of a resin to maintain tensile strength, elongation, toughness, impact strength, and the like even when it contains a high proportion of incompatible components. Resin composition (Z-2) contains a thermoplastic resin (A) containing polyvinyl chloride resin and a plasticizer (C), as well as fibers (B), and in some cases, a filler. As a result, resin composition (Z-2) tends to lose various physical properties, such as elongation at break, that are expected from a flexible polyvinyl chloride resin composition containing polyvinyl chloride resin and plasticizer (C). For these reasons, it is believed that adding chlorinated polyethylene with high fillability can improve mechanical properties such as elongation at break and tear strength. In addition, the property of chlorinated polyethylene, which is a soft material similar to rubber, also contributes to improving the elongation at break of resin composition (Z-2). Elongation at break, tear strength, etc. are mechanical properties particularly necessary for the backing layer of a tile carpet, as they are less likely to break during installation, etc.

[0058] <Other Components> In addition to the thermoplastic resin (A), the fiber (B), the plasticizer (C), and the chlorinated polyolefin (Y), the resin composition (Z-2) may further contain other components such as a filler, a lubricant, a stabilizer for polyvinyl chloride resin, a pigment, a flame retardant, an ultraviolet absorber, and a stabilizer for chlorinated polyolefin.

[0059] Fillers are typically particulate substances that are blended to increase the amount of polyvinyl chloride resin and reduce costs. The filler is not particularly limited, and fillers commonly used in polyvinyl chloride resins can be used. In the present invention, the filler is a material different from the fiber (B). Examples of fillers include calcium carbonate, talc, mica, clay, silicon dioxide, aluminum hydroxide, magnesium hydroxide, and carbon black. Fillers can be used singly or in combination. Resin composition (Z-2) preferably further contains at least one filler selected from the group consisting of calcium carbonate, talc, mica, clay, silicon dioxide, aluminum hydroxide, magnesium hydroxide, and carbon black. The filler content is preferably 70.0% by mass or less, more preferably 60.0% by mass or less, based on 100% by mass of resin composition (Z-2).

[0060] Examples of the lubricant include fatty acid metal soap-based lubricants, ester compound-based lubricants, hydrocarbon-based lubricants, fatty acid-based lubricants, and higher alcohol-based lubricants.

[0061] Examples of the pigment include titanium oxide and organic pigments. Examples of the flame retardant include diantimony trioxide, halogen-based flame retardants, phosphorus-based flame retardants, and composite flame retardants. Examples of the ultraviolet absorber include benzotriazole-based ultraviolet absorbers.

[0062] Examples of stabilizers for chlorinated polyolefins include metal soaps, organotin compounds, inorganic acid salts, composite stabilizers, and hydrotalcite. The stabilizers for chlorinated polyolefins may be used alone or in combination of two or more. The amount of the stabilizer for chlorinated polyolefins added is preferably 1.0 part by mass or more and 20.0 parts by mass or less, more preferably 3.0 parts by mass or more and 15.0 parts by mass or less, per 100 parts by mass of the chlorinated polyolefin (Y).

[0063] The method for producing the resin composition (Z-2) is not particularly limited, and the resin composition (Z-2) can be obtained by mixing the thermoplastic resin (A), the fiber (B), the plasticizer (C), and the chlorinated polyolefin (Y), but is preferably obtained by adding the chlorinated polyolefin (Y) to a mixture of the thermoplastic resin (A), the fiber (B), and the plasticizer (C) and mixing them together. The mixing can be carried out by a method commonly used for mixing resins, such as kneading using a mixing roll, a Banbury mixer, a kneader, an extrusion molding machine, or the like.

[0064] The conditions for producing the resin composition (Z-2) can be appropriately set in consideration of the properties of each component such as the thermoplastic resin (A), the fiber (B), the plasticizer (C), and the chlorinated polyolefin (Y). The resin composition (Z-2) can be produced by mixing each component including the thermoplastic resin (A), the fiber (B), the plasticizer (C), and the chlorinated polyolefin (Y) at 50°C or higher and 180°C or lower for about 1 minute or higher and 10 minutes or lower.

[0065] One embodiment of the present invention is a method for producing a resin composition (Z-2), comprising the step of mixing a thermoplastic resin (A), a fiber (B), a plasticizer (C), and a chlorinated polyolefin (Y).

[0066] <<Uses of Resin Composition (Z)>> The uses of the resin composition (Z) are not particularly limited, but the resin composition (Z) has excellent elongation at break, tear strength, and low-temperature properties, is resistant to cracking when bent, and is resistant to cracking even when used or installed in low-temperature environments. Therefore, it is preferably used as a carpet backing layer such as a PVC backing layer of a carpet tile, a long PVC floor sheet, a PVC homogeneous style, a PVC waterproof sheet for construction, a surface resin layer of PVC wallpaper, a waterproof PVC sheet for civil engineering, a PVC leather sheet for vehicle interiors, a PVC covering material for agriculture, and a sound-insulating PVC sheet. More preferably, the resin composition (Z) is used as a carpet backing layer. When the resin composition (Z-1) is used for these purposes, if the resin material (X) is a waste-derived material, a product made from recycled polyvinyl chloride resin can be obtained. When the resin composition (Z-2) is used for these applications, if the thermoplastic resin (A), the fiber (B), and the plasticizer (C) are derived from waste, a product made from recycled polyvinyl chloride resin can be obtained.

[0067] Another embodiment of the present invention is a carpet backing layer such as a PVC backing layer of a carpet tile, a long PVC floor sheet, a PVC homogeneous style, a PVC waterproof sheet for construction, a surface resin layer of PVC wallpaper, a waterproof PVC sheet for civil engineering, a PVC leather sheet for vehicle interiors, a PVC covering material for agricultural use, and a soundproof PVC sheet, which contains the resin composition (Z), and preferably a carpet backing layer containing the resin composition (Z).

[0068] The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to these examples in any way. [Methods for measuring various physical properties] <Chlorine content> The chlorine content was measured by the following method. A sample was heated and burned in a glass tube with the flame of a gas burner to remove hydrochloric acid and decompose, and the generated hydrochloric acid gas was absorbed in distilled water and quantified by neutralization titration with a 0.1 mol / l normal solution of caustic soda.

[0069] <MFR (Melt Flow Rate)> MFR was measured in accordance with JIS K7210-1999, Method A. The measurement conditions were a temperature of 180°C and a load of 211.8 N (21.6 kgf).

[0070] <Specific Gravity> Specific gravity was measured in accordance with JIS K7112-1-2023, Method A. The temperature of the immersion liquid was 23°C.

[0071] <Tensile Properties> Tensile properties were measured in accordance with JIS K6251-2017. However, the measurement was performed at a gripping speed of 200 mm / min. Specifically, a dumbbell-shaped No. 3 test piece described in JIS K6251-2017 was prepared by punching out a sheet-like sample to be measured. Analysis was performed using this test piece at a measurement temperature of 23°C and a humidity of 50% RH to measure the tensile stress at yield point (Sy), tensile strength at break (Tb), and elongation at break (Eb).

[0072] <Tear Strength> The tear strength was measured in accordance with the method using an unnotched angle-shaped test piece in Test Method B-Procedure (a) of JIS K6252-1-2015.

[0073] <Low-temperature impact embrittlement temperature> The low-temperature impact embrittlement temperature was measured in accordance with JIS K6261-2-2017 as a 50% impact embrittlement temperature (method B), with the temperature being measured at 5°C intervals.

[0074] <Hardness> The hardness was measured at 23°C using a Type D durometer in accordance with JIS K7215-1986. Here, as samples used for the measurement, four sheets with a thickness of 2 mm and a smooth surface were used, and the flat portions were stacked to form a thickness of approximately 8 mm.

[0075] [Example 1] Polyvinyl chloride resin, plasticizer, and fiber-containing resin material (XI) (manufactured by Refineverse Co., Ltd., IVP-1108) 100 parts by mass, chlorinated polyethylene as a chlorinated polyolefin (manufactured by Resonac Co., Ltd., Eraslen (registered trademark) 301MA) 5 parts by mass, and a hydrotalcite compound as a stabilizer (manufactured by Sakai Chemical Industry Co., Ltd., STABIACE (registered trademark) HT-P) 1 part by mass was hand-blended at room temperature, and then the mixing roll temperature was set to 150 ° C. and kneaded with a mixing roll for 3 minutes, and a sheet of about 2.5 mm thick was produced by sheeting out a resin composition (recycled (recycled) resin composition). Then, this resin composition was preheated at 170 ° C. for 3 minutes in a compression molding machine, pressurized for 3 minutes, cooled and pressurized for 3 minutes, and a smooth 2.0 mm thick sheet was produced.

[0076] IVP-1108 is a powdery material derived from the backing layer of discarded tile carpet. The composition of IVP-1108 was 18.1% by mass of polyvinyl chloride resin, 6.6% by mass of fiber, 16.5% by mass of di-2-ethylhexyl phthalate as a plasticizer, and 58.8% by mass of calcium carbonate as a filler.

[0077] Examples 2 to 14 and Comparative Examples 1 and 2 were carried out in the same manner as Example 1, except that the types and amounts of stabilizer and chlorinated polyolefin, and the mixing of the mixing roll during mixing were changed to the amounts shown in Table 1 below. Here, the various Elaslen (registered trademark) products shown in Table 1 below are chlorinated polyethylenes manufactured by Resonac Corporation.

[0078]

[0079] The physical properties of the chlorinated polyethylene used in each example are shown in Table 2. Here, the "chlorine content," "MFR," and "specific gravity" shown in Table 2 below are values ​​measured by the method described in the above "Methods for measuring various physical properties," respectively.

[0080]

[0081] The evaluation results for the sheets obtained in each of the Examples and Comparative Examples are summarized in Table 3. Here, the values ​​shown in the items "specific gravity," "tensile properties," "tear strength," "impact embrittlement temperature," and "hardness" in Table 3 below are values ​​measured by the methods described above in the "methods for measuring various physical properties" for "specific gravity," "tensile properties," "tear strength," "low-temperature impact embrittlement temperature," and "hardness," respectively.

[0082]

[0083] As shown in Table 3, in Examples 1 to 14, in which a chlorinated polyolefin having the specified physical properties was mixed with a resin material containing polyvinyl chloride resin as a thermoplastic resin, fibers, and a plasticizer, the elongation at break (Eb) and tear strength were significantly improved and the impact embrittlement temperature was not impaired, compared to the cases in which no chlorinated polyolefin was contained as in Comparative Examples 1 and 2, and a resin composition with performance suitable for the backing layer of a tile carpet was obtained. Examples 1 to 14 also had values ​​for tensile stress at yield point (Sy), tensile strength at break (Tb), and hardness that were sufficient for practical use.

[0084] The surfaces of the sheets produced in Example 4 and Comparative Example 1 were observed at 70x magnification using a digital microscope (Dino-Lite Edge EDR / EDOF Polarizer (polarized)), and the results are shown in Figures 1 and 2, respectively. In Figure 2, fibers of various colors are lined up with their long axes oriented from the upper right to the lower left of the photograph, confirming orientation by the mixing roll. On the other hand, in Figure 1, the long axes of the fibers are random, and no orientation by the mixing roll is observed, confirming that the fibers and calcium carbonate are dispersed in the mixture of the resin material and chlorinated polyolefin in a state where they are not compatible with the mixture but are highly uniform.

Claims

1. A resin composition comprising a resin material (X) containing a thermoplastic resin (A) including a polyvinyl chloride resin, fibers (B), and a plasticizer (C), and a chlorinated polyolefin (Y).

2. The resin composition according to claim 1, comprising 1.0 part by mass or more and 80.0 parts by mass or less of the chlorinated polyolefin (Y) per 100 parts by mass of the resin material (X).

3. The resin composition according to claim 1, wherein the fiber (B) is at least one selected from the group consisting of nylon fiber, polyester fiber, acrylic fiber, polypropylene fiber, glass fiber, and carbon fiber.

4. The resin composition according to claim 1, comprising 0.1 mass % or more and 40.0 mass % or less of the fiber (B) per 100 mass % of the resin material (X).

5. The resin composition according to claim 1, wherein the content of the plasticizer (C) in the resin material (X) is 20.0 parts by mass or more and 200.0 parts by mass or less per 100 parts by mass of the thermoplastic resin (A).

6. The resin composition according to claim 1, wherein the resin material (X) further comprises at least one filler selected from the group consisting of calcium carbonate, talc, mica, clay, silicon dioxide, aluminum hydroxide, magnesium hydroxide, and carbon black.

7. The resin composition according to claim 1, wherein the resin material (X) is a material derived from waste.

8. The resin composition according to claim 1, wherein the chlorinated polyolefin (Y) is a chlorinated polyethylene.

9. The resin composition according to claim 1, wherein the melt flow rate of the chlorinated polyolefin (Y) at 180° C. and 211.8 N is 150 g / 10 min or less.

10. A carpet backing layer comprising the resin composition according to any one of claims 1 to 9.

11. A resin composition comprising a thermoplastic resin (A) containing a polyvinyl chloride resin, a fiber (B), a plasticizer (C), and a chlorinated polyolefin (Y).

12. The resin composition according to claim 11, wherein the resin composition contains 1.0 mass % or more and 45.0 mass % or less of the chlorinated polyolefin (Y).

13. The resin composition according to claim 11 or 12, wherein the fiber (B) is at least one selected from the group consisting of nylon fiber, polyester fiber, acrylic fiber, polypropylene fiber, glass fiber, and carbon fiber.

14. A resin composition according to claim 11 or 12, wherein the resin composition contains 0.01 mass % or more and 20.0 mass % or less of the fiber (B).

15. A resin composition according to claim 11 or 12, comprising 3.0 mass % or more and 80.0 mass % or less of a plasticizer (C) in the resin composition.

Citation Information

Patent Citations

  • Environmentally-friendly wood fiber reinforced PVC composite template and production method thereof

    CN105001657A

  • Novel building organic composite board and production process thereof

    CN113881160A

  • Preparation method of antistatic modified regenerated plastic particles

    CN114456479A

  • Flame-retardant resin composition

    JP1984068359A

  • Vinyl chloride resin composition

    JP1985177054A