Synthetic leather and method for producing synthetic leather
The synthetic leather composition, featuring a urethane resin with specific polyol and aromatic polyisocyanate compounds, addresses the issues of short pot life and inadequate peel strength and light resistance in existing adhesives, resulting in a product with improved processing capabilities and performance.
Patent Information
- Application Number
- PCT/JP2024/016183
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-11
- Filing Date
- 2024-04-25
- Publication Date
- 2024-11-14
AI Technical Summary
Existing synthetic leather adhesives with water-based polyurethane resin compositions have a short pot life and inadequate peel strength and light resistance, making them difficult to process effectively.
A synthetic leather composition comprising an adhesive layer formed from a mixture of a specific water-based urethane resin composition, including a urethane resin with a polyol compound and an aromatic polyisocyanate compound, and an aqueous medium, with a urea bond concentration of 100 mmol/kg or less, and a weight average molecular weight of 100,000 or more, which enhances pot life, peel strength, and light resistance.
The synthetic leather exhibits a longer pot life, improved peel strength, and enhanced light resistance, making it suitable for use in adhesive layers and coating applications.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Synthetic leather and manufacturing method thereof
[0001] The present invention relates to a synthetic leather and a method for producing the synthetic leather.
[0002] Because aqueous urethane resin compositions can reduce volatile organic compounds compared to conventional solvent-based urethane resin compositions, in recent years they have been considered for use as environmentally friendly materials in a variety of applications, such as artificial leather, synthetic leather, coating agents, glove coatings and membranes, and adhesives.
[0003] Among these, for use in adhesive layers of synthetic leather, an aqueous polyurethane resin-based adhesive containing an aqueous polyurethane resin (PUD) having a softening temperature of 50°C or less and a melt viscosity at 50°C of 60,000 Pa·s or less, and a polyisocyanate compound, is known (see, for example, Patent Document 1). However, two-component adhesives that combine a PUD base with an isocyanate crosslinking agent have the problem that the usable time (pot life) of the blended liquid is short, making it difficult to process stably.
[0004] Therefore, there has been a demand for a material that has a long pot life, excellent peel strength and light resistance.
[0005] Japanese Patent Application Laid-Open No. 2000-108289
[0006] The problem to be solved by the present invention is to provide a synthetic leather having an adhesive layer that has a long pot life and is excellent in peel strength and light resistance, and a method for producing said synthetic leather.
[0007] As a result of intensive research to solve the above problems, the inventors discovered that the above problems can be solved by using a mixture of specific aqueous urethane resin compositions as an adhesive layer-forming material, and thus completed the present invention.
[0008] That is, the present invention relates to a synthetic leather having at least a base fabric (i), an adhesive layer (ii), and a surface layer (iii), wherein the adhesive layer (ii) is formed from a mixture containing an aqueous urethane resin composition (A) and an aqueous urethane resin composition (B) other than the aqueous resin composition (A), the aqueous urethane resin composition (A) contains a urethane resin (a1), an aqueous medium (a2), and an emulsifier (a3), the urethane resin (a1) comprises, as essential raw materials, a polyol compound (a1-1) containing a nonionic polyol and an aromatic polyisocyanate compound (a1-2), the urea bond concentration in the urethane resin (a1) is 100 mmol / kg or less, and the weight-average molecular weight of the aqueous urethane resin composition (B) is 100,000 or more.
[0009] The synthetic leather of the present invention has an adhesive layer that has a long pot life and excellent peel strength and light resistance, and therefore can be used as a coating agent or adhesive, and is particularly suitable for use in the adhesive layer of synthetic leather.
[0010] The synthetic leather of the present invention is characterized by having at least a base fabric (i), an adhesive layer (ii), and a surface layer (iii).
[0011] The synthetic leather of the present invention may have, for example, the following configurations (1) to (4).
[0012] Synthetic leather (1): Base fabric (i), adhesive layer (ii), skin layer (iii) Synthetic leather (2): Base fabric (i), adhesive layer (ii), intermediate layer, skin layer (iii) Synthetic leather (3): Base fabric (i), porous layer, adhesive layer (ii), skin layer (iii) Synthetic leather (4): base fabric (i), porous layer, adhesive layer (ii), intermediate layer, skin layer (iii)
[0013] Examples of the base fabric (i) include nonwoven fabrics, woven fabrics, knitted fabrics, and the like made from polyester fibers, polyethylene fibers, nylon fibers, acrylic fibers, polyurethane fibers, acetate fibers, rayon fibers, polylactic acid fibers, cotton, hemp, silk, wool, glass fibers, carbon fibers, and blends thereof.
[0014] The adhesive layer (ii) is formed from a mixture containing the aqueous urethane resin composition (A) and an aqueous urethane resin composition (B) other than the aqueous resin composition (A).
[0015] The aqueous urethane resin composition (A) contains a urethane resin (a1), an aqueous medium (a2), and an emulsifier (a3).
[0016] The urethane resin (a1) is made from a polyol compound (a1-1) containing a nonionic polyol and an aromatic polyisocyanate compound (a1-2) as essential raw materials.
[0017] Examples of the nonionic polyol include compounds having an oxyethylene structure. These nonionic polyols can be used alone or in combination of two or more. Among these, compounds having an oxyethylene structure are preferred because they can provide synthetic leather having an adhesive layer with a long pot life and excellent peel strength and light resistance.
[0018] Examples of the compound having an oxyethylene structure include polyether polyols having an oxyethylene structure, such as polyethylene glycol, polyoxyethylene polyoxypropylene glycol, polyoxyethylene polyoxytetramethylene glycol, and polyethylene glycol dimethyl ether. These compounds having an oxyethylene structure can be used alone or in combination of two or more. Among these, polyethylene glycol and polyethylene glycol dimethyl ether are preferred because they provide synthetic leather having an adhesive layer with a long pot life and excellent peel strength and light resistance.
[0019] The number-average molecular weight of the nonionic polyol is preferably in the range of 200 to 10,000, more preferably in the range of 300 to 3,000, and even more preferably in the range of 300 to 2,000, since this allows for a synthetic leather having a long pot life and an adhesive layer that is excellent in peel strength and light resistance. In the present invention, the number-average molecular weight is a value measured by gel permeation column chromatography (GPC).
[0020] The proportion of the nonionic polyol used in the polyol compound (a1-1) is preferably in the range of 1 to 30% by mass, more preferably 2 to 10% by mass, because this allows for the production of a synthetic leather having an adhesive layer that has a long pot life and is excellent in peel strength and light resistance.
[0021] Furthermore, as the polyol compound (a1-1), polyols other than the nonionic polyols (hereinafter abbreviated as "other polyol compounds") can also be used, if necessary.
[0022] Examples of the other polyol compounds include polyether polyols, polyester polyols, polyacrylic polyols, polycarbonate polyols, polybutadiene polyols, etc., other than the nonionic polyols. These other polyol compounds can be used alone or in combination of two or more. Among these, polyether polyols, polyester polyols, and polycarbonate polyols are preferred because they can provide synthetic leather having an adhesive layer with a long pot life and excellent peel strength and light resistance.
[0023] The amount of the polyol compound (a1-1) used in the raw materials for the urethane resin (a1) is preferably in the range of 40 to 90% by mass, more preferably 50 to 80% by mass, in order to obtain a synthetic leather having a long pot life and an adhesive layer that is excellent in peel strength and light resistance.
[0024] Examples of the aromatic polyisocyanate compound (a1-2) include phenylene diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate, naphthalene diisocyanate, polymethylene polyphenyl polyisocyanate, and carbodiimidized diphenylmethane polyisocyanate. These aromatic polyisocyanate compounds can be used alone or in combination of two or more. Among these, toluene diisocyanate is preferred because it allows the production of synthetic leather having an adhesive layer that has a long pot life and excellent peel strength and light resistance.
[0025] The amount of the aromatic polyisocyanate compound (a1-2) used in the raw material of the urethane resin (a1) is preferably in the range of 5 to 60% by mass, more preferably 10 to 50% by mass, in order to obtain a synthetic leather having a long pot life and an adhesive layer that is excellent in peel strength and light resistance.
[0026] If necessary, polyisocyanate compounds other than the aromatic polyisocyanate compound (a1-2) (hereinafter abbreviated as "other polyisocyanate compounds") can also be used in combination.
[0027] Examples of the other polyisocyanate compounds include aliphatic polyisocyanates such as hexamethylene diisocyanate, lysine diisocyanate, cyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, xylylene diisocyanate, tetramethylxylylene diisocyanate, dimer acid diisocyanate, and norbornene diisocyanate; and alicyclic diisocyanates such as norbornane diisocyanate, isophorone diisocyanate, hydrogenated xylylene diisocyanate, and hydrogenated diphenylmethane diisocyanate. These other polyisocyanate compounds can be used alone or in combination of two or more.
[0028] The amount of the other polyisocyanate compounds used is preferably in the range of 0.1 to 30% by mass, more preferably 1 to 20% by mass, in the raw material of the urethane resin (a1).
[0029] The urea bond concentration of the urethane resin (a1) is 100 mmol / kg or less, and is preferably 50 mmol / kg or less, more preferably 30 mmol / kg or less, and particularly preferably 0 mmol / kg, because this allows for the production of a synthetic leather having an adhesive layer that has a long pot life and is excellent in peel strength and light resistance.
[0030] The average particle size of the urethane resin (a1) is preferably in the range of 0.01 to 1 μm, more preferably in the range of 0.05 to 0.9 μm, since this allows for the production of synthetic leather having an adhesive layer that has a long pot life and is excellent in peel strength and light resistance.
[0031] In addition to the polyol compound (a1-1) and the aromatic polyisocyanate compound (a1-2), a chain extender not having an amino group may be used as the urethane resin (a1), if necessary. In particular, it is preferable to use a chain extender having a hydroxyl group, since this allows the production of synthetic leather having an adhesive layer that has a long pot life and excellent peel strength and light resistance.
[0032] Examples of the chain extender having a hydroxyl group include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, hexamethylene glycol, sucrose, methylene glycol, glycerin, sorbitol, bisphenol A, 4,4'-dihydroxydiphenyl, 4,4'-dihydroxydiphenyl ether, and trimethylolpropane. These chain extenders can be used alone or in combination of two or more. Among these, it is preferable to use an aliphatic polyol compound because discoloration can be easily suppressed and even better light resistance can be obtained.
[0033] The method for producing the urethane resin (a1) is not particularly limited, and any method may be used. For example, the urethane resin (a1) may be produced by reacting all of the reaction raw materials containing the polyol compound (a1-1) and the aromatic polyisocyanate compound (a1-2) at once, or by reacting the reaction raw materials sequentially. These reactions are preferably carried out at a temperature of 50 to 100°C for 3 to 10 hours.
[0034] The molar ratio of the total number of moles of hydroxyl groups in the polyol compound (a1-1) and hydroxyl groups in the chain extender to the number of moles of isocyanate groups in the aromatic polyisocyanate compound (a1-2) [(isocyanate groups) / (hydroxyl groups)] is preferably in the range of 0.80 to 1.00, more preferably in the range of 0.85 to 0.98.
[0035] In addition, when producing the urethane resin (a1), an organic solvent can be used. However, from the viewpoint of environmental friendliness, it is preferable to carry out the reaction between the polyol compound (a1-1) and the aromatic polyisocyanate compound (a1-2) in the absence of a solvent.
[0036] Examples of the organic solvent that can be used include ketone compounds such as acetone and methyl ethyl ketone; ether compounds such as tetrahydrofuran and dioxane; acetate compounds such as ethyl acetate and butyl acetate; nitrile compounds such as acetonitrile; and amide compounds such as dimethylformamide and N-methylpyrrolidone. These organic solvents may be used alone or in combination of two or more. The organic solvent is preferably removed by distillation or the like when obtaining the aqueous urethane resin composition.
[0037] The weight-average molecular weight of the urethane resin (a1) is preferably in the range of 2,000 to 150,000, more preferably in the range of 4,000 to 100,000, still more preferably in the range of 6,000 to 70,000, and particularly preferably in the range of 8,000 to 50,000, in order to obtain synthetic leather having an adhesive layer that has a long pot life and excellent peel strength and light resistance. The weight-average molecular weight of the urethane resin (a1) is a value obtained by measurement by GPC, similar to the number-average molecular weight of the polyol (a1-1).
[0038] Examples of the aqueous medium (a2) include ion-exchanged water, distilled water, etc. These aqueous media can be used alone or in combination of two or more.
[0039] The mass ratio [(a1) / (a2)] of the urethane resin (a1) to the aqueous medium (a2) is preferably in the range of 30 / 70 to 80 / 20, more preferably 40 / 60 to 70 / 30, because this allows for the production of synthetic leather having an adhesive layer that has a long pot life and is excellent in peel strength and light resistance.
[0040] Examples of the emulsifier (a3) include nonionic emulsifiers such as polyoxyethylene nonylphenyl ether, polyoxyethylene lauryl ether, polyoxyethylene styrylphenyl ether, polyoxyethylene sorbitol tetraoleate, and polyethylene-polypropylene copolymer; anionic emulsifiers such as fatty acid salts such as sodium oleate, alkyl sulfate ester salts, alkylbenzene sulfonates, alkyl sulfosuccinates, naphthalene sulfonates, polyoxyethylene alkyl sulfates, sodium alkanesulfonates, and sodium alkyldiphenyl ether sulfonates; and cationic emulsifiers such as alkylamine salts, alkyltrimethylammonium salts, and alkyldimethylbenzylammonium salts. These emulsifiers can be used alone or in combination of two or more. Among these, anionic emulsifiers are preferred because they provide synthetic leather with an adhesive layer that has a long pot life and is excellent in peel strength and light resistance.
[0041] The amount of the emulsifier (a3) used is preferably 10 parts by mass or less, more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the urethane resin (a1), in order to obtain a synthetic leather having an adhesive layer that has a long pot life and is excellent in peel strength and light resistance.
[0042] The weight average molecular weight of the aqueous urethane resin composition (A) is preferably in the range of 2,000 to 150,000, more preferably in the range of 4,000 to 100,000, because synthetic leather having an adhesive layer with a long pot life and excellent peel strength and light resistance can be obtained.
[0043] The method for producing the aqueous urethane resin composition (A) is not particularly limited, and any method may be used, for example, a method of mixing the urethane resin (a1), the aqueous medium (a2), and the emulsifier (a3).
[0044] Examples of methods for mixing the urethane resin (a1), the aqueous medium (a2), and the emulsifier (a3) include methods using a reaction vessel equipped with a stirring blade; a kneader such as a kneader, a continuous kneader, a taper roll, a single-screw extruder, a twin-screw extruder, a triple-screw extruder, a universal mixer, a Plastomill, or a Bodeta-type kneader; a rotary dispersion mixer such as a homomixer, a static mixer, FILMICS, an Ebara Milder, a Clearmix, an Ultra-Turrax, a Cavitron, or a Biomixer; an ultrasonic dispersion device; or a device such as an in-line mixer that has no moving parts and can mix by the flow of the fluid itself.
[0045] The aqueous urethane resin composition (A) may contain other additives as needed.
[0046] Examples of the other additives include surfactants, thickeners, urethanization catalysts, fillers, pigments, dyes, flame retardants, leveling agents, antiblocking agents, etc. These additives can be used alone or in combination of two or more. It is preferable that the urethane resin (a1) is produced without substantially containing an organic solvent, but an organic solvent may be added as an additive.
[0047] Examples of the surfactant include nonionic surfactants such as polyoxyethylene nonylphenyl ether, polyoxyethylene lauryl ether, polyoxyethylene styrylphenyl ether, polyoxyethylene sorbitol tetraoleate, and polyethylene-polypropylene copolymer; anionic surfactants such as fatty acid salts such as sodium oleate, alkyl sulfate ester salts, alkylbenzene sulfonates, alkyl sulfosuccinates, naphthalene sulfonates, polyoxyethylene alkyl sulfates, sodium alkanesulfonates, and sodium alkyldiphenyl ether sulfonates; and cationic surfactants such as alkylamine salts, alkyltrimethylammonium salts, and alkyldimethylbenzylammonium salts.
[0048] Examples of the thickener include associative and acid thickeners.
[0049] Examples of the urethane catalyst include organotin catalysts and bismuth catalysts.
[0050] Examples of the filler include calcium carbonate and silica.
[0051] Examples of the pigment include carbon black.
[0052] Examples of the dye include azo dyes.
[0053] Examples of the flame retardant include phosphorus-based flame retardants.
[0054] Examples of the leveling agent include silicon-based leveling agents.
[0055] Examples of the anti-blocking agent include acrylic agents and cellulose ester agents.
[0056] The aqueous urethane resin composition (B) used has a weight-average molecular weight of 100,000 or more. Because this allows for the production of synthetic leather having an adhesive layer with a long pot life and excellent peel strength and light resistance, the weight-average molecular weight is preferably 100,000 to 700,000, and more preferably 150,000 to 500,000. In the present invention, the weight-average molecular weight is a value measured by gel permeation column chromatography (GPC).
[0057] The aqueous urethane resin composition (B) may, for example, be one containing a urethane resin (b1) and an aqueous medium (b2).
[0058] The urethane resin (b1) may, for example, be one containing a polyol compound (b1-1) and a polyisocyanate compound (b1-2) as essential raw materials.
[0059] Examples of the polyol compound (b1-1) include polyether polyols, polyester polyols, polycarbonate polyols, polycaprolactone polyols, polyacrylic polyols, and silicon-modified polyols. These polyol compounds can be used alone or in combination of two or more. These polyol compounds may be derived from petroleum or biomass.
[0060] Examples of the polyether polyols include polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polyoxyethylene polyoxypropylene glycol, polyoxyethylene polyoxytetramethylene glycol, etc. These polyether polyols can be used alone or in combination of two or more.
[0061] Examples of the polyester polyol include those obtained by esterifying a polycarboxylic acid with a polyhydric alcohol.
[0062] Examples of the polycarboxylic acid include aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, and naphthalenedicarboxylic acid, and esters thereof, and aliphatic dicarboxylic acids such as succinic acid, glutaric acid, adipic acid, maleic acid, pimelic acid, suberic acid, azelaic acid, itaconic acid, sebacic acid, chlorendic acid, 1,2,4-butanetricarboxylic acid, decanedicarboxylic acid, cyclohexanedicarboxylic acid, dimer acid, and fumaric acid, and esters thereof. These polycarboxylic acids and esters thereof can be used alone or in combination of two or more.
[0063] Examples of the polyhydric alcohol include aromatic diols such as benzenedimethanol, toluenedimethanol, and xylene dimethanol, and aliphatic polyols such as ethylene glycol, propylene glycol, 1,3-propylene diol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, diethylene glycol, triethylene glycol, cyclohexane-1,4-diol, cyclohexane-1,4-dimethanol, and neopentyl glycol ethylene glycol. These polyhydric alcohols can be used alone or in combination of two or more.
[0064] In the esterification reaction for producing the polyester polyol, it is preferable to use an esterification catalyst for the purpose of accelerating the esterification reaction. Examples of the esterification catalyst include metals such as titanium, tin, zinc, aluminum, zirconium, magnesium, hafnium, and germanium; and metal compounds such as titanium tetraisopropoxide, titanium tetrabutoxide, titanium oxyacetylacetonate, dibutyltin oxide, dibutyltin diacetate, dibutyltin dilaurate, tin octoate, 2-ethylhexanetin, zinc acetylacetonate, zirconium tetrachloride, zirconium tetrachloride tetrahydrofuran complex, hafnium tetrachloride, hafnium tetrachloride tetrahydrofuran complex, germanium oxide, and tetraethoxygermanium. These esterification catalysts can be used alone or in combination of two or more.
[0065] Examples of the polycarbonate polyol include a reaction product of a carbonate ester and / or phosgene with a compound having two or more hydroxyl groups.
[0066] Examples of the carbonate ester include dimethyl carbonate, diethyl carbonate, diphenyl carbonate, ethylene carbonate, propylene carbonate, etc. These carbonate esters can be used alone or in combination of two or more.
[0067] Examples of the compound having two or more hydroxyl groups include ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 1,2-butanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 1,5-hexanediol, 3-methyl-1,5-pentanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,8-nonanediol, 2-ethyl-2-butyl-1,3-propanediol, 1,10-decanediol, 1,12-dodecanediol, 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, trimethylolpropane, 3-methylpentanediol, neopentyl glycol, trimethylolethane, and glycerin. These compounds can be used alone or in combination of two or more.
[0068] The number average molecular weight of the polyol compound (b1-1) is preferably in the range of 500 to 5,000, since this allows for the production of synthetic leather having an adhesive layer that has a long pot life and is excellent in peel strength and light resistance.
[0069] The content of the polyol compound (b1-1) in the raw materials of the urethane resin (b1) is preferably in the range of 50 to 95% by mass, more preferably in the range of 60 to 90% by mass, because this allows for the production of synthetic leather having an adhesive layer that has a long pot life and is excellent in peel strength and light resistance.
[0070] Examples of the polyisocyanate compound (b1-2) include aliphatic polyisocyanates such as hexamethylene diisocyanate, lysine diisocyanate, cyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, xylylene diisocyanate, tetramethylxylylene diisocyanate, dimer acid diisocyanate, and norbornene diisocyanate; alicyclic diisocyanates such as norbornane diisocyanate, isophorone diisocyanate, hydrogenated xylylene diisocyanate, and hydrogenated diphenylmethane diisocyanate; and aromatic polyisocyanates such as phenylene diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate, naphthalene diisocyanate, polymethylene polyphenyl polyisocyanate, and carbodiimidized diphenylmethane polyisocyanate. These polyisocyanate compounds can be used alone or in combination of two or more. Among these, hexamethylene diisocyanate, isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, and hydrogenated diphenylmethane diisocyanate are preferred because they provide synthetic leather having a long pot life and an adhesive layer that is excellent in peel strength and light resistance.
[0071] The content of the polyisocyanate compound (b1-2) in the raw material of the urethane resin (b1) is preferably in the range of 5 to 50% by mass, more preferably in the range of 10 to 30% by mass, because this allows for the production of synthetic leather having an adhesive layer that has a long pot life and is excellent in peel strength and light resistance.
[0072] The urethane resin (b1) may further contain a chain extender (b1-3) as needed.
[0073] The chain extender (b1-3) preferably has a molecular weight of less than 500. The molecular weight of the chain extender (a3) is a value calculated from the chemical structural formula.
[0074] Examples of the chain extender (a3) include a chain extender having a hydroxyl group, a chain extender having an amino group, etc. These chain extenders can be used alone or in combination of two or more.
[0075] Examples of the chain extender having a hydroxyl group include aliphatic polyol compounds such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, hexamethylene glycol, sucrose, methylene glycol, glycerin, and sorbitol; aromatic polyol compounds such as bisphenol A, 4,4'-dihydroxydiphenyl, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl sulfone, hydrogenated bisphenol A, and hydroquinone; and water. These chain extenders can be used alone or in combination of two or more.
[0076] Examples of the chain extender having an amino group include ethylenediamine, 1,2-propanediamine, 1,6-hexamethylenediamine, piperazine, 2-methylpiperazine, 2,5-dimethylpiperazine, isophoronediamine, 4,4'-dicyclohexylmethanediamine, 3,3'-dimethyl-4,4'-dicyclohexylmethanediamine, 1,2-cyclohexanediamine, 1,4-cyclohexanediamine, aminoethylethanolamine, hydrazine, diethylenetriamine, triethylenetetramine, etc. These chain extenders can be used alone or in combination of two or more.
[0077] The amount of the chain extender (b1-3) used is preferably in the range of 0.2 to 20% by mass, more preferably 0.5 to 10% by mass, of the solid content of the urethane resin composition (B), because a synthetic leather having an adhesive layer with a long pot life and excellent peel strength and light resistance can be obtained.
[0078] The method for producing the urethane resin (b1) is not particularly limited, and any method may be used. For example, the urethane resin (b1) may be produced by reacting all of the reactant materials, including the polyol compound (b1-1), the polyisocyanate compound (b1-2), and, if necessary, the chain extender (b1-3), all at once, or by sequentially reacting the reactant materials. These reactions are preferably carried out at a temperature of 50 to 100°C for 3 to 10 hours, for example.
[0079] Regarding the reaction ratio of the polyol compound (b1-1), the polyisocyanate compound (b1-2), and the chain extender (b1-3), the molar ratio of the total number of moles of hydroxyl groups in the polyol compound (b1-1) and the hydroxyl groups and amino groups in the chain extender (b1-3) to the number of moles of isocyanate groups in the polyisocyanate compound (b1-2) [(isocyanate groups) / (hydroxyl groups and amino groups)] is preferably in the range of 0.90 to 1.30, more preferably 0.95 to 1.20, because a synthetic leather can be obtained that has a long pot life and an adhesive layer that is excellent in peel strength and light resistance.
[0080] When producing the urethane resin (b1), an organic solvent may also be used.
[0081] Examples of the organic solvent that can be used include ketone compounds such as acetone and methyl ethyl ketone; ether compounds such as tetrahydrofuran and dioxane; acetate compounds such as ethyl acetate and butyl acetate; nitrile compounds such as acetonitrile; and amide compounds such as dimethylformamide and N-methylpyrrolidone. These organic solvents may be used alone or in combination of two or more. The organic solvent is preferably removed by distillation or the like when obtaining the aqueous urethane resin composition.
[0082] As the aqueous medium (b2), the same aqueous medium as exemplified above as the aqueous medium (a2) can be used, and these aqueous media can be used alone or in combination of two or more kinds.
[0083] The mass ratio [(b1) / (b2)] of the urethane resin (b1) to the aqueous medium (b2) is preferably in the range of 30 / 70 to 80 / 20, more preferably in the range of 40 / 60 to 70 / 30, since this allows for the production of synthetic leather having an adhesive layer that has a long pot life and is excellent in peel strength and light resistance.
[0084] The method for producing the aqueous urethane resin composition (B) is not particularly limited, and any method may be used, such as a method of mixing the urethane resin (b1) with the aqueous medium (b2).
[0085] Examples of methods for mixing the urethane resin (b1) and the aqueous medium (b2) include methods using a reaction vessel equipped with a stirring blade; a kneader such as a kneader, a continuous kneader, a taper roll, a single-screw extruder, a twin-screw extruder, a triple-screw extruder, a universal mixer, a Plastomill, or a Bodeta-type kneader; a rotary dispersion mixer such as a homomixer, a static mixer, FILMICS, an Ebara Milder, a Clearmix, an Ultra-Turrax, a Cavitron, or a Biomixer; an ultrasonic dispersion device; or a device such as an in-line mixer that has no moving parts and can mix by the flow of the fluid itself.
[0086] The aqueous urethane resin composition (B) may contain other additives as needed.
[0087] As the other additives, the same additives as those exemplified above can be used, and the other additives can be used alone or in combination of two or more.
[0088] The mixing ratio of the aqueous urethane resin composition (A) to the aqueous urethane resin composition (B) is preferably in the range of 51 / 49 to 97 / 3, more preferably in the range of 60 / 40 to 95 / 5, because this allows for the production of synthetic leather having an adhesive layer that has a long pot life and is excellent in peel strength and light resistance.
[0089] The thickness of the adhesive layer (ii) is, for example, in the range of 30 to 60 μm.
[0090] Examples of the material for forming the surface layer (iii) (hereinafter, sometimes referred to as "surface layer-forming resin") include known aqueous urethane resins, solvent-based urethane resins, solventless urethane resins, aqueous acrylic resins, silicone resins, polypropylene resins, polyester resins, etc. These materials can be used alone or in combination of two or more.
[0091] A surface treatment layer may be further provided on the surface layer (iii) to prevent scratches, etc. Examples of materials for forming the surface treatment layer include known aqueous urethane resins, solvent-based urethane resins, solventless urethane resins, aqueous acrylic resins, silicone resins, polypropylene resins, polyester resins, and vinyl chloride resins. These materials may be used alone or in combination of two or more.
[0092] The porous layer may be formed from a solvent-based urethane resin composition by a known wet film-forming method; a water-based urethane resin composition that has been made porous by a known method; or a solventless urethane resin composition that has been foamed by a known method.
[0093] Examples of materials for forming the intermediate layer include known aqueous urethane resins, solvent-based urethane resins, solventless urethane resins, aqueous acrylic resins, silicone resins, polypropylene resins, polyester resins, vinyl chloride resins, etc. These materials can be used alone or in combination of two or more.
[0094] The synthetic leather may be produced by any method without any particular limitation. Examples thereof include a method (1) in which a resin for forming a surface layer is applied to a release-treated substrate, followed by drying and processing to obtain a surface layer (iii), and then the aqueous urethane resin composition of the present invention is applied to the surface layer (iii) and dried to form an adhesive layer (ii), which is then laminated to a base fabric (i), and a method (2) in which a resin for forming a surface layer is applied to a release-treated substrate, followed by drying and processing to obtain a surface layer (iii), and then the aqueous urethane resin composition of the present invention is applied to the surface layer (iii), which is then laminated to a base fabric (i), followed by drying to form an adhesive layer (ii).
[0095] Examples of methods for applying the resin for forming the surface layer and the aqueous urethane resin composition include methods using an applicator, a roll coater, a spray coater, a T-die coater, a knife coater, a comma coater, and the like.
[0096] After the synthetic leather is produced, it may be aged, for example, at 30 to 100° C. for 1 to 10 days, if necessary.
[0097] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the examples given below.
[0098] The weight average molecular weight of the aqueous urethane resin composition and the number average molecular weight of the polyol compound used in the examples and comparative examples were measured by gel permeation chromatography (GPC) under the following conditions.
[0099] Measurement apparatus: High-speed GPC apparatus ("HLC-8220GPC" manufactured by Tosoh Corporation) Column: The following columns manufactured by Tosoh Corporation were used, connected in series: "TSKgel G5000" (7.8 mm I.D. x 30 cm) x 1, "TSKgel G4000" (7.8 mm I.D. x 30 cm) x 1, "TSKgel G3000" (7.8 mm I.D. x 30 cm) x 1, "TSKgel G2000" (7.8 mm I.D. x 30 cm) x 1 Detector: RI (differential refractometer) Column temperature: 40°C Eluent: Tetrahydrofuran (THF) Flow rate: 1.0 mL / min Injection volume: 100 μL (tetrahydrofuran solution with a sample concentration of 0.4% by mass) Standard sample: A calibration curve was prepared using the following standard polystyrene.
[0100] (Standard polystyrene) "TSKgel Standard Polystyrene A-500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-1000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-2500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-5000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-1" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-2" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-4" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-10" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-20" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-40" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-80" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-128" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-288" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-550" manufactured by Tosoh Corporation
[0101] Synthesis Example 1 Preparation of Aqueous Urethane Resin Composition (A1) In a four-neck flask equipped with a stirrer, a reflux condenser, a thermometer, and a nitrogen inlet tube, 1,000 parts by mass of polyether polyol ("PTMG1000" manufactured by Mitsubishi Chemical Corporation, number average molecular weight: 1,000, hereinafter abbreviated as "PTMG1000"), 61 parts by mass of methoxypolyethylene glycol ("UNIOX M1000" manufactured by NOF Corporation, number average molecular weight: 1,000, hereinafter abbreviated as "MPEG"), and 163 parts by mass of toluene diisocyanate (hereinafter abbreviated as "TDI") were reacted under a nitrogen stream at 120°C for 3 hours to obtain a urethane resin (a1) ([NCO] / [OH] ratio: 0.90). Next, urethane resin (a1) heated to 70°C was mixed with 141 parts by mass of a 35% by mass aqueous solution of sodium alkylnaphthalenesulfonate ("Pelex NBL" manufactured by Kao Corporation) and 309 parts by mass of water, and further water was added to finally obtain an aqueous urethane resin composition (A1) having a urethane resin content of 50% by mass. The urea bond group concentration in this aqueous urethane resin composition (A1) was 0 mmol / kg.
[0102] Synthesis Example 2 Preparation of Aqueous Urethane Resin Composition (B1) In a four-neck flask equipped with a stirrer, a reflux condenser, a thermometer, and a nitrogen inlet tube, 1,000 parts by mass of polyether polyol ("PTMG2000" manufactured by Mitsubishi Chemical Corporation, number average molecular weight: 2,000, hereinafter abbreviated as "PTMG2000"), 24 parts by mass of 2,2-dimethylolpropionic acid (hereinafter abbreviated as "DMPA"), and 262 parts by mass of dicyclohexylmethane diisocyanate (hereinafter abbreviated as "HMDI") were reacted at 100°C in the presence of 0.1 parts by mass of stannous octoate under a nitrogen stream until the NCO% reached 2.1% by mass, to obtain a urethane resin (b1). Next, the urethane resin (b1) heated to 70°C was mixed with 25 parts by mass of triethylamine, 322 parts by mass of a 20% by mass aqueous solution of sodium dodecylbenzenesulfonate ("Neogen S-20F" manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), and 670 parts by mass of water. Immediately thereafter, a water-diluted solution of isophoronediamine (hereinafter abbreviated as "IPDA") having an amino group content equivalent to 95% of the NCO groups was added to carry out chain extension, ultimately obtaining an aqueous urethane resin composition (B1) having a urethane resin content of 50% by mass.
[0103] Example 1: Production of synthetic leather (1) A blended liquid consisting of 100 parts by mass of an aqueous urethane resin composition for a surface layer (HYDRAN WLS-250 manufactured by DIC Corporation), 10 parts by mass of a water-dispersible black pigment (DIC Corporation's DIRAC HS-9530), and 1 part by mass of an associative thickener (DIC Corporation's HYDRAN ASISTOR T10) was applied to a flat release paper (Ajinomoto Co., Inc.'s DN-TP-155T) so that the film would have a dry thickness of 30 μm, and the coating was dried at 70° C. for 2 minutes and then at 120° C. for 2 minutes. Next, 90 parts by mass of the aqueous urethane resin composition (A1) obtained in Synthesis Example 1 and 10 parts by mass of the aqueous urethane resin composition (B1) obtained in Synthesis Example 2 were mixed, to which 14 parts by mass of a polyisocyanate-based crosslinking agent (BURNOCK DNW-5500 manufactured by DIC Corporation) was added, and the mixture was stirred and mixed for 5 minutes. This mixture was applied to a solid film thickness of 50 μm and dried for 3 minutes at 90° C. After laminating with a T / R raised fabric, it was heat-treated at 130° C. for 10 minutes, and the release paper was peeled off to obtain synthetic leather (1).
[0104] (Examples 2 to 5: Production of synthetic leathers (2) to (5)) Synthetic leathers (2) to (5) were obtained in the same manner as in Example 1, except that the blending amounts of the "aqueous urethane resin composition (A1)" and the "aqueous urethane resin composition (B1)" used in Example 1 were changed as shown in Table 1.
[0105] Comparative Example 1: Production of synthetic leather (R1) Synthetic leather (R1) was obtained in the same manner as in Example 1, except that the blending amounts of the "aqueous urethane resin composition (A1)" and the "aqueous urethane resin composition (B1)" used in Example 1 were changed as shown in Table 1.
[0106] [Method for measuring dry peel strength] A 2.5 cm wide hot melt tape ("BW-2" manufactured by Sun Chemical Industry Co., Ltd.) was placed on the synthetic leather obtained in the Examples and Comparative Examples and heated at 150°C for 3 minutes to adhere it. A sample was cut along the width of the hot melt tape. A portion of this sample was peeled off, and the substrate and hot melt tape were clamped with a zipper. The peel strength was measured using an autograph ("AG-1" manufactured by Shimadzu Corporation) and evaluated according to the following criteria.
[0107] A: The peel strength was 3.5 kgf / 25 mm or more. B: The peel strength was 2.5 kgf / 25 mm or more and less than 3.5 kgf / 25 mm. C: The peel strength was less than 2.5 kgf / 25 mm.
[0108] [Method for measuring wet peel strength] A 2.5 cm wide hot melt tape ("BW-2" manufactured by Sun Chemical Industry Co., Ltd.) was placed on the synthetic leather obtained in the Examples and Comparative Examples and heated at 150°C for 3 minutes to adhere it. A sample was cut along the width of the hot melt tape. After immersing this sample in water at 23°C for 3 hours, a portion of this sample was peeled off, and the substrate and hot melt tape were clamped with a zipper. The peel strength was measured using an autograph ("AG-1" manufactured by Shimadzu Corporation) and evaluated according to the following criteria.
[0109] A: The peel strength was 3.5 kgf / 25 mm or more. B: The peel strength was 2.5 kgf / 25 mm or more and less than 3.5 kgf / 25 mm. C: The peel strength was less than 2.5 kgf / 25 mm.
[0110] [Method for Evaluating Pot Life] 10 parts by mass of a polyisocyanate-based crosslinking agent (Burnoc DNW-5500 manufactured by DIC Corporation) was added to 100 parts by mass of each of the aqueous urethane resin compositions (A1) and (B1) obtained in the Synthesis Examples, and the mixture was left at 40°C for 4 hours. Synthetic leathers were then prepared in the same manner as in Example 1. A 2.5 cm wide hot melt tape (BW-2 manufactured by Sun Chemical Industry Co., Ltd.) was placed on the synthetic leather and heated at 150°C for 3 minutes to adhere the tape. A sample was then cut along the width of the hot melt tape. A portion of the sample was peeled off, and the substrate and hot melt tape were clamped with a zipper. The peel strength was measured using an autograph (AG-1 manufactured by Shimadzu Corporation) and evaluated according to the following criteria.
[0111] A: The peel strength was 3.5 kgf / 25 mm or more. B: The peel strength was 2.5 kgf / 25 mm or more and less than 3.5 kgf / 25 mm. C: The peel strength was less than 2.5 kgf / 25 mm.
[0112] [Method for evaluating light resistance] The synthetic leathers obtained in the examples and comparative examples were irradiated with light for 100 hours using a fade meter "U48AU" (63°C, humidity 50%) manufactured by Suga Test Instruments Co., Ltd. Thereafter, the synthetic leathers were visually observed and evaluated according to the following criteria.
[0113] A: No change in appearance. B: Slight yellowing was observed in appearance. C: Significant yellowing was observed in appearance.
[0114] The blending amounts of the aqueous urethane resin compositions used in the adhesive layer-forming materials of the synthetic leathers (1) to (5), (R1) and (R2) obtained in the above Examples and Comparative Examples, and the evaluation results are shown in Tables 1 and 2.
[0115]
[0116] Examples 1 to 5 shown in Table 1 are examples in which the synthetic leather of the present invention was used. It was confirmed that the adhesive layer of these synthetic leathers had a long pot life and was excellent in peel strength and light resistance.
[0117] On the other hand, Comparative Example 1 shown in Table 1 is an example of synthetic leather in which the aqueous urethane resin composition (B) was not used as the adhesive layer-forming material. It was confirmed that the adhesive layer of this synthetic leather had significantly insufficient wet peel strength.
Claims
1. A synthetic leather having at least a base fabric (i), an adhesive layer (ii), and a surface layer (iii), wherein the adhesive layer (ii) is formed from a mixture containing an aqueous urethane resin composition (A) and an aqueous urethane resin composition (B) other than the aqueous resin composition (A), the aqueous urethane resin composition (A) contains a urethane resin (a1), an aqueous medium (a2), and an emulsifier (a3), the urethane resin (a1) contains a polyol compound (a1-1) containing a nonionic polyol and an aromatic polyisocyanate compound (a1-2) as essential raw materials, the urea bond concentration in the urethane resin (a1) is 100 mmol / kg or less, and the weight average molecular weight of the aqueous urethane resin composition (B) is 100,000 or more.
2. The synthetic leather according to claim 1, wherein the mixing ratio of the aqueous urethane resin composition (A) to the aqueous urethane resin composition (B) is in the range of 51 / 49 to 97 / 3.
3. The synthetic leather according to claim 1, wherein the aromatic polyisocyanate compound (a1-2) is toluene diisocyanate.
4. The synthetic leather according to claim 1 or 2, wherein the emulsifier (a3) contains an anionic emulsifier.
5. The synthetic leather according to claim 1, wherein the amount of the emulsifier (a3) used is 10 parts by mass or less per 100 parts by mass of the urethane resin (a1).
6. A method for producing synthetic leather according to any one of claims 1 to 5, wherein the urethane resin (a1) is obtained by reacting raw materials containing the polyol compound (a1-1) and the aromatic polyisocyanate compound (a1-2) in the absence of a solvent.
Citation Information
Patent Citations
Manufacture of fibrous laminate and synthetic leather obtained thereby
JP2000108289A
Emulsifying agent, water-emulsified isocyanate curing agent and water-emulsified curable composition using the same
JP2004315598A
Method for producing vinyl polymer and method for producing polyurethane
JP2012201730A
Urethane resin composition, leather-like sheet, and laminate
JP2015040286A
Manufacturing method of solid