Resist underlayer film-forming composition

The use of a polymer with a polycyclic aromatic structure and a crosslinking agent in the resist underlayer film composition addresses the issue of amine diffusion from nitrogen-containing substrates, maintaining pattern resolution and precision over time, enhancing semiconductor manufacturing accuracy.

WO2024232380A1PCT designated stage expired Publication Date: 2024-11-14NISSAN CHEM CORP
View PDF 65 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017062
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-09
Filing Date
2024-05-08
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

In semiconductor manufacturing, the use of nitrogen-containing substrates leads to diffusion of amine components, which reduces the resolution and precision of resist patterns formed by resist underlayer films, especially over time.

Method used

A composition for forming a resist underlayer film that includes a polymer with a polycyclic aromatic structure and a crosslinking agent, which helps to maintain the resolution and precision of resist patterns even when the film is formed on nitrogen-containing substrates and has aged.

Benefits of technology

The composition effectively suppresses the deterioration of resist pattern resolution over time, ensuring high accuracy and precision in microfabrication processes even after extended periods, thereby improving the quality of semiconductor elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The present invention pertains to a resist underlayer film-forming composition containing a polymer and a crosslinking agent. The polymer has a structural unit (A) having a polycyclic aromatic structure. The resist underlayer film-forming composition is for, in lithography using a photo-resist film or an electron beam-resist film, forming, on a nitrogen atom-containing substrate, an underlayer film of the resist film.
Need to check novelty before this filing date? Find Prior Art

Description

Composition for forming resist underlayer film

[0001] The present invention relates to a composition for forming a resist underlayer film, an underlayer film, and a method for producing a semiconductor device.

[0002]

[0003] With the progress of semiconductor manufacturing processes and the miniaturization of large-scale integrated circuits (LSIs), microfabrication is also being carried out in lithography using resist compositions. Specifically, a processing method is being used in which a thin film of a photoresist composition is formed on a semiconductor substrate such as a silicon wafer, and the thin film is irradiated with active light such as ultraviolet light through a mask pattern on which a device pattern is drawn, and developed, and the substrate is then etched using the obtained photoresist pattern as a protective film, thereby forming fine irregularities corresponding to the photoresist pattern on the surface of the substrate.

[0003] In order to further improve the precision of microfabrication using such resist compositions, there is a need for higher quality and improved properties of resist underlayer films. For example, when nitrogen atoms are contained in the substrate on which the resist underlayer film is formed or in the film on the substrate, amine components may diffuse from the substrate, resulting in a decrease in resist resolution (Patent Documents 1 to 3).

[0004] JP 2008-39811 A JP 2008-39815 A JP 2010-134437 A

[0005] The present invention provides a composition for forming a resist underlayer film that can form a photoresist pattern with high accuracy even when a substrate containing nitrogen atoms is used, and that can be used as an antireflective film during exposure.Furthermore, the present invention provides a composition that can suppress a decrease in the accuracy of the photoresist pattern, which would otherwise occur if, for example, several days or more pass after the resist underlayer film formed on a substrate using the composition of the present invention is formed and before the pattern is formed.

[0006] The present inventors have conducted extensive research to solve the above problems, and as a result have found that the above problems can be solved, and have completed the present invention having the following gist.

[0007] That is, the present invention encompasses the following aspects. [1] A composition for forming a resist underlayer film, comprising a polymer and a crosslinking agent, wherein the polymer has a structural unit (A) having a polycyclic aromatic structure, and is used in lithography using a photoresist film or an electron beam resist film to form an underlayer film of the resist film on a nitrogen-atom-containing substrate. [2] The composition for forming a resist underlayer film according to [1], wherein the polymer has the polycyclic aromatic structure in a side chain of the polymer. [3] The composition for forming a resist underlayer film according to [1] or [2], wherein the polycyclic aromatic structure is selected from optionally substituted naphthalene, anthracene, phenanthrene, pyrene, triphenylene, chrysene, naphthacene, biphenylene, fluorene, and carbazole. [4] The composition for forming a resist underlayer film according to any of [1] to [3], wherein the unit structure (A) is a unit structure represented by the following formula (A-1): (In formula (A-1), R 1 represents a hydrogen atom or a methyl group. 1 represents a single bond, an ester group, or an amide group. 1 represents a single bond or an alkylene group having 1 to 6 carbon atoms. Ar represents a monovalent group obtained by removing a hydrogen atom from naphthalene, anthracene, phenanthrene, pyrene, triphenylene, chrysene, naphthacene, biphenylene, fluorene, or carbazole, which may be substituted.) [5] The composition for forming a resist underlayer film according to any one of [1] to [4], wherein the polymer further has a unit structure (B) having a reactive group, and the crosslinking agent has a functional group capable of reacting with the reactive group. [6] The composition for forming a resist underlayer film according to [5], wherein the unit structure (B) is at least one of a unit structure represented by the following formula (B-1) and a unit structure represented by the following formula (B-2): (In formula (B-1), R 11 represents a hydrogen atom or a methyl group. 11 represents an ester group or an amide group. 12 represents a monovalent group having 1 to 12 carbon atoms and having the reactive group. 13represents a monovalent group having 1 to 12 carbon atoms and having the reactive group.) [7] The composition for forming a resist underlayer film according to any one of [1] to [6], wherein the polymer further has at least one unit structure (C) selected from a unit structure (C-1) having a monocyclic aromatic structure and a unit structure (C-2) derived from a maleimide structure. [8] The composition for forming a resist underlayer film according to [7], wherein the unit structure (C-1) is a unit structure represented by the following formula (C-1-1): (In formula (C-1-1), R 21 represents a hydrogen atom or a methyl group. 21 represents a single bond, an ester group, or an amide group. 21 represents a single bond or an alkylene group having 1 to 6 carbon atoms. 22 represents a halogen atom, an alkyl group having 1 to 6 carbon atoms which may be substituted with a halogen atom, or an alkoxy group having 1 to 6 carbon atoms which may be substituted with a halogen atom. n represents an integer of 0 to 5. R 22 When there are two or more, there are two or more R 22 may be the same or different. 23represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be substituted with a halogen atom, or an aryl group having 6 to 10 carbon atoms which may be substituted with a halogen atom.) [9] The composition for forming a resist underlayer film according to any one of [1] to [8], wherein the molar ratio of the unit structure (A) to all unit structures of the polymer is 40 mol % or more.

[10] The composition for forming a resist underlayer film according to any one of [5] to [9], wherein the molar ratio of the unit structure (B) to all unit structures of the polymer is 5 mol % to 40 mol %.

[11] The composition for forming a resist underlayer film according to any one of [1] to

[10] , wherein the polymer further has a unit structure (B) having a reactive group, and at least one unit structure (C) selected from a unit structure (C-1) having a monocyclic aromatic structure and a unit structure (C-2) derived from a maleimide structure; the crosslinking agent has a functional group capable of reacting with the reactive group; the unit structure (A) is a unit structure represented by the following formula (A-1); the unit structure (B) is at least one unit structure represented by the following formula (B-1) and a unit structure represented by the following formula (B-2); the unit structure (C-1) is a unit structure represented by the following formula (C-1-1); and the unit structure (C-2) is a unit structure represented by the following formula (C-2-1); the molar ratio of the unit structure (A) to all unit structures of the polymer is 40 mol % or more; and the molar ratio of the unit structure (B) to all unit structures of the polymer is 5 mol % to 40 mol %. (In formula (A-1), R 1 represents a hydrogen atom or a methyl group. 1 represents a single bond, an ester group, or an amide group. 1 represents a single bond or an alkylene group having 1 to 6 carbon atoms. Ar represents a monovalent group obtained by removing a hydrogen atom from naphthalene, anthracene, phenanthrene, pyrene, triphenylene, chrysene, naphthacene, biphenylene, fluorene, or carbazole, which may be substituted. (In formula (B-1), R 11 represents a hydrogen atom or a methyl group. 11 represents an ester group or an amide group. 12represents a monovalent group having 1 to 6 carbon atoms and having the reactive group. 13 represents a monovalent group having 1 to 6 carbon atoms and having the reactive group. (In formula (C-1-1), R 21 represents a hydrogen atom or a methyl group. 21 represents a single bond, an ester group, or an amide group. 21 represents a single bond or an alkylene group having 1 to 6 carbon atoms. 22 represents a halogen atom, an alkyl group having 1 to 6 carbon atoms which may be substituted with a halogen atom, or an alkoxy group having 1 to 6 carbon atoms which may be substituted with a halogen atom. n represents an integer of 0 to 5. R 22 When there are two or more, there are two or more R 22 may be the same or different. 23represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be substituted with a halogen atom, or an aryl group having 6 to 10 carbon atoms which may be substituted with a halogen atom.)

[12] The composition for forming a resist underlayer film according to any one of [1] to

[11] , wherein the content of the crosslinking agent is 20% by mass to 50% by mass of the polymer.

[13] An underlayer film formed on the nitrogen-atom-containing substrate using the composition for forming a resist underlayer film according to any one of [1] to

[12] .

[14] The underlayer film according to

[13] , wherein the film has a thickness of less than 10 nm.

[15] A method for producing a resist patterned substrate, comprising: forming an underlayer film on the nitrogen-atom-containing substrate using the composition for forming a resist underlayer film according to any one of [1] to

[12] ; forming a resist film, which is either a photoresist film or an electron beam resist film, on the underlayer film; and irradiating the resist film with light or an electron beam and then developing the resist film to obtain a resist pattern.

[16] A method for producing a substrate having a resist pattern according to

[15] , comprising the step of forming the resist film 12 hours or more after the formation of the underlayer film.

[17] A method for producing a semiconductor device, comprising the steps of: forming an underlayer film on the nitrogen-containing substrate using the composition for forming a resist underlayer film according to any one of [1] to

[12] , forming a resist film, which is either a photoresist film or an electron beam resist film, on the underlayer film, irradiating the resist film with light or an electron beam and then developing the resist film to obtain a resist pattern, and etching the underlayer film using the resist pattern as a mask to form a patterned underlayer film.

[0008] According to the present invention, it is possible to form a resist underlayer film that can suppress a decrease in resist resolution due to diffusion of an amine component.Furthermore, according to the present invention, it is possible to form a resist underlayer film that is resistant to a decrease in resolution even when a predetermined period of time has passed between the formation of the resist underlayer film on a substrate and the formation of a pattern.

[0009] (Composition for forming a resist underlayer film) The composition for forming a resist underlayer film of the present invention is used in lithography using a photoresist film or an electron beam resist film, for forming an underlayer film of the resist film on a nitrogen atom-containing substrate. The composition for forming a resist underlayer film of the present invention contains a polymer and a crosslinking agent. The polymer has a unit structure (A) having a polycyclic aromatic structure.

[0010] The resist underlayer film-forming composition contains a polymer and a crosslinking agent, and the polymer has a unit structure (A) having a polycyclic aromatic structure, thereby forming a resist underlayer film that can suppress a decrease in resist resolution. Furthermore, a resist underlayer film that is resistant to a decrease in resolution can be formed even after a predetermined period of time has passed since the resist underlayer film was formed. The predetermined period of time is, for example, 12 hours or more, 24 hours or more, 48 hours or more, 72 hours or more, or 92 hours or more. The storage temperature is, for example, 20°C to 30°C, and the storage humidity is, for example, 30 to 70% RH, 30 to 60% RH, or 35 to 55% RH.

[0011] <Polymer> The polymer has a unit structure (A) having a polycyclic aromatic structure. The polymer preferably has a polycyclic aromatic structure in a side chain. The polymer preferably has a unit structure (B) having a reactive group. The crosslinking agent preferably has a reactive group capable of reacting with the reactive group. Hereinafter, this polymer may be referred to as a "specific polymer."

[0012] <<Unit Structure (A)>> The unit structure (A) is a unit structure having a polycyclic aromatic structure. In this specification, the polycyclic aromatic structure refers to a structure composed of two or more aromatic rings exhibiting aromaticity, and includes a fused polycyclic aromatic structure having a fused ring, and an aromatic ring assembly structure in which multiple aromatic rings are directly bonded by single bonds. The polycyclic aromatic structure may be a structure composed only of hydrocarbons, or may be a structure having a heteroatom (e.g., an oxygen atom, a nitrogen atom, or a sulfur atom).

[0013] The condensed polycyclic aromatic structure is not particularly limited, but examples thereof include a naphthalene structure, an anthracene structure, a phenanthrene structure, a pyrene structure, a triphenylene structure, a chrysene structure, a naphthacene structure, a biphenylene structure, and a fluorene structure.

[0014] The aromatic ring assembly structure is not particularly limited, but examples thereof include a carbazole structure, a biphenyl structure, a terphenyl structure, a quaterphenyl structure, a binaphthalene structure, a phenylnaphthalene structure, a phenylfluorene structure, and a diphenylfluorene structure.

[0015] The polycyclic aromatic structure is preferably selected from optionally substituted naphthalene, anthracene, phenanthrene, pyrene, triphenylene, chrysene, naphthacene, biphenylene, fluorene, and carbazole.

[0016] The polycyclic aromatic structure (condensed polycyclic aromatic structure, aromatic ring assembly structure) may be substituted with a substituent. The optionally substituted substituent is not particularly limited, and examples thereof include a halogen atom, a hydroxy group, an alkyl group, an alkoxy group, a thiol group, a cyano group, a carboxy group, an amino group, an amide group, an alkoxycarbonyl group, and a thioalkyl group. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Examples of the alkyl group include an alkyl group having 1 to 6 carbon atoms. Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, an s-butyl group, a t-butyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, a 1-ethyl-n-propyl group, an n-hexyl group, a 1-methyl-n-pentyl group, a 2-methyl-n-pentyl group, a 3-methyl- Examples include an n-pentyl group, a 4-methyl-n-pentyl group, a 1,1-dimethyl-n-butyl group, a 1,2-dimethyl-n-butyl group, a 1,3-dimethyl-n-butyl group, a 2,2-dimethyl-n-butyl group, a 2,3-dimethyl-n-butyl group, a 3,3-dimethyl-n-butyl group, a 1-ethyl-n-butyl group, a 2-ethyl-n-butyl group, a 1,1,2-trimethyl-n-propyl group, a 1,2,2-trimethyl-n-propyl group, a 1-ethyl-1-methyl-n-propyl group, and a 1-ethyl-2-methyl-n-propyl group.Furthermore, a cyclic alkyl group can also be used as the alkyl group. Examples of cyclic alkyl groups having 1 to 10 carbon atoms include cyclopropyl, cyclobutyl, 1-methylcyclopropyl, 2-methylcyclopropyl, cyclopentyl, 1-methylcyclobutyl, 2-methylcyclobutyl, 3-methylcyclobutyl, 1,2-dimethylcyclopropyl, 2,3-dimethylcyclopropyl, 1-ethylcyclopropyl, 2-ethylcyclopropyl, cyclohexyl, 1-methylcyclopentyl, 2-methylcyclopentyl, 3-methylcyclopentyl, 1-ethylcyclobutyl, 2-ethylcyclobutyl, 3-ethylcyclobutyl, 1,2-dimethyl Examples of the alkoxy group include 1-methyl-2-cyclopropyl, 2-ethyl-1-methyl-cyclopropyl, 2-ethyl-2-methyl-cyclopropyl, and 2-ethyl-3-methyl-cyclopropyl groups. Examples of the alkoxy group include 1-methyl-2-cyclopropyl, 2-ethyl-1-methyl-cyclopropyl, 2-ethyl-2-methyl-cyclopropyl, and 2-ethyl-3-methyl-cyclopropyl groups. Examples of the alkoxy group include 1-methyl-2-cyclopropyl, 2-ethyl-1-methyl-cyclopropyl, 2-ethyl-2-methyl-cyclopropyl, and 2-ethyl-3-methyl-cyclopropyl groups. Examples of the alkoxy group include 1-methyl-2-cyclopropyl, 2-ethyl-1-methyl-cyclopropyl, and 2-ethyl-3-methyl-cyclopropyl groups. Examples of the alkoxy group include 1-methyl-2-cyclopropyl, 2-ethyl-1-methyl-cyclopropyl, and 2-ethyl-2-methyl-cyclopropyl groups. Examples of the amide group include amide groups having 1 to 12 carbon atoms. Examples of the amide group having 1 to 12 carbon atoms include formamide, acetamide, propionamide, isobutylamide, benzamide, naphthylamide, and acrylamide. Examples of the alkoxycarbonyl group include alkoxycarbonyl groups having 2 to 12 carbon atoms. Examples of the alkoxycarbonyl group having 2 to 12 carbon atoms include methoxycarbonyl, ethoxycarbonyl, and benzyloxycarbonyl.Examples of the thioalkyl group include thioalkyl groups having 1 to 6 carbon atoms, such as methylthio, ethylthio, butylthio, and hexylthio groups.

[0017] From the viewpoint of suitably obtaining the effects of the present invention, the polycyclic aromatic structure is preferably a naphthalene structure, an anthracene structure, a phenanthrene structure, a pyrene structure, a triphenylene structure, a chrysene structure, a naphthacene structure, a biphenylene structure, a fluorene structure, or a carbazole structure, more preferably a naphthalene structure, an anthracene structure, a phenanthrene structure, a pyrene structure, or a carbazole structure, and even more preferably a naphthalene structure or a carbazole structure. The polycyclic aromatic structure may be one type or two or more types, but is preferably one or two types.

[0018] The unit structure (A) is not particularly limited, but from the viewpoint of suitably obtaining the effects of the present invention, a unit structure represented by the following formula (A-1) is preferred. (In formula (A-1), R 1 represents a hydrogen atom or a methyl group. 1 represents a single bond, an ester group, or an amide group. 1 represents a single bond or an alkylene group having 1 to 6 carbon atoms. Ar represents a monovalent group obtained by removing a hydrogen atom from naphthalene, anthracene, phenanthrene, pyrene, triphenylene, chrysene, naphthacene, biphenylene, fluorene, or carbazole, which may be substituted.

[0019] The unit structure represented by formula (A-1) includes vinylnaphthalene having naphthalene as Ar in the side chain.

[0020] Examples of the substituent that Ar may have include a halogen atom, a hydroxy group, an alkyl group, an alkoxy group, a thiol group, a cyano group, a carboxy group, an amino group, an amide group, an alkoxycarbonyl group, and a thioalkyl group.

[0021] The unit structure represented by formula (A-1) is not particularly limited, but from the viewpoint of suitably achieving the effects of the present invention, the unit structure represented by the following formula (A-1-1) is preferred. (In formula (A-1-1), R 1 represents a hydrogen atom or a methyl group. 2 represents a halogen atom, a hydroxy group, an alkyl group, an alkoxy group, a thiol group, a cyano group, a carboxy group, an amino group, an amido group, an alkoxycarbonyl group, or a thioalkyl group. n represents an integer of 0 to 7. 2 When there are two or more, there are two or more R 2 may be the same or different.)

[0022] Examples of the unit structure represented by formula (A-1) include the following:

[0023] The unit structure (A) in the specific polymer may be of one or more types, preferably one or two types.

[0024] <<Unit Structure (B)>> The unit structure (B) is a unit structure having a reactive group. The unit structure (B) is a structure different from the unit structure (A). For example, the unit structure (B) does not have a polycyclic aromatic structure.

[0025] The reactive group contained in the unit structure (B) is not particularly limited, and examples thereof include a hydroxy group, an epoxy group, an acyl group, an acetyl group, a formyl group, a benzoyl group, a carboxy group, a carbonyl group, an amino group, an imino group, a cyano group, an azo group, an azido group, a thiol group, a sulfo group, and an allyl group.

[0026] The unit structure (B) is not particularly limited, but from the viewpoint of suitably obtaining the effects of the present invention, it is preferably at least one of a unit structure represented by the following formula (B-1) and a unit structure represented by the following formula (B-2): (In formula (B-1), R 11 represents a hydrogen atom or a methyl group. 11 represents an ester group or an amide group. 12represents a monovalent group having 1 to 12 carbon atoms and having a reactive group. 13 represents a monovalent group having 1 to 12 carbon atoms and having a reactive group.

[0027] R 12 and R 13 In the above formula, examples of the monovalent group having 1 to 12 carbon atoms and having a reactive group include hydroxyalkyl groups having 1 to 12 carbon atoms. Examples of the hydroxyalkyl groups having 1 to 12 carbon atoms include hydroxyalkyl groups having 1 to 6 carbon atoms. Examples of the hydroxyalkyl groups having 1 to 12 carbon atoms include hydroxymethyl groups, 1-hydroxyethyl groups, 2-hydroxyethyl groups, 1-hydroxypropyl groups, 2-hydroxypropyl groups, 3-hydroxypropyl groups, 1-hydroxybutyl groups, 2-hydroxybutyl groups, 3-hydroxybutyl groups, 4-hydroxybutyl groups, hydroxycyclohexyl groups, dihydroxycyclohexyl groups, and 3-hydroxy-1-adamantyl groups. The number of hydroxy groups in the hydroxyalkyl groups having 1 to 12 carbon atoms may be one or two or more.

[0028] Examples of the unit structure represented by formula (B-1) include the unit structure represented by formula (B-1-1) below. (In formula (B-1-1), R 11 and R 12 respectively represent R in formula (B-1). 11 and R 12 is synonymous with

[0029] Examples of the unit structure represented by formula (B-1) include the following:

[0030] Examples of the unit structure represented by formula (B-2) include the following:

[0031] Examples of unit structures containing an epoxy group as a reactive group include unit structures derived from compounds represented by general formulas (I) to (XVII) described in JP-A-2012-62365.

[0032] The unit structure (B) in a specific polymer may be of one or more types, preferably one or two types.

[0033] <<Unit Structure (C)>> The specific polymer may have a unit structure other than the unit structure (A) and the unit structure (B). From the viewpoint of suitably achieving the effects of the present invention, such a unit structure is preferably at least one of the unit structure (C) of the unit structure (C-1) having a monocyclic aromatic structure and the unit structure (C-2) derived from a maleimide structure. The unit structure (C) is a unit structure different from the unit structure (A) and the unit structure (B). For example, the unit structure (C) does not have a polycyclic aromatic structure or the reactive group possessed by the unit structure (B).

[0034] The monocyclic aromatic ring contained in the unit structure (C-1) may be an aromatic hydrocarbon ring or an aromatic heterocyclic ring, but is preferably an aromatic hydrocarbon ring. Examples of such aromatic hydrocarbon rings include a benzene ring.

[0035] The unit structure (C) is not particularly limited, but from the viewpoint of suitably obtaining the effects of the present invention, it is preferably at least one of a unit structure (C-1) represented by the following formula (C-1-1) and a unit structure (C-2) represented by the following formula (C-1-2): (In formula (C-1-1), R 21 represents a hydrogen atom or a methyl group. 21 represents a single bond, an ester group, or an amide group. 21 represents a single bond or an alkylene group having 1 to 6 carbon atoms. 22 represents a halogen atom, an alkyl group having 1 to 6 carbon atoms which may be substituted with a halogen atom, or an alkoxy group having 1 to 6 carbon atoms which may be substituted with a halogen atom. n represents an integer of 0 to 5. R 22 When there are two or more, there are two or more R 22 may be the same or different. 23 represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be substituted with a halogen atom, or an aryl group having 6 to 10 carbon atoms which may be substituted with a halogen atom.

[0036] Examples of the unit structure represented by formula (C-1-1) include a unit structure represented by formula (C-1-1-1) below and a unit structure represented by formula (C-1-1-2) below. (In formula (C-1-1-1) and formula (C-1-1-2), R 21 represents a hydrogen atom or a methyl group. 21 represents a single bond or an alkylene group having 1 to 6 carbon atoms. 22 represents a halogen atom, an alkyl group having 1 to 6 carbon atoms which may be substituted with a halogen atom, or an alkoxy group having 1 to 6 carbon atoms which may be substituted with a halogen atom. n represents an integer of 0 to 5. R 22 When there are two or more, there are two or more R 22 may be the same or different.)

[0037] In formula (C-1-1-2), n is preferably an integer of 1 to 5.

[0038] Examples of the unit structure represented by formula (C-1-1) include the following:

[0039] Examples of the unit structure represented by formula (C-1-2) include the following:

[0040] The unit structure (C) in the specific polymer may be of one or more types, preferably one or two types.

[0041] The molar ratio of the unit structure (A) to all unit structures of the specific polymer is not particularly limited, but from the viewpoint of suitably obtaining the effects of the present invention, it is preferably 40 mol% or more, more preferably 45 mol% or more, and particularly preferably 50 mol% or more. The molar ratio of the unit structure (A) to all unit structures of the specific polymer is preferably 95 mol% or less, more preferably 90 mol% or less, and particularly preferably 80 mol% or less.

[0042] When the specific polymer has the unit structure (B), the molar ratio of the unit structure (B) to all the unit structures of the specific polymer is not particularly limited, but from the viewpoint of suitably obtaining the effects of the present invention, it is preferably 5 mol% or more, more preferably 10 mol% or more, and particularly preferably 15 mol% or more. The molar ratio of the unit structure (B) to all the unit structures of the specific polymer is preferably 40 mol% or less, more preferably 35 mol% or less, and particularly preferably 30 mol% or less.

[0043] When the specific polymer has the unit structure (C), the molar ratio of the unit structure (C) to all the unit structures of the specific polymer is not particularly limited, but from the viewpoint of suitably obtaining the effects of the present invention, it is preferably 5 mol% or more, more preferably 10 mol% or more, and particularly preferably 15 mol% or more. The molar ratio of the unit structure (C) to all the unit structures of the specific polymer is preferably 40 mol% or less, more preferably 35 mol% or less, and particularly preferably 30 mol% or less.

[0044] The molar ratio of the unit structure (A) to the unit structure (B) in the specific polymer (unit structure (A) / unit structure (B)) is not particularly limited, but is preferably 1 to 9, and more preferably 1.5 to 5.

[0045] The distribution of the unit structures in the specific polymer is not particularly limited, and the specific polymer may be a block copolymer or a random copolymer.

[0046] The molecular weight of the specific polymer is not particularly limited, but the weight average molecular weight determined by gel permeation chromatography (hereinafter sometimes abbreviated as GPC) is preferably 1,500 to 100,000, and more preferably 2,000 to 50,000.

[0047] <<Method for Producing Specific Polymer>> The method for producing the specific polymer is not particularly limited, but for example, the specific polymer of the present embodiment can be obtained by reacting a carbon-carbon double bond contained in a monomer that provides unit structure (A), a carbon-carbon double bond contained in a monomer that provides unit structure (B), and a carbon-carbon double bond contained in a monomer that provides any unit structure (C).

[0048] As a polymerization method for the specific polymer, known polymerization methods such as radical polymerization, anionic polymerization, cationic polymerization, etc., and various known techniques such as solution polymerization, suspension polymerization, emulsion polymerization, and bulk polymerization can be used.

[0049] The polymerization initiator used in the polymerization is not particularly limited, and examples thereof include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2 , 2'-azobis(isobutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 1-[(1-cyano-1-methylethyl)azo]formamide, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane], and 2,2'-azobis(2-methylpropionamidine)dihydrochloride, etc., can be used.

[0050] The solvent used during polymerization is not particularly limited, and examples thereof include dioxane, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, and butyl lactate. These may be used alone or in combination.

[0051] The reaction temperature is not particularly limited, but may be, for example, 20° C. to 150° C. The reaction time is not particularly limited, but may be, for example, 1 hour to 72 hours.

[0052] The resulting solution containing the polymer can be used as is for preparing a composition for forming a resist underlayer film, or the polymer can be recovered by precipitation and isolation in a poor solvent such as methanol, ethanol, isopropanol, or water, or a mixed solvent thereof, and then used.

[0053] The content of the specific polymer in the composition for forming a resist underlayer film is not particularly limited, but from the viewpoint of solubility, it is preferably 0.1% by mass to 50% by mass, and more preferably 0.1% by mass to 10% by mass, based on the entire composition for forming a resist underlayer film. Furthermore, the content of the specific polymer in the composition for forming a resist underlayer film is preferably 50% by mass to 95% by mass, more preferably 55% by mass to 90% by mass, and particularly preferably 60% by mass to 85% by mass, based on the film-constituting components. The film-constituting components refer to components other than the solvent contained in the composition.

[0054] <Crosslinking Agent> The composition for forming a resist underlayer film contains a crosslinking agent. The crosslinking agent preferably has a functional group capable of reacting with the reactive group of the unit structure (B). The number of functional groups in the crosslinking agent is not particularly limited and may be one, or two or more.

[0055] The functional group capable of reacting with the reactive group contained in the unit structure (B) is not particularly limited, and examples thereof include a hydroxy group, an epoxy group, an acyl group, an acetyl group, a formyl group, a benzoyl group, a carboxy group, a carbonyl group, an amino group, an imino group, a cyano group, an azo group, an azido group, a thiol group, a sulfo group, an allyl group, and a structure represented by the following formula (D): (In formula (D), R 101 represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkoxyalkyl group having 2 to 6 carbon atoms. * represents a bond.) The bond is bonded to, for example, a nitrogen atom or a carbon atom constituting an aromatic hydrocarbon ring.

[0056] When the reactive group contained in the unit structure (B) is a hydroxy group or a thiol group, examples of the functional group capable of reacting with the reactive group contained in the unit structure (B) include a structure represented by formula (D).

[0057] When the reactive group of the unit structure (B) is an epoxy group, examples of the functional group capable of reacting with the reactive group of the unit structure (B) include a carboxy group, an amino group, and a thiol group.

[0058] The crosslinking agent may be, for example, a compound having two or more structures represented by the above formula (D).

[0059] R 101 is preferably a hydrogen atom, a methyl group, an ethyl group or a group represented by the following structure. (In the structure, R 102 represents a hydrogen atom, a methyl group, or an ethyl group. * represents a bond.

[0060] As the crosslinking agent, a melamine compound, a guanamine compound, a glycoluril compound, a urea compound, or a compound having a phenolic hydroxy group is preferred. These may be used alone or in combination of two or more.

[0061] The melamine compound is not particularly limited as long as it has a group capable of reacting with the reactive group (e.g., hydroxy group) of the unit structure (B). Examples of the melamine compound include hexamethylol melamine, hexamethoxymethyl melamine, a compound in which one to six methylol groups of hexamethylol melamine are methoxymethylated, or a mixture thereof, hexamethoxyethyl melamine, hexaacyloxymethyl melamine, a compound in which one to six methylol groups of hexamethylol melamine are acyloxymethylated, or a mixture thereof.

[0062] The guanamine compound is not particularly limited as long as it has a group capable of reacting with the reactive group (e.g., hydroxy group) of the unit structure (B). Examples of the guanamine compound include tetramethylolguanamine, tetramethoxymethylguanamine, a compound in which one to four methylol groups of tetramethylolguanamine are methoxymethylated, or a mixture thereof, tetramethoxyethylguanamine, tetraacyloxyguanamine, a compound in which one to four methylol groups of tetramethylolguanamine are acyloxymethylated, or a mixture thereof.

[0063] The glycoluril compound is not particularly limited as long as it has a group capable of reacting with the reactive group (e.g., hydroxy group) of the unit structure (B). Examples of the glycoluril compound include tetramethylol glycoluril, tetramethoxy glycoluril, tetramethoxymethyl glycoluril, a compound in which one to four methylol groups of tetramethylol glycoluril are methoxymethylated or a mixture thereof, and a compound in which one to four methylol groups of tetramethylol glycoluril are acyloxymethylated or a mixture thereof.

[0064] The glycoluril compound may be, for example, a glycoluril derivative represented by the following formula (1E). (In formula (1E), four R 1 each independently represents a methyl group or an ethyl group, R 2 and R 3 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a phenyl group.

[0065] Examples of the glycoluril derivative represented by the formula (1E) include compounds represented by the following formulas (1E-1) to (1E-6).

[0066] The glycoluril derivative represented by formula (1E) can be obtained, for example, by reacting a glycoluril derivative represented by the following formula (2E) with at least one compound represented by the following formula (3d).

[0067] (In formula (2E), R 2 and R 3 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a phenyl group; R 4 each independently represents an alkyl group having 1 to 4 carbon atoms.

[0068] (In formula (3d), R 1 represents a methyl group or an ethyl group.)

[0069] Examples of glycoluril derivatives represented by formula (2E) include compounds represented by formulas (2E-1) to (2E-4) below. Furthermore, examples of compounds represented by formula (3d) include compounds represented by formulas (3d-1) and (3d-2) below.

[0070] The urea compound is not particularly limited as long as it has a group capable of reacting with the reactive group (e.g., hydroxy group) of the unit structure (B). Examples of the urea compound include tetramethylol urea, tetramethoxymethyl urea, a compound in which one to four methylol groups of tetramethylol urea are methoxymethylated, or a mixture thereof, and tetramethoxyethyl urea.

[0071] Examples of the compound having a phenolic hydroxy group include compounds represented by the following formula (111) or (112). (In formula (111) and formula (112), Q 2 represents a single bond or a divalent organic group. 8 , R 9 , R 11 and R 12 R represents a hydrogen atom or a methyl group. 7 and R 10 n represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 40 carbon atoms. 9 is 1≦n 9 an integer ≦3, n 10 is 2≦n 10 an integer ≦5, n 11 is 0≦n 11 an integer ≦3, n 12 is 0≦n 12 an integer ≦3, 3≦(n 9 +n 10 +n 11 +n 12 ) represents an integer ≦6. 13 is 1≦n 13 an integer ≦3, n 14 is 1≦n 14 n is an integer ≦4 15 is 0≦n 15an integer ≦3, n 16 is 0≦n 16 an integer ≦3, 2≦(n 13 +n 14 +n 15 +n 16 ) represents an integer of ≦5. m2 represents an integer of 2 to 10. 2 In the above, the m2-valent organic group includes, for example, an m2-valent organic group having 1 to 4 carbon atoms.

[0072] Examples of the compound represented by formula (111) or formula (112) include the following compounds. The above compound is available as a product of Asahi Organic Chemicals Co., Ltd. and Honshu Chemical Industry Co., Ltd. An example of the product is TMOM-BP, a product name of Asahi Organic Chemicals Co., Ltd.

[0073] Among these, glycoluril compounds are preferred, specifically tetramethylol glycoluril, tetramethoxy glycoluril, tetramethoxymethyl glycoluril, tetramethylol glycoluril compounds in which one to four methylol groups are methoxymethylated or mixtures thereof, and tetramethylol glycoluril compounds in which one to four methylol groups are acyloxymethylated or mixtures thereof, with tetramethoxymethyl glycoluril being preferred.

[0074] The molecular weight of the crosslinking agent is not particularly limited, but is preferably 500 or less.

[0075] The content of the crosslinking agent in the composition for forming a resist underlayer film is not particularly limited, but is preferably 5% by mass to 60% by mass, more preferably 10% by mass to 55% by mass, and particularly preferably 20% by mass to 50% by mass of the specific polymer.

[0076] <Curing Catalyst> The curing catalyst contained as an optional component in the composition for forming a resist underlayer film may be either a thermal acid generator or a photoacid generator, but it is preferable to use a thermal acid generator.

[0077] Examples of the thermal acid generator include sulfonic acid compounds and carboxylic acid compounds such as p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium-p-toluenesulfonate (pyridinium-p-toluenesulfonic acid), pyridinium phenolsulfonic acid, pyridinium-p-hydroxybenzenesulfonic acid (pyridinium p-phenolsulfonate salt), pyridinium-trifluoromethanesulfonic acid, salicylic acid, camphorsulfonic acid, 5-sulfosalicylic acid, 4-chlorobenzenesulfonic acid, 4-hydroxybenzenesulfonic acid, benzenedisulfonic acid, 1-naphthalenesulfonic acid, citric acid, benzoic acid, hydroxybenzoic acid, N-methylmorpholine-p-toluenesulfonic acid, N-methylmorpholine-p-hydroxybenzenesulfonic acid, and N-methylmorpholine-5-sulfosalicylic acid.

[0078] Examples of the photoacid generator include an onium salt compound, a sulfonimide compound, and a disulfonyldiazomethane compound.

[0079] Examples of the onium salt compound include iodonium salt compounds such as diphenyliodonium hexafluorophosphate, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium nonafluoro-normal butanesulfonate, diphenyliodonium perfluoro-normal octanesulfonate, diphenyliodonium camphorsulfonate, bis(4-tert-butylphenyl)iodonium camphorsulfonate, and bis(4-tert-butylphenyl)iodonium trifluoromethanesulfonate; and sulfonium salt compounds such as triphenylsulfonium hexafluoroantimonate, triphenylsulfonium nonafluoro-normal butanesulfonate, triphenylsulfonium camphorsulfonate, and triphenylsulfonium trifluoromethanesulfonate.

[0080] Examples of the sulfonimide compound include N-(trifluoromethanesulfonyloxy)succinimide, N-(nonafluoronormalbutanesulfonyloxy)succinimide, N-(camphorsulfonyloxy)succinimide, and N-(trifluoromethanesulfonyloxy)naphthalimide.

[0081] Examples of the disulfonyldiazomethane compound include bis(trifluoromethylsulfonyl)diazomethane, bis(cyclohexylsulfonyl)diazomethane, bis(phenylsulfonyl)diazomethane, bis(p-toluenesulfonyl)diazomethane, bis(2,4-dimethylbenzenesulfonyl)diazomethane, and methylsulfonyl-p-toluenesulfonyldiazomethane.

[0082] The curing catalyst may be used alone or in combination of two or more.

[0083] When a curing catalyst is used, the content of the curing catalyst is, for example, 0.1% by mass to 50% by mass, and preferably 1% by mass to 30% by mass, relative to the crosslinking agent.

[0084] <Other Components> A surfactant may be further added to the composition for forming a resist underlayer film in order to prevent pinholes, striations, and the like from occurring and to further improve the coatability against surface irregularities.

[0085] Examples of surfactants include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether; polyoxyethylene alkylaryl ethers such as polyoxyethylene octylphenol ether and polyoxyethylene nonylphenol ether; polyoxyethylene-polyoxypropylene block copolymers; sorbitan fatty acid esters such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan trioleate, and sorbitan tristearate; polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate; nonionic surfactants such as polyoxyethylene sorbitan fatty acid esters, such as polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan tristearate; fluorine-based surfactants such as Eftop EF301, EF303, and EF352 (trade names, manufactured by Tochem Products Co., Ltd.), Megafac F171, F173, and R-30 (trade names, manufactured by DIC Corporation), Fluorad FC430 and FC431 (trade names, manufactured by Sumitomo 3M Limited), Asahiguard AG710, Surflon S-382, SC101, SC102, SC103, SC104, SC105, and SC106 (trade names, manufactured by AGC Inc.); and organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.). The amount of these surfactants to be added is not particularly limited, but is usually 2.0 mass % or less, and preferably 1.0 mass % or less, based on the composition for forming a resist underlayer film. These surfactants may be added alone or in combination of two or more.

[0086] <Solvent> The composition for forming a resist underlayer film may contain a solvent. As the solvent, an organic solvent generally used in a chemical solution for a semiconductor lithography process is preferred. Specifically, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, cyclohexane, cyclohexane-1, cyclohexane-2, cyclohexane-3, cyclohexane-4, cyclohexane-5, cyclohexane-6, cyclohexane-7, cyclohexane-8, cyclohexane-9, cyclohexane-11, cyclohexane-12, cyclohexane-13, cyclohexane-14, cyclohexane-15, cyclohexane-16, cyclohexane-17, cyclohexane-18, cyclohexane-19, cyclohexane-20, cyclohexane-21, cyclohexane-22, cyclohexane-23, cyclohexane-24, cyclohexane-25, cyclohexane-26, cyclohexane-27, cyclohexane-28, cyclohexane-29, cyclohexane-30, cyclohexane-31, cyclohexane-32, cyclohexane-33, cyclohexane-34, cyclohexane-35, cyclohexane-36, cyclohexane-37, cyclohexane-38, cyclohexane-39, cyclohexane-40, cyclohexane-41, cyclohexane-42, cyclohexane-43, cyclohexane-44, cyclohexane-45, cyclohexane-45, cyclohexane-46, cyclohexane-47, cyclohexane-48, cyclohexane-49, cyclohexane-51, cyclohexane Examples of suitable solvents include heptanone, 4-methyl-2-pentanol, methyl 2-hydroxyisobutyrate, ethyl 2-hydroxyisobutyrate, ethyl ethoxyacetate, 2-hydroxyethyl acetate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, 2-heptanone, methoxycyclopentane, anisole, γ-butyrolactone, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide. These solvents may be used alone or in combination of two or more.

[0087] Among these solvents, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, ethyl lactate, butyl lactate, and cyclohexanone are preferred, with propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate being particularly preferred.

[0088] The content of the solvent in the composition for forming a resist underlayer film is not particularly limited, but is preferably 80% by mass to 99.99% by mass, more preferably 90% by mass to 99.95% by mass, and particularly preferably 95% by mass to 99.9% by mass.

[0089] <Nitrogen Atom-Containing Substrate> The substrate on which the underlayer film of the resist film is formed using the resist underlayer film-forming composition of the present invention as described above is a nitrogen atom-containing substrate. Examples of nitrogen atom-containing substrates include substrates made of a compound having a bond between a metal atom or a metalloid atom and a nitrogen atom, and substrates having a nitrogen atom-containing film made of a compound having a bond between a metal atom or a metalloid atom and a nitrogen atom. Nitrogen atoms may be contained in both the substrate and the film on the substrate. The metal atom is not particularly limited, and examples thereof include titanium, gallium, tungsten, hafnium, zirconium, aluminum, copper, etc. The metalloid atom is not particularly limited, and examples thereof include boron, silicon, germanium, arsenic, antimony, tellurium, etc.

[0090] For example, examples of the substrate include silicon wafers, germanium wafers, and compound semiconductor wafers such as gallium arsenide, indium phosphide, gallium nitride, indium nitride, and aluminum nitride. Among these, examples of substrates made of compounds having bonds with nitrogen atoms include gallium nitride, indium nitride, and aluminum nitride. Furthermore, when a film is formed on the substrate, examples of the film include polysilicon films, silicon oxide films, silicon nitride films, BPSG (Boro-Phospho Silicate Glass) films, titanium nitride films, titanium nitride oxide films, tungsten films, gallium nitride films, and gallium arsenide films formed by, for example, ALD (atomic layer deposition), CVD (chemical vapor deposition), reactive sputtering, ion plating, vacuum deposition, and spin coating (spin-on glass: SOG). Among these, examples of nitrogen-atom-containing films made of compounds having bonds with nitrogen atoms include silicon nitride films, titanium nitride films, titanium nitride oxide films, and gallium nitride films.

[0091] The upper limit of the film thickness of the nitrogen atom-containing film is, for example, 200 nm, 150 nm, or 100 nm, and the lower limit is 5 nm or 10 nm.

[0092]

[0013] Conventionally, when a resist film is formed on the above-mentioned nitrogen-atom-containing substrate and then irradiated with light or an electron beam to obtain a resist pattern, the precision of the pattern may be reduced. This is thought to be due to the diffusion of amine components derived from the nitrogen-atom-containing substrate from the substrate side to the resist side in some process. In contrast, when an underlayer film is formed using the composition for forming a resist underlayer film of the present invention, it is possible to suppress the above-mentioned reduction in precision of the photoresist pattern.

[0093] The underlayer film of the present invention (also referred to as a resist underlayer film) is a cured product of the composition for forming a resist underlayer film described above. The resist underlayer film can be produced, for example, by applying the composition for forming a resist underlayer film described above onto a nitrogen atom-containing substrate and baking the applied composition.

[0094] Specifically, the composition for forming a resist underlayer film of the present invention is applied to a nitrogen-atom-containing substrate by a suitable application method such as a spinner or coater. The underlayer film is then formed by baking using a heating means such as a hot plate. The baking conditions are appropriately selected from a baking temperature of 100°C to 400°C and a baking time of 0.3 to 60 minutes. A baking temperature of 120°C to 350°C and a baking time of 0.5 to 30 minutes are preferred, and a baking temperature of 150°C to 300°C and a baking time of 0.8 to 10 minutes are more preferred.

[0095] The thickness of the underlayer film may be, for example, 0.001 μm (1 nm) to 10 μm, 0.002 μm (2 nm) to 1 μm, 0.005 μm (5 nm) to 0.5 μm (500 nm), 0.001 μm (1 nm) to 0.05 μm (50 nm), 0.002 μm (2 nm) to 0.05 μm (50 nm), 0.003 μm (3 nm) to 0.05 μm (50 nm), 0.004 μm (4 nm) to 0.05 μm (50 nm), 0.005 μm (5 nm) to 0.05 μm (50 nm), 0.003 μm (3 nm) to 0.05 μm (50 nm), 0.003 μm (3 nm) to 0.01 μm (10 nm), 0.005 μm (5 nm) to 0.02 μm (20 nm), 0.005 μm (5 nm) to 0.02 μm (20 nm), 0.003 μm (3 nm) to 0.01 μm (10 nm), 0.005 μm (5 nm) to 0.01 μm (10 nm), 0.003 μm (3 nm) to 0.006 μm (6 nm), 0.003 μm (3 nm) to 0.01 μm (10 nm), or 0.005 μm (5 nm).

[0096] The method for measuring the thickness of the underlayer film in this specification is as follows: Measurement device name: Ellipso film thickness measurement device RE-3100 (SCREEN Corporation) SWE (single wavelength ellipsometer) mode Arithmetic mean of 8 points (for example, measuring 8 points at 1 cm intervals in the X direction of the wafer)

[0097] (Method for manufacturing a semiconductor device) The method for manufacturing a semiconductor device of the present invention includes at least the following steps: forming an underlayer film on a nitrogen atom-containing substrate using the composition for forming a resist underlayer film of the present invention, forming a resist film, which is either a photoresist film or an electron beam resist film, on the underlayer film, irradiating the resist film with light or an electron beam, and then developing the resist film to obtain a resist pattern, and etching the underlayer film using the resist pattern as a mask to form a patterned underlayer film.

[0098] Typically, a resist film is formed on the underlayer film. The thickness of the resist film is, for example, 3,000 nm or less, 2,000 nm or less, 1,800 nm or less, 1,500 nm or less, or 1,000 nm or less. The lower limit is 100 nm, 80 nm, 50 nm, 30 nm, 20 nm, or 10 nm.

[0099] The resist film formed on the underlayer film by a known method (e.g., coating and baking a resist composition) is not particularly limited as long as it is responsive to light or electron beam (EB) irradiation. Both negative and positive photoresists can be used. In this specification, resists responsive to EB are also referred to as photoresists. Examples of photoresists include positive photoresists composed of a novolak resin and a 1,2-naphthoquinone diazide sulfonic acid ester; chemically amplified photoresists composed of a binder having a group that decomposes in the presence of an acid to increase the alkaline dissolution rate and a photoacid generator; chemically amplified photoresists composed of a low-molecular-weight compound that decomposes in the presence of an acid to increase the alkaline dissolution rate of the photoresist, an alkali-soluble binder, and a photoacid generator; chemically amplified photoresists composed of a binder having a group that decomposes in the presence of an acid to increase the alkaline dissolution rate, a low-molecular-weight compound that decomposes in the presence of an acid to increase the alkaline dissolution rate of the photoresist, and a photoacid generator; and resists containing metal elements. Examples of such photoresists include V146G (trade name) manufactured by JSR Corporation, APEX-E (trade name) manufactured by Shipley Co., Ltd., PAR710 (trade name) manufactured by Sumitomo Chemical Co., Ltd., and AR2772 and SEPR430 (trade names) manufactured by Shin-Etsu Chemical Co., Ltd. Further examples include fluorine-containing polymer photoresists such as those described in Proc. SPIE, Vol. 3999, 330-334 (2000), Proc. SPIE, Vol. 3999, 357-364 (2000), and Proc. SPIE, Vol. 3999, 365-374 (2000).

[0100] Also, WO2019 / 188595, WO2019 / 187881, WO2019 / 187803, WO2019 / 167737, WO2019 / 167725, WO2019 / 187445, WO2019 / 167419, WO2019 / 123842, WO2019 / 054282, WO2019 / 058945, WO2019 / 058890, WO2019 / 039290, WO2019 / 044259, WO2019 / 044231, WO2019 / 026549, WO2018 / 193954, WO201 9 / 172054, WO2019 / 021975, WO2018 / 230334, WO2018 / 194123, JP 2018-180525, WO2018 / 190088, JP 2018-070596, JP 2018-028090, JP 2016-153409, JP 2016-130240, JP 2016-108325, JP 2016-047920, JP 2016-035570, JP 2016-035567, JP 2016-035565, JP 2019-101417, JP 2019-117373, JP 2019-052294, JP 2019-008280, JP 2019-008279, JP 2019-003176, JP 2019-003175, JP 2018-197853, JP 2019-191298, JP 2019-061217, JP 2018-045152, JP 2018-022039, JP 2016-090441, JP 2015-10878, JP 2012-168279, JP 2012-022261, JP 2012-022258, JP 2011-043749, JP 2010-18 1857, JP 2010-128369, WO2018 / 031896, JP 2019-113855, WO2017 / 156388, WO2017 / 066319, JP 2018-41099, WO2016 / 065120, WO2015 / 026482, JP 2016-29498, JP 2011-253185, etc., radiation-sensitive resin compositions, so-called resist compositions such as high-resolution patterning compositions based on organometallic solutions, and metal-containing resist compositions can be used, but are not limited to these.

[0101] Examples of the resist composition include the following compositions.

[0102] An actinic ray-sensitive or radiation-sensitive resin composition comprising: Resin A having a repeating unit having an acid-decomposable group in which a polar group is protected with a protecting group that is cleaved by the action of an acid; and a compound represented by the following general formula (121):

[0103] In the general formula (121), m represents an integer of 1 to 6. 1 and R 2 each independently represents a fluorine atom or a perfluoroalkyl group. 1 is -O-, -S-, -COO-, -SO 2 - or -SO 3 - represents. 2 represents an alkylene group which may have a substituent or a single bond. 1 represents a cyclic organic group which may have a substituent. + represents a cation.

[0104] A metal-containing film-forming composition for extreme ultraviolet or electron beam lithography, comprising a compound having a metal-oxygen covalent bond and a solvent, wherein the metal element constituting the compound belongs to Periods 3 to 7 of Groups 3 to 15 of the periodic table.

[0105] A radiation-sensitive resin composition comprising: a polymer having a first structural unit represented by the following formula (31) and a second structural unit represented by the following formula (32) containing an acid-dissociable group; and an acid generator.

[0106] In formula (31), Ar is a group obtained by removing (n+1) hydrogen atoms from an arene having 6 to 20 carbon atoms. 1 is a hydroxy group, a sulfanyl group, or a monovalent organic group having 1 to 20 carbon atoms. n is an integer of 0 to 11. When n is 2 or more, multiple R 1 are the same or different. 2 is a hydrogen atom, a fluorine atom, a methyl group, or a trifluoromethyl group. 3 is a monovalent group having 1 to 20 carbon atoms containing the above acid-dissociable group. Z is a single bond, an oxygen atom, or a sulfur atom. R 4is a hydrogen atom, a fluorine atom, a methyl group, or a trifluoromethyl group.

[0107] A resist composition comprising: a resin (A1) containing a structural unit having a cyclic carbonate structure, a structural unit represented by the following formula, and a structural unit having an acid labile group; and an acid generator.

[0108] [In the formula, R 2 represents an alkyl group having 1 to 6 carbon atoms which may have a halogen atom, a hydrogen atom or a halogen atom; X 1 represents a single bond, —CO—O—*, or —CO—NR 4 -*, * represents a bond to -Ar, R 4 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and Ar represents an aromatic hydrocarbon group having 6 to 20 carbon atoms which may have one or more groups selected from the group consisting of a hydroxy group and a carboxyl group.]

[0109] Examples of the resist film include the following.

[0110] A resist film comprising a base resin comprising a repeating unit represented by the following formula (a1) and / or a repeating unit represented by the following formula (a2), and a repeating unit that generates an acid bonded to a polymer main chain upon exposure:

[0111] (In formula (a1) and formula (a2), R A are each independently a hydrogen atom or a methyl group. 1 and R 2 are each independently a tertiary alkyl group having 4 to 6 carbon atoms. 3 are each independently a fluorine atom or a methyl group, and m is an integer of 0 to 4. 1 X is a single bond, a phenylene group, or a naphthylene group, or a linking group having 1 to 12 carbon atoms and containing at least one selected from an ester bond, a lactone ring, a phenylene group, and a naphthylene group. 2 is a single bond, an ester bond, or an amide bond.

[0112] Examples of resist materials include the following:

[0113] A resist material comprising a polymer having a repeating unit represented by the following formula (b1) or (b2):

[0114] (In formula (b1) and formula (b2), R A is a hydrogen atom or a methyl group. 1 is a single bond or an ester group. 2 is a linear, branched or cyclic alkylene group having 1 to 12 carbon atoms or an arylene group having 6 to 10 carbon atoms, and some of the methylene groups constituting the alkylene group may be substituted with an ether group, an ester group or a lactone ring-containing group; and X 2 At least one hydrogen atom contained in X is substituted with a bromine atom. 3 Rf is a single bond, an ether group, an ester group, or a linear, branched, or cyclic alkylene group having 1 to 12 carbon atoms, and some of the methylene groups constituting the alkylene group may be substituted with an ether group or an ester group. 1 ~Rf 4 are each independently a hydrogen atom, a fluorine atom, or a trifluoromethyl group, but at least one is a fluorine atom or a trifluoromethyl group. 1 and Rf 2 may combine to form a carbonyl group. 1 ~R 5 are each independently a linear, branched, or cyclic alkyl group having 1 to 12 carbon atoms, a linear, branched, or cyclic alkenyl group having 2 to 12 carbon atoms, an alkynyl group having 2 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, or an aryloxyalkyl group having 7 to 12 carbon atoms, in which some or all of the hydrogen atoms may be substituted with a hydroxy group, a carboxy group, a halogen atom, an oxo group, a cyano group, an amide group, a nitro group, a sultone group, a sulfone group, or a sulfonium salt-containing group, and in which some of the methylene groups constituting these groups may be substituted with an ether group, an ester group, a carbonyl group, a carbonate group, or a sulfonate ester group. 1 and R 2may be bonded to form a ring together with the sulfur atom to which they are attached.

[0115] A resist material comprising a base resin containing a polymer containing a repeating unit represented by the following formula (a):

[0116] (In formula (a), R A is a hydrogen atom or a methyl group. 1 is a hydrogen atom or an acid labile group. 2 is a linear, branched or cyclic alkyl group having 1 to 6 carbon atoms, or a halogen atom other than bromine. 1 X is a single bond, a phenylene group, or a linear, branched or cyclic alkylene group having 1 to 12 carbon atoms which may contain an ester group or a lactone ring. 2 is -O-, -O-CH 2 - or -NH-. m is an integer of 1 to 4. u is an integer of 0 to 3. However, m+u is an integer of 1 to 4.

[0117] A resist composition that generates an acid upon exposure, and whose solubility in a developer changes due to the action of the acid, comprising: a base component (A) whose solubility in a developer changes due to the action of the acid; and a fluorine additive component (F) that exhibits decomposition in an alkaline developer, wherein the fluorine additive component (F) comprises a fluororesin component (F1) that has a structural unit (f1) that includes a base dissociable group, and a structural unit (f2) that includes a group represented by the following general formula (f2-r-1):

[0118] [In formula (f2-r-1), Rf 21 are each independently a hydrogen atom, an alkyl group, an alkoxy group, a hydroxy group, a hydroxyalkyl group, or a cyano group. n" is an integer of 0 to 2. * is a bond.

[0119] The structural unit (f1) includes a structural unit represented by the following general formula (f1-1) or a structural unit represented by the following general formula (f1-2).

[0120] [In formulas (f1-1) and (f1-2), each R is independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. X is a divalent linking group that does not have an acid-dissociable site. A aryl represents a divalent aromatic cyclic group which may have a substituent. 01 is a single bond or a divalent linking group. 2 are each independently an organic group having a fluorine atom.

[0121] Coatings, coating solutions, and coating compositions include, for example:

[0122] A coating comprising a metal oxo-hydroxo network having organic ligands with metal carbon and / or metal carboxylate bonds.

[0123] Inorganic oxo / hydroxo-based compositions.

[0124] a coating solution comprising an organic solvent; a first organometallic composition having the formula R z SnO (2-(z/2)-(x/2)) (OH) x (where 0<z≦2 and 0<(z+x)≦4), formula R′ n SnX 4-n wherein n=1 or 2, or mixtures thereof, where R and R′ are independently hydrocarbyl groups having 1 to 31 carbon atoms, and X is a ligand having a hydrolyzable bond to Sn, or a combination thereof; and a hydrolyzable metal compound having the formula MX′ v wherein M is a metal selected from groups 2 to 16 of the periodic table of the elements, v is a number from 2 to 6, and X' is a ligand having a hydrolyzable M-X bond or a combination thereof.

[0125] an organic solvent and a solution of the formula RSnO (3/2-x/2) (OH) xand a first organometallic compound of the formula: wherein 0<x<3, wherein the solution contains from about 0.0025M to about 1.5M tin, and R is an alkyl or cycloalkyl group having from 3 to 31 carbon atoms, the alkyl or cycloalkyl group being bonded to the tin at a secondary or tertiary carbon atom.

[0126] An aqueous inorganic patterning precursor solution comprising a mixture of water, metal suboxide cations, polyatomic inorganic anions, and radiation-sensitive ligands comprising peroxide groups.

[0127] Irradiation with light or electron beams is carried out, for example, through a mask (reticle) for forming a predetermined pattern. For example, i-line, KrF excimer laser, ArF excimer laser, EUV (extreme ultraviolet), or EB (electron beam) can be used. The composition for forming a resist underlayer film of the present invention is preferably applied for EB (electron beam) or EUV (extreme ultraviolet: 13.5 nm) irradiation, more preferably for EUV (extreme ultraviolet) exposure. The irradiation energy of the electron beam and the exposure dose of light are not particularly limited.

[0128] After irradiation with light or electron beams and before development, baking (PEB: Post Exposure Bake) may be performed. The baking temperature is not particularly limited, but is preferably 60° C. to 150° C., more preferably 70° C. to 120° C., and particularly preferably 75° C. to 110° C. The baking time is not particularly limited, but is preferably 1 second to 10 minutes, more preferably 10 seconds to 5 minutes, and particularly preferably 30 seconds to 3 minutes.

[0129] For example, an alkaline developer is used for development. The development temperature can be, for example, 5°C to 50°C. The development time can be, for example, 10 seconds to 300 seconds. Examples of alkaline developers that can be used include aqueous solutions of alkalis such as inorganic alkalis (e.g., sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, and aqueous ammonia); primary amines (e.g., ethylamine and n-propylamine); secondary amines (e.g., diethylamine and di-n-butylamine); tertiary amines (e.g., triethylamine and methyldiethylamine); alcohol amines (e.g., dimethylethanolamine and triethanolamine); quaternary ammonium salts (e.g., tetramethylammonium hydroxide, tetraethylammonium hydroxide, and choline); and cyclic amines (e.g., pyrrole and piperidine). Furthermore, the aqueous solutions of the alkalis can be used by adding an appropriate amount of alcohols (e.g., isopropyl alcohol) or a nonionic surfactant. Among these, preferred developers are aqueous solutions of quaternary ammonium salts, more preferably aqueous solutions of tetramethylammonium hydroxide and choline. Furthermore, surfactants and the like can also be added to these developers. Alternatively, development may be carried out with an organic solvent such as butyl acetate instead of an alkaline developer, and the portions of the photoresist where the alkaline dissolution rate is not improved may be developed.

[0130] Next, the underlayer film is etched using the formed resist pattern as a mask. The etching may be dry etching or wet etching, but dry etching is preferred. If a film is formed on the surface of the nitrogen-containing substrate used, the surface of the film is exposed. If no film is formed on the surface of the substrate used, the surface of the substrate is exposed. Thereafter, the substrate is processed by a known method (e.g., dry etching), thereby manufacturing a semiconductor device.

[0131] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples.

[0132] The weight-average molecular weights of the polymers shown in Synthesis Examples 1 to 6 and Comparative Synthesis Example 1 below in this specification are the results of measurement by gel permeation chromatography (hereinafter abbreviated as GPC). A GPC device manufactured by Tosoh Corporation was used for the measurement, and the measurement conditions were as follows: GPC column: TSKgel Super-Multipore HZ-N (2 columns) Column temperature: 40°C Solvent: tetrahydrofuran (THF) Flow rate: 0.35 ml / min Standard sample: polystyrene (manufactured by Tosoh Corporation)

[0133] Synthesis Example 1 5.68 g of 2-vinylnaphthalene (75% by molar ratio to the total of Polymer 1), 1.60 g of 2-hydroxyethyl methacrylate (25% by molar ratio to the total of Polymer 1), and 0.73 g of 2,2'-azobisisobutyronitrile were dissolved in 32.00 g of propylene glycol monomethyl ether acetate. After replacing the atmosphere in the reaction vessel with nitrogen, the solution was heated and stirred at 140°C for approximately 4 hours. The reaction liquid was added dropwise to isopropyl alcohol, and the precipitate was recovered by suction filtration and then dried under reduced pressure at 60°C to recover Polymer 1. The weight average molecular weight Mw measured by GPC in terms of polystyrene was 8,500. The structure present in Polymer 1 is shown in the following formula.

[0134]

[0135] Synthesis Example 2 4.75 g of 2-vinylnaphthalene (55% by molar ratio to the total of Polymer 2), 2.96 g of benzyl methacrylate (30% by molar ratio to the total of Polymer 2), 1.21 g of 2-hydroxypropyl methacrylate (15% by molar ratio to the total of Polymer 2), and 1.07 g of 2,2'-azobisisobutyronitrile were dissolved in 40.00 g of propylene glycol monomethyl ether acetate. After replacing the atmosphere in the reaction vessel with nitrogen, the solution was heated and stirred at 140°C for approximately 4 hours. The reaction solution was added dropwise to isopropyl alcohol, and the precipitate was recovered by suction filtration. After that, the precipitate was dried under reduced pressure at 60°C to recover Polymer 2. The weight average molecular weight Mw measured by GPC in terms of polystyrene was 5900. The structure present in Polymer 2 is shown in the following formula.

[0136]

[0137] Synthesis Example 3 5.00 g of 2-vinylnaphthalene (55% by molar ratio to the total polymer 3), 2.91 g of 2-phenylethyl methacrylate (26% by molar ratio to the total polymer 3), 1.61 g of 2-hydroxypropyl methacrylate (19% by molar ratio to the total polymer 3), and 0.48 g of 2,2'-azobisisobutyronitrile were dissolved in 40.00 g of propylene glycol monomethyl ether acetate. After replacing the atmosphere in the reaction vessel with nitrogen, the solution was heated and stirred at 140°C for approximately 4 hours. The reaction solution was added dropwise to methanol, and the precipitate was recovered by suction filtration and then dried under reduced pressure at 60°C to recover polymer 3. The weight average molecular weight Mw measured by GPC in terms of polystyrene was 6,600. The structure present in polymer 3 is shown in the following formula.

[0138]

[0139] Synthesis Example 4 2.94 g of 2-vinylnaphthalene (50% by molar ratio to the total of Polymer 4), 1.24 g of hydroxyethyl methacrylate (25% by molar ratio to the total of Polymer 4), 1.71 g of N-cyclohexylmaleimide (25% by molar ratio to the total of Polymer 4), and 0.12 g of 2,2'-azobisisobutyronitrile were dissolved in 24.00 g of propylene glycol monomethyl ether acetate. After replacing the atmosphere in the reaction vessel with nitrogen, the solution was heated and stirred at 140°C for approximately 4 hours. The reaction solution was added dropwise to isopropyl alcohol, and the precipitate was recovered by suction filtration. After that, the precipitate was dried under reduced pressure at 60°C to recover Polymer 4. The weight average molecular weight Mw measured by GPC in terms of polystyrene was 16,300. The structure present in Polymer 4 is shown in the following formula.

[0140]

[0141] Synthesis Example 5 2.86 g of 2-vinylnaphthalene (50% by molar ratio to the total of Polymer 5), 1.68 g of N-cyclohexylmaleimide (25% by molar ratio to the total of Polymer 5), 1.32 g of N-hydroxyethylmaleimide (25% by molar ratio to the total of Polymer 5), and 0.12 g of 2,2'-azobisisobutyronitrile were dissolved in 24.00 g of propylene glycol monomethyl ether acetate. After replacing the atmosphere in the reaction vessel with nitrogen, the solution was heated and stirred at 140°C for approximately 4 hours. The reaction solution was added dropwise to isopropyl alcohol, and the precipitate was recovered by suction filtration and then dried under reduced pressure at 60°C to recover Polymer 5. The weight average molecular weight Mw measured by GPC in terms of polystyrene was 11,900. The structure present in Polymer 5 is shown in the following formula.

[0142]

[0143] Synthesis Example 6 7.22 g of 2-vinylnaphthalene (71% by molar ratio to the total of Polymer 6), 0.50 g of 4-tert-butylstyrene (10% by molar ratio to the total of Polymer 6), 1.80 g of 2-hydroxypropyl methacrylate (19% by molar ratio to the total of Polymer 6), and 0.48 g of 2,2'-azobisisobutyronitrile were dissolved in 40.00 g of propylene glycol monomethyl ether acetate. After replacing the atmosphere in the reaction vessel with nitrogen, the solution was heated and stirred at 140°C for approximately 4 hours. The reaction solution was added dropwise to methanol, and the precipitate was recovered by suction filtration and then dried under reduced pressure at 60°C to recover Polymer 6. The weight average molecular weight Mw measured by GPC in terms of polystyrene was 7,300. The structure present in Polymer 6 is shown in the following formula.

[0144]

[0145] Comparative Synthesis Example 1 100.00 g of monoallyl diglycidyl isocyanurate (manufactured by Shikoku Chemicals Corporation), 66.4 g of 5,5-diethylbarbituric acid (manufactured by Tateyama Chemicals Co., Ltd.), and 4.1 g of benzyltriethylammonium chloride were added to 682.00 g of propylene glycol monomethyl ether in a reaction vessel and dissolved. After replacing the atmosphere in the reaction vessel with nitrogen, the reaction was carried out at 130°C for 24 hours to obtain a solution containing comparative polymer 1. GPC analysis showed that the obtained comparative polymer 1 had a weight average molecular weight of 6,800 in terms of standard polystyrene. The structure present in comparative polymer 1 is shown in the following formula.

[0146]

[0147] (Preparation of underlayer film-forming composition 1) The components were mixed in the proportions shown in Table 1 and filtered using a polyethylene microfilter with a pore size of 0.05 μm to prepare the underlayer film-forming compositions of Examples 1 to 6 and Comparative Example 1, respectively.

[0148] The abbreviations in Table 1 are as follows: PyPTS: pyridinium-p-toluenesulfonic acid PGME: propylene glycol monomethyl ether PGMEA: propylene glycol monomethyl ether acetate

[0149] PL-LI: 1,3,4,6-tetrakis(methoxymethyl)glycoluril (structural formula below)

[0150]

[0151] (Resist Patterning Evaluation) <Formation of Underlayer Film> Each of the compositions for forming an underlayer film in Examples 1 to 6 and Comparative Example 1 was applied using a spinner onto a nitrogen-containing substrate on which a 31.5 nm SiON film had been formed. The wafer was baked on a hot plate at 205 to 250°C for 60 seconds, yielding an underlayer film with a thickness of 5 nm for each of Examples 1 to 6 and Comparative Example 1.

[0152] An underlayer film-coated wafer was prepared in the same manner as above, and stored in a clean room for 48 hours to prepare an underlayer film.

[0153] <Resist Pattern Formation Test Using an ArF Scanner> A commercially available ArF resist solution (manufactured by Shin-Etsu Chemical Co., Ltd., product name: SAIL X-206) was applied to the underlayer films of Examples 1 to 6 and Comparative Example 1 that had been stored in a clean room for the predetermined period of time described above, and baked at 85°C for 60 seconds to form a photoresist film with a thickness of 100 nm. Using a Nikon Corporation NSR-S307E scanner (wavelength 193 nm, NA=0.85, σ=0.93 / 0.85), the resist film was exposed through a mask designed to form dense lines with a photoresist line width and space width of 0.1 μm after development, i.e., a 0.1 μm line-and-space (L / S) ratio of 1 / 1. The resist film was then baked on a hot plate at 95°C for 60 seconds, cooled, and developed using butyl acetate for 60 seconds to form a negative pattern on the resist underlayer film.

[0154] For the obtained photoresist patterns, a photoresist film was immediately formed on the underlayer film-coated wafer without storing it in a clean room, and then exposed and developed. The resist pattern was observed from above, and a 100 nm line / 200 nm pitch (line and space (L / S=1 / 1) pattern was formed. Separately, a photoresist film was formed on the underlayer film of an underlayer film-coated wafer that had been stored in a clean room for 48 hours using the same method, and then exposed and developed, and the line size of the resist pattern was confirmed. The exposure was carried out at the optimum irradiation energy for each example. The pattern length was measured using a scanning electron microscope (CG4100, manufactured by Hitachi High-Technologies Corporation). The change in pattern size between the pattern size after 48 hours of storage in a clean room (after 48 hours) and the pattern size after continuous exposure (after 0 hours) was confirmed, and the results are shown in Table 2.

[0155]

[0156] In Examples 1 to 6, the amount of change in pattern size was smaller than in Comparative Example 1, even when the underlayer film-coated wafers were stored for 48 hours. The reason for the small amount of change in pattern size in each Example is believed to be that the composition was able to block the amine component even when it diffused from the underlying substrate, which had a film such as SiON, SiN, or TiN. Furthermore, in each Example, it was believed to be able to suppress damage caused by the diffusion of the amine component and suppress change in pattern size even when the underlayer film was left for several days after coating. Therefore, the composition for forming a resist underlayer film of this embodiment is expected to be a material that can be widely applied in coating applications on nitrogen-containing substrates for a variety of semiconductor manufacturing processes.

Claims

1. A composition for forming a resist underlayer film, comprising a polymer and a crosslinking agent, the polymer having a structural unit (A) having a polycyclic aromatic structure, and used in lithography using a photoresist film or an electron beam resist film to form an underlayer film of the resist film on a nitrogen atom-containing substrate.

2. The composition for forming a resist underlayer film according to claim 1, wherein the polymer has the polycyclic aromatic structure in a side chain of the polymer.

3. The composition for forming a resist underlayer film according to claim 1, wherein the polycyclic aromatic structure is selected from the group consisting of optionally substituted naphthalene, anthracene, phenanthrene, pyrene, triphenylene, chrysene, naphthacene, biphenylene, fluorene, and carbazole.

4. The composition for forming a resist underlayer film according to claim 1, wherein the unit structure (A) is a unit structure represented by the following formula (A-1): (In formula (A-1), R 1 represents a hydrogen atom or a methyl group. 1 represents a single bond, an ester group or an amide group. 1 represents a single bond or an alkylene group having 1 to 6 carbon atoms. Ar represents a monovalent group obtained by removing a hydrogen atom from naphthalene, anthracene, phenanthrene, pyrene, triphenylene, chrysene, naphthacene, biphenylene, fluorene, or carbazole, which may be substituted.

5. The composition for forming a resist underlayer film according to claim 1, wherein the polymer further comprises a unit structure (B) having a reactive group, and the crosslinking agent has a functional group capable of reacting with the reactive group.

6. The composition for forming a resist underlayer film according to claim 5, wherein the unit structure (B) is at least one of a unit structure represented by the following formula (B-1) and a unit structure represented by the following formula (B-2): (In formula (B-1), R 11 represents a hydrogen atom or a methyl group. 11 represents an ester group or an amide group. 12 represents a monovalent group having 1 to 12 carbon atoms and having the reactive group. 13 represents a monovalent group having 1 to 12 carbon atoms and having the reactive group.

7. The composition for forming a resist underlayer film according to claim 1, wherein the polymer further has at least any one of a unit structure (C) of a unit structure (C-1) having a monocyclic aromatic structure and a unit structure (C-2) derived from a maleimide structure.

8. The composition for forming a resist underlayer film according to claim 7, wherein the unit structure (C-1) is a unit structure represented by the following formula (C-1-1), and the unit structure (C-2) is a unit structure represented by the following formula (C-2-1): (In formula (C-1-1), R 21 represents a hydrogen atom or a methyl group. 21 represents a single bond, an ester group or an amide group. 21 represents a single bond or an alkylene group having 1 to 6 carbon atoms. 22 represents a halogen atom, an alkyl group having 1 to 6 carbon atoms which may be substituted with a halogen atom, or an alkoxy group having 1 to 6 carbon atoms which may be substituted with a halogen atom. n represents an integer of 0 to 5. 22 When there are two or more, there are two or more R 22 may be the same or different. In formula (C-1-2), R 23 represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be substituted with a halogen atom, or an aryl group having 6 to 10 carbon atoms which may be substituted with a halogen atom.

9. The composition for forming a resist underlayer film according to claim 1, wherein the molar ratio of the unit structure (A) to all unit structures of the polymer is 40 mol % or more.

10. The composition for forming a resist underlayer film according to claim 5, wherein the molar ratio of the unit structure (B) to all unit structures of the polymer is 5 mol % to 40 mol %.

11. The composition for forming a resist underlayer film according to claim 1, wherein the polymer further has a unit structure (B) having a reactive group, and at least one unit structure (C) selected from a unit structure (C-1) having a monocyclic aromatic structure and a unit structure (C-2) derived from a maleimide structure, the crosslinking agent has a functional group capable of reacting with the reactive group, the unit structure (A) is a unit structure represented by the following formula (A-1), the unit structure (B) is at least one unit structure represented by the following formula (B-1) and a unit structure represented by the following formula (B-2), the unit structure (C-1) is a unit structure represented by the following formula (C-1-1), the unit structure (C-2) is a unit structure represented by the following formula (C-2-1), a molar ratio of the unit structure (A) to all unit structures of the polymer is 40 mol % or more, and a molar ratio of the unit structure (B) to all unit structures of the polymer is 5 mol % to 40 mol %. (In formula (A-1), R 1 represents a hydrogen atom or a methyl group. 1 represents a single bond, an ester group or an amide group. 1 represents a single bond or an alkylene group having 1 to 6 carbon atoms. Ar represents a monovalent group obtained by removing a hydrogen atom from naphthalene, anthracene, phenanthrene, pyrene, triphenylene, chrysene, naphthacene, biphenylene, fluorene, or carbazole, which may be substituted. (In formula (B-1), R 11 represents a hydrogen atom or a methyl group. 11 represents an ester group or an amide group. 12 represents a monovalent group having 1 to 6 carbon atoms and having the reactive group. 13 represents a monovalent group having 1 to 6 carbon atoms and having the reactive group. (In formula (C-1-1), R 21 represents a hydrogen atom or a methyl group. 21 represents a single bond, an ester group or an amide group. 21 represents a single bond or an alkylene group having 1 to 6 carbon atoms. 22 represents a halogen atom, an alkyl group having 1 to 6 carbon atoms which may be substituted with a halogen atom, or an alkoxy group having 1 to 6 carbon atoms which may be substituted with a halogen atom. n represents an integer of 0 to 5. 22 When there are two or more, there are two or more R 22 may be the same or different. In formula (C-1-2), R 23 represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be substituted with a halogen atom, or an aryl group having 6 to 10 carbon atoms which may be substituted with a halogen atom.

12. The composition for forming a resist underlayer film according to claim 1, wherein the content of the crosslinking agent is 20% by mass to 50% by mass of the polymer.

13. An underlayer film formed on the nitrogen atom-containing substrate using the composition for forming a resist underlayer film according to any one of claims 1 to 12.

14. The underlayer film of claim 13, having a thickness of less than 10 nm.

15. A method for producing a substrate having a resist pattern, comprising the steps of: forming an underlayer film on the nitrogen-atom-containing substrate using a composition for forming a resist underlayer film according to any one of claims 1 to 12; forming a resist film, which is either a photoresist film or an electron beam resist film, on the underlayer film; and irradiating the resist film with light or an electron beam, and then developing the resist film to obtain a resist pattern.

16. The method for producing a substrate provided with a resist pattern according to claim 15, further comprising the step of forming the resist film 12 hours or more after the formation of the underlayer film.

17. A method for manufacturing a semiconductor device, comprising: a step of forming an underlayer film on the nitrogen atom-containing substrate using a composition for forming a resist underlayer film according to any one of claims 1 to 12; a step of forming a resist film, which is either a photoresist film or an electron beam resist film, on the underlayer film; a step of irradiating the resist film with light or an electron beam, and then developing the resist film to obtain a resist pattern; and a step of etching the underlayer film using the resist pattern as a mask, to form a patterned underlayer film.

Citation Information

Patent Citations

  • Resist undercoat film material, and resist undercoat film substrate and pattern forming method using the same

    JP2008039811A

  • Resist undercoat film material, and resist undercoat film substrate and pattern forming method using the same

    JP2008039815A

  • Positive resist composition and resist pattern forming method

    JP2010128369A

  • Photoresist undercoat-forming material and patterning process

    JP2010134437A

  • Positive resist composition, resist pattern forming method, and polymer compound

    JP2010181857A