Resin composition

The resin composition, comprising olefin and polyhydroxyalkanoate polymers, addresses the adhesion and rigidity challenges of aliphatic polyester films by applying a resin film to the surface, resulting in a product with enhanced mechanical properties and processing capabilities.

WO2024232343A1PCT designated stage expired Publication Date: 2024-11-14SUMITOMO CHEM CO LTD +1
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016901
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-11
Filing Date
2024-05-02
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Conventional aliphatic polyester films face challenges in achieving high rigidity and excellent adhesion of the resin film applied to their surface.

Method used

A resin composition comprising an olefin polymer and a polyhydroxyalkanoate polymer, with specific mass ratios and properties, is used to create a molded product with a resin film applied to its surface, enhancing both rigidity and adhesion.

Benefits of technology

The resin composition achieves high rigidity and excellent adhesion of the resin film to the molded product, improving paintability and printability, and can be processed using methods like injection molding and extrusion molding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016901_14112024_PF_FP_ABST
    Figure JP2024016901_14112024_PF_FP_ABST
Patent Text Reader

Abstract

This resin composition for a molded body to which a resin film is applied on a front surface thereof contains an olefin-based polymer A and a polyhydroxyalkanoate-based polymer B. The content of the olefin-based polymer A is 51 to 99.9 parts by mass and the content of the polyhydroxyalkanoate-based polymer B is 0.1 to 49 parts by mass with respect to a total of 100 parts by mass of the olefin-based polymer A and the polyhydroxyalkanoate-based polymer B.
Need to check novelty before this filing date? Find Prior Art

Description

resin composition

[0001] The present invention relates to a resin composition.

[0002] Aliphatic polyester films have been known as biodegradable resin molded articles.

[0003] Patent No. 3206747

[0004] However, conventional aliphatic polyester films still have room for improvement in the adhesion of the resin film applied to the film surface.

[0005] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a resin composition for a molded body to be provided with a resin film on its surface, which has high rigidity and excellent adhesion of the resin film provided on the surface of the molded body.

[0006] [1] A resin composition for a molded article to be provided with a resin film on its surface, comprising an olefin polymer A and a polyhydroxyalkanoate polymer B, wherein the content of the olefin polymer A is 51 to 99.9 parts by mass and the content of the polyhydroxyalkanoate polymer B is 0.1 to 49 parts by mass relative to a total of 100 parts by mass of the olefin polymer A and the polyhydroxyalkanoate polymer B. [2] The resin composition according to [1], wherein the content of the olefin polymer A is 60.1 to 99.9 parts by mass and the content of the polyhydroxyalkanoate polymer B is 0.1 to 39.9 parts by mass relative to a total of 100 parts by mass of the olefin polymer A and the polyhydroxyalkanoate polymer B. [3] The resin composition according to any one of [1] to [2], wherein the polyhydroxyalkanoate polymer B is a poly(3-hydroxyalkanoate) polymer. [4] The resin composition according to any one of [1] to [3], wherein the polymer A is a propylene-based polymer. [5] An injection-molded article of the resin composition according to any one of [1] to [4]. [6] An extrusion-molded article of the resin composition according to any one of [1] to [4]. [7] An article comprising a resin composition molded article and a resin film provided on a surface of the resin composition molded article, wherein the resin composition molded article contains an olefin-based polymer A and a polyhydroxyalkanoate-based polymer B, and wherein the content of the olefin-based polymer A is 51 to 99.9 parts by mass and the content of the polyhydroxyalkanoate-based polymer B is 0.1 to 49 parts by mass, relative to 100 parts by mass of the total of the olefin-based polymer A and the polyhydroxyalkanoate-based polymer B.

[0007] According to the present invention, there is provided a resin composition for a molded article to be provided with a resin film on its surface, which has high rigidity and excellent adhesion of the resin film to be provided on the surface of the molded article.

[0008] 1 is a schematic cross-sectional view of a resin film-applied resin composition molded article according to one embodiment.

[0009] Hereinafter, several embodiments of the present invention will be described in detail, but the present invention is not limited to the following embodiments.

[0010] (Resin Composition for Molded Article to be Provided with a Resin Film on the Surface) The resin composition according to the present invention contains an olefin polymer A and a polyhydroxyalkanoate polymer B.

[0011] <Olefin Polymer A> Olefin polymer A is a polymer containing 50% by mass or more of structural units derived from an olefin having from 2 to 10 carbon atoms (wherein the total amount of the olefin polymer is taken as 100% by mass). Examples of olefins having from 2 to 10 carbon atoms include ethylene, propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, and 1-decene.

[0012] The olefin polymer A may contain a structural unit derived from a monomer other than an olefin having from 2 to 10 carbon atoms. Examples of the monomer other than an olefin having from 2 to 10 carbon atoms include aromatic vinyl monomers such as styrene, unsaturated carboxylic acids such as acrylic acid and methacrylic acid, unsaturated carboxylic acid esters such as methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate and ethyl methacrylate, vinyl ester compounds such as vinyl acetate, conjugated dienes such as 1,3-butadiene and 2-methyl-1,3-butadiene (isoprene), and non-conjugated dienes such as dicyclopentadiene and 5-ethylidene-2-norbornene.

[0013] The olefin polymer A may be at least one selected from the group consisting of an ethylene polymer, a propylene polymer, and a butene polymer, or may be a combination of any two or more of these.

[0014] An ethylene-based polymer is a polymer containing 50% by mass or more of structural units derived from ethylene, and examples thereof include ethylene homopolymer, ethylene-1-butene copolymer, ethylene-1-hexene copolymer, ethylene-1-octene copolymer, and ethylene-1-butene-1-hexene copolymer. The ethylene-based polymer may be a combination of two or more ethylene-based polymers.

[0015] The propylene-based polymer is a polymer containing 50% by mass or more of structural units derived from propylene, and examples thereof include a propylene homopolymer, a propylene-ethylene copolymer, a propylene-1-butene copolymer, a propylene-1-hexene copolymer, a propylene-1-octene copolymer, a propylene-ethylene-1-butene copolymer, a propylene-ethylene-1-hexene copolymer, and a propylene-ethylene-1-octene copolymer. The propylene-based polymer may be a combination of two or more propylene-based polymers. It is preferable that the olefin-based polymer A is a propylene-based polymer.

[0016] The butene polymer is a polymer containing 50% by mass or more of structural units derived from 1-butene, and examples thereof include 1-butene homopolymer, 1-butene-ethylene copolymer, 1-butene-propylene copolymer, 1-butene-1-hexene copolymer, 1-butene-1-octene copolymer, 1-butene-ethylene-propylene copolymer, 1-butene-ethylene-1-hexene copolymer, 1-butene-ethylene-1-octene copolymer, 1-butene-propylene-1-hexene copolymer, and 1-butene-propylene-1-octene copolymer. The butene polymer may be a combination of two or more butene polymers.

[0017] The olefin polymer A can be produced by a known polymerization method using a known polymerization catalyst.

[0018] The melt mass flow rate (MFR) of the olefin polymer A measured according to JIS K7210-2014 at a temperature of 230°C or 190°C under a load of 2.16 kgf is preferably 0.1 g / 10 min or more and 200 g / 10 min or less.

[0019] <Polyhydroxyalkanoate Polymer B> The polyhydroxyalkanoate polymer is a polyester of a hydroxyalkanoic acid. Examples of the hydroxyalkanoic acid include 2-hydroxyalkanoic acid, 3-hydroxyalkanoic acid, and 4-hydroxyalkanoic acid.

[0020] Examples of 2-hydroxyalkanoic acids are glycolic acid, lactic acid, and 2-hydroxybutyric acid. Examples of polyesters of 2-hydroxyalkanoic acids, that is, poly(2-hydroxyalkanoate)-based polymers, are polyglycolic acid and polylactic acid.

[0021] Examples of 3-hydroxyalkanoic acids are 3-hydroxybutyric acid, 3-hydroxypropionic acid, 3-hydroxypentanoic acid, and 3-hydroxyhexanoic acid. Polyesters of 3-hydroxyalkanoic acids, i.e., poly(3-hydroxyalkanoate) polymers, will be described in detail later.

[0022] Examples of 4-hydroxyalkanoic acids are 4-hydroxybutyric acid, 4-hydroxypentanoic acid, and 4-hydroxyhexanoic acid.

[0023] The polyhydroxyalkanoate polymer may be a homopolymer of a hydroxyalkanoic acid, or a polymer of two or more kinds of hydroxyalkanoic acids.

[0024] (Poly(3-hydroxyalkanoate)-based polymer) The polyhydroxyalkanoate-based polymer B can be a poly(3-hydroxyalkanoate)-based polymer.

[0025] The poly(3-hydroxyalkanoate) polymer is a polyhydroxyalkanoate, i.e., a polycondensate (polyester) of hydroxyalkanoic acid, and necessarily contains a 3-hydroxyalkanoate repeating unit represented by formula (1). In formula (1), R represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 15 carbon atoms, a cyano group, an amino group having 1 to 11 carbon atoms, an alkoxy group (alkyloxy group) having 1 to 11 carbon atoms, an amide group having 2 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, or a monovalent heterocyclic group having 1 to 9 carbon atoms. These groups may have a substituent. In particular, from the viewpoint of compatibility with components other than the polyhydroxyalkanoate polymer B contained in the composition (e.g., the olefin polymer A), R is preferably an alkyl group having 1 to 8 carbon atoms, an amide group having 1 to 20 carbon atoms, or an aryl group having 6 to 8 carbon atoms.

[0026] [-O-CHR-CH 2 -CO-]... (1)

[0027] Examples of halogen atoms are F, Cl, Br, and I.

[0028] The alkyl group having 1 to 15 carbon atoms may be linear or branched. The number of carbon atoms in the alkyl group is preferably 1 to 8, and more preferably 1 to 4. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a 2-methylbutyl group, a 1-methylbutyl group, a hexyl group, an isohexyl group, a 3-methylpentyl group, a 2-methylpentyl group, a 1-methylpentyl group, a heptyl group, an octyl group, an isooctyl group, a 2-ethylhexyl group, a 3,7-dimethyloctyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, a tetradecyl group, and a pentadecyl group.

[0029] Examples of the amino group having 1 to 18 carbon atoms include an amino group, an alkylamino group, a dialkylamino group, an arylamino group, an alkylarylamino group, a benzylamino group, and a dibenzylamino group.

[0030] Examples of the alkylamino group include a methylamino group, an ethylamino group, a propylamino group, a butylamino group, a pentylamino group, a hexylamino group, a heptylamino group, an octylamino group, a nonylamino group, a decylamino group, a dodecylamino group, an isopropylamino group, an isopentylamino group, a sec-butylamino group, a tert-butylamino group, a sec-pentylamino group, a tert-pentylamino group, a tert-octylamino group, a neopentylamino group, a cyclopropylamino group, a cyclobutylamino group, a cyclopentylamino group, a cyclohexylamino group, a cycloheptylamino group, a cyclooctylamino group, a 1-adamantamino group, and a 2-adamantamino group.

[0031] Examples of the dialkylamino group include a dimethylamino group, a diethylamino group, a dipropylamino group, a dibutylamino group, a dipentylamino group, a diisopropylamino group, a diisobutylamino group, a diisopentylamino group, a methylethylamino group, a methylpropylamino group, a methylbutylamino group, a methylisobutylamino group, a dicyclopropylamino group, a pyrrolidino group, a piperidino group, and a piperazino group.

[0032] Examples of the arylamino group include an anilino group, a 1-naphthylamino group, a 2-naphthylamino group, an o-toluidino group, an m-toluidino group, a p-toluidino group, a 1-fluoreneamino group, a 2-fluoreneamino group, a 2-thiazoleamino group, and a p-terphenylamino group.

[0033] The alkylarylamino group includes an N-methylanilino group, an N-ethylanilino group, an N-propylanilino group, an N-butylanilino group, an N-isopropylanilino group, and an N-pentylanilino group.

[0034] Examples of the alkoxy group having 1 to 11 carbon atoms include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, a cyclopropoxy group, a cyclobutoxy group, and a cyclopentoxy group.

[0035] The term "amide group" refers to a group in which one hydrogen atom bonded to a nitrogen atom has been removed from a carboxylic acid amide. Examples of the amide group having 1 to 20 carbon atoms include -NH-C(=O)-R groups such as formamide, acetamide, propionamide, butylamide, benzamide, trifluoroacetamide, and pentafluorobenzamide. A (wherein R A represents a hydrogen atom or a monovalent organic group), and -N(-C(=O)-R such as a diformamide group, a diacetamide group, a dipropionamide group, a dibutyroamide group, a dibenzamide group, a ditrifluoroacetamide group, and a dipentafluorobenzamide group. A )(-C(=O)-R B ) (wherein R A 、 RB are each independently a hydrogen atom or a monovalent organic group. The organic group may be an alkyl group, an alkoxy group, or an aryl group, each of which may be substituted with a halogen atom. Of these, preferred amide groups are formamide, acetamide, propionamide, butyromide, and benzamide.

[0036] Examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a tolyl group, a xylyl group, a naphthyl group, and a biphenyl group, with the phenyl group, the tolyl group, and the xylyl group being more preferred.

[0037] Examples of heteroatoms in monovalent heterocyclic groups having 1 to 9 carbon atoms include N, O, and S. The heterocyclic groups may be saturated or unsaturated, and may contain a single heteroatom or multiple heteroatoms, or different types of heteroatoms. Examples of such heterocyclic groups include thienyl, pyrrolyl, furyl, pyridyl, piperidinyl, quinolinyl, isoquinolinyl, pyrimidinyl, triazinyl, and thiazolyl groups.

[0038] The repeating units of the polyhydroxyalkanoate polymer B may consist solely of one or more types of 3-hydroxyalkanoates represented by formula (1), or may contain one or more types of 3-hydroxyalkanoates represented by formula (1) and one or more types of other hydroxyalkanoates.

[0039] The polyhydroxyalkanoate polymer B preferably contains 50 mol % or more, more preferably 70 mol % or more, of the 3-hydroxyalkanoate repeating units represented by the formula (1) relative to the total repeating units of the hydroxyalkanoate (100 mol %).

[0040] Examples of 3-hydroxyalkanoates represented by formula (1) are those in which R is a hydrogen atom or C n H 2n+1where n is an integer of 1 to 15, examples thereof include 3-hydroxybutyrate (hereinafter, sometimes referred to as 3HB) where n=1, 3-hydroxyvalerate (hereinafter, sometimes referred to as 3HV) where n=2, 3-hydroxyhexanoate (hereinafter, sometimes referred to as 3HH) where n=3, 3-hydroxyoctanoate where n=5, 3-hydroxyoctadecanoate where n=15, and 3-hydroxypropionate where R is a hydrogen atom.

[0041] An example of polymer B having only one type of repeating unit represented by formula (1) is poly(3-hydroxybutyrate) (hereinafter, sometimes referred to as P3HB).

[0042] Examples of polymer B having only multiple types of repeating units represented by formula (1) include poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (hereinafter, sometimes referred to as P3HB3HH), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (hereinafter, sometimes referred to as P3HB3HV), and poly(3-hydroxybutyrate-co-3-hydroxypropionate) (hereinafter, sometimes referred to as P3HB3HP).

[0043] Examples of hydroxyalkanoates other than the 3-hydroxyalkanoate represented by formula (1) include repeating units represented by formula (2) (wherein R 1 is a hydrogen atom or C n H 2n+1 where n is an integer of 1 or more and 15 or less, and m is an integer of 2 to 10.

[0044] [—O—CHR 1 -C m H 2m+1 -CO-]... (2)

[0045] An example of polymer B containing repeating units of formula (1) and formula (2) is poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (for example, the following formula (P3HB4HB)).

[0046] From the viewpoint of increasing the melting point, it is preferable that the repeating unit of the polyhydroxyalkanoate polymer B contains at least 3-hydroxybutyrate among the 3-hydroxyalkanoates represented by the formula (1).

[0047] The polyhydroxyalkanoate polymer B preferably contains 3-hydroxybutyrate repeating units in an amount of 50 mol % or more, more preferably 70 mol % or more, based on the total repeating units of hydroxyalkanoate (100 mol %).

[0048] The polyhydroxyalkanoate polymer B may have two or more types of ester repeating units, and may be, for example, a di-polymer having two types of repeating units, a tri-copolymer having three types of repeating units, or a tetra-copolymer having four types of repeating units, as described above.

[0049] For example, an example of a tri-copolymer is poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate) (hereinafter, sometimes referred to as (P3HB3HV3HH)).

[0050] As described above, the polyhydroxyalkanoate polymer B preferably contains 3-hydroxybutyrate among the 3-hydroxyalkanoate repeating units represented by formula (1). The proportion XX of 3-hydroxybutyrate repeating units relative to 100 moles of all hydroxyalkanoate ester repeating units is preferably 90 mol% or more, more preferably 95 mol% or more, and even more preferably 98.0 mol% or more.

[0051] The proportion XX is usually 100 mol % or less, preferably 99.9 mol % or less, and more preferably 99.8 mol % or less.

[0052] The arrangement of the copolymer may be any of a random copolymer, an alternating copolymer, a block copolymer, a graft copolymer, and the like.

[0053] The polyhydroxyalkanoate polymer B may have ester repeating units other than those of the formulae (1) and (2), but the main chain of the other ester repeating units does not contain an aromatic hydrocarbon structure. That is, the polyhydroxyalkanoate polymer B is an aliphatic polyester. However, it is possible for a group having an aromatic hydrocarbon group to be bonded to a carbon atom in the main chain of the other ester repeating units.

[0054] The constituent ratio of the repeating units in the polyhydroxyalkanoate polymer B can be determined by calculation from the results of NMR measurements such as H-NMR and C-NMR, as described in L. Tripathi, M. C. Factories, 11, 44 (2012).

[0055] The polyhydroxyalkanoate polymer B may also be a mixture of two or more types of poly(3-hydroxyalkanoate) polymers.

[0056] The weight-average molecular weight (Mw) of the polyhydroxyalkanoate polymer B can be from 10,000 to 1,000,000, preferably from 20,000 to 800,000, and more preferably from 30,000 to 600,000. By setting the weight-average molecular weight (Mw) to 10,000 or more, it is possible to obtain a molded product excellent in impact strength and tensile elongation. Furthermore, by setting the weight-average molecular weight to 500,000 or less, dispersibility in the olefin polymer A is improved. The weight-average molecular weight may be 400,000 or less, 300,000 or less, 200,000 or less, or 100,000 or less. In this specification, the weight-average molecular weight (Mw) is measured by GPC using standard polystyrene as a molecular weight standard.

[0057] The polyhydroxyalkanoate polymer B is a thermoplastic resin and may be crystalline.

[0058] The melt mass flow rate (MFR(B)) of the polyhydroxyalkanoate polymer B, measured in accordance with JIS K7210-2014 at a temperature of 190°C or 170°C and a load of 2.16 kgf, is preferably 0.1 g / 10 min or more and 200 g / 10 min or less. MFR(B) may be 1 g / 10 min or more, 3 g / 10 min or more, 5 g / 10 min or more, 7 g / 10 min or more, 8 g / 10 min or more, 10 g / 10 min or more, or 20 g / 10 min or more. MFR(B) may be 150 g / 10 min or less, or 100 g / 10 min or less.

[0059] The melting point (Tm) of the polyhydroxyalkanoate polymer B is preferably 150° C. or higher, and may be 155° C. or higher, 160° C. or higher, 165° C. or higher, 170° C. or higher, or 175° C. or higher. The melting point (Tm) of the polymer B may be 220° C. or lower, or may be 200° C. or lower, or may be 190° C. or lower.

[0060] The melting point (Tm) of the polyhydroxyalkanoate polymer B is measured by a differential scanning calorimeter (DSC) in accordance with JIS K7121, based on the position of the main peak due to the melting of crystals.

[0061] The poly(3-hydroxyalkanoate) polymer may be produced by a microorganism or may be derived from a compound (such as a cyclic lactone) derived from petroleum or plant materials.

[0062] The poly(3-hydroxyalkanoate) polymer may be one in which each repeating unit of hydroxyalkanoate is composed only of the D-form (R-form), as in those produced from microorganisms, or one in which the repeating unit of hydroxyalkanoate contains both the D-form (R-form) and the L-form (S-form), as in those derived from a mixture of the D-form (R-form) and the L-form (S-form).

[0063] In the poly(3-hydroxyalkanoate) polymer produced from a microorganism, the repeating unit of formula (1) can be represented by the following formula: (BI-1) In formula (BI-1), n ​​represents the degree of polymerization.

[0064]

[0065] For example, poly-(3-hydroxybutyrate) produced from a microorganism has the following structure: (BI-2) where n represents the degree of polymerization.

[0066]

[0067] Furthermore, poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) produced from a microorganism has the following structure: (BI-3) where m and n represent the degree of polymerization.

[0068]

[0069] Furthermore, poly-(3-hydroxybutyrate-co-4-hydroxybutyrate) produced from a microorganism has the following structure: (BI-4) where m and n represent the degree of polymerization.

[0070]

[0071] The polyhydroxyalkanoate polymer B can be biodegradable.

[0072] For example, poly(3-hydroxyalkanoate) polymers can be produced by microorganisms such as Alcaligeneseutrophus AC32 strain (international deposit under the Budapest Treaty, international depository authority: National Institute of Advanced Industrial Science and Technology International Patent Organism Depositary (6-1 Central, 1-1 Higashi, Tsukuba, Ibaraki Prefecture, Japan), original deposit date: August 12, 1996, transferred on August 7, 1997, accession number FERMBP-6038 (transferred from original deposit FERMP-15786)) (J. Bacteriol., 179, 4821 (1997)).

[0073] <Composition of Resin Composition> The resin composition contains 51 to 99.9 parts by mass of the olefin polymer A and 0.1 to 49 parts by mass of the polyhydroxyalkanoate polymer B relative to 100 parts by mass in total of the olefin polymer A and the polyhydroxyalkanoate polymer B.

[0074] The resin composition may contain 60.1 to 99.9 parts by mass of olefin polymer A and 0.1 to 39.9 parts by mass of polyhydroxyalkanoate polymer B relative to 100 parts by mass in total of olefin polymer A and polyhydroxyalkanoate polymer B, 70 to 99.9 parts by mass of olefin polymer A and 0.1 to 30 parts by mass of polyhydroxyalkanoate polymer B, or 75 to 99.9 parts by mass of olefin polymer A and 0.1 to 25 parts by mass of polyhydroxyalkanoate polymer B.

[0075] The resin composition may be such that, relative to 100 parts by mass of the total of the olefin polymer A and the polyhydroxyalkanoate polymer B, the content of the olefin polymer A is 80 to 99.9 parts by mass and the content of the polyhydroxyalkanoate polymer B is 0.1 to 20 parts by mass, the content of the olefin polymer A is 85 to 99.9 parts by mass and the content of the polyhydroxyalkanoate polymer B is 0.1 to 15 parts by mass, or the content of the olefin polymer A is 90 to 99.9 parts by mass and the content of the polyhydroxyalkanoate polymer B is 0.1 to 10 parts by mass.

[0076] The total proportion of the olefin polymer A and the polyhydroxyalkanoate polymer B in the entire resin composition can be 50% by mass or more, preferably 60% by mass or more, and more preferably 70% by mass or more.

[0077] In the resin composition, the polyhydroxyalkanoate polymer B may or may not form a dispersed phase. The polyhydroxyalkanoate polymer B forming a dispersed phase means that the resin composition has a sea-island structure in which the olefin polymer A forms a continuous phase (sea portion) and the polyhydroxyalkanoate polymer B forms a dispersed phase (islands portion). The average equivalent circle diameter of the dispersed phase (islands portion) can be 10 nm to 400 μm.

[0078] (Additives) The resin composition may contain additives as needed. The additives may be at least one selected from the group consisting of stabilizers, antibacterial agents, antifungal agents, dispersants, plasticizers, flame retardants, tackifiers, colorants, metal powders, organic powders, inorganic fibers, organic fibers, organic and inorganic composite fibers, inorganic whiskers, and fillers.

[0079] Examples of the stabilizer include at least one selected from the group consisting of lubricants, antioxidants, heat stabilizers, light stabilizers, weathering agents, metal deactivators, ultraviolet absorbers, light stabilizers, and copper inhibitors. Examples of the light stabilizer include hindered amine-based light stabilizers.

[0080] An example of the colorant is at least one selected from the group consisting of titanium oxide, carbon black, and organic pigments. An example of the metal powder is ferrite.

[0081] An example of an organic powder is protein. Examples of inorganic fibers are glass fibers and metal fibers. Examples of organic fibers are carbon fibers and aramid fibers. An example of an inorganic whisker is potassium titanate whisker.

[0082] Examples of the filler include at least one selected from the group consisting of glass beads, glass balloons, glass flakes, asbestos, mica, calcium carbonate, talc, silica, calcium silicate, hydrotalcite, kaolin, diatomaceous earth, graphite, pumice, ebonized powder, cotton flock, cork powder, barium sulfate, fluororesin, cellulose powder, and wood flour.

[0083] The resin composition may contain only one of the above additives, or may contain a combination of two or more of them.

[0084] In the resin composition, the additive may be contained in either the olefin polymer A or the polyhydroxyalkanoate polymer B. The additive may form a dispersed phase separate from the polyhydroxyalkanoate polymer B in the continuous phase of the olefin polymer A.

[0085] (Method for producing resin composition) The resin composition can be obtained by melt-kneading an olefin polymer A, a polyhydroxyalkanoate polymer B, and additives added as needed. The kneading temperature (the set temperature of the kneader) is preferably 150 to 300°C, more preferably 170 to 280°C. Alternatively, a composition can be obtained by melt-kneading a portion of each of the olefin polymer A and the polyhydroxyalkanoate polymer B to obtain a pre-kneaded mixture, and then adding the remainder of the olefin polymer A and the polyhydroxyalkanoate polymer B to the pre-kneaded mixture and further melt-kneading the mixture.

[0086] (Attributes and Uses of Resin Composition) The resin composition according to this embodiment not only provides a molded article with high rigidity, but also provides excellent adhesion between the molded article and the resin film when the resin film is applied to the surface of the molded article after molding. The reason for this is not clear, but is thought to be due to the resin composition according to this embodiment containing an appropriate amount of polyhydroxyalkanoate polymer B.

[0087] The resin composition of the present embodiment is used for a molded article to be provided with a resin film on the surface.

[0088] (Molded Article of Resin Composition) A molded article can be obtained by using the above-described resin composition by a known method.

[0089] Specifically, the obtained resin composition can be molded into a molded article having a desired shape using a known resin molding method such as injection molding, extrusion molding, vacuum molding, pressure molding, press molding, foam molding, blow molding, or rotational molding.

[0090] From the viewpoint of the adhesion of the resin film applied to the surface of the molded article, i.e., paintability and printability, the molding methods are preferably injection molding, extrusion molding, blow molding, and rotational molding, and more preferably injection molding and extrusion molding, which can produce injection molded articles and extrusion molded articles. Extrusion molding can be used to form films, plates, fibers, etc.

[0091] From the viewpoint of adhesion of the resin film applied to the surface of the molded article, i.e., paintability and printability, the maximum shear rate during heat molding to obtain a molded article from the composition of the present invention is 1 to 10,000 sec. -1 is preferable, and more preferably 10 to 5000 seconds -1 , and even more preferably 15 to 3000 seconds -1 is.

[0092] Furthermore, the above composition can be laminated with other materials such as other resins, metals, paper, leather, etc. to obtain a multi-layer structure.

[0093] The surface of the article molded from the composition of the present invention may be subjected to a surface treatment such as embossing, corona discharge treatment, flame treatment, plasma treatment, or ozone treatment.

[0094] The shape of the molded article of the resin composition is not particularly limited, and examples thereof include plates, films, fibers, cloth, nonwoven fabrics, containers, and pipes. Furthermore, molded articles of any complex shape can be produced by injection molding or the like.

[0095] 1 , a resin film is applied to at least a portion of the surface of a resin composition molded body 10 by painting with a paint or printing with ink, thereby obtaining a resin composition molded body 10 and a resin film-applied resin composition molded body (article) 100, which has a resin film 20 such as a coating film or ink film applied to at least a portion of the surface of the resin composition molded body 10. There are no particular limitations on the thickness of the resin film 20, but it can be 0.01 to 100 μm.

[0096] The resin film 20 includes a film containing a resin. The resin film 20 preferably has a primer layer 22 that contacts the surface of the resin composition molded body 10.

[0097] The material of the primer layer 22 is not particularly limited, but may include, for example, chlorinated polyolefin resins such as chlorinated polyethylene and chlorinated polypropylene, and maleated polyolefin resins obtained by modifying polyethylene resins and chlorinated polyolefin resins with maleic acid.

[0098] The resin film 20 preferably has a topcoat layer 23 on the primer layer 22. The topcoat layer 23 may be a single layer or may have multiple layers. For example, the topcoat layer 23 may include, in order from the primer layer 22 side, a base layer 24 and a clear layer 26, as shown in Figure 1, and such a topcoat layer configuration may be called a coating film.

[0099] The material of the base layer 24 is not particularly limited, but may include, for example, resins such as ethyl methacrylate resins, methyl methacrylate resins, urethane resins, epoxy resins, ester resins, olefin resins, fluorine resins, silicone resins, styrene resins, and melamine resins; pigments such as metal particles such as aluminum and mineral particles such as mica; and various additives.

[0100] There are no particular limitations on the material of the clear layer 26, but it may contain, for example, resins such as ethyl methacrylate resins, methyl methacrylate resins, urethane resins, epoxy resins, ester resins, olefin resins, fluorine resins, silicone resins, styrene resins, and melamine resins; and various additives.

[0101] To obtain such a resin film-applied resin composition molded body, a primer layer-forming liquid (a liquid in which a primer resin is dissolved / dispersed in a solvent (toluene, isopropyl alcohol, etc.)) is applied to the surface of the above-mentioned resin composition molded body and dried, then a base layer-forming paint is applied to the primer layer and dried, and then a clear layer-forming paint is applied to the base layer and dried.

[0102] When the topcoat layer 23 has a base layer 24 and a clear layer 26, there may be a plurality of base layers 24 or a plurality of clear layers 26. Alternatively, the topcoat layer 23 may have only one of the base layer 24 and the clear layer 26.

[0103] The base layer 24 of the overcoat layer 23 may contain a resin and a colorant selected from the group consisting of dyes and pigments, and such a base layer 24 is sometimes called an ink film. The overcoat layer 23 may include a single base layer 24 containing a resin and a colorant, or may include multiple base layers 24 containing a resin and a colorant, and may or may not include a clear layer 26.

[0104] Examples of resins for the base layer containing resin and colorant include ethyl methacrylate-based resins, methyl methacrylate-based resins, urethane-based resins, epoxy-based resins, ester-based resins, olefin-based resins, fluorine-based resins, silicone-based resins, styrene-based resins, and melamine-based resins.

[0105] Examples of dyes and pigments are carbon black, zinc oxide, white lead, lithopone, titanium dioxide, precipitated barium sulfate and baryte powder, red lead, iron oxide red, yellow lead, zinc yellow type 1, zinc yellow type 2, ultramarine blue, potassium ferrocyanide, YInMn blue, organic pigments, polycyclic pigments, azo pigments, lake pigments, and fluorescent pigments.

[0106] Examples of the dye include acid dyes, basic dyes, direct dyes, sulfur dyes, vat dyes, naphthol dyes, reactive dyes, disperse dyes, etc., and can be selected from dyes conventionally known for use in color filters. Examples of the dye include those described in JP-A-64-90403, JP-A-64-91102, JP-A-1-94301, JP-A-6-11614, JP-A-2592207, U.S. Pat. No. 4,808,501, U.S. Pat. No. 5,667,920, U.S. Pat. No. 5,059,500, JP-A-5-333207, JP-A-6-35183, JP-A-6-51115, and JP-A-6-194828. Examples of the chemical structure of the dye include pyrazole azo dyes, anilino azo dyes, arylazo dyes, pyrazolotriazole azo dyes, pyridone azo dyes, triphenylmethane dyes, anthraquinone dyes, anthrapyridone dyes, benzylidene dyes, oxonol dyes, cyanine dyes, polymethine dyes, phenothiazine dyes, pyrrolopyrazole azomethine dyes, xanthene dyes, phthalocyanine dyes, quinophthalone dyes, benzopyran dyes, indigo dyes, dioxazine dyes, coumarin dyes, and squarylium dyes. Preferred examples include pyrazole azo dyes, anilino azo dyes, pyrazolotriazole azo dyes, pyridone azo dyes, anthraquinone dyes, anthrapyridone dyes, phthalocyanine dyes, dioxazine dyes, quinophthalone dyes, and xanthene dyes. More preferred examples include pyrazole azo dyes, pyridone azo dyes, phthalocyanine dyes, quinophthalone dyes, and xanthene dyes.

[0107] Such a resin film 20 can be obtained by applying a primer layer forming liquid (a liquid in which a primer resin is dissolved / dispersed in a solvent (toluene, isopropyl alcohol, etc.)) to the surface of a resin composition molded body, drying it, and then printing an ink raw material containing a resin, a colorant, and a solvent on the primer layer and drying it.

[0108] There is no particular limitation on the thickness of the resin film 20, but it can be set to 0.01 to 100 μm. The thickness of the primer layer 22 may be 0.001 to 50 μm.

[0109] (Surface Condition of Molded Article of Resin Composition) The molded article of the above-described resin composition can satisfy at least one of the following requirements (i) to (vi).

[0110] (i): The oxygen atomic content on the surface of a resin composition molded article, as determined by X-ray photoelectron spectroscopy, is 0.01 atom% or more and 8.5 atom% or less. The oxygen atomic content may be 0.05 atom% or more, 0.10 atom% or more, or 0.20 atom% or more. The oxygen atomic content may be 8.0 atom% or less, 5.0 atom% or less, 3 atom% or less, 2.0 atom% or less, or 1.0 atom% or less.

[0111] (ii): The wet tension of the surface of the resin composition molded article is 25 mN / m or more and 45 mN / m or less. In this specification, the wet tension is the wet tension defined in JIS K6768 1999. This wet tension may be 27 mN / m or more, 29 mN / m or more, or 30 mN / m or more. The wet tension may be 40 mN / m or less, or 37 mN / m or less.

[0112] When requirement (i) and / or requirement (ii) are satisfied, the amount of oxygen atoms on the surface and / or the wetting tension on the surface are appropriate, and thus the resin film applied to the surface of the resin composition molded article can have higher rigidity and have higher adhesion.

[0113] The reason for this is not clear, but the following is thought to be the reason: If the amount of oxygen atoms on the surface is too small, the thickness of the primer layer decreases and the adhesion to the resin film decreases, whereas if the amount of oxygen atoms on the surface is too large, the strength of the surface of the resin composition molded article tends to decrease.

[0114] If the surface wet tension is too high, the thickness of the primer layer decreases, resulting in poor adhesion to the resin film.If the surface wet tension is too low, the uniformity of the primer layer thickness tends to decrease, resulting in poor adhesion uniformity to the resin film.

[0115] (iii): In the infrared absorption spectrum of the surface of a molded product of the resin composition measured by an infrared spectrophotometer, the ratio RCO / RCH of the peak intensity RCO of the stretching vibration of the C=O bond to the peak intensity RCH of the stretching vibration of the C-H bond is 0.05 or more. This ratio RCO / RCH may be 0.07 or more, 0.10 or more, or 0.12 or more. There is no particular upper limit to this ratio RCO / RCH, but it may be 1.0 or less, 0.8 or less, or 0.5 or less.

[0116] The peak intensity RCO is 1600-1800 cm -1 In the IR absorption spectrum of the surface of the resin composition molded article, which is base corrected in the range of 1600 to 1800 cm -1 This is the maximum absorbance of the peak observed at 1000 kJ / cm2, and corresponds to the C=O stretching vibration intensity of the carbonyl.

[0117] The peak intensity RCH is 2700 to 3000 cm -1 In the IR absorption spectrum of the surface of the resin composition molded article, which is base corrected in the range of 2700 to 3000 cm -1 This is the maximum absorbance of the peak observed at 1000 kJ / cm2, and corresponds to the C—H stretching vibration peak intensity of the alkane.

[0118] The IR spectrum of the surface of the resin composition molded article can be obtained by the attenuated total reflection (ATR) method using an FTIR device.

[0119] An RCO / RCH ratio of 0.05 or more means that a certain amount of C═O bonds are present on the surface of the resin composition molded article. It is believed that C═O bonds contribute more to adhesion to the resin film than O—H bonds, and that satisfying formula (iii) further improves the adhesion of the resin film.

[0120] (Uses of Articles) Uses of the articles of the present invention include textile materials, exterior construction members, furniture and interior decoration members, house members, toy members, gardening members, automobile members, and packaging materials. Examples of textile materials include fabric materials for clothing, fabric materials for interior use, and industrial textile materials; examples of exterior construction materials include carport materials, fence materials, gate materials, gatepost materials, post materials, cycle port materials, deck materials, sunroom materials, roof materials, terrace materials, handrail materials, shade materials, and awning materials; examples of furniture and interior decoration materials include sofa materials, table materials, chair materials, bed materials, chest of drawers materials, cabinet materials, and dresser materials; examples of home appliance materials include clock materials, mobile phone materials, and white goods home appliance materials; examples of toy materials include plastic model materials, diorama materials, and video game console materials; examples of gardening materials include planter materials, vase materials, and flowerpot materials; examples of automobile materials include bumper materials, instrument panel materials, and airbag cover materials; and examples of packaging materials include food packaging materials, textile packaging materials, and miscellaneous goods packaging materials. Further, other uses include, for example, monitor components, office automation (OA) equipment components, medical components, drain pans, toiletry components, bottles, containers, snow removal equipment components, and various construction components.

[0121] The present invention will be described below with reference to Examples and Comparative Examples. The olefin polymer A and polyhydroxyalkanoate polymer B used in the Examples and Comparative Examples are shown below.

[0122] (1) Olefin Polymer A (A-1) Propylene homopolymer MFR (230°C, 2.16 kg load): 20 g / 10 min Melting point (Tm): 163°C

[0123] (2) Polyhydroxyalkanoate Polymer B (B-1) Poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) Structural formula: (BI-3) Comonomer (3HH) content (mol%): 0.2 mol% Weight average molecular weight (Mw): 104,000 MFR (190°C, 2.16 kg load): 7.8 g / 10 min Melting point (Tm): 175°C

[0124] The physical properties of each polymer and composition were measured according to the methods shown below.

[0125] (1) Melt mass flow rate (MFR, unit: g / 10 min) was measured according to the method specified in JIS K7210-2014. The measurement temperature was 230°C or 190°C, and the load was 2.16 kg.

[0126] (2) Weight-average molecular weight (Mw) The weight-average molecular weight (Mw) was calculated based on the results of gel permeation chromatography (GPC). In the GPC measurement, a Waters GPC-150C was used as the measuring device, an ortho-dichlorobenzene solution with a polymer concentration of 0.05 wt % was used, and a mixed polystyrene gel column (Tosoh PSKgel GMH6-HT) was used as the column, at a measurement temperature of 135°C.

[0127] (3) Melting point (Tm) of polymer: Measured according to the method specified in JIS K 7121. The measurement temperature was −50° C. to 200° C. or −50° C. to 250° C., and the temperature rise rate was 10° C. / min.

[0128] (4) Content of Comonomer Component in Polyhydroxyalkanoate Polymer B The content of the comonomer component refers to the molar ratio of repeating units other than 3-hydroxybutyrate (3-hydroxyhexanoate (3HH) or 4-hydroxybutyrate (4HB)) to the total number of ester repeating units of hydroxyalkanoate in Polymer B.

[0129] The content of the comonomer component was determined by a method using 1H-NMR spectrum described in L. Tripathi, M. C. Factories, 11, 44 (2012). [Measurement conditions] Model: Bruker AVANCE 600 Probe: 10 mm cryoprobe Measurement temperature: 135°C Pulse repetition time: 1 second Pulse width: 45° Number of accumulations: 700 Magnetic field strength: 600 MHz

[0130] (5) Measurement of Tg of Composition A temperature-storage modulus curve of the composition was obtained using a viscoelasticity device (SII Nanotechnology Inc.; DMS200), and the number of peaks was counted.

[0131] (6) Oxygen Atom Content on the Surface of Resin Composition Molded Article The oxygen atom content on the surface of the resin composition molded article was measured using an X-ray photoelectron spectroscopy device, AXIS ULTRA DLD, manufactured by Shimadzu Corporation / KRATOS. The degree of vacuum in the device during measurement was 10 -8 ~10 -9 The X-ray source was set to a range of 1000 torr. The excitation light was monochromated Al Kα (1486.6 eV), and the output was set to a tube current of 10 mA, a tube voltage of 15 kV, and a photoelectron take-off angle of 0°. After charging correction based on the binding energy of the carbon 1s level (1486.6 eV), the background of the spectrum was removed by the Shirley method. Peak separation of the oxygen atom component was performed on the obtained carbon 1s narrow spectrum using a Gauss-Lorentz composite function (Lorentz function ratio: 30%). [Measurement conditions] Apparatus: X-ray photoelectron spectroscopy apparatus (AXIS ULTRA DLD manufactured by Shimadzu / KRATOS) Light source: Monochromatic Al Kα (1486.6 eV) Tube current: 10 mA Tube voltage: 15 kV Vacuum degree inside the apparatus: 10-8 to 10-9 torr Neutralization gun: Used Spot size: 300 μm × 700 μm Scan mode (element): Narrow (C1s, O1s, P2p) Pass energy: 20 eV Step: 0.1 eV Dwell time: 260 ms (C1s), 332 (O1s), 426 (P2p) Number of accumulations: 5 times (C1s), 10 times (O1s), 20 times (P2p) Charge correction: Carbon 1s level binding energy (284.6 eV) Background: Shirley method

[0132] (7) Ratio RCO / RCH Using an infrared spectrophotometer JASCO FT / IR 6200, infrared spectroscopy was performed on the surface of a resin composition molded article by the attenuated total reflection (ATR) method according to the measurement procedure described below, and the ratio was calculated from the obtained IR spectrum using the formula XXX. [Measurement conditions] Measurement mode: ATR method Prism: Diamond Measurement wavelength: 600 to 4000 cm -1 Number of times accumulated: 64 times RCO / RCH = 1600-1800 cm -1 In the base-corrected IR spectrum in the range of 1600 to 1800 cm -1 Maximum absorbance of the peak observed at (carbonyl C=O stretching vibration intensity) / 2700-3000 cm -1 In the base-corrected IR spectrum in the range of 2700 to 3000 cm -1 Maximum absorbance of the peak observed at (C-H stretching vibration peak intensity of alkane) ...XXX

[0133] (9) Wet Tension Wet tension was measured by dropping wetting reagents (wet tension test mixtures, manufactured by Wako Pure Chemical Industries, Ltd.) having various wetting tensions onto the surface of a resin composition molded body, spreading the wetting reagents with a cotton swab, and visually observing the spreading of the reagent. Specifically, first, a wet tension test mixture No. 65.0 with a wet tension of 65 mN / m was dropped onto the surface of the molded body and spread with a cotton swab. The state of the reagent was visually observed 20 seconds after spreading. If the reagent was repelled, the test was repeated using a wet tension test mixture with a gradually smaller wet tension in the same manner until the reagent was no longer repelled. The wet tension of the reagent used when the reagent no longer repelled was recorded as the wet tension value.

[0134] (10) Initial Adhesion <Painting Conditions> For initial adhesion, a primer (Kansai Paint Plastic Primer (NE)) was spray-coated (dry film thickness 6 μm) on the surface of the resin composition molded body using a low-pressure spray gun (ANEST IWATA LPH101-S34) at an air pressure of 0.1 MPa, and then dried at 60 ° C. for 3 minutes. Then, a water-based base paint (Kansai Paint 202 Sun Metallic) was spray-coated (dry film thickness 10 μm) using a spray gun (ANEST IWATA W101) at an air pressure of 0.25 MPa, and then dried at 60 ° C. for 3 minutes. On top of that, a clear paint (consisting of Kansai Paint HS Clear Base Main Agent, Kansai Paint HS Clear G Curing Agent, and Kansai Paint Thinner 30) was spray-coated (dry film thickness 15 μm) using a spray gun (ANEST IWATA W101) at an air pressure of 0.15 MPa. Thereafter, the coating was dried at 60° C. for 60 minutes to form a multi-layer resin film.

[0135] <Evaluation conditions> One hundred 2 mm square grids (10 vertical x 10 horizontal) were cut with a razor blade into the resin film of a resin composition molded article that had formed a multilayer resin film according to the coating conditions, and a 24 mm wide cellophane tape (registered trademark) (manufactured by Nichiban Co., Ltd.) was pressed onto the grids with the fingers. The tape was then grasped by the edge and pulled off in one go, and the number of grids remaining was evaluated as the remaining rate (%).

[0136] <Flexural Modulus> Using a Toyo Machinery Metal PLASTAR Si30 injection molding machine with a clamping force of 30 tons, rectangular injection-molded articles measuring 80 mm x 10 mm x 4 mm thick were produced under conditions of a molding temperature of 210°C, an injection speed of 20 mm / sec, and a mold temperature of 50°C, and the flexural modulus was measured in accordance with JIS K 7203. Specifically, the flexural modulus was measured at a span length of 64 mm, a juice velocity of 2.0 mm / min, and a measurement temperature of 23°C.

[0137] (Example 1) 5.0% by mass of polymer (B-1) and 95% by mass of polymer (A-1) were mixed and melt-kneaded using a 15 mm twin-screw extruder KZW15-45MG (manufactured by Technovel) under the conditions of cylinder set temperature: 210 ° C., screw rotation speed: 500 rpm, extrusion rate: about 4 kg / hour to obtain a resin composition (Q-1). The resin composition (Q-1) raw material was molded into a plate using a 220 ton injection molding machine (IS220EN, manufactured by Toshiba Machine Co., Ltd.) under the conditions of cylinder set temperature: 210 ° C., injection speed: 31 mm / sec, thickness: 2 mm, length: 150 mm, width: 70 mm, to obtain a resin composition molded body.

[0138] Example 2 The same procedure as in Example 1 was carried out except that 10% by mass of the polymer (B-1) and 90% by mass of the polymer (A-2) were used.

[0139] Comparative Example 1 The procedure was the same as in Example 1, except that 100% by mass of the polymer (A-1) was used.

[0140] (Comparative Example 2) Polymer (A-1) was melt-kneaded using a 15 mm twin-screw extruder KZW15-45MG (manufactured by Technovel) under conditions of cylinder set temperature: 210 ° C., screw rotation speed: 500 rpm, and extrusion rate: approximately 4 kg / hour to obtain a resin composition (Q-1). The resin composition (Q-1) raw material was molded using a 220 ton injection molding machine (IS220EN, manufactured by Toshiba Machine Co., Ltd.) under conditions of cylinder set temperature: 210 ° C., injection speed: 31 mm / sec, thickness: 2 mm, length: 150 mm, and width: 70 mm to obtain a resin composition molded article. The obtained resin composition molded article was subjected to plasma treatment using an NVC-103 (manufactured by Nitto Denshi) under conditions of an oxygen-containing argon gas atmosphere, 100 W, and 5 minutes.

[0141] The results are shown in Table 1.

[0142]

[0143] 10...resin composition molded body, 20...resin film, 22...primer layer, 23...top coat layer, 24...base layer, 26...clear layer, and 100...resin film-applied resin composition molded body.

Claims

1. A resin composition for a molded article to be provided with a resin film on its surface, comprising an olefin polymer A and a polyhydroxyalkanoate polymer B, wherein the content of the olefin polymer A is 51 to 99.9 parts by mass and the content of the polyhydroxyalkanoate polymer B is 0.1 to 49 parts by mass relative to a total of 100 parts by mass of the olefin polymer A and the polyhydroxyalkanoate polymer B.

2. The resin composition according to claim 1, wherein the content of the olefin polymer A is 60.1 to 99.9 parts by mass and the content of the polyhydroxyalkanoate polymer B is 0.1 to 39.9 parts by mass, relative to 100 parts by mass in total of the olefin polymer A and the polyhydroxyalkanoate polymer B.

3. The resin composition according to claim 1 or 2, wherein the polyhydroxyalkanoate polymer B is a poly(3-hydroxyalkanoate) polymer.

4. The resin composition according to any one of claims 1 to 3, wherein the polymer A is a propylene-based polymer.

5. An injection molded article made from the resin composition according to any one of claims 1 to 4.

6. An extrusion molded product of the resin composition according to any one of claims 1 to 4.

7. An article comprising a resin composition molded body and a resin film provided on a surface of the resin composition molded body, wherein the resin composition molded body contains an olefin polymer A and a polyhydroxyalkanoate polymer B, and the content of the olefin polymer A is 51 to 99.9 parts by mass and the content of the polyhydroxyalkanoate polymer B is 0.1 to 49 parts by mass per 100 parts by mass in total of the olefin polymer A and the polyhydroxyalkanoate polymer B.

Citation Information

Patent Citations

  • Color mosaic filter

    JP1989090403A

  • Color mosaic filter

    JP1989091102A

  • Color mosaic filter

    JP1989094301A

  • Color filter

    JP1993333207A

  • Manufacture of color filter array having finished coat layer, which can be patternized