Curable fluorosilicone rubber composition

The curable fluorosilicone rubber composition, featuring organohydrogenpolysiloxane and α,ω-organopolysiloxane diol, addresses the adhesion issues between fluorosilicone and dimethylsilicone rubber layers, ensuring strong interfacial bonding and preventing delamination in applications like turbo hoses.

WO2024232369A1PCT designated stage expired Publication Date: 2024-11-14SHIN ETSU CHEMICAL CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017019
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-10
Filing Date
2024-05-08
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The existing fluorosilicone rubber compositions exhibit poor adhesion with dimethylsilicone rubber when laminated and cured, leading to potential delamination issues, particularly in applications like turbo hoses, where a two-layer structure is required for optimal performance.

Method used

A curable fluorosilicone rubber composition is developed, incorporating organohydrogenpolysiloxane with a trifluoropropyl group and α,ω-organopolysiloxane diol, along with fine powder silica and an organic peroxide curing agent, to enhance interfacial adhesion with dimethylsilicone rubber, allowing for suitable use in two-layer structures under various molding conditions.

Benefits of technology

The composition achieves excellent adhesion between fluorosilicone and dimethylsilicone rubber layers, preventing delamination and ensuring the durability and performance of materials in applications like turbo hoses, even under low-pressure molding conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

Provided is a fluorosilicone rubber composition for a fluorosilicone rubber having excellent interfacial adhesion to a dimethyl silicone rubber. The fluorosilicone rubber composition comprises: (A) 100 parts by mass of a raw rubber-like organopolysiloxane having at least one fluoroalkyl group or fluoropolyether group in one molecule and at least one C2-8 alkenyl group in one molecule and having an average degree of polymerization of at least 1,000; (B) 10-60 parts by mass of fine powder silica having a BET specific surface area of at least 50 m2 / g; (C) 0.1-30 parts by mass of an organo-hydrogen polysiloxane having at least one methyl trifluoropropyl siloxane unit and at least one methyl hydrogen siloxane unit in one molecule; (D) 0.5-30 parts by mass of an α,ω-organopolysiloxanediol having a degree of polymerization of 1-30; and (E) a required amount of an organic peroxide curing agent.
Need to check novelty before this filing date? Find Prior Art

Description

Curable fluorosilicone rubber composition

[0001] The present invention relates to a fluorosilicone rubber composition that provides a fluorosilicone rubber that has excellent adhesion, particularly to dimethylsilicone rubber.

[0002] Fluorosilicone rubber has excellent heat resistance, cold resistance, oil resistance, fuel resistance, compression recovery, and other properties, and is widely used in transportation equipment parts such as automobiles and aircraft, as well as petroleum and marine transport equipment parts. When used in automobiles, particularly as turbo hose material, it is sometimes molded into a two-layer structure consisting of a dimethylsilicone rubber composition and a fluorosilicone rubber composition. The inner layer of the turbo hose requires particular oil resistance, so fluorosilicone rubber is selected. Meanwhile, the outer layer of the turbo hose has superior resilience and ironing resistance to fluorosilicone rubber, resulting in a two-layer structure of dimethylsilicone rubber and fluorosilicone rubber for the entire hose material. However, due to differences in compatibility between the two compositions, even when the fluorosilicone rubber composition and the dimethylsilicone rubber composition are laminated and cured, the adhesion at the interface is very poor and the hose is prone to peeling.

[0003] Therefore, Patent Document 1 describes an invention in which the adhesion between dimethylsilicone rubber and fluorosilicone rubber is improved by adding to a fluorosilicone rubber composition an organopolysiloxane having a branched structure (T units) and having a viscosity of 2,000 mPa·s or less at 25° C. However, the invention of Patent Document 1 requires the addition of a relatively large amount of the organopolysiloxane, and as a result, the rubber itself may not ultimately achieve the desired physical strength or elongation.

[0004] Patent Document 2 describes an invention in which a fluorosilicone rubber composition containing an organohydrogenpolysiloxane is co-vulcanized with a dimethylsilicone rubber composition, but the adhesive strength between the fluorosilicone rubber composition and the dimethylsilicone rubber composition was not sufficient.

[0005] Patent Document 3 describes a method for manufacturing a laminate of fluorosilicone rubber and silicone rubber, in which the fluorosilicone rubber is first cured by a hydrosilylation reaction, and then a silicone rubber composition containing a fluorine-free organopolysiloxane and an organic peroxide is laminated on the surface, and the silicone rubber composition is then cured. However, this method requires that the fluorosilicone rubber be cured in advance, making the process complicated.

[0006] Japanese Patent Application Laid-Open No. 2006-328303 Japanese Patent Application Laid-Open No. 2010-126712 International Publication No. 2020-022406

[0007] Therefore, an object of the present invention is to provide a fluorosilicone rubber composition that, when laminated together with a dimethylsilicone rubber composition and a fluorosilicone rubber composition, yields a fluorosilicone rubber that exhibits excellent adhesion at the interface with the dimethylsilicone rubber when cured, as well as a laminate (laminate structure) of fluorosilicone rubber and dimethylsilicone rubber that is made from a cured product of the fluorosilicone rubber composition.

[0008] As a result of extensive research conducted by the inventors in order to achieve the above object, they discovered that by adding specific amounts of an organohydrogenpolysiloxane having trifluoropropyl groups and an α,ω-organopolysiloxanediol having no fluorine atoms to a fluorosilicone rubber composition, a fluorosilicone rubber with excellent interfacial adhesion with dimethylsilicone rubber can be obtained, leading to the completion of the present invention.

[0009] Accordingly, the present invention provides the following fluorosilicone rubber composition, and a laminate of fluorosilicone rubber and dimethylsilicone rubber, which is made from a cured product of the fluorosilicone rubber composition: [1] (A) 100 parts by mass of a raw rubber-like organopolysiloxane having an average degree of polymerization of 1,000 or more and containing one or more fluoroalkyl or fluoropolyether groups per molecule and one or more alkenyl groups having 2 to 8 carbon atoms per molecule; (B) a cured product of the fluorosilicone rubber composition having a BET specific surface area of ​​50 m 2 / g or more: 10 to 60 parts by mass of finely powdered silica, (C) the following formulas (1) and (2): (D) 0.1 to 30 parts by mass of an organohydrogenpolysiloxane having one or more siloxane units represented by the following formula (3): (In formula (3), R 1 are each independently a group selected from alkyl groups having 1 to 8 carbon atoms and aryl groups having 6 to 10 carbon atoms, and p is a number in the range of 1 to 30.) 0.5 to 30 parts by mass of an α,ω-organopolysiloxanediol represented by the formula (I), and (E) a required amount of an organic peroxide curing agent. [2] The curable fluorosilicone rubber composition according to [1], wherein component (A) is a raw rubber-like organopolysiloxane represented by any one of formulas (4) to (6): (In formulas (4) to (6), R 2 are each independently an alkyl group having 1 to 8 carbon atoms or an alkenyl group having 2 to 8 carbon atoms, each Rf is independently a perfluoroalkyl group having 1 to 10 carbon atoms or a perfluoropolyether group having 3 to 30 carbon atoms, each X is independently a divalent organic group, each m is independently a number from 0 to 200, and each n is independently a number from 1,000 to 10,000, with the proviso that 1,000≦m+n≦10,000.) [3] The curable fluorosilicone rubber composition according to [1] or [2], wherein component (C) is an organohydrogenpolysiloxane represented by the following formula (15): (In formula (15), R 2 are each independently an alkyl group having 1 to 8 carbon atoms or an alkenyl group having 2 to 8 carbon atoms, x is a number of 1 or more, and y is a number of 1 or more.) [4] A laminate having a fluorosilicone rubber layer formed from the curable fluorosilicone rubber composition according to any one of [1] to [3], and a dimethylsilicone rubber layer formed from a dimethylsilicone rubber composition.

[0010] The cured product of the curable fluorosilicone rubber composition of the present invention exhibits excellent adhesion at the interface between the fluorosilicone and dimethylsilicone rubber when press-vulcanized, even when the molding pressure is low, such as in steam vulcanization or atmospheric hot air vulcanization, making it suitable for use as a material for automotive turbo hoses, particularly those molded with a two-layer structure of fluorosilicone rubber and dimethylsilicone rubber. Furthermore, because the curable fluorosilicone rubber composition of the present invention has better compatibility with dimethylsilicone rubber compositions than ordinary fluorosilicone rubber compositions, it can also be used in blends with organosilicone rubber compositions without causing delamination.

[0011] 1A is a schematic diagram illustrating a method for measuring the adhesive strength of a two-layer laminate of fluorofluorosilicone rubber and dimethylsilicone rubber according to the present invention, and FIG. 1B is a diagram showing the state during adhesive strength measurement.

[0012] The present invention will be described in detail below, but the present invention is not limited thereto. Note that the "base compound" refers to a mixture of components (A), (B), and (D).

[0013] [(A) Raw Rubber-Like Organopolysiloxane] In the present invention, component (A) is the main component (base polymer) in the composition, and is a raw rubber-like organopolysiloxane having one or more fluoroalkyl groups or fluoropolyether groups per molecule and one or more alkenyl groups having 2 to 8 carbon atoms per molecule. Component (A) differs from component (C), described below, in that it does not have any hydrogen atoms bonded to silicon atoms.

[0014] The raw rubber-like organopolysiloxane of component (A) has an average degree of polymerization of 1,000 or more, preferably 1,000 to 100,000, more preferably 2,000 to 50,000, and particularly preferably 2,000 to 10,000. An average degree of polymerization of less than 1,000 is undesirable because the silicone rubber composition of the present invention will no longer satisfy the properties required for millable rubber and roll kneading properties, etc., will be significantly impaired. In the present invention, the average degree of polymerization is calculated from the weight average molecular weight in terms of polystyrene in GPC (gel permeation chromatography) analysis measured under the following conditions:

[0015] [Measurement conditions] Developing solvent: tetrahydrofuran (THF) Flow rate: 1 mL / min Detector: refractive index detector (RI) Column: 4 TSKGEL SUPERMULTIPORE HZ-H columns (manufactured by Tosoh Corporation) Column temperature: 25°C Sample injection volume: 10 μL (THF solution with a concentration of 0.1% by mass) In the present invention, the component (A) is preferably a non-liquid organopolysiloxane gum that has a high degree of polymerization (high viscosity) and does not have self-flowing properties at room temperature (25°C).

[0016] The proportion of siloxane units having a fluoroalkyl group or a fluoropolyether group to the total number of siloxane units in component (A) is preferably 40% or more, more preferably 45% or more. The upper limit of the proportion of siloxane units having a fluoroalkyl group or a fluoropolyether group is not particularly limited as long as it is 100% or less, preferably less than 100%, more preferably 99.8% or less, and may even be 98% or less.

[0017] Preferred examples of component (A) include crude rubber-like organopolysiloxanes represented by any of the following formulas (4) to (6).

[0018]

[0019] In formulas (4) to (6), R 2are each independently an alkyl group having 1 to 8 carbon atoms or an alkenyl group having 2 to 8 carbon atoms, Rf are each independently a perfluoroalkyl group having 1 to 10 carbon atoms or a perfluoropolyether group having 3 to 30 carbon atoms, X is a divalent organic group, m is a number from 0 to 200, n is a number from 1,000 to 10,000, and m+n is 1,000 to 10,000. 2 At least one of the groups is an alkenyl group having 2 to 8 carbon atoms.

[0020] R 2 Examples of the alkyl group having 1 to 8 carbon atoms include alkyl groups such as methyl, ethyl, propyl, and butyl, and cycloalkyl groups such as cyclohexyl, and examples of the alkenyl group having 2 to 8 carbon atoms include vinyl, allyl, butenyl, and hexenyl. 2 Among these, in the case of an alkyl group, a methyl group is preferred, and in the case of an alkenyl group, a vinyl group is preferred.

[0021] The perfluoroalkyl group having 1 to 10 carbon atoms represented by Rf is a group represented by the following formula C k F 2k+1 - (k is an integer of 1 to 10). Examples of the perfluoropolyether group having 3 to 30 carbon atoms for Rf include those represented by the following formula: (wherein s and t are each an integer of 1 to 9) Examples of the divalent organic group for X include groups represented by the following formulas. (* indicates the bonding site to the Rf group, and ** indicates the bonding site to the silicon atom.)

[0022] In the curable fluorosilicone rubber composition of the present invention, the content of component (A) is preferably 50 to 90 mass %, more preferably 60 to 90 mass %, and even more preferably 65 to 85 mass %.

[0023] [(B) Finely powdered silica] Component (B) is a reinforcing filler that is essential for obtaining a curable fluorosilicone rubber composition with excellent mechanical strength. This finely powdered silica has a BET specific surface area of ​​50 m 2 / g or more, preferably 100 to 400m 2 / g. Examples of this finely powdered silica include fumed silica (dry silica), fired silica, and precipitated silica (wet silica). The surface of these finely powdered silicas may be hydrophobized with organopolysiloxane, organopolysilazane, chlorosilane, alkoxysilane, or the like. These finely powdered silicas may be used alone or in combination of two or more.

[0024] The amount of finely powdered silica blended is characterized by being 10 to 60 parts by mass per 100 parts by mass of component (A), and preferably 20 to 50 parts by mass. An amount less than 10 parts by mass is too small to achieve a sufficient reinforcing effect, while an amount greater than 60 parts by mass is undesirable because it results in poor processability and also reduces the physical properties of the resulting silicone rubber.

[0025] [(C) Organohydrogenpolysiloxane] The organohydrogenpolysiloxane of component (C) is the most important component for achieving adhesion to a dimethylsilicone interface. In the present invention, the organohydrogenpolysiloxane of component (C) has a different purpose of use from the crosslinking agents compounded in typical addition-curable silicone rubber compositions. This organohydrogenpolysiloxane contains at least one unit (bifunctional siloxane unit) represented by the following formulas (1) and (2) per molecule, preferably at least two (e.g., 2 to 100), and more preferably 3 to 50 of each.

[0026]

[0027] The siloxane unit (methyltrifluoropropylsiloxane unit) represented by formula (1) above enhances the affinity with fluorosilicone, while the siloxane unit (methylhydrogensiloxane unit) represented by formula (2) enhances the affinity with dimethylsilicone. Therefore, by incorporating component (C) into fluorosilicone, the siloxane unit represented by formula (2) is preferentially present at the interface, thereby enhancing the affinity with dimethylsilicone at the fluorosilicone interface. Generally, in molding methods that apply a certain pressure during molding, such as press vulcanization, co-vulcanization at the interface results in strong adhesion, making interfacial delamination less likely to occur. However, since steam vulcanization and atmospheric hot air vulcanization are more suitable for molding hose materials, the composition of the present invention incorporating component (C) is more effective because component (C) reduces interfacial delamination even when the molding pressure is low. It is preferable that component (C) have a viscosity of 2,000 mPa·s or less at 25°C. If the viscosity of component (C) exceeds 2,000 mPa·s, the dispersibility of the component (C) when added to a base compound may be poor, or the surface may no longer have a portion that preferentially has one of the functional groups, making it difficult to achieve an effect on interfacial adhesion.

[0028] The proportion of methyltrifluoropropylsiloxane units represented by the above formula (1) in one molecule (i.e., the ratio of the number of methyltrifluoropropylsiloxane units represented by formula (1) to the total number of siloxane units in one molecule; the same applies hereinafter) is preferably 1 to 90%, more preferably 5 to 80%. If this proportion is less than 1%, it may be difficult to achieve effective adhesion, and if it exceeds 90%, it may also be difficult to achieve effective adhesion. Furthermore, the proportion of hydrogensiloxane units represented by the above formula (2) in one molecule is preferably 1 to 90%, more preferably 5 to 80%. Again, if this proportion is less than 1%, it may be difficult to achieve effective adhesion, and if it exceeds 90%, it may also be difficult to achieve effective adhesion.

[0029] Furthermore, for the purpose of improving adhesion, component (C) may contain a monofunctional siloxane unit (vinyldimethylsiloxy unit, divinylmethylsiloxy unit, or trivinylsiloxy unit) of the following formula (7), (8), or (9), or a difunctional siloxane unit (vinylmethylsiloxane unit) of the following formula (10):

[0030] By incorporating the vinyl groups in formulas (7) to (10) into the crosslinks of the organosilicone rubber or fluorosilicone rubber, the adhesiveness of the composition containing component (C) having any of the groups represented by formulas (7) to (10) is further improved.

[0031] Representative examples of the organohydrogenpolysiloxane of component (C) include linear siloxane copolymers in which both molecular chain terminals are blocked with triorganosiloxy groups such as trimethylsiloxy groups, vinyldimethylsiloxy groups, divinylmethylsiloxy groups, and trivinylsiloxy groups, and the main chain portion composed of repeating bifunctional siloxane units is a combination of methyltrifluoropropylsiloxane units represented by formula (1) and methylhydrogensiloxane units represented by formula (2), or a combination of methyltrifluoropropylsiloxane units represented by formula (1) and methylhydrogensiloxane units and vinylmethylsiloxane units represented by formula (2). Furthermore, these siloxane copolymers can be suitably used as long as the number of silicon atoms (or degree of polymerization) per molecule is 4 to 200, preferably 8 to 100, and more preferably 20 to 50. The component (C) is preferably an organohydrogenpolysiloxane represented by the following formula (15). In formula (15), R 2 are each independently an alkyl group having 1 to 8 carbon atoms or an alkenyl group having 2 to 8 carbon atoms, x is a number of 1 or more, and y is a number of 1 or more. 2 As in the formulas (4) to (6), examples of the alkyl group having 1 to 8 carbon atoms include alkyl groups such as a methyl group, an ethyl group, a propyl group, and a butyl group, and cycloalkyl groups such as a cyclohexyl group. 2As in the formulas (4) to (6), examples of the alkenyl group having 2 to 8 carbon atoms include a vinyl group, an allyl group, a butenyl group, and a hexenyl group. 2 In particular, when x is an alkyl group, a methyl group is preferred, and when x is an alkenyl group, a vinyl group is preferred. In formula (15), x is preferably a number from 1 to 50, and more preferably a number from 3 to 30. In formula (15), y is preferably a number from 1 to 50, and more preferably a number from 3 to 30. Furthermore, 4≦x+y≦200 is preferred, 8≦x+y≦100 is more preferred, and 20≦x+y≦50 is even more preferred.

[0032] The blend amount of component (C) is 0.1 to 30 parts by weight, preferably 0.5 to 20 parts by weight, and more preferably 1.0 to 10 parts by weight, per 100 parts by weight of component (A).

[0033] [(D) α,ω-organopolysiloxanediol] The component (D) is an α,ω-organopolysiloxanediol represented by the following formula (3): (In the formula, R 1 are each independently a group selected from an alkyl group having 1 to 8 carbon atoms and an aryl group having 6 to 10 carbon atoms, and p is a number satisfying 1≦p≦30.

[0034] Here, R 1 Examples of the alkyl group include alkyl groups such as methyl, ethyl, propyl and butyl groups, and aryl groups such as phenyl, α-naphthyl and β-naphthyl groups, with methyl and phenyl groups being preferred.

[0035] p is a number between 1 and 30, preferably between 1 and 25, and particularly preferably between 1 and 20. If p is a number greater than 30, a large amount of component (D) must be added to achieve adhesion to the dimethyl silicone, which impairs the inherent oil resistance and fuel oil resistance of the fluorosilicone rubber.

[0036] Furthermore, component (D) is characterized by the absence of a fluorine atom-containing group (fluoroalkyl group) like the Rf group in component (A), and it is believed that component (D) migrates the organohydrogenpolysiloxane of component (C) to the interface with the dimethylsilicone, improving adhesion. The blending amount of component (D) is 0.5 to 30 parts by mass, and preferably 1 to 20 parts by mass, per 100 parts by mass of the organopolysiloxane of component (A). If the blending amount of component (D) is less than 0.5 part by mass, the desired adhesive strength with dimethylsilicone rubber will not be achieved, while if it exceeds 30 parts by mass, the oil resistance and fuel resistance inherent to fluorosilicone rubber will be impaired.

[0037] [(E) Organic Peroxide Curing Agent] The organic peroxide curing agent (E) is a component that is mixed with the other components constituting the curable fluorosilicone rubber composition of the present invention and cured by conventional methods to produce a cured product. Specific examples include benzoyl peroxide, tert-butyl perbenzoate, o-methylbenzoyl peroxide, p-methylbenzoyl peroxide, di-tert-butyl peroxide, dicumyl peroxide, 1,1-bis(tert-butylperoxy)3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne. These may be used alone or in combination of two or more. The amount of the organic peroxide curing agent may be any amount necessary to cure the composition; for example, it is preferably 0.1 to 5 parts by mass per 100 parts by mass of the total of the above components (A), (B), (C), and (D).

[0038] [Other Optional Components] The curable fluorosilicone rubber composition of the present invention may optionally contain additives such as non-reinforcing silica such as crushed quartz or diatomaceous earth, carbon black such as acetylene black, furnace black or channel black, fillers such as calcium carbonate, colorants, heat resistance improvers, flame retardancy improvers, acid acceptors, thermal conductivity improvers, and mold release agents, alkoxysilanes, diphenylsilanediol, and carbon functional silanes.

[0039] Furthermore, in the present invention, known alkoxysilanes having functional groups effective for adhesion, such as acryloxy groups, methacryloxy groups, 3-aminopropyl groups, N-2 (aminoethyl) 3-aminopropyl groups, and epoxy groups, may be added.

[0040] [Production Method] The curable fluorosilicone rubber composition of the present invention can be obtained by uniformly mixing the above-mentioned components using a rubber mixer such as a two-roll mill, a Banbury mixer, a Dew mixer (kneader), etc. A preferred method for producing the curable fluorosilicone rubber composition of the present invention is to first mix components (A), (B), and (D) to prepare a base compound, then mix component (C) into this base compound, and finally mix in component (E).

[0041] There are no particular restrictions on the molding method for the curable fluorosilicone rubber composition of the present invention, and it can be molded into the desired shape using common rubber molding methods such as compression molding, transfer molding, injection molding, extrusion molding, and calendar molding, to produce molded rubber products such as O-rings, diaphragms, packings, and gaskets. In this case, the molding method aimed at in this invention is preferably a vulcanization method such as steam vulcanization or atmospheric hot air vulcanization using extrusion molding or calendar molding. If necessary, secondary vulcanization can be carried out at 180-250°C for about 1-10 hours.

[0042] [Laminate] When the curable fluorosilicone rubber composition of the present invention is laminated with a dimethylsilicone rubber composition and cured, it can form a fluorosilicone rubber that has good adhesion to the dimethylsilicone rubber, and is therefore suitable for use in forming a laminate structure (laminate) of fluorosilicone rubber and dimethylsilicone rubber. That is, the laminate of the present invention has a fluorosilicone rubber layer composed of the curable fluorosilicone rubber composition of the present invention and a dimethylsilicone rubber layer composed of a dimethylsilicone rubber composition.

[0043] Examples of dimethylsilicone rubber compositions include, but are not limited to, organic peroxide-curing dimethylsilicone rubber compositions containing an alkenyl group-containing dimethylpolysiloxane as the main component (base polymer) and containing a silica-based inorganic filler (reinforcing filler) and an organic peroxide (curing catalyst). The dimethylsilicone rubber composition may contain the organohydrogenpolysiloxane of component (C).

[0044] Furthermore, examples of methods for producing laminated structures (laminates) of fluorosilicone rubber and dimethylsilicone rubber include dispensing the fluorosilicone rubber composition and the dimethylsilicone rubber composition into sheets using a calendar roll, then laminating and wrapping them around a mandrel, followed by steam vulcanization or atmospheric hot air vulcanization (HAV). Alternatively, the compositions can be layered and charged (filled) into a molding die, followed by compression molding. The vulcanization conditions are 100 to 200°C for 10 minutes to 2 hours for steam vulcanization, 150 to 500°C for 10 seconds to 1 hour for atmospheric hot air vulcanization (HAV), and 100 to 200°C at a pressure of 5.0 to 15.0 MPa for 1 minute to 1 hour for compression molding.

[0045] EXAMPLES The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0046] (Examples 1 and 2, Comparative Examples 1 to 3) First, a base compound was prepared by the following method.

[0047] [Base Compound A] 100 parts by mass of trifluoropropylmethylpolysiloxane A-1 represented by the following formula (11), fumed silica A (manufactured by Nippon Aerosil Co., Ltd., trade name: Aerosil 200, BET specific surface area 200 m), 2 40 parts by mass of trifluoropropylmethylpolysiloxane A-1 (1 / g) and 7 parts by mass of dimethylpolysiloxane diol D-1 represented by the following formula (12) as a dispersant were added and kneaded uniformly, followed by heat treatment at 150°C for 4 hours and kneading with a two-roll mill to obtain base compound A. (m and n are numbers that satisfy the conditions m+n=4,000 and m / (m+n)=0.001 to 0.002.) Dimethylpolysiloxanediol D-1

[0048] [Base Compound B] In the preparation of Base Compound A, 10 parts by mass of dimethylpolysiloxanediol D-2 represented by the following formula (13) was added as a dispersant instead of the dimethylpolysiloxanediol represented by the formula (12) above, and the mixture was uniformly kneaded, heat-treated at 150°C for 4 hours, and then kneaded with a two-roll mill to obtain Base Compound B. Dimethylpolysiloxanediol D-2

[0049] [Base Compound C] In the preparation of Base Compound A, instead of the dimethylpolysiloxanediol represented by the formula (12) above, 7 parts by mass of trifluoropropylmethylpolysiloxanediol D-3 represented by the following formula (14) was added as a dispersant, and the mixture was uniformly kneaded, heat-treated at 150°C for 4 hours, and then kneaded with a two-roll mill to obtain Base Compound C. Trifluoropropylmethylpolysiloxanediol D-3

[0050] Next, organohydrogensiloxane C-1 represented by the following formula (15-1) was blended into each of the above base compounds A, B, and C in the amount shown in Table 2 using a twin roll mill to obtain mixtures containing components (A) to (D). Each curable fluorosilicone rubber composition was prepared by blending 100 parts by mass of each mixture containing components (A) to (D) with 0.5 parts by mass of a paste containing 80% by mass of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane using a twin roll mill. Each resulting curable fluorosilicone rubber composition was tested for initial physical properties and adhesion using the methods described below.

[0051] Initial physical properties: The resulting curable fluorosilicone rubber composition was pressure molded at 165°C for 10 minutes and then post-cured at 200°C for 4 hours to prepare a 2mm thick sheet for measuring physical properties. The measurement method was in accordance with JIS K6249:2003.

[0052] Adhesion Test: First, the obtained curable fluorosilicone rubber composition was cut out using a twin roll roller into strips measuring 25 mm x 175 mm and 1.0 to 1.2 mm thick (hereinafter referred to as "(strip) fluorosilicone rubber"). Furthermore, a curable dimethylsilicone rubber was prepared by blending 100 parts by mass of a dimethylsilicone rubber composition (KE-561-U, manufactured by Shin-Etsu Chemical Co., Ltd.) with 0.4 parts by mass of a paste containing 80% 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane using a twin roll roller. The obtained dimethylsilicone rubber was cut out using a twin roll roller into strips measuring 25 mm x 175 mm and 1.0 to 1.2 mm thick (hereinafter referred to as "(strip) dimethylsilicone rubber"). Next, a 0.2 mm thick, 25 mm x 30 mm polytetrafluoroethylene resin sheet was placed on one of the short sides of the dimethylsilicone rubber strip, with the edge aligned. A strip of fluorosilicone rubber was then placed on top of the strip of dimethylsilicone rubber. This was press-vulcanized under the molding conditions shown in Table 2 to obtain a two-layer laminate (test piece) of fluorosilicone rubber and dimethylsilicone rubber. An end view of this two-layer laminate is shown in FIG. 1(A). The laminate had dimethylsilicone rubber 1 and fluorosilicone rubber 2, with a polytetrafluoroethylene resin sheet 3 interposed between one of the short sides of the dimethylsilicone rubber 1 and the fluorosilicone rubber 2. Next, the polytetrafluoroethylene resin sheet 3 was peeled off from the laminate, and the fluorosilicone rubber 2 was fixed with a fixture 4 as shown in FIG. 1(B). The strength of the dimethylsilicone rubber 1 when pulled at a constant speed of 50 mm / min was taken as the adhesive strength. The arrow in FIG. 1(B) indicates the direction in which the dimethylsilicone rubber 1 was pulled.

[0053]

[0054]

[0055] The results of observing the state of the test pieces after the adhesive strength test are shown in the column for peeling state in Table 2. In Table 2, for peeling state, A indicates complete cohesive failure, B indicates partial cohesive failure, and C indicates interfacial peeling (poor adhesion). Peeling state A or B was evaluated as good adhesion, and peeling state C was evaluated as poor adhesion.

[0056] The examples and comparative examples demonstrate that when the curable fluorosilicone rubber composition of the present invention is co-vulcanized with a dimethylsilicone rubber composition under the same molding conditions, it exhibits superior interfacial adhesion with the dimethylsilicone rubber compared to a composition of the present invention that uses trifluoropropylmethylpolysiloxanediol instead of component (D), a composition of the present invention that does not contain components (C) and (D), and a composition of the present invention that does not contain component (C).

[0057] REFERENCE SIGNS LIST 10 Laminate 1 Dimethyl silicone rubber 2 Fluorosilicone rubber 3 Polytetrafluoroethylene resin sheet 4 Fixing jig

Claims

1. (A) 100 parts by mass of a raw rubber-like organopolysiloxane having one or more fluoroalkyl groups or fluoropolyether groups per molecule and one or more alkenyl groups having 2 to 8 carbon atoms per molecule, and an average degree of polymerization of 1,000 or more; (B) a BET specific surface area of ​​50 m 2 / g or more: 10 to 60 parts by mass, (C) the following formulas (1) and (2): (D) an organohydrogenpolysiloxane having at least one siloxane unit represented by the following formula (3): 0.1 to 30 parts by mass (In formula (3), R 1 each independently represents a group selected from an alkyl group having 1 to 8 carbon atoms and an aryl group having 6 to 10 carbon atoms, and p is a number that satisfies 1≦p≦30; and (E) an organic peroxide curing agent: a required amount.

2. The curable fluorosilicone rubber composition according to claim 1, wherein component (A) is a raw rubber-like organopolysiloxane represented by any one of formulas (4) to (6). (In formulas (4) to (6), R 2 are each independently an alkyl group having 1 to 8 carbon atoms or an alkenyl group having 2 to 8 carbon atoms, Rf are each independently a perfluoroalkyl group having 1 to 10 carbon atoms or a perfluoropolyether group having 3 to 30 carbon atoms, X are each independently a divalent organic group, m are each independently a number from 0 to 200, and n are each independently a number from 1,000 to 10,000, with 1,000≦m+n≦10,000. 2 At least one of the groups is an alkenyl group having 2 to 8 carbon atoms.

3. A curable fluorosilicone rubber composition according to claim 1, wherein component (C) is an organohydrogenpolysiloxane represented by the following formula (15): (In formula (15), R 2 are each independently an alkyl group having 1 to 8 carbon atoms or an alkenyl group having 2 to 8 carbon atoms, x is a number of 1 or more, and y is a number of 1 or more.

Citation Information

Patent Citations

  • Production of fluoropolydiorganosiloxane-based composition

    JP1997165513A

  • Fluorosilicone rubber composition and its adhesion

    JP1997268257A

  • Fluorosilicone rubber composition

    JP2001002923A

  • Fluorosilicone rubber composition and rubber molded product

    JP2006328303A

  • Adhesion of fluorosilicone rubber

    JP2008540754A