Composition containing siloxane bond-containing polymer compound that has host group and / or guest group
The composition of siloxane bond-containing polymer compounds with specific cyclic oligosaccharide-modified organopolysiloxane compounds addresses the limitations of conventional films by enhancing self-healing and film-forming properties, resulting in resilient and transparent resin sheets.
Patent Information
- Application Number
- PCT/JP2024/016265
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-09
- Filing Date
- 2024-04-25
- Publication Date
- 2024-11-14
AI Technical Summary
Conventional compositions containing siloxane bond-containing polymer compounds with host and guest groups lack improved self-healing and film-forming properties, limiting their effectiveness in forming resilient and durable films.
A composition comprising a host body and a guest body, both containing siloxane bonds, with specific cyclic oligosaccharide-modified organopolysiloxane compounds, where the content of these compounds ranges from 1% to 25% by mass, enhancing compatibility and fluidity for improved self-healing and film-forming capabilities.
The composition achieves excellent self-healing properties and enhanced film-forming characteristics, including elasticity and transparency, with the specific content of siloxane bond-containing compounds optimizing the resin sheet's performance.
Smart Images

Figure JP2024016265_14112024_PF_FP_ABST
Abstract
Description
Composition containing a siloxane bond-containing polymer compound having a host group and / or a guest group
[0001] The present disclosure relates to compositions comprising siloxane bond-containing polymeric compounds having host groups and / or guest groups.
[0002] It is known that films can be formed by using crosslinked polymer compounds. In particular, film-forming agents containing crosslinked silicone resins are widely used in various coating agents and cosmetics.
[0003] Patent Document 1 discloses a cosmetic composition containing trimethylsiloxysilicate or the like as a film-forming agent.
[0004] It is also known that a host body made of a polymer compound having a host group and a guest body made of a polymer compound having a guest group, or a host-guest body made of a polymer compound having a host group and a guest group, can reversibly form a bond depending on the combination of the host group and the guest group (Patent Document 2).
[0005] Patent Documents 3 and 4 respectively describe a resin material and a cosmetic containing a siloxane bond-containing polymer compound having a host group and / or a guest group.
[0006] JP 2019-99576 A International Publication No. 2012 / 036069 International Publication No. 2021 / 172463 International Publication No. 2021 / 172468
[0007] Films formed based on host-guest interactions can have self-repairing properties. For example, cosmetic coating films formed based on host-guest interactions can have self-repairing properties due to the reversible recombination of polymeric compounds via host-guest interactions.
[0008] The present invention aims to achieve improved self-repairing properties compared to conventional compositions containing siloxane bond-containing polymeric compounds having host groups and / or guest groups. In particular, the present invention also aims to achieve improved film-forming properties compared to conventional compositions containing siloxane bond-containing polymeric compounds having host groups and / or guest groups.
[0009] The invention according to the present disclosure can solve the above-mentioned problems by the invention including the following aspects: <Aspect 1> A composition containing a host entity made of a polymer compound having a host group and a guest entity made of a polymer compound having a guest group, or a host-guest entity made of a polymer compound having a host group and a guest group, and a compound represented by the following chemical formula DP1, wherein at least one of the polymer compound having a host group and the polymer compound having a guest group, or the polymer compound having a host group and a guest group, contains a siloxane bond, and the content of the compound represented by the chemical formula DP1 in the composition is 1 mass % to 25 mass % with respect to the total mass of the composition: Composition: (In formula DP1, x is an integer of 0 to 200, and y is an integer of 1 to 200.) <Aspect 2> The host group is α-cyclodextrin, β-cyclodextrin, or γ-cyclodextrin, and / or the guest group is (1) a linear alkyl group having 4 to 18 carbon atoms, (2) a linear alkyl group having 4 to 18 carbon atoms and having a hydroxyl group, (3) a linear alkyl group having 4 to 18 carbon atoms and having a carboxyl group, (4) a linear alkyl group having 4 to 18 carbon atoms and having an amino group, (5) a cyclic alkyl group, (6) a phenyl group, (7) an azobenzene group, (8) a cinnamic acid group, (1') a t-butyl group, (2') an adamantyl group, (3') an aryl group, (4') an aryl group having a hydroxyl group, (5') an aryl group having a carboxyl group, (6') an aryl group having an amino group, (7') a phenyl group, (8') a phenyl group, (9) a phenyl group, (10) a phenyl group, (11) a phenyl group, (12) a phenyl group, (13) a phenyl group, (14) a phenyl group, (15) a phenyl group, (16) a phenyl group, (17) a phenyl group, (18) a phenyl group, (19) a phenyl group, (20) a phenyl group, (21) a phenyl group, (22) a phenyl group, (23) a phenyl group, (24) a phenyl group, (25) a phenyl group, (26) a phenyl group, (27) a phenyl group, (28) a phenyl group, (29) a phenyl group, (30) a phenyl group, (31) a phenyl group, (32) a phenyl group, (3 (8) a ferrocenyl group, (9) a dansyl group, (1") an alkyl group having up to 18 carbon atoms, (2") an alkyl group having up to 18 carbon atoms and a hydroxyl group, (3") an alkyl group having up to 18 carbon atoms and a carboxyl group, (4") an alkyl group having up to 18 carbon atoms and an amino group, (5") an adamantyl group, (6") a group having a cluster of carbon atoms, (7") a dansyl group having an aryl group, (8") a ferrocenyl group, and (9") an anthracenyl group. <Aspect 3> The composition according to Aspect 1 or 2, wherein the polymeric compound having a host group or the polymeric compound having a host group and a guest group is a cyclic oligosaccharide-modified organopolysiloxane that is an addition reaction product of the following A and B: (A) an organohydrogenpolysiloxane having one or more hydrosilyl groups per molecule; and (B) a cyclic oligosaccharide derivative having an unsaturated group represented by the following general formula (1): (In formula 1, L is an alkenyl group having 2 to 12 carbon atoms, R 1 are independently a group selected from an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 2 represents an alkylene group having 1 to 4 carbon atoms, R 3are independently selected from alkyl groups having 1 to 4 carbon atoms or acyl groups having 1 to 4 carbon atoms, a is an integer of 0 to 8, b is an integer of 5 to 7, and x is 0 or 1.) <Aspect 4> The organohydrogenpolysiloxane has a kinematic viscosity of 50 mm at 25°C. 2 / s or more and its number average molecular weight is 8,000 or more. <Aspect 5> The composition according to Aspect 3 or 4, wherein the cyclic oligosaccharide-modified organopolysiloxane is an addition reaction product of (C) an α-olefin having 2 to 16 carbon atoms in addition to (A) and (B). <Aspect 6> The composition according to Aspect 1 or 2, wherein at least one of the polymer compound having a host group and the polymer compound having a guest group, or the polymer compound having a host group and a guest group, is represented by the following formula 2: (In formula 2, R 4 are independently a group selected from an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 5 are independently an alkyl group having 5 to 16 carbon atoms; R 6 are independently a group having a cyclic oligosaccharide structure represented by the following formula 3, and R 7 are independently R 4 or R 6 is a group selected from the groups described above with respect to (c), where c is an integer of 100 to 600, d is an integer of 0 to 50, e is an integer of 0 to 50, and f is an integer of 0 to 20. However, at least one of d and e is 1 or greater, and the range of c+d+e is satisfied, i.e., 101 to 700, and the bonding order of the siloxane units bounded by c, d, e, and f may be block or random. (In Formula 3, L' is an alkylene group having 2 to 12 carbon atoms, and R 1 are independently a group selected from an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 2 represents an alkylene group having 1 to 4 carbon atoms, R 3are independently a group selected from an alkyl group having 1 to 4 carbon atoms or an acyl group having 1 to 4 carbon atoms, a is an integer of 0 to 8, b is an integer of 5 to 7, and x is 0 or 1. * is a free group that bonds to the silicon atom of the siloxane unit. <Aspect 7> In the formula 3, R 1 is a methyl group, R 3 is an acetyl group, and in the formula 2, R 4 and R 7 is a methyl group. <Aspect 8> The composition according to aspect 6 or 7, wherein x is 0 in formula 3. <Aspect 9> The composition according to any one of aspects 6 to 8, wherein the polymer compound having a host group or the polymer compound having a host group and a guest group is represented by formula 2, wherein e = 1 to 50 in formula 2. <Aspect 10> The composition according to any one of aspects 6 to 9, wherein the polymer compound represented by formula 2 has a glass transition temperature of 30 to 130°C as measured by dynamic viscoelasticity measurement. <Aspect 11> The composition according to any one of aspects 1 to 10, further comprising a solvent. <Aspect 12> The composition according to aspect 11, wherein the solvent is a volatile silicone or a volatile hydrocarbon compound. <Aspect 13> The composition according to any one of aspects 1 to 12, for use as a cosmetic. Aspect 14: A method for producing a resin sheet, comprising: applying the composition according to any one of Aspects 1 to 12 onto a substrate and shaping the composition into a sheet; and drying the composition shaped into a sheet to form a resin sheet. Aspect 15: The method according to Aspect 14, wherein the resin sheet is a film.
[0010] According to the present invention, a composition containing a siloxane bond-containing polymer compound having a host group and / or a guest group can achieve improved self-repairing properties compared to conventional compositions. In particular, according to the present invention, a composition containing a siloxane bond-containing polymer compound having a host group and / or a guest group can achieve improved film-forming properties compared to conventional compositions.
[0011] <<Composition>> The composition according to the present disclosure is a composition containing a host entity made of a polymeric compound having a host group and a guest entity made of a polymeric compound having a guest group, or a host-guest entity made of a polymeric compound having a host group and a guest group, and a compound represented by the following formula DP1, wherein at least one of the polymeric compound having a host group and the polymeric compound having a guest group, or the polymeric compound having a host group and a guest group, contains a siloxane bond, and the content of the compound represented by the chemical formula DP1 in the composition is 1% by mass to 25% by mass with respect to the total mass of the composition.
[0012] The present inventors have discovered that a resin sheet (e.g., a coating) exhibiting excellent self-repairing properties can be obtained by incorporating a specific amount of a compound represented by the following formula DP1 into a composition containing a siloxane bond-containing polymer compound having a host group and / or a guest group. The siloxane bond-containing polymer compound is, for example, an organopolysiloxane.
[0013] For self-repair through host-guest interactions, it is believed that ensuring a certain level of fluidity of the components in the film is important. Without intending to be limited by theory, in the present invention, by incorporating a specific amount of a compound represented by the following formula DP1 into a composition containing a siloxane bond-containing polymer compound having a host group and / or a guest group, it is believed that good compatibility between the components in the composition is ensured and the fluidity of the components in the formed film is improved, resulting in a film with excellent self-repair properties.
[0014] The composition according to the present invention may also have particularly excellent film-forming properties due to the inclusion of a specific amount of the compound represented by the following formula DP1. Furthermore, a resin sheet (e.g., a film) formed from the composition according to the present invention may also have excellent elasticity and / or transparency.
[0015] <Compound Represented by Formula DP1> As described above, the composition of the present invention contains a compound represented by the following chemical formula DP1. (In formula DP1, x is an integer from 0 to 200, and y is an integer from 1 to 200).
[0016] When x=0, the compound represented by formula DP1 is phenyl trimethicone. In this case, y is preferably an integer of 1 to 50, more preferably 1 to 20, from the viewpoint of the viscosity of phenyl trimethicone.
[0017] When x>0, the compound represented by formula DP1 is diphenylsiloxyphenyl trimethicone, in which case it is preferred that x=an integer from 1 to 100 and y=an integer from 1 to 100, more preferably x and y are each independently an integer from 2 to 50, an integer from 3 to 25, or even an integer from 4 to 15.
[0018] The content of the compound represented by the chemical formula DP1 in the composition is 1 to 25% by mass, preferably 2 to 20% by mass, and more preferably 3 to 18% by mass, based on the total mass of the composition.
[0019] In a particularly preferred embodiment, the content of the compound represented by the chemical formula DP1 in the composition is 5% by mass or more (or even 6% by mass or more) relative to the total mass of the composition. In this case, particularly good self-repairing properties may be obtained for a resin sheet or the like formed from the composition.
[0020] In another particularly preferred embodiment, the content of the compound represented by the chemical formula DP1 in the composition is 15% by mass or less (or even 12% by mass or less) relative to the total mass of the composition. In this case, particularly good self-repairing properties may be obtained for a resin sheet or the like formed from the composition, and particularly excellent film-forming properties may be obtained.
[0021] The compound represented by Formula DP1 may be contained in an amount of 5 to 150 parts by mass, preferably 10 to 120 parts by mass, more preferably 30 to 90 parts by mass, particularly preferably 40 to 80 parts by mass, and most particularly preferably 40 to 70 parts by mass, relative to 100 parts by mass of the total of the host group- and / or guest group-containing polymeric compounds in the composition. In particular, the compound represented by Formula DP1 is contained in an amount of 10 to 120 parts by mass, more preferably 30 to 90 parts by mass, particularly preferably 40 to 80 parts by mass, and most particularly preferably 40 to 70 parts by mass, relative to 100 parts by mass of the polymeric compounds having host groups and guest groups in the composition.
[0022] In one preferred embodiment, the compound represented by formula DP1 has a viscosity of 10 to 20 mm when measured at 25°C according to Method 1 of the Viscosity Measurement Method for Quasi-drug Raw Materials. 2 / s, and in particular, 15 mm 2 In one preferred embodiment, the compound represented by formula DP1 has a refractive index of 1.4, particularly 1.49, when measured at 25°C according to the refractive index measurement method for quasi-drug raw materials.
[0023] <Host entity, guest entity, host-guest entity> The composition according to the present disclosure contains a host entity made of a polymer compound having a host group and a guest entity made of a polymer compound having a guest group, or a host-guest entity made of a polymer compound having a host group and a guest group. Note that these polymer compounds are different from the compound represented by formula DP1 above.
[0024] When the composition contains a solvent, the total content of the host entity consisting of a polymeric compound having a host group and the guest entity consisting of a polymeric compound having a guest group, and / or the host-guest entity consisting of a polymeric compound having a host group and a guest group (i.e., the total content of the host group- and / or guest group-containing polymeric compounds) may be 5% by mass to 40% by mass, preferably 8% by mass to 30% by mass, and more preferably 10% by mass to 25% by mass, relative to the total mass of the composition.
[0025] <Polymer Compound> The term "polymer compound" refers to a polymer consisting of one or more types of monomer units, and in particular, a polymer having a molecular weight distribution and a number average molecular weight in terms of polystyrene of 1×10 3 or more (for example, 1 x 10 3 ~1 x 10 8 The polymer compound may be any of a block copolymer, a random copolymer, an alternating copolymer, a graft copolymer, or other forms.
[0026] The polymeric compound having a host group and / or a guest group according to the present disclosure may be a polymer consisting of a single monomer unit, or may be a copolymer, a block copolymer, or a graft copolymer.
[0027] <Host Group and Guest Group> "Host-guest interaction" refers to a bond formed between a host group and a guest group. The host group binds to the guest group by including the guest group. A host-guest interaction occurs when the size of the guest group is suitable for incorporation into the internal space of the host group and the host group and the guest group have an interaction involving at least one of hydrophobic interaction, hydrogen bonding, electrostatic interaction, and coordinate bonding.
[0028] (Host Group) The host group is preferably a cyclic oligosaccharide (cyclodextrin, CD), specifically, α-cyclodextrin, β-cyclodextrin, and γ-cyclodextrin. When these groups are used as the host group, particularly stable host-guest interactions can be formed.
[0029] (Guest Group) The guest group is not particularly limited as long as it is a group that can act as a guest group for the corresponding host group. Examples of the guest group include alkyl groups and aryl groups. Examples of the guest group include trialkylsilyl groups (e.g., trimethylsilyl groups, triethylsilyl groups, and tripropylsilyl groups, particularly trimethylsilyl groups). These guest groups may have a substituent.
[0030] Among the guest groups, examples of the alkyl group include linear, branched, or cyclic C1-18 alkyl groups. The alkyl group is preferably an alkyl group having 3 to 18 carbon atoms, more preferably an alkyl group having 5 to 16 carbon atoms, and these are preferably linear. Specific examples include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, cyclopentyl, hexyl, cyclohexyl, isohexyl, heptyl, octyl, dodecyl, octadecyl, and adamantyl. The alkyl group may have 1 to 3 substituents, such as a halogen atom (e.g., fluorine, chlorine, bromine, etc.), a carboxyl group, an ester group, an amide group, or an optionally protected hydroxyl group. The alkyl group may also be an alkyl group to which ferrocene, an organometallic complex, is bonded as a substituent.
[0031] Among the guest groups, the aryl group includes, for example, a monocyclic or bicyclic or more cyclic aryl group, preferably an aryl group having 6 to 18 carbon atoms, more preferably an aryl group having 6 to 12 carbon atoms, and specific examples thereof include phenyl, toluyl, xylyl, naphthyl, anthryl, phenanthryl, etc. This aryl group may have 1 to 3 substituents such as an alkyl group (e.g., a C1 to 18 alkyl group), a halogen atom (e.g., fluorine, chlorine, bromine, etc.), a carboxyl group, an ester group, an amide group, an azo group having an aryl group, or an optionally protected hydroxyl group.
[0032] (Combination of Host Group and Guest Group) In one embodiment according to the present disclosure, with regard to the host group and the guest group in the composition, the host group is α-cyclodextrin, β-cyclodextrin, or γ-cyclodextrin, and / or the guest group is (1) a linear alkyl group having 4 to 18 carbon atoms, (2) a linear alkyl group having 4 to 18 carbon atoms and having a hydroxyl group, (3) a linear alkyl group having 4 to 18 carbon atoms and having a carboxyl group, (4) a linear alkyl group having 4 to 18 carbon atoms and having an amino group, (5) a cyclic alkyl group, (6) a phenyl group, (7) an azobenzene group, (8) a cinnamic acid group, (1') a t-butyl group, (2') an adamantyl group, (3') an aryl group, (4') an aryl group having a hydroxyl group, (5') an aryl group having a carboxyl group, (6') an aryl group having an amino group, (7') a phenyl group, (8 ... (8) azobenzene group, (9) dansyl group, (1") alkyl group having up to 18 carbon atoms, (2") alkyl group having up to 18 carbon atoms and having a hydroxyl group, (3") alkyl group having up to 18 carbon atoms and having a carboxyl group, (4") alkyl group having up to 18 carbon atoms and having an amino group, (5") adamantyl group, (6") group having a cluster composed of carbon atoms, (7") dansyl group having an aryl group, (8") ferrocenyl group, and (9") anthracenyl group.
[0033] The guest group is preferably an alkyl group having 5 to 16 carbon atoms, more preferably an alkyl group having 6 to 14 carbon atoms, and particularly preferably an alkyl group having 7 to 12 carbon atoms. These groups are preferably linear.
[0034] <Siloxane Bond> In the composition according to the present disclosure, at least one of the polymer compound having a host group and the polymer compound having a guest group, or the polymer compound having a host group and a guest group, contains a siloxane bond.
[0035] In the siloxane bond according to the present disclosure, the silicon atom (Si) constituting the siloxane bond is preferably a hydrogen atom or R S In this case, R Srepresents an alkyl group, a cycloalkyl group, an alkenyl group, an alkoxy group, a cycloalkoxy group, a hydroxy group, a carboxy group, an aldehyde group, an aryl group, an aryloxy group, or a monovalent heterocyclic group, and these groups may have a substituent; R S When there are a plurality of R, they may be the same or different. S In particular, R may be an alkyl group having 1 to 12 carbon atoms or an aryl group which may have a substituent. S is preferably an alkyl group having 1 to 12 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, and particularly preferably a methyl group.
[0036] Preferably, at least one of the polymer compound having a host group and the polymer compound having a guest group, or the polymer compound having a host group and the guest group, contains a polyorganosiloxane main chain, particularly a polyorganosiloxane.When the polymer compound contained in the composition according to the present disclosure contains a polyorganosiloxane main chain, the chemical stability of the composition may be further improved, and it is also preferable because it shows better solubility in hydrocarbon oils and silicone oils.
[0037] The polymer compound according to the present disclosure may have a polyorganosiloxane unit in the main chain or side chain. When the polymer compound according to the present disclosure contains a polyorganosiloxane unit, the proportion of the polyorganosiloxane unit may be 20% by weight or more, 30% by weight or more, or 40% by weight or more, and / or 100% by weight or less, 90% by weight or less, 80% by weight or less, 70% by weight or less, or 60% by weight or less, based on the entire polymer compound. When the proportion of the polyorganosiloxane unit is within this range, the chemical stability and solubility of the polymer compound are further improved.
[0038] When the composition according to the present disclosure contains a polymer compound having a host group and a polymer compound having a guest group, preferably, both of these polymer compounds contain siloxane bonds in the main chain, and in particular, both are polyorganosiloxanes.
[0039] Examples of polymeric compounds having host groups and / or guest groups according to the present disclosure include polyorganosiloxanes. Other examples include block copolymers of polyorganosiloxanes with vinyl resins, acrylic resins, urethane resins, epoxy resins, polyimide resins, polyester resins, or polycarbonate resins; and graft copolymers in which polyorganosiloxanes are grafted onto vinyl resins, acrylic resins, urethane resins, epoxy resins, polyimide resins, polyester resins, or polycarbonate resins. Other examples include acrylic silicone resins, acrylic-silicone graft copolymers, copolymers of polynorbornene and silicone, copolymers of pullulan and silicone, and the like. These resins and / or polyorganosiloxanes may have substituents other than the host group and / or guest group.
[0040] Examples of polyorganosiloxanes include methylpolysiloxane, phenylpolysiloxane, and methylphenylpolysiloxane. These polysiloxanes may have a substituent other than the host group and / or the guest group. The polymer compound according to the present disclosure particularly preferably has a methylpolysiloxane skeleton.
[0041] (Host Group / Guest Group Content) The ratio of the host group to the guest group in the composition is not particularly limited. H and the number of guest groups N G The ratio (N H / N G ) may be 0.1 to 10, may be 0.2 to 5, 0.3 to 3, or 0.4 to 2.5.
[0042] (Positions of Host Group and Guest Group) In one embodiment of the composition according to the present disclosure, the polymer compound having a host group has the host group on a side chain, and the polymer compound having a guest group has the guest group on a side chain.
[0043] In another embodiment of the composition according to the present disclosure, the polymer compound having a host group has a host group on a side chain, and the polymer compound having a guest group has a guest group at a terminal.
[0044] In yet another embodiment of the composition according to the present disclosure, the polymer compound having a host group has a host group at its terminal, and the polymer compound having a guest group has a guest group on its side chain.
[0045] (Polymer Compounds Not Containing Siloxane Bonds) In one embodiment of the present disclosure, either the polymer compound having a host group or the polymer compound having a guest group contained in the composition does not contain a siloxane bond. In this embodiment, polymer compounds not containing siloxane bonds (hereinafter also referred to as "non-siloxane polymer compounds") include, for example, polymers and copolymers of at least one monomer selected from vinyl compounds, acrylic compounds, olefins, styrenes, acrylic acid esters, and methacrylic acid esters, as well as block copolymers containing these polymers and copolymers, such as vinyl resins, acrylic resins, urethane resins, epoxy resins, polyimide resins, polyester resins, or polycarbonate resins. These resins may have substituents other than the host group and / or guest group. For polymer compounds having a guest group and / or host group and not containing a siloxane bond, see Patent Document 2.
[0046] (Combination of polymer compounds contained in composition) For example, the composition according to the present disclosure may contain at least one of the following (i) to (iv): (i) a siloxane bond-free polymer compound having a host group, and a siloxane bond-containing polymer compound having a guest group; (ii) a siloxane bond-containing polymer compound having a host group, and a siloxane bond-free polymer compound having a guest group; (iii) a siloxane bond-containing polymer compound having a host group, and a siloxane bond-containing polymer compound having a guest group; (iv) a siloxane bond-containing polymer compound having a host group and a guest group.
[0047] <Method for Producing Non-Siloxane Polymer Compound Having a Host Group> A polymer compound having a host group but not containing a siloxane bond (non-siloxane polymer compound having a host group) can be produced by a known method, for example, by the method described in Patent Document 2.
[0048] <Method for Producing Non-Siloxane Polymer Compound Having Guest Group> A polymer compound having a guest group but not containing a siloxane bond (non-siloxane polymer compound having a guest group) can be produced by a known method, for example, by the method described in Patent Document 2. (Crosslinking) In one embodiment of the composition according to the present disclosure, at least one of the polymer compound having a host group and the polymer compound having a guest group, or the polymer compound having a host group and the polymer compound having a guest group, is crosslinked. The crosslinking may be crosslinking by a covalent bond other than host-guest interaction (e.g., siloxane crosslinking).
[0049] Any reaction commonly used for crosslinking main-chain silicones can be used, such as a hydrosilylation reaction in which a hydrosilyl group and a vinyl group are added together in the presence of a catalyst. Condensation reactions can also be used to synthesize crosslinked products.
[0050] <Cyclic Oligosaccharide-Modified Organopolysiloxane> In one preferred embodiment according to the present disclosure, the polymeric compound having a host group, or the polymeric compound having a host group and a guest group, is a cyclic oligosaccharide-modified organopolysiloxane that is an addition reaction product of the following components A and B: (A) an organohydrogenpolysiloxane having one or more hydrosilyl groups per molecule; (B) a cyclic oligosaccharide derivative having an unsaturated group represented by the following general formula 1: (In formula 1, L is an alkenyl group having 2 to 12 carbon atoms, R 1 are independently a group selected from an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 2 represents an alkylene group having 1 to 4 carbon atoms, R 3are independently a group selected from alkyl groups having 1 to 4 carbon atoms or acyl groups having 1 to 4 carbon atoms, a is an integer of 0 to 8, b is an integer of 5 to 7, and x is 0 or 1.
[0051] In a preferred embodiment of the present disclosure, the organohydrogenpolysiloxane used as component A has a kinematic viscosity at 25°C of 50 mm 2 / s or more, and / or the number average molecular weight is 8,000 or more. The kinematic viscosity at 25°C can be measured in accordance with Method 1 of the Viscosity Measurement Method for Quasi-drug Raw Materials.
[0052] Although there is no intention to be limited by theory, it is believed that when the molecular weight of the organohydrogenpolysiloxane is relatively large, the proportion of polymeric compounds having multiple host groups and / or guest groups in one molecule increases, making it easier to form the composition into a film.
[0053] (Addition Reaction) The manner of the addition reaction of Components A and B is not particularly limited and can be carried out by known methods. Specifically, for example, cyclic oligosaccharide-modified organopolysiloxane can be produced by mixing Components A and B, a catalyst, and an optional solvent, and optionally heating and / or stirring the mixture to cause the reaction. Platinum, for example, can be used as the catalyst for the addition reaction. In the addition reaction, the addition reaction proceeds via the hydrosilyl group of Component A and the unsaturated group (e.g., vinyl group) of Component B.
[0054] (Component A) Component A used in forming the addition reaction product is an organohydrogenpolysiloxane having one or more hydrosilyl groups per molecule, such as polyorganohydrogenmethylsiloxane.
[0055] (Component B) Regarding component B used in forming the addition reaction product, in the above formula 1, L is an alkenyl group having 2 to 12 carbon atoms. Preferably, in the above formula 1, L is an alkenyl group having 2 to 8 carbon atoms, 2 to 6 carbon atoms, or 2 to 4 carbon atoms, more preferably CH 3 =CH 2 -CH 2 - or CH 3 =CH2 -, most preferably CH 3 =CH 2 - is.
[0056] In formula 1, R 1 are independently a group selected from an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms. 1 is preferably an alkyl group having 1 to 4 carbon atoms, more preferably an alkyl group having 1 to 2 carbon atoms, and particularly preferably a methyl group.
[0057] In formula 1, R 2 is an alkylene group having 1 to 4 carbon atoms. 2 is preferably —(CH 2 ) 2 - or - (CH 2 ) 3 -, and particularly preferably -(CH 2 ) 3 - is.
[0058] In formula 1, R 3 is a group selected from an alkyl group having 1 to 4 carbon atoms or an acyl group having 1 to 4 carbon atoms. 3 is preferably an acetyl group (Ac group).
[0059] In formula 1, a is an integer of 0 to 8. a is preferably 0 or 1, and particularly preferably 0.
[0060] In formula 1, b is an integer of 5 to 7. Preferably, b is 6.
[0061] In formula 1, x is 0 or 1.
[0062] In a preferred embodiment of the present disclosure, the cyclic oligosaccharide-modified organopolysiloxane, which is an addition reaction product of the above-mentioned Components A and B, is an addition reaction product of (Component C) an α-olefin having 2 to 16 carbon atoms in addition to the above-mentioned Components A and B.
[0063] An example of the α-olefin having 2 to 16 carbon atoms is 1-octene.
[0064] In a preferred embodiment according to the present disclosure, at least one of the polymer compound having a host group and the polymer compound having the guest group, or the polymer compound having a host group and a guest group, is represented by the following formula 2: (In formula 2, R 4 are independently a group selected from an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 5 are independently an alkyl group having 5 to 16 carbon atoms; R 6 are independently a group having a cyclic oligosaccharide structure represented by the following formula 3, and R 7 are independently R 4 or R 6 is a group selected from the groups described above with respect to (c), where c is an integer of 100 to 600, d is an integer of 0 to 50, e is an integer of 0 to 50, and f is an integer of 0 to 20. However, at least either e or d is 1 or greater, and the range of c+d+e is satisfied, i.e., c+d+e=10 to 700, and the bonding order of the siloxane units bounded by c, d, e, and f may be block or random.
[0065] When d=1 to 50 and e=0, the compound represented by formula 2 is a polymer compound having a guest group.
[0066] Such a polymeric compound having a guest group can be produced, for example, by adding a compound such as an alkene to an organopolysiloxane having a Si—H group. The alkene is preferably an alkene having 5 to 16 carbon atoms. A platinum catalyst, for example, can be used as a catalyst for the addition reaction.
[0067] When d=0 and e=1 to 50, the compound represented by formula 2 is a cyclic oligosaccharide-modified organopolysiloxane, and is a polymer compound having a host group.
[0068] When d=1 to 50 and e=1 to 50, the compound represented by formula 2 is a cyclic oligosaccharide-modified organopolysiloxane, which is a polymeric compound having a host group and a guest group.
[0069] The specific method for producing such a polymeric compound having a host group or a polymeric compound having a host group and a guest group is not particularly limited, but it can be produced, for example, by the method described above for the cyclic oligosaccharide-modified organopolysiloxane, which is the addition reaction product of components A and B.
[0070] In formula 2, R 4 is preferably a group selected from an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms. 4 is more preferably an alkyl group having 1 to 4 carbon atoms, and particularly preferably a methyl group.
[0071] In formula 2, R 5 is an alkyl group having 5 to 16 carbon atoms. 5 is preferably an alkyl group having 6 to 12 carbon atoms, more preferably an alkyl group having 6 to 10 carbon atoms, and particularly preferably an alkyl group having 7 to 9 carbon atoms.
[0072] In formula 2, R 7 is R 4 or R 6 is a group selected from the groups described above with respect to R 7 is preferably an alkyl group having 1 to 4 carbon atoms, more preferably a methyl group.
[0073] In formula 2, c is an integer of 100 to 600. c is preferably 200 to 580, more preferably 300 to 550, and particularly preferably 400 to 500.
[0074] In formula 2, d is an integer of 0 to 50. d is preferably 1 to 50, more preferably 1 to 20, and particularly preferably 2 to 10.
[0075] In formula 2, e is an integer of 0 to 50. e is preferably 1 to 50, more preferably 1 to 20, and particularly preferably 2 to 10.
[0076] In formula 2, f is an integer of 0 to 20. f is preferably 0 to 10, more preferably 0 to 5, and particularly preferably f=0.
[0077] In formula 2, R6 are independently a group having a cyclic oligosaccharide structure represented by the following formula 3: (In Formula 3, L' is an alkylene group having 2 to 12 carbon atoms, and R 1 , R 2 , R 3 , a, b, and x are as described above with respect to Formula 1. * indicates a bond to the silicon atom of the siloxane unit.
[0078] In Formula 3, L' is an alkylene group having 2 to 12 carbon atoms. Preferably, L' is an alkylene group having 2 to 8 carbon atoms, 2 to 6 carbon atoms, or 2 to 4 carbon atoms, and most preferably -(CH 2 ) 3 - is.
[0079] In formula 3, R 1 , R 2 , R 3 For the values and preferred ranges of a, b, and x, see the description of Formula 1 above.
[0080] In a particularly preferred embodiment of the present disclosure, in the above formula 3, R 1 is a methyl group, R 3 is an acetyl group, and / or in the above formula 2, R 4 and R 7 are all methyl groups.
[0081] In a preferred embodiment of the present disclosure, the cyclic oligosaccharide-modified organopolysiloxane has a glass transition temperature (Tg) measured by dynamic viscoelasticity measurement of 30 to 130° C. The Tg is preferably 40 to 100° C.
[0082] In one embodiment according to the present disclosure, the composition contains a polymeric compound having a host group and a polymeric compound having a guest group, and the polymeric compound having a host group is the above-mentioned cyclic oligosaccharide-modified organopolysiloxane.
[0083] In a particularly preferred embodiment of the present disclosure, the composition contains a polymeric compound having a host group and a guest group, and the polymeric compound is the above-mentioned cyclic oligosaccharide-modified organopolysiloxane.
[0084] <Uses> The use of the composition according to the present disclosure is not particularly limited, and it can be used, for example, as a cosmetic. The composition according to the present disclosure can be suitably used, in particular, as UV protection cosmetics such as sunscreen emulsions and sunscreen creams; and makeup cosmetics such as base makeup, foundations, concealers, blushers, eye shadows, mascaras, eyeliners, eyebrow pencils, overcoats, and lipsticks.
[0085] When the composition according to the present disclosure is used as a cosmetic, it is believed that the self-repairing properties based on the host-guest interaction result in excellent physical properties such as improved cosmetic wear. Without intending to be limited by theory, for example, when the composition according to the present disclosure is used for a cosmetic coating, the polymer compounds reversibly recombine with each other via the host-guest interaction, thereby sealing scratches in the cosmetic coating (including tiny scratches that cannot be seen with the naked eye), resulting in further improvement in cosmetic wear.
[0086] <<Method for Producing Composition>> The composition according to the present disclosure can be produced by mixing a polymer compound having a host group and / or a guest group and a compound represented by formula DP1.
[0087] The conditions for mixing the polymer compound having a host group and / or a guest group with the compound represented by Formula DP1 are not particularly limited. For example, the mixing temperature, mixing time, mixing means, etc. may be appropriately set.
[0088] The composition according to the present disclosure may further contain a solvent in addition to the above-mentioned components. By further containing a solvent, it is possible to provide a composition that has particularly excellent applicability to a substrate.
[0089] In one embodiment of the composition according to the present disclosure, the composition is in a paste state at room temperature. A paste-like composition can be obtained by selecting a polymer compound that is in a paste state at room temperature as the polymer compound contained in the composition. Alternatively, a liquid composition may be obtained by dissolving the polymer compound in a solvent. A composition that is in a liquid or paste state at room temperature is particularly preferred because it is relatively easy to form a film.
[0090] Examples of polymeric compounds that are liquid at room temperature include polymeric compounds having polyorganosiloxane in the main chain, particularly dimethylpolysiloxane.
[0091] <Solvent> The solvent that can be contained in the composition is not particularly limited, but examples thereof include water, alcohols, silicones, hydrocarbon compounds, ester compounds, ethers, and waxes.
[0092] Alcohols include glycerin, butylene glycol (BG), propylene glycol (PG), dipropylene glycol (DPG), polyethylene glycol (PEG), ethanol, and oleyl alcohol.
[0093] Examples of silicones include dodecamethylcyclohexasiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, dimethylpolysiloxane, caprylyl methicone, methylpolysiloxane, methylphenylpolysiloxane, cyclopentasiloxane, aminoethylaminopropylmethylsiloxane-dimethylsiloxane copolymer, aminopropyldimethicone, methyltrimethicone, tris(trimethylsilyl)methylsilane, tetrakis(trimethylsilyl)silane, amodimethicone, and cyclomethicone. Among these, one or more selected from decamethylcyclopentasiloxane and dimethylpolysiloxane are more preferred, and dimethylpolysiloxane with a degree of polymerization of 10 or less is even more preferred.
[0094] Examples of hydrocarbon compounds include hydrogenated polyisobutene, petrolatum, mineral oil, squalane, paraffin, isoparaffin, alkyl benzoate, polyisobutene, isododecane, isotridecane, isohexadecane, and light isoparaffins, with isododecane being preferred.
[0095] Examples of the ester compounds include isopropyl palmitate, ethylhexyl palmitate, isopropyl myristate, and octyldodecyl myristate. Examples of the ethers include ethyl perfluorobutyl ether.
[0096] It is particularly preferable that the solvent is volatile. When the composition according to the present disclosure contains a volatile solvent, the solvent evaporates when the composition is applied to a substrate, and the composition becomes a film, so that a resin sheet can be formed relatively easily.
[0097] Examples of volatile solvents include, in addition to the above alcohols, silicones such as dimethylpolysiloxane, methyltrimethicone, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexasiloxane, tris(trimethylsilyl)methylsilane, and tetrakis(trimethylsilyl)silane; hydrocarbon compounds such as isododecane, isotridecane, isohexadecane, light isoparaffin, and hydrogenated polyisobutene; and ethers such as ethyl perfluorobutyl ether.
[0098] The content of the solvent in the composition is not particularly limited and can be appropriately set depending on the types and amounts of the polymer compound and the compound represented by formula DP1.
[0099] The solvent may be present in an amount of 50 to 90% by weight, preferably 55 to 85% by weight, particularly preferably 60 to 80% by weight, based on the total weight of the composition.
[0100] The solvent is preferably contained in an amount of 10 to 1,000 parts by mass, more preferably 100 to 800 parts by mass, and particularly preferably 200 to 600 parts by mass, per 100 parts by mass of the total of the host group- and / or guest group-containing polymer compounds in the composition. In particular, the solvent is contained in an amount of 10 to 1,000 parts by mass, more preferably 100 to 800 parts by mass, and particularly preferably 200 to 600 parts by mass, per 100 parts by mass of the polymer compounds having a host group and a guest group in the composition.
[0101] <Other Additives> The composition according to the present disclosure (particularly a cosmetic composition) may contain other main components besides those described above to the extent that the effects of the present invention are not impaired, and may contain, as appropriate, lower alcohols, higher alcohols, spherical powders, film-forming agents, cooling agents, oily components, surfactants, aqueous components, water-soluble polymers, UV absorbers, moisturizers, browning inhibitors, antioxidants, antifoaming agents, cosmetic ingredients, preservatives, sequestering agents, blood circulation promoters, various extracts, inorganic pigments, organic pigments, minerals, colorants such as organic dyes, pigments, thickeners, pH adjusters, cooling agents, antiperspirants, disinfectants, skin activators, fragrances, etc. The content of these other additives (i.e., other components other than the host group- and / or guest group-containing polymeric compound, the compound represented by Formula DP1, and the solvent) in the composition is preferably 10% by mass or less (more preferably 5% by mass or less, and even more preferably 1% by mass or less) relative to the mass of the total composition.
[0102] Lower alcohols are widely used in cosmetics as usability adjusters and preservative aids, and examples of lower alcohols include ethanol and isopropyl alcohol.
[0103] Examples of spherical powders include inorganic powders such as spherical silicic anhydride, spherical polymethyl methacrylate, spherical cellulose, spherical nylon, spherical polyethylene, and spherical silicone powder.
[0104] When a film-forming agent is additionally contained, the film-forming agent may be an oil-based film-forming agent, which is preferably one that can be dissolved or dispersed in a non-polar volatile solvent, such as a silicone-based film-forming agent such as trimethylsiloxysilicate.
[0105] Examples of the cooling agent include menthol derivatives, camphor derivatives, and essential oils.
[0106] <Resin Sheet> The composition can be formed into a film. When the composition is in the form of a film, the thickness is not particularly limited and can be set to an appropriate thickness depending on the application. For example, the thickness of the composition can be adjusted to 1 nm to 1 cm, and in terms of good film-forming properties, it can be adjusted to 1 μm to 100 μm. When the composition is a cosmetic, by forming it into a film, it can be used as a cosmetic coating film to be applied to the skin, etc.
[0107] The present disclosure also includes a method for producing a resin sheet, which method includes: applying a composition to a substrate and shaping the composition into a sheet (shaping step); and drying the composition shaped into a sheet to form a resin sheet (forming step).
[0108] (Shaping Step) In the shaping step, the composition is applied onto a substrate and shaped into a sheet (or film).
[0109] The substrate is not particularly limited, and may be human skin.
[0110] The specific method for applying the composition to a substrate and forming it into a sheet is not particularly limited, and an appropriate method can be selected depending on the application of the composition, etc. Specifically, for example, the composition can be formed into a sheet by dropping the composition onto a substrate and spreading it with a coater or fingers.
[0111] The composition may be in a paste or liquid form. The composition may be made into a paste or liquid form by containing a solvent, which may improve the applicability.
[0112] (Forming Step) In the forming step, the composition formed into a sheet shape is dried to form a resin sheet. The drying method is not particularly limited, and can be performed by a known method.
[0113] (Decorative Coating Film) Preferably, the resin sheet is a film, particularly a decorative coating film.
[0114] The method for forming the cosmetic composition into a cosmetic coating film is not particularly limited. For example, a cosmetic coating film can be formed by preparing a solution or dispersion of a polymer compound and a compound represented by formula DP1 and applying the solution or dispersion.
[0115] The method for forming the cosmetic coating may include, for example, the following steps: applying the composition to a target (e.g., skin) with a finger and allowing it to dry to form a cosmetic coating.
[0116] The present invention will be specifically described below with reference to examples.
[0117] <<Synthesis Examples and Production Examples>> The following Production Examples 1 and 2 specifically describe the production of Compound E and Compound F. Both Compound E and Compound F are polymeric compounds having a host group and a guest group that can be used in the composition of the present disclosure. Synthesis Examples 1 to 4 specifically describe the synthesis of the compound (Compound B or D) used to produce Compound E or Compound F.
[0118] Synthesis Example 1: Synthesis of cyclic oligosaccharide derivative having unsaturated bonds. 50.0 g of mono-6-O(p-toluenesulfonyl)-β-cyclodextrin (C6-Ts-β-CD) and 500.0 g of allylamine were placed in a four-neck flask equipped with a stirrer, thermometer, reflux condenser, and dropping funnel. After replacing the atmosphere in the flask with nitrogen, the mixture was stirred at 53°C for 7 hours, cooled to room temperature, and stirred overnight. The mixture was concentrated using an evaporator, and 1000 mL of acetonitrile was added to the resulting solid, and the precipitate was collected by filtration. 1000 mL of distilled water was added to dissolve the resulting precipitate, and the resulting solution was added dropwise to 1000 mL of acetonitrile, and the precipitate was collected by filtration. The precipitate was washed with acetone and then dried in a vacuum dryer at 40°C to obtain vinyl-modified compound A (white solid, 42.7 g).
[0119] Synthesis Example 2: Synthesis of Cyclic Oligosaccharide Derivative Having Unsaturated Bonds 30.0 g of vinyl-modified compound A, 110.0 g of acetic anhydride, and 170.0 g of pyridine were charged into a four-neck flask equipped with a stirrer, thermometer, reflux condenser, and dropping funnel. After replacing the atmosphere in the flask with nitrogen, the mixture was stirred at 60 ° C for 7 hours, cooled to room temperature, and stirred overnight. 170 mL of toluene was added to the solution in the flask, washed twice with 170 mL of 1 mM hydrochloric acid and once with 170 mL of saturated saline. The resulting solution was separated and concentrated using an evaporator. The recovered solid was then dissolved in 50 mL of acetone, and the resulting solution was added dropwise to 500 mL of distilled water. The precipitate was collected by filtration. The precipitate was dried in a vacuum dryer at 40 ° C to obtain vinyl-modified compound B (white solid, 31.8 g).
[0120] Synthesis Example 3: Synthesis of cyclic oligosaccharide derivative having unsaturated bonds. 48.0 g of mono-6-O-(p-toluenesulfonyl)-β-cyclodextrin (C6-Ts-β-CD), 300.0 g of 1-vinyl, 3-(3-aminopropyl)tetramethyldisiloxane, and 60.0 g of N,N-dimethylformamide were placed in a four-neck flask equipped with a stirrer, thermometer, reflux condenser, and dropping funnel. After replacing the atmosphere in the flask with nitrogen, the mixture was stirred at 75°C for 7 hours, cooled to room temperature, and stirred overnight. The solution in the flask was added dropwise to 1200 mL of acetonitrile, and the precipitate was collected by filtration. 60.0 g of N,N-dimethylformamide was added to the resulting precipitate to dissolve it, and the resulting solution was added dropwise to 1200 mL of toluene, and the precipitate was collected by filtration. The precipitate was washed with acetone and then dried in a vacuum dryer at 40° C. to obtain a vinyl-modified compound C (white solid, 42.5 g).
[0121] Synthesis Example 4: Synthesis of Cyclic Oligosaccharide Derivative Having Unsaturated Bonds. 42.0 g of the vinyl-modified compound A, 134.4 g of acetic anhydride, and 210.0 g of pyridine were charged into a four-neck flask equipped with a stirrer, thermometer, reflux condenser, and dropping funnel. After purging the flask with nitrogen, the mixture was stirred at 60°C for 7 hours, cooled to room temperature, and stirred overnight. 210 mL of toluene was added to the solution in the flask, washed twice with 210 mL of 1 mM hydrochloric acid and once with 210 mL of saturated saline. The resulting solution was separated and concentrated using an evaporator. The recovered solid was then dissolved in 150 mL of toluene, and the resulting solution was added dropwise to 300 mL of hexane. The precipitate was collected by filtration. The precipitate was dried in a vacuum dryer at 40°C to obtain vinyl-modified compound D (white solid, 50.1 g).
[0122] <Production Example 1> A four-neck flask equipped with a stirrer, thermometer, reflux condenser, and dropping funnel was charged with 100.0 g of polyorganohydrogensiloxane represented by the following formula (4) (hydrosilyl group amount: 0.040 mol), 24.9 g of the vinyl-modified compound B (vinyl group amount: 0.012 mol), and 200.0 g of toluene. After replacing the atmosphere in the flask with nitrogen, the temperature was raised to 90°C, and 1.3 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration: 0.5 wt%) was added to the flask, followed by stirring at 90°C for 4 hours. 1 The progress of the reaction was confirmed by the disappearance of the vinyl group peak (5.6-6.1 ppm) by H-NMR. Subsequently, 6.4 g (0.057 mol) of 1-octene and 0.7 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration: 0.5 wt%) were added to the flask and stirred at 90°C for 4 hours. The reaction solution was then cooled to room temperature, and the toluene was distilled off under reduced pressure using an evaporator. The resulting solid was added with 250 g of methanol, and the solid was washed at 50°C. This process was repeated three times. Finally, the solid was dried in a vacuum dryer at 40°C to obtain cyclic oligosaccharide-modified organopolysiloxane E (light brown solid, 119.7 g).
[0123] <Production Example 2> A four-neck flask equipped with a stirrer, thermometer, reflux condenser, and dropping funnel was charged with 128.3 g of polyorganohydrogensiloxane represented by the following formula (4) (hydrosilyl group amount: 0.052 mol), 45.0 g of the vinyl-modified compound D (vinyl group amount: 0.016 mol), and 256.0 g of toluene. After replacing the atmosphere in the flask with nitrogen, the temperature was raised to 90°C, and 1.7 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration: 0.5 wt%) was added to the flask, followed by stirring at 90°C for 2 hours. 1 The progress of the reaction was confirmed by the disappearance of the vinyl group peak (5.6-6.1 ppm) by H-NMR. Subsequently, 8.2 g (0.073 mol) of 1-octene and 0.9 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration 0.5 wt%) were added to the flask and stirred at 90°C for 4 hours. The reaction solution was then cooled to room temperature, and the toluene was distilled off under reduced pressure using an evaporator. The resulting solid was added with 300 g of methanol, and the solid was washed at 50°C. This process was repeated three times. Finally, the solid was dried in a vacuum dryer at 40°C to obtain cyclic oligosaccharide-modified organopolysiloxane F (light brown solid, 148.3 g).
[0124] <<Examples 1 to 5 and Comparative Examples 1 to 6>> In Examples 1 to 5 and Comparative Examples 1 to 6, compositions were prepared from polymers (P1 to P3) having a host group and / or a guest group, additives shown in Table 1 below, and isododecane as a solvent, and the solubility, film-forming ability, and self-repairing ability were evaluated.
[0125] <Production of Polymer P1> Polymer P1 is a polymer represented by the following formula 2, 4 =CH 3 , R 5 = (CH 2 ) 7 CH 3 , R 7 =CH 3 and R 6represented by the following formula H1, and had a structure in which d = 4, e = 4, c = 458, and f = 0. Polymer P1 was produced by the same methods as those described in Synthesis Examples 3 and 4 and Production Example 2 above.
[0126]
[0127] (In Formula H1, * indicates a bond to the silicon atom of the siloxane unit.)
[0128] <Polymer P2> Polymer P2 is a polymer represented by the formula 2 above, where R 4 =CH 3 , R 7 =CH 3 and R 6 represented by the above formula H1, and had a structure in which d = 0, e = 4, f = 3, and c = 458. Polymer P2 was produced in the same manner as in Synthesis Examples 3 and 4 and Production Example 2, except that the hydrosilylation reaction with 1-octene carried out in Production Example 2 was not carried out without adding 1-octene.
[0129] <Preparation of Polymer P3> Polymer P3 is a polymer represented by the formula 2 above, where R 4 =CH 3 , R 5 = (CH 2 ) 7 CH 3 , R 7 =CH 3 , d=4, e=4, c=458, f=0, and R 6 had the structure represented by H2 below: Polymer P3 was produced by the same method as described in Synthesis Examples 1 and 2 and Production Example 1 above.
[0130] (In Formula H2, * indicates a bond to the silicon atom of the siloxane unit.)
[0131] <Compound Represented by Formula DP1> The diphenylsiloxyphenyl trimethicone (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KF56A) used in Examples 1 to 3 and 5 and Comparative Example 6 was one in which x = 1 to 20 and y = 1 to 20 in the following formula DP1.
[0132] The phenyl trimethicone used in Example 4 (manufactured by Dow Toray Industries, Inc., product name: Dowsil SH-556) was represented by the following formula DP1, where x = 0 and y = 1 to 30.
[0133]
[0134] Example 1 (Preparation of Composition) In Example 1, a composition containing 1 part by mass of polymer P1 as a polymeric compound having a host group and a guest group and having a siloxane bond, 0.25 parts by mass of diphenylsiloxyphenyl trimethicone (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KF56A), and 4 parts by mass of isododecane (manufactured by Maruzen Petrochemical Co., Ltd., product name: Marukasol R) as a solvent was prepared. Specifically, the composition according to Example 1 was prepared by heating and mixing at 90°C.
[0135] In polymer P1, the host group is a cyclic oligosaccharide of formula H1 above, and the guest group is an octene group (=R 5 Polymer P1 had a disiloxy bond (—Si—O—Si—) in the linker portion between the silicone main chain and the cyclic oligosaccharide.
[0136] (Solubility) The solubility of the ingredients (polymer compound and diphenylsiloxyphenyl trimethicone) in the solvent (isododecane) was evaluated based on the following evaluation criteria: ◯: All ingredients dissolved Δ: Some ingredients remained undissolved ×: None of the ingredients dissolved.
[0137] (Preparation of Resin Sheet) A resin sheet was prepared from the composition according to Example 1 obtained as described above. Specifically, this composition was heated and mixed at 90°C, poured into a 5 cm x 5 cm mold made of Teflon (registered trademark), and dried overnight in a windy oven at 50°C to solidify, thereby obtaining a resin sheet according to Example 1. The obtained resin sheet was an elastomeric sheet with high elasticity. The thickness of the resin sheet was 0.4 mm.
[0138] (Film-forming ability) Film-forming ability was evaluated according to the following criteria. ⊚: A film could be obtained from the resin composition, and was a clean, continuous film when removed from the mold. ◯: A film could be obtained from the composition, but was somewhat soft when removed from the mold. ◯△: A film could be obtained from the composition, and was soft when removed from the mold, and was easily torn when removed. △: A film could be obtained from the composition, but was very weak and brittle. ×: A film could not be obtained from the composition, or oil bled out onto the surface, making it so brittle that it could not be removed.
[0139] (Evaluation of self-repairing property) The self-repairing property of the obtained resin sheet was evaluated as follows: (1) The resin sheet was cut to form a strip-shaped sheet with a width of 6 mm and a length of 30 mm, and this strip-shaped sheet was cut in the center to form two pieces, and the two pieces were brought into contact with each other via their cut surfaces, and the contacted pieces were sandwiched between overlapping Teflon ("Teflon" is a registered trademark) plates, and the peripheral edges of the overlapping Teflon plates were fixed with clips, and the result was left to stand overnight at room temperature or 50°C to obtain a test specimen. (2) Both ends of the obtained test specimen were held by two grips of a tensile tester, and a tensile stress was applied to the test specimen along the length direction of the test specimen, and the energy required for the test specimen to break (fracture energy kJ / m 3 ) was measured. The test piece broke at the point where the cut surfaces were joined. The repair rate was calculated by calculating the ratio of the fracture energy measured with a strip-shaped film that had not been cut. The repair rate at 50°C in Example 2 was 72%.
[0140] The evaluation results of the self-repairing property are shown in Table 1. The self-repairing property was evaluated according to the following criteria: ◯: When the repair rate was 40% or more △: When the repair rate was 20% or more but less than 40% ×: When the repair rate was less than 20% -: When the self-repairing property could not be evaluated as a film
[0141] The results are shown in Table 1 below.
[0142] In Examples 2 and 3, except that the content of diphenylsiloxyphenyl trimethicone was changed, compositions and resin sheets were formed and evaluated in the same manner as in Example 1. The results are shown in Table 1 below.
[0143] In Example 4, a composition and a resin sheet were formed and evaluated in the same manner as in Example 1, except that phenyl trimethicone was used instead of diphenylsiloxyphenyl trimethicone. The results are shown in Table 1 below.
[0144] In Example 5, except that polymer P3 was used instead of polymer P1, a composition and a resin sheet were formed and evaluated in the same manner as in Example 2. The results are shown in Table 1 below.
[0145] In Comparative Examples 1 to 5, compositions and resin sheets were formed and evaluated in the same manner as in Example 1, except that dimethicone, diphenyldimethicone, triphenyldimethylvinyldisiloxane, pentaphenyltrimethyltrisiloxane, or phenyltrimethicone was used instead of diphenylsiloxytrimethicone. The results are shown in Table 1 below.
[0146] In Comparative Example 6, a composition and a resin sheet were formed and evaluated in the same manner as in Example 2, except that Polymer P2 was used instead of Polymer P1. The results are shown in Table 1 below.
[0147]
[0148] The compositions of Examples 1 to 4 contained a modified silicone (polymer P1) having a cyclic oligosaccharide (cyclodextrin) as a host group and an octyl group as a guest group, as well as diphenylsiloxyphenyl trimethicone or phenyl trimethicone as an additive in a proportion of 4.8% to 16.7% by mass relative to the total composition. As can be seen in Table 1, Examples 1 to 4 exhibited excellent solubility and film-forming properties, and the resin sheets formed from the compositions exhibited excellent self-repairing properties. The modified silicone used in Examples 1 to 4 had a disiloxy bond in the linker portion between the silicone main chain and the cyclic oligosaccharide.
[0149] Furthermore, as can be seen in Table 1, when the composition of Example 5 was used, which had a linker of a linear alkylene group having 3 carbon atoms instead of a disiloxy bond as the linker part between the silicone main chain and the cyclic oligosaccharide, results similar to those of Example 2 were obtained.
[0150] In contrast, the compositions of Comparative Examples 1 to 5, which contained the same polymer P1 as in Examples 1 to 4 but did not contain diphenylsiloxyphenyl trimethicone or phenyl trimethicone, were relatively poor in solubility and / or film-forming ability, and even when resin sheets could be formed from the compositions, the self-repairing properties of the resin sheets were relatively poor. In particular, even when dimethicone having the same viscosity as diphenylsiloxyphenyl trimethicone was used (Comparative Example 1), the same effects as in the Examples were not observed.
[0151] Comparative Example 6 is an example in which a modified silicone (polymer P2) containing diphenylsiloxyphenyl trimethicone but having only a host group and no guest group was used. Although a resin sheet could be formed, the self-repairing properties of the resulting resin sheet were poor.
Claims
1. A composition containing a host body made of a polymeric compound having a host group and a guest body made of a polymeric compound having a guest group, or a host-guest body made of a polymeric compound having a host group and a guest group, and a compound represented by the following chemical formula DP1, wherein at least one of the polymeric compound having a host group and the polymeric compound having a guest group, or the polymeric compound having a host group and a guest group, contains a siloxane bond, and the content of the compound represented by the chemical formula DP1 in the composition is 1% by mass to 25% by mass with respect to the total mass of the composition: (In formula DP1, x is an integer from 0 to 200, and y is an integer from 1 to 200.) 2. The host group is α-cyclodextrin, β-cyclodextrin, or γ-cyclodextrin, and / or the guest group is (1) a linear alkyl group having 4 to 18 carbon atoms, (2) a linear alkyl group having 4 to 18 carbon atoms and a hydroxyl group, (3) a linear alkyl group having 4 to 18 carbon atoms and a carboxyl group, (4) a linear alkyl group having 4 to 18 carbon atoms and an amino group, (5) a cyclic alkyl group, (6) a phenyl group, (7) an azobenzene group, (8) a cinnamic acid group, (1') a t-butyl group, (2') an adamantyl group, (3') an aryl group, (4') an aryl group having a hydroxyl group, (5') an aryl group having a carboxyl group, (6') an aryl group having an amino group, (7') a phenyl group, (8') a phenyl group, (9) a phenyl group, (10) a phenyl group, (11) a phenyl group, (12) a phenyl group, (13) a phenyl group, (14) a phenyl group, (15) a phenyl group, (16) a phenyl group, (17) a phenyl group, (18) a phenyl group, (19) a phenyl group, (20) a phenyl group, (21) a phenyl group, (22) a phenyl group, (23) a phenyl group, (24) a phenyl group, (25) a phenyl group, (26) a phenyl group, (27) a phenyl group, (28) a phenyl group, (29) a phenyl group, (30) a phenyl group, (31) a phenyl group, (32) a phenyl group, (33) a phenyl group, (34) a phenyl group, (35) a phenyl group, (36) a phenyl group, (37) a phenyl group The composition according to claim 1, wherein the aryl group is at least one selected from the group consisting of a ferrocenyl group, (8') an azobenzene group, (9') a dansyl group, (1'') an alkyl group having up to 18 carbon atoms, (2'') an alkyl group having up to 18 carbon atoms and a hydroxyl group, (3'') an alkyl group having up to 18 carbon atoms and a carboxyl group, (4'') an alkyl group having up to 18 carbon atoms and an amino group, (5'') an adamantyl group, (6'') a group having a cluster constituted of carbon atoms, (7'') a dansyl group having an aryl group, (8'') a ferrocenyl group, and (9'') an anthracenyl group.
3. The composition according to claim 1 or 2, wherein the polymeric compound having a host group or the polymeric compound having a host group and a guest group is a cyclic oligosaccharide-modified organopolysiloxane which is an addition reaction product of the following A and B: (A) an organohydrogenpolysiloxane having one or more hydrosilyl groups in one molecule; (B) a cyclic oligosaccharide derivative having an unsaturated group represented by the following general formula 1: (In formula 1, L is an alkenyl group having 2 to 12 carbon atoms, R 1 are independently selected from an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 2 represents an alkylene group having 1 to 4 carbon atoms, R 3 are independently a group selected from an alkyl group having 1 to 4 carbon atoms or an acyl group having 1 to 4 carbon atoms, a is an integer of 0 to 8, b is an integer of 5 to 7, and x is 0 or 1.
4. The organohydrogenpolysiloxane has a kinetic viscosity of 50 mm at 25°C. 2 4. The composition of claim 3, wherein said copolymer has a molecular weight of 1,000 or more and a number average molecular weight of 8,000 or more.
5. The composition according to claim 3, wherein the cyclic oligosaccharide-modified organopolysiloxane is an addition reaction product of (C) an α-olefin having 2 to 16 carbon atoms in addition to (A) and (B).
6. The composition according to claim 1 or 2, wherein at least one of the polymer compound having a host group and the polymer compound having a guest group, or the polymer compound having a host group and a guest group, is represented by the following formula 2: (In formula 2, R 4 are independently selected from an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 5 are independently an alkyl group having 5 to 16 carbon atoms; R 6 are independently a group having a cyclic oligosaccharide structure represented by the following formula 3, R 7 are independently R 4 Or R 6 is a group selected from the groups described above with respect to c, c being an integer of 100 to 600, d being an integer of 0 to 50, e being an integer of 0 to 50, and f being an integer of 0 to 20. However, at least one of d and e is 1 or more, and the range of c+d+e=101 to 700 is satisfied, and the bonding order of the siloxane units bounded by c, d, e, and f may be block or random. (In formula 3, L' is an alkylene group having 2 to 12 carbon atoms, R 1 are independently selected from an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 2 represents an alkylene group having 1 to 4 carbon atoms, R 3 are independently a group selected from an alkyl group having 1 to 4 carbon atoms or an acyl group having 1 to 4 carbon atoms, a is an integer of 0 to 8, b is an integer of 5 to 7, and x is 0 or 1. * is a free group that bonds to the silicon atom of the siloxane unit.
7. In the above formula 3, R 1 is a methyl group, R 3 is an acetyl group, and in the formula 2, R 4 and R 7 The composition of claim 6 , wherein is a methyl group.
8. The composition according to claim 6, wherein in formula 3, x is 0.
9. The composition according to claim 6, wherein the polymer compound having a host group or the polymer compound having a host group and a guest group is represented by formula 2, in which e=1 to 50.
10. The composition according to claim 6, wherein the polymer compound represented by formula 2 has a glass transition temperature of 30 to 130° C. as measured by dynamic viscoelasticity measurement.
11. The composition of claim 1 or 2, further comprising a solvent.
12. The composition of claim 11, wherein the solvent is a volatile silicone or a volatile hydrocarbon compound.
13. A composition according to claim 1 or 2 for use as a cosmetic preparation.
14. A method for producing a resin sheet, comprising: applying the composition according to claim 1 or 2 onto a substrate and shaping the composition into a sheet; and drying the composition shaped into a sheet to form a resin sheet.
15. The method of claim 14, wherein the resin sheet is a film.
Citation Information
Patent Citations
COMPLEX OF beta- OR gamma-CYCLODEXTRIN AND alpha-TOCOPHEROL AND METHOD FOR PRODUCING THE SAME AND COSMETIC CONTAINING THE SAME
JP2003238402A
Cosmetic
JP2015105249A
Water-in-oil emulsion cosmetic
JP2022064534A
Aqueous dispersed composition
WO2013145870A1
Cited By
Method for producing cyclic oligosaccharide-modified organopolysiloxane
JP2024162026A
Method for producing cyclic oligosaccharide-modified organopolysiloxanes
JP7863067B2