Epoxy resin composition
The epoxy resin composition, featuring epoxy resin, solid castor oil particles, and a curing agent, addresses the strength issues in epoxy resin compositions by integrating the plasticizer, resulting in improved tensile shear adhesive strength and environmental sustainability.
Patent Information
- Application Number
- PCT/JP2024/016893
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-09
- Filing Date
- 2024-05-02
- Publication Date
- 2024-11-14
AI Technical Summary
Epoxy resin compositions containing plasticizers face challenges in achieving high tensile shear adhesive strength due to plasticizer bleeding and lack of incorporation into the crosslinked network, resulting in reduced strength at the interface between adherends and cured products.
An epoxy resin composition is developed with specific components, including epoxy resin, solid castor oil particles, and a curing agent or accelerator, which improves tensile shear adhesive strength by incorporating the plasticizer into the network and maintaining stability.
The composition enhances tensile shear adhesive strength and maintains storage stability while being environmentally friendly with a high biomass content, improving the bonding performance of epoxy resin compositions.
Smart Images

Figure JPOXMLDOC01-APPB-M000002 
Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Epoxy resin composition
[0001] The present invention relates to an epoxy resin composition.
[0002] It is known that a plasticizer is added to an epoxy resin composition to impart flexibility and toughness to the cured product, and such an epoxy resin composition is used for so-called structural adhesion to bond vehicle body structures, as disclosed in JP-A-2020-533441.
[0003] However, because plasticizers do not have functional groups, they are not incorporated into the crosslinked network of the curable resin. Furthermore, plasticizers are generally liquid at 25°C. For these reasons, when an epoxy resin composition cures, the plasticizer often bleeds out onto the surface of the cured product, resulting in the plasticizer remaining at the interface between the adherend and the cured product, which reduces the tensile shear bond strength. Therefore, it has been difficult to improve the tensile shear bond strength of epoxy resin compositions containing plasticizers.
[0004] As a result of intensive investigations aimed at solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by preparing an epoxy resin composition containing the specified components (A) to (C) in specified amounts, and have thus completed the present invention.
[0005] The gist of the present invention is described below. A first aspect of the present invention is an epoxy resin composition comprising the following components (A) to (C), with 10 to 50 parts by mass of component (B) per 100 parts by mass of component (A): Component (A): epoxy resin Component (B): castor oil particles that are solid at 25°C Component (C): curing agent and / or curing accelerator.
[0006] A second aspect of the present invention is the epoxy resin composition according to the first aspect, wherein the average particle size of component (B) is 5 to 20 μm.
[0007] A third aspect of the present invention is the epoxy resin composition according to the first or second aspect, wherein the component (C) contains an epoxy adduct compound.
[0008] A fourth aspect of the present invention is the epoxy resin composition according to any one of the first to third aspects, further comprising a filler (excluding the above-mentioned component (B)) as component (D).
[0009] A fifth aspect of the present invention is the epoxy resin composition according to the fourth aspect, which contains 0.1 to 200 parts by mass of the component (D) per 100 parts by mass of the component (A).
[0010] A sixth aspect of the present invention is the epoxy resin composition according to the fourth or fifth aspect, wherein the component (D) is an inorganic powder derived from a natural marine product.
[0011] A seventh aspect of the present invention is the epoxy resin composition according to any one of the fourth to sixth aspects, wherein the average particle size of the component (D) is 1 to 20 μm.
[0012] An eighth aspect of the present invention is the epoxy resin composition according to any one of the first to seventh aspects, wherein the biomass degree is 10 or more.
[0013] Hereinafter, embodiments of the present invention will be described. However, the present invention is not limited to only the following embodiments. Furthermore, in this specification, unless otherwise specified, operations and measurements of physical properties are performed under conditions of room temperature (20°C or higher and 25°C or lower) and relative humidity of 40% RH or higher and 50% RH or lower.
[0014] The details of the present invention will now be described.
[0015] One embodiment of the present invention is an epoxy resin composition comprising the following components (A) to (C), with 10 to 50 parts by mass of component (B) per 100 parts by mass of component (A): component (A): epoxy resin, component (B): castor oil particles that are solid at 25°C, and component (C): curing agent and / or curing accelerator.
[0016] According to the present invention, an epoxy resin composition containing a plasticizer can be obtained that improves the tensile shear adhesive strength.
[0017] <Component (A)> The component (A) that can be used in the present invention is an epoxy resin. The component (A) is an epoxy resin that does not contain the component (B) described below. Preferably, the component (A) is a compound having two or more epoxy groups per molecule. The component (A) may be a single compound or a mixture of two or more compounds. The component (A) is preferably liquid at 25°C. The component (A) may be obtained by dissolving an epoxy resin that is solid at 25°C in an epoxy resin that is liquid at 25°C. The epoxy resin preferably has a chloride ion concentration (also referred to as total chlorine content) of 1000 ppm by mass or less, more preferably 700 ppm by mass or less, even more preferably 600 ppm by mass or less, and even more preferably 500 ppm by mass or less. A chloride ion concentration (total chlorine content) of 1000 ppm by mass or less allows the resin to maintain storage stability. The lower limit of the chloride ion concentration (total chlorine content) is not particularly limited, but is, for example, 10 ppm by mass or more. The epoxy resin preferably has a halogen ion concentration (total concentration of halogen ions such as chloride ions, fluoride ions, bromide ions, and iodide ions, also referred to as total halogen amount) of 1000 mass ppm or less, more preferably 700 mass ppm or less, even more preferably 600 mass ppm or less, and even more preferably 500 mass ppm or less. When the halogen ion concentration (total halogen amount) is 1000 mass ppm or less, storage stability can be maintained. The lower limit of the halogen ion concentration (total halogen amount) is not particularly limited, but is, for example, 10 mass ppm or more.
[0018] Specific examples of component (A) include glycidyl ether epoxy resins obtained by condensation of epichlorohydrin with polyhydric phenols such as bisphenols or polyhydric alcohols, such as bisphenol A, brominated bisphenol A, hydrogenated bisphenol A, bisphenol F, bisphenol S, bisphenol AF, biphenyl, naphthalene, fluorene, novolac, phenol novolac, orthocresol novolac, tris(hydroxyphenyl)methane, and tetraphenylolethane. Other examples include glycidyl ester epoxy resins obtained by condensation of epichlorohydrin with carboxylic acids such as phthalic acid derivatives or fatty acids, glycidyl amine epoxy resins obtained by reaction of epichlorohydrin with amines, cyanuric acids, or hydantoins, and epoxy resins modified by various methods, but are not limited to these.
[0019] Commercially available epoxy resins include, but are not limited to, 827, 828EL, etc. manufactured by Mitsubishi Chemical Corporation, EPICLON (registered trademark) 830, EXA-835LV, etc. manufactured by DIC Corporation, and Epotohto YD-128, YDF-170, etc. manufactured by Nippon Steel Chemical & Material Co., Ltd. In terms of cost, epoxy resins having a bisphenol A skeleton or a bisphenol F skeleton are preferred, and from the viewpoint of being able to maintain a liquid state at 25°C as a raw material, a mixture of an epoxy resin having a bisphenol A skeleton (bisphenol A-type epoxy resin) and an epoxy resin having a bisphenol F skeleton (bisphenol F-type epoxy resin) is preferred.
[0020] The content of component (A) in the epoxy resin composition of this embodiment is not particularly limited, but is, for example, 20 to 80 parts by mass, and preferably 30 to 70 parts by mass, relative to 100 parts by mass of the total mass of the epoxy resin composition. When the epoxy resin composition contains two or more types of component (A), the content of component (A) means the total content of these.
[0021] <Component (B)> The component (B) that can be used in the present invention is castor oil particles that are solid at 25°C. The epoxy resin composition of this embodiment contains 10 to 50 parts by mass of the component (B) per 100 parts by mass of the component (A). When the epoxy resin composition contains two or more types of the component (A), the content of the component (A) refers to the total content of these components. When the epoxy resin composition contains two or more types of the component (B), the content of the component (B) refers to the total content of these components. Here, castor oil is a triglyceride formed by esterification of a fatty acid and glycerin. For example, approximately 90% of the fatty acid may be composed of ricinoleic acid. Examples of castor oil include modified castor oils such as hydrogenated castor oil and hydrogenated castor oil, but are not limited to these. Hydrogenated castor oil or hydrogenated castor oil is preferred, with hydrogenated castor oil being more preferred. The castor oil used as component (B) is not particularly limited, but preferably does not contain reactive functional groups such as epoxy groups. Among the castor oils used as component (B), those containing reactive functional groups such as epoxy groups are excluded from component (A). Furthermore, component (B) preferably exists in an epoxy resin composition in a state in which it is incompatible with other components at 25°C. The average particle size of component (B) is not particularly limited, but is preferably 50 μm or less, more preferably 5 to 20 μm, even more preferably 8 to 20 μm, and particularly preferably 8 to 12 μm. In this specification, the term "average particle size" refers to the 50% particle size (D50 value; also referred to as the 50% average particle size) in the number-integrated distribution measured using a laser diffraction particle size analyzer.
[0022] Specific examples of component (B) include, but are not limited to, hydrogenated castor oil particles such as NatureFine H325 manufactured by MP Gokyo Food & Chemical Co., Ltd., and hydrogenated castor oil particles such as A-S-A T-20SF manufactured by Ito Oil Mills, Ltd.
[0023] Here, component (B) preferably contains biomass (resources that are organic matter derived from plants and animals (excluding crude oil, petroleum gas, combustible natural gas, and coal)), and more preferably consists of biomass. The biomass degree of component (B) is not particularly limited. The biomass degree of component (B) can be a value obtained by multiplying the mass proportion of components derived from biomass contained in component (B) by 100.
[0024] In the epoxy resin composition of this embodiment, the content of component (B) is 10 to 50 parts by mass, preferably 10 to 45 parts by mass, and more preferably 10 to 40 parts by mass, per 100 parts by mass of component (A). If the content of component (B) is less than 10 parts by mass per 100 parts by mass of component (A), sufficient tensile shear bond strength cannot be obtained, while if it exceeds 50 parts by mass, the viscosity cannot be sufficiently reduced. Furthermore, although component (B) corresponds to a plasticizer, the epoxy resin composition preferably does not contain any plasticizer other than component (B) in order to avoid a decrease in tensile shear bond strength. According to one embodiment, the epoxy resin composition preferably does not contain any biodegradable resin such as poly(hydroxybutyrate-co-valerate) (PHBV), or particles such as polyethylene wax, carnauba wax, or rice wax.
[0025] Furthermore, since component (B) is a plasticizer, toughness can be imparted to the epoxy resin composition by including component (B) in a predetermined content.
[0026] <Component (C)> The component (C) that can be used in the present invention is a curing agent and / or curing accelerator (particularly a latent curing agent). Examples of curing agents include polyamine compounds, polyphenol compounds, polythiol compounds, and acid anhydrides. A curing accelerator can be further used to improve the reactivity of the epoxy resin composition of this embodiment. Alternatively, a curing accelerator may be used alone as component (C). The curing agent and curing accelerator may each be liquid or solid (including powder) at 25°C.
[0027] The polyamine compound is not particularly limited as long as it is a compound having two or more amino groups. The two or more amino groups in the polyamine compound may be primary amino groups, secondary amino groups, or tertiary amino groups. Specific examples of polyamine compounds include, but are not limited to, diethylenetriamine, triethylenetetramine, m-xylylenediamine, isophoronediamine, 1,3-bisaminomethylcyclohexane, 4,4'-diaminodiphenylmethane, m-phenylenediamine, diaminodiphenylsulfone, dicyandiamide, and organic acid dihydrazides. The polyamine compound is preferably liquid at 25°C. These polyamine compounds can also be used as curing accelerators.
[0028] Specific examples of polyphenol compounds include, but are not limited to, novolac-type phenolic resins obtained by reacting phenols such as phenol and alkylphenols with aldehydes such as formaldehyde and paraformaldehyde, as well as polyhydric phenolic resins such as zylog-type phenolic resins, dicyclopentadiene-type phenolic resins, and polyfunctional phenolic resins, which are modified phenol novolac resins. The polyphenol compound is preferably liquid at room temperature. The polyphenol compound is preferably liquid at 25°C.
[0029] The polythiol compound is not particularly limited as long as it is a compound having two or more thiol groups. Specific examples of the polythiol compound include trimethylolpropane tristhiopropionate, pentaerythritol tetrakisthiopropionate, ethylene glycol bisthioglycolate, 1,4-butanediol bisthioglycolate, trimethylolpropane tristhioglycolate, pentaerythritol tetrakisthioglycolate, di(2-mercaptoethyl)ether, 1,4-butanedithiol, 1,3,5-trimercaptomethylbenzene, 1,3,5-trimercaptomethyl-2,4,6-trimethylbenzene, terminal thiol group-containing polyethers, terminal thiol group-containing polythioethers, thiol compounds obtained by reacting an epoxy compound with hydrogen sulfide, and thiol compounds having terminal thiol groups obtained by reacting a polythiol compound with an epoxy compound, but are not limited thereto. The polythiol compound is preferably liquid at 25°C.
[0030] Specific examples of acid anhydrides include, but are not limited to, cyclic acid anhydrides such as dodecenyl succinic anhydride, polyazelaic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenonetetracarboxylic anhydride, tetrabromophthalic anhydride, and hexahydrophthalic anhydride. The acid anhydride is preferably liquid at 25° C.
[0031] In order to promote the reactivity of the curing agent, a tertiary amine compound or the like may be used as a curing accelerator (latent curing agent). In some cases, the curing accelerator alone can be used as the curing agent. Curing accelerators are generally solid at room temperature, and examples include fine powders obtained by pulverizing a solid compound having an imidazole skeleton or fine powders obtained by pulverizing an epoxy adduct compound. Commonly known examples of epoxy adduct compounds include those in which a tertiary amine is added to an epoxy resin to stop the reaction midway (epoxy adduct compounds in which an epoxy resin and a tertiary amine compound have reacted partway through).
[0032] From the viewpoint of enhancing dispersibility in the epoxy resin, the curing agent and / or curing accelerator of component (C) preferably has an average particle size of 1.0 to 50 μm, more preferably 1.0 to 10 μm, even more preferably 2 to 8 μm, and most preferably 3 to 7 μm.
[0033] The epoxy resin composition of this embodiment preferably contains an epoxy adduct compound (excluding component (A)) as component (C). The epoxy resin composition of this embodiment can use an epoxy adduct-based latent curing agent containing an epoxy adduct compound as component (C).
[0034] The epoxy resin composition of this embodiment may use a commercially available epoxy adduct latent curing agent as component (C). Examples of commercially available epoxy adduct latent curing agents include PN-23 from the Amicure series manufactured by Ajinomoto Fine-Techno Co., Ltd., FXR-1081 and FXR-1020 from the Fujicure series manufactured by T&K Toka Corporation, and HXA3932HP from the Novacure series manufactured by Asahi Kasei Corporation. Also known as curing accelerators that are liquid at room temperature are organic phosphorus compounds, organic amine compounds, and imidazole derivative compounds.
[0035] In the epoxy resin composition of this embodiment, the content of component (C) is preferably 1 to 30 parts by mass, more preferably 5 to 30 parts by mass, even more preferably 10 to 30 parts by mass, and even more preferably 15 to 25 parts by mass, per 100 parts by mass of component (A). When the content of component (C) is 1 part by mass or more per 100 parts by mass of component (A), curability is exhibited, and when it is 30 parts by mass or less, storage stability can be maintained. When the epoxy resin composition contains two or more types of component (A), the content of component (A) refers to the total content of these. When the epoxy resin composition contains two or more types of component (C), the content of component (C) refers to the total content of these.
[0036] <Component (D)> The component (D) that can be used in the present invention is a filler. However, the component (D) does not include the component (B). The epoxy resin composition of this embodiment may or may not contain the component (D) in the mixture of the components (A) to (C). By including the component (D), the elastic modulus, fluidity, etc. of the cured product obtained by curing the epoxy resin composition can be improved. Examples of fillers include, but are not limited to, organic powders and inorganic powders. From the viewpoint of improving tensile shear adhesive strength, the component (D) is preferably an inorganic powder.
[0037] Examples of inorganic powders include, but are not limited to, glass powder, fumed silica powder, alumina powder, mica powder, ceramic powder, silicone rubber powder, calcium carbonate powder, aluminum nitride powder, carbon powder, kaolin clay, dried clay minerals, and dried diatomaceous earth. These may be used alone or in combination of two or more. Considering the environment, component (D) is preferably an inorganic powder derived from natural marine products. Among these, uncalcined scallop shell powder (calcium carbonate powder) is more preferred as the inorganic powder derived from natural marine products, and it is even more preferred that this powder be produced from scallop waste. These may be used alone or in combination of two or more.
[0038] The component (D) preferably contains biomass (resources that are organic matter derived from plants and animals (excluding crude oil, petroleum gas, combustible natural gas, and coal)), and more preferably consists of biomass. The component (D) preferably has a biomass degree of 95 or more, and more preferably 100. The biomass degree of the component (D) can be calculated by multiplying the mass proportion of components derived from biomass contained in the component (D) by 100.
[0039] The epoxy resin composition may contain fumed silica powder as one of the inorganic powders, and the fumed silica powder can be blended for the purpose of adjusting the viscosity of the epoxy resin composition or improving the mechanical strength of the cured product of the epoxy resin composition. As the fumed silica powder, fumed silica surface-treated with dimethylsilane, trimethylsilane, alkylsilane, methacryloxysilane, organochlorosilane, polydimethylsiloxane, hexamethyldisilazane, or the like is preferably used. Commercially available fumed silica powders include, but are not limited to, Aerosil (registered trademark) R972, R972V, R972CF, R974, R976, R976S, R9200, RX50, NAX50, NX90, RX200, RX300, R812, R812S, R8200, RY50, NY50, RY200S, RY200, RY300, R104, R106, R202, R805, R816, T805, R711, RM50, and R7200 (manufactured by Nippon Aerosil Co., Ltd.). These may be used alone or in combination of two or more.
[0040] The epoxy resin composition may contain a conductive filler as one of the inorganic powders. Examples of conductive fillers include, but are not limited to, gold, silver, platinum, nickel, palladium, and plated particles in which organic polymer particles are coated with a thin metal film. These may be used alone or in combination of two or more.
[0041] Examples of organic powders other than component (B) include, but are not limited to, polyethylene powder, polypropylene powder, nylon powder, cross-linked acrylic powder, cross-linked polystyrene powder, polyester powder, polyvinyl alcohol powder, polyvinyl butyral powder, polycarbonate powder, etc. These may be used alone or in combination of two or more.
[0042] In order not to impair the storage stability of the epoxy resin composition of this embodiment, the content of component (D) is preferably 0.1 to 200 parts by mass, more preferably 0.1 to 150 parts by mass, even more preferably 50 to 150 parts by mass, even more preferably 80 to 150 parts by mass, even more preferably 100 to 150 parts by mass, even more preferably 110 to 140 parts by mass, and particularly preferably 110 to 130 parts by mass, per 100 parts by mass of component (A). When the epoxy resin composition contains two or more types of component (A), the content of component (A) refers to the total content of these. When the epoxy resin composition contains two or more types of component (D), the content of component (D) refers to the total content of these. Furthermore, in consideration of dispersion in component (A), the average particle size of component (D) is preferably 1 to 20 μm, more preferably 1 to 15 μm, even more preferably 3 to 15 μm, even more preferably 3 to 13 μm, even more preferably 3 to 12 μm, even more preferably 3 to 10 μm, and particularly preferably 4 to 8 μm.
[0043] The epoxy resin composition of the present invention may further contain a storage stabilizer, an antioxidant, a light stabilizer, a heavy metal deactivator, a silane coupling agent, an antifoaming agent, a colorant such as a pigment or a dye, a rust inhibitor, a leveling agent, a dispersant, a rheology modifier, a flame retardant, etc., within the scope of the present invention.
[0044] The storage stabilizer is not particularly limited as long as it improves storage stability, but examples include borate ester compounds, phosphoric acid, alkyl phosphate esters, p-toluenesulfonic acid, etc. Examples of borate ester compounds include trimethyl borate, triethyl borate, tri-n-propyl borate, triisopropyl borate, tri-n-butyl borate, tris(2-ethylhexyloxy)borane, and triphenyl borate. Commercially available borate ester compounds include "Cureduct L-07N" (manufactured by Shikoku Chemicals Corporation). Examples of alkyl phosphate esters that can be used include, but are not limited to, trimethyl phosphate and tributyl phosphate. Storage stabilizers may be used alone or in combination. Considering storage stability, phosphoric acid, tributyl borate, trimethoxyboroxine, or methyl p-toluenesulfonate are preferred. In the epoxy resin composition, the content of the storage stabilizer is preferably 0.01 to 5.0 parts by mass per 100 parts by mass of component (A). When the content of the storage stabilizer is 0.01 parts by mass or more per 100 parts by mass of the component (A), good storage stability is exhibited, and when it is 5.0 parts by mass or less, high curability can be maintained.
[0045] Examples of antioxidants include quinone compounds such as β-naphthoquinone, 2-methoxy-1,4-naphthoquinone, methylhydroquinone, hydroquinone, hydroquinone monomethyl ether, mono-tert-butylhydroquinone, 2,5-di-tert-butylhydroquinone, p-benzoquinone, 2,5-diphenyl-p-benzoquinone, and 2,5-di-tert-butyl-p-benzoquinone; 2,2-methylene-bis(4-methyl-6-tert-butylphenol), catechol, tert-butylcatechol, and 2-butyl-4-hydroxybenzoquinone; Nisole, 2,6-di-tert-butyl-p-cresol, 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate, 4,4'-butylidenebis(6-tert-butyl-3-methylphenol), 4,4'-thiobis(6-tert-butyl-3-methylphenol), 3,9-bis[2-[3-(3-tert-butyl-4-hydroxyphenyl)methyl]phenyl] hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, N,N'-hexane-1,6-diylbis[3-(3,5-di-tert -butyl-4-hydroxyphenyl)propionamide], benzenepropanoic acid, 3,5-bis(1,1-dimethylethyl)-4-hydroxy, C7-C9 side chain alkyl ester, 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl [[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphonate, 3,3',3",5,5',5"-hexa-tert-butyl-a,a',a"-(mesitylene-2,4,6-tolyl)tri-p-cresol, calcium diethylbis[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphonate, 4,6-bis(octylthiomethyl)-o-cresol, ethylene bis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], hexamethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3, 5-triazine-2,4,6(1H,3H,5H)-trione, 1,3,5-tris[(4-tert-butyl-3-hydroxy-2,6-xylyl)methyl]-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, reaction products of N-phenylbenzenamine and 2,4,6-trimethylpentene, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol, picric acid phenols such as citric acid; tris(2,4-di-tert-butylphenyl)phosphite, tris[2-[[2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphen-6-yl]oxy]ethyl]amine, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis[2,4-bis(1,1-dimethylethyl)-6-methylphenyl]ethyl ester phosphorous acid, Phosphorus compounds such as tetrakis(2,4-di-tert-butylphenyl)[1,1-bisphenyl]-4,4'-diylbisphosphonite and 6-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-tert-butyldibenz[d,f][1,3,2]dioxaphosphene; dilauryl 3,3'-thiodipropionate, dimyristyl 3,3'-thiodipropionate, distearyl 3,Examples of suitable compounds include, but are not limited to, sulfur compounds such as 3'-thiodipropionate, pentaerythrityl tetrakis(3-laurylthiopropionate), and 2-mercaptobenzimidazole; amine compounds such as phenothiazine; lactone compounds; and vitamin E compounds. These compounds may be used alone or in combination of two or more. Of these, phenols are preferred.
[0046] Examples of silane coupling agents include, but are not limited to, γ-chloropropyltrimethoxysilane, octenyltrimethoxysilane, glycidoxyoctyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, γ-ureidopropyltriethoxysilane, and p-styryltrimethoxysilane. These may be used alone or in combination of two or more. The content of the silane coupling agent is preferably 0.05 to 30 parts by mass, more preferably 0.2 to 10 parts by mass, per 100 parts by mass of component (A).
[0047] The dispersant is not particularly limited, but a wetting dispersant can be preferably used. Commercially available dispersants include, but are not limited to, DISPERBYK (registered trademark)-111, BYK-019, BYK-020, BYK-023, BYK-024, BYK-065, BYK-066, BYK-067, BYK-070, BYK-088, and BYK-080A manufactured by BYK Corporation. These dispersants may be used alone or in combination of two or more. The content of the dispersant is not particularly limited, but is, for example, 0.1 to 10 parts by mass, preferably 0.5 to 5 parts by mass, and more preferably 1 to 3 parts by mass, per 100 parts by mass of component (A). Examples of colorants include pigments and dyes, with pigments being preferred from the viewpoint of durability. Among pigments, black pigments are preferred. Examples of black pigments include carbon black, black titanium oxide, copper chromium black, cyanine black, and aniline black. There are no particular restrictions on the amount of colorant contained, but it is, for example, 0.01 to 10 parts by mass, and preferably 0.1 to 5 parts by mass, per 100 parts by mass of component (A). Note that the colorant does not include the above-mentioned component (D).
[0048] The epoxy resin composition of the present invention is preferably an epoxy resin composition containing only the components (A) to (D), a dispersant, a silane coupling agent, a storage stabilizer, and a colorant, and more preferably an epoxy resin composition containing only the components (A) to (D) and a dispersant.
[0049] In one embodiment, the total content of the components (A) to (D), dispersant, silane coupling agent, storage stabilizer, and colorant in the epoxy resin composition is, for example, 95 parts by mass or more, preferably 97 parts by mass or more, and most preferably 100 parts by mass, based on 100 parts by mass of the total amount of the epoxy resin composition. In one embodiment, the total content of the components (A) to (D) and dispersant in the epoxy resin composition is, for example, 95 parts by mass or more, preferably 97 parts by mass or more, and most preferably 100 parts by mass, based on 100 parts by mass of the total amount of the epoxy resin composition.
[0050] The biomass degree of the epoxy resin composition of this embodiment is not particularly limited, but is preferably 10 or more, more preferably 15 or more, even more preferably 20 or more, and even more preferably 25 or more. If it is within the above range, an environmentally friendly epoxy resin composition can be obtained. The upper limit of the biomass degree is not particularly limited, but is, for example, 80 or less.
[0051] The curing conditions for the epoxy resin composition of the present invention are not particularly limited. The heating temperature for curing is preferably 50 to 200°C, more preferably 70 to 150°C, and most preferably 70 to 100°C. The heating time is preferably 5 to 180 minutes, and more preferably 10 to 90 minutes.
[0052] The epoxy resin composition of the present invention can be applied to an adherend by known methods for applying sealants or adhesives. For example, methods such as needle application, non-contact jet dispensing, spraying, screen printing, gravure printing, dipping, and spin coating can be used. Considering ease of application and other workability, the viscosity (25°C) of the epoxy resin composition of the present invention is preferably 500 Pa·s or less, more preferably 400 Pa·s or less, and even more preferably 380 Pa·s or less. The viscosity (25°C) of the epoxy resin composition can be measured by the method described in the Examples below. The lower limit of the viscosity (25°C) of the epoxy resin composition is not particularly limited, but is, for example, 30 Pa·s or more, preferably 50 Pa·s or more, and even more preferably 70 Pa·s or more.
[0053] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples. Hereinafter, the epoxy resin composition will also be referred to simply as the composition.
[0054] [Examples 1 to 4, Comparative Examples 1 to 9] The following components were prepared to prepare epoxy resin compositions.
[0055] Component (A): Epoxy resin - Mixed epoxy resin of bisphenol A type epoxy resin and bisphenol F type epoxy resin (biomass degree: 0) (total halogen content: 500 mass ppm) (EPICLON (registered trademark) EXA-835LV manufactured by DIC Corporation) Component (B): Castor oil particles that are solid at 25°C - Hydrogenated castor oil particles with an average particle size of 8 to 12 μm (biomass degree: 100) (NatureFine H325 MP manufactured by Gokyo Food & Chemical Co., Ltd.) - Hydrogenated castor oil particles with an average particle size of 10 to 20 μm (biomass degree: 100) (A-S-A T-20SF manufactured by Ito Oil Mills Co., Ltd.) Component (B'): Particles that are solid at 25°C other than component (B).・Poly(hydroxybutyrate-co-valerate) (PHBV) particles having an average particle size of 7.5 to 10.5 μm (biomass degree: 100) (Naturematte 31 MP, manufactured by Gokyo Food & Chemical Co., Ltd.) ・Rice wax particles having an average particle size of 6 to 10 μm (biomass degree: 100) (NatureFine R331 MP, manufactured by Gokyo Food & Chemical Co., Ltd.) ・Carnauba wax particles having an average particle size of 6 to 8 μm (biomass degree: 100) (MicroKlear 418, manufactured by Micro Powders) Component (C): curing agent and / or curing accelerator ・Epoxy adduct-based latent curing agent (biomass degree: 0) (average particle size: 5 μm) (Fujicure FXR-1081, manufactured by T&K TOKA Corporation) Component (D): filler - Unbaked scallop shell powder (calcium carbonate powder) with an average particle size of 13 μm and 95% or more passing through a 300 mesh (biomass degree: 100) (Scallop powder, manufactured by NC Corporation) - Unbaked scallop shell powder (calcium carbonate powder) with an average particle size of 6 μm and 95% or more passing through a 500 mesh (biomass degree: 100) (Scallop Powder S, manufactured by NC Corporation) Dispersants - Wetting dispersant (biomass degree: 0) (DISPERBYK (registered trademark)-111, manufactured by BYK).
[0056] To prepare the compositions, component (A), component (B) (or component (B')), component (D), and dispersant were weighed and placed in a stirring vessel for a mixer. These components were stirred for 30 minutes to homogenize, after which component (C) was weighed and placed in the same stirring vessel, and the resulting mixture was stirred for an additional 30 minutes to obtain the epoxy resin compositions of each Example and Comparative Example. Detailed amounts prepared are shown in Table 1 below, with all values expressed in parts by mass.
[0057]
[0058] Viscosity (25°C) measurement, tensile shear adhesive strength measurement, and biomass content confirmation were carried out for Examples 1 to 4 and Comparative Examples 1 to 9. The results are summarized in Table 2.
[0059] [Viscosity (25°C) Measurement] Viscosity was measured using a cone-plate rotational viscometer (E-type viscometer) adjusted to 25°C using a circulating thermostatic bath. 0.5 cc of the epoxy resin composition prepared in each Example and Comparative Example was sampled and dispensed into the center of a sample cup. The sample cup was attached to the viscometer body, and measurement was performed for 3 minutes at 1 rpm (5 rpm for low viscosity) using a 3°×R14 cone plate, and the viscosity was recorded as "viscosity (Pa s)." Considering workability, the viscosity is preferably 500 Pa s or less.
[0060] [Measurement of Tensile Shear Adhesion Strength] Using SPCC-SD (cold-rolled steel plate, dull finish) material measuring 25 mm wide x 100 mm long x 1.6 mm thick, two pieces of material were bonded together with an epoxy resin composition over a bonding area of 25 mm x 10 mm and secured with clips. The material was then left in a hot air drying oven at 80°C for 1 hour to cure the epoxy resin composition, producing a test piece. The test piece was pulled in the shear direction at a tensile speed of 10 mm / min using a tensile tester, the maximum strength was measured, and the "tensile shear adhesion strength (MPa)" was calculated from the bonding area. Details were in accordance with JIS K 6850:1999. Evaluation was based on the following criteria. To maintain stable adhesion, an initial adhesion strength of 15 MPa or greater is preferred.
[0061] [Confirmation of Biomass Degree] The biomass degree of the composition was calculated using the following mathematical formula 1, and was taken as the "biomass degree." In consideration of the environment, the biomass degree is preferably 10 or more.
[0062]
[0063]
[0064] When comparing the compositions of Examples 1 to 4, which contain 10 to 50 parts by mass of component (B) per 100 parts by mass of component (A), with the compositions of Comparative Examples 1 to 3, which do not contain component (B), and the compositions of Comparative Examples 4 to 6, which contain less than 10 parts by mass of component (B) per 100 parts by mass of component (A), it is clear that the compositions of Examples 1 to 4 have higher tensile shear bond strengths. This indicates that the inclusion of a specific content range of castor oil particles that are solid at 25°C improves the tensile shear bond strength of an epoxy resin composition. Furthermore, when comparing the composition of Example 3, which contains component (B), with the compositions of Comparative Examples 7 to 9, which contain component (B'), it is clear that no improvement in tensile shear bond strength was observed when the plasticizer was particles other than castor oil particles that are solid at 25°C.
[0065] According to the present invention, an epoxy resin composition containing a plasticizer can be obtained which has improved tensile shear bond strength, and furthermore, since the biomass content is high, an environmentally friendly epoxy resin composition can be obtained.
[0066] This application is based on Japanese Patent Application No. 2023-077057, filed on May 9, 2023, the disclosure of which is incorporated herein by reference in its entirety.
Claims
1. An epoxy resin composition comprising the following components (A) to (C), containing 10 to 50 parts by mass of component (B) per 100 parts by mass of component (A): component (A): epoxy resin; component (B): castor oil particles that are solid at 25°C; and component (C): curing agent and / or curing accelerator.
2. The epoxy resin composition according to claim 1, wherein the average particle size of component (B) is 5 to 20 μm.
3. The epoxy resin composition according to claim 1, wherein the component (C) comprises an epoxy adduct compound.
4. The epoxy resin composition according to claim 1, further comprising a filler as component (D) (excluding component (B)).
5. The epoxy resin composition according to claim 4, comprising 0.1 to 200 parts by mass of said component (D) per 100 parts by mass of said component (A).
6. The epoxy resin composition according to claim 4, wherein the component (D) is an inorganic powder derived from a natural marine product.
7. The epoxy resin composition according to claim 4, wherein the average particle size of component (D) is 1 to 20 μm.
8. The epoxy resin composition according to claim 1, having a biomass degree of 10 or more.
Citation Information
Patent Citations
Nontar epoxy resin coating composition and heavy-duty corrosionproof coating film
JP1998259351A
Castor oil / epoxidized soybean oil based elastomer composition
JP2006516998A
Latent curing type epoxy resin composition of photo-heat combination type
JP2009079216A
Resin composition for screen printing
JP2012017411A
Epoxy adhesives, their manufacture, and uses
JP2015514149A