Method for producing resin composition, and resin composition
The twin-screw kneading extruder method addresses the challenge of residual fiber bundles by optimizing screw design, enhancing productivity and mechanical strength in fiber-reinforced thermoplastic resin compositions for precision molding.
Patent Information
- Application Number
- PCT/JP2024/017164
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-14
AI Technical Summary
Existing methods for producing fiber-reinforced thermoplastic resin compositions struggle to balance the reduction of residual unfibrillated fiber bundles, fiber length, and productivity, particularly in precision molded products where the presence of undefinated fibers can lead to defects and poor performance.
A method using a twin-screw kneading extruder with specific screw designs, including a first and second kneading zone with defined flight clearances and resistance sections, to efficiently melt-knead thermoplastic resin and fibrous fillers, reducing the residual rate of unfibrillated fiber bundles while maintaining long fiber lengths and enhancing productivity.
The method effectively reduces the residual rate of unfibrillated fiber bundles, improves mechanical strength, and maintains long fiber lengths, resulting in improved resin composition properties suitable for precision molding applications.
Smart Images

Figure JP2024017164_14112024_PF_FP_ABST
Abstract
Description
Resin composition manufacturing method and resin composition
[0001] The present invention relates to a method for producing a resin composition and a resin composition.
[0002] Thermoplastic resin compositions containing a thermoplastic resin and a fibrous filler have superior physical properties such as mechanical strength compared to thermoplastic resins that do not contain a fibrous filler. For this reason, thermoplastic resin compositions containing a fibrous filler are used as raw materials for automobile parts, parts for electric and electronic products, etc.
[0003] Examples of methods for producing fiber-filler-reinforced thermoplastic resin composition pellets by mixing and kneading a fiber-based filler with a thermoplastic resin include the following: First, a thermoplastic resin is fed into an extruder and melted. Next, a fiber-based filler is fed into the molten thermoplastic resin, and the thermoplastic resin and the fiber-based filler are mixed and kneaded in the extruder. Finally, the mixture is cooled and granulated. For example, a single-screw extruder or a twin-screw extruder (such as a co-rotating intermeshing twin-screw extruder) is used as the extruder. Compared to a single-screw extruder, a twin-screw extruder tends to have higher productivity and operating flexibility. Therefore, a twin-screw extruder is more preferably used for producing fiber-filler-reinforced thermoplastic resin composition pellets.
[0004] The fiber filler used in the production of the fiber-based filler reinforced thermoplastic resin composition pellets is, for example, a roving wound with about 300 to 3,000 monofilaments having a diameter of 6 to 20 μm, or chopped strands obtained by cutting the roving to a length of 1 to 6 mm, etc. Chopped strands are used. Because chopped strands are easier to use, when industrially producing fiber-based filler reinforced thermoplastic resin composition pellets, the most common method is to supply a thermoplastic resin to a twin-screw extruder, melt the thermoplastic resin, and then supply chopped strands from the middle of the twin-screw extruder. The molten thermoplastic resin and the fiber-based filler are mixed and kneaded, the mixture is extruded, and then cooled and solidified.
[0005] The productivity of fiber-filler-reinforced thermoplastic resin composition pellets produced using the twin-screw extruder is determined by the extruder's plasticizing and mixing capabilities. The plasticizing capability of a twin-screw extruder depends on the screw design, the torque generated by the screw, the screw groove depth (the difference between the outer diameter and the root diameter of the screw), the screw rotation speed, etc. Patent Document 1 defines the torque density as the value obtained by dividing the center distance between the two screws by the cube, and discloses a twin-screw extruder with high plasticizing capability and excellent productivity.
[0006] The mixing and kneading capacity of a twin-screw extruder also depends on the screw design. As the plasticizing capacity of twin-screw extruders has improved, the residence time has decreased. This has led to a demand for the development of screw designs that can efficiently mix and knead in a short time. As such, research is being conducted into technologies to improve the plasticizing and kneading capacity of twin-screw extruders.
[0007] Generally, as described above, bundles of monofilaments are used as fibrous fillers. This is because, when fibrous fillers are fed into a twin-screw extruder without bundling the monofilaments, the monofilaments tend to become cotton-like, lose fluidity, and become difficult to handle. The chopped strands are, for example, mixed and kneaded in the twin-screw extruder until they are defibrated into monofilaments, and at the same time, the chopped strands are broken by a screw or the like until the monofilaments have an average length of 200 to 500 μm.
[0008] If mixing and kneading in the twin-screw extruder is insufficient, some or all of the chopped strands, which are not defibrated into monofilaments but are in the form of an aggregate of monofilaments (undefibrated fiber filler bundles), will remain in the resin composition pellets. If some or all of the chopped strands remain in the fiber-filler-reinforced thermoplastic resin composition pellets, some or all of the chopped strands will clog the gate during injection molding, making injection molding impossible, or even if injection molding is possible, some or all of the chopped strands will be present in the molded product, which is likely to cause poor appearance or reduced functionality.
[0009] In particular, with the recent advances in electronics-related technology, fiber-based filler reinforced thermoplastic resin compositions used in parts are required to be molded into thin, complex shapes. The gate nozzles of molding machines used in such precision molding are often 1 mm or less. In precision molded products, the presence of unresolved fiber-based filler bundles is a very serious defect.
[0010] Use of the twin-screw extruder of Patent Document 1 is said to improve productivity; however, particularly in the case of precision molded products such as those described above, the residence time tends to be shorter under conditions of high discharge rate, making it more difficult to completely defibrate chopped strands into monofilaments and shorten the fiber length.
[0011] By combining a large number of kneading segments such as kneading disks, it is possible to some extent to increase the kneading intensity and defibrate the fiber bundles into monofilaments. On the other hand, increasing the kneading intensity tends to significantly shorten the fiber length and reduce strength. Therefore, Patent Document 2 discloses a method of using a kneading segment whose flight section has an arc-shaped top with a predetermined radius of curvature to promote the reaction between the glass-based inorganic filler and the thermoplastic resin in the molding machine and improve adhesion between the glass-based inorganic filler and the thermoplastic resin. Patent Document 3 discloses that using a single progressive screw segment whose flight section has an arc-shaped notch formed therein significantly reduces the probability of remaining undefibrated glass fiber bundles.
[0012] JP-T-11-512666A JP-A-2012-140526 JP-A-2012-213996
[0013] However, none of the above manufacturing methods are sufficient in terms of the balance between the remaining rate of unfibrillated fiber bundles, the remaining fiber length, and the improvement in productivity.
[0014] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for producing a resin composition that can reduce the rate of remaining undefibrated fiber bundles.
[0015] The present inventors have conducted extensive research and have completed the present invention.
[0016] That is, the present invention relates to the following: [1] A method for producing a resin composition by melt-kneading a thermoplastic resin and a fibrous filler using a twin-screw kneading extruder, wherein the twin-screw kneading extruder is provided with, in order from upstream as viewed in the direction of flow of the materials to be melt-kneaded, a first supply port, a first kneading zone, a second supply port, and a second kneading zone, the thermoplastic resin and the fibrous filler are supplied to the twin-screw kneading extruder from the first supply port and the second supply port, respectively, and 50 mass % or more of the thermoplastic resin supplied from the first supply port is melted in the first kneading zone, and the second kneading zone has: (A) a single flight and a resistance portion downstream of the single flight that generates a pressure of 2 MPa or more, and (B) a double flight with a clearance between the cylinder and the second flight that is 1.3% or more of the cylinder diameter, and a resistance portion downstream of the double flight that generates a pressure of 2 MPa or more. (C) a single-flight flight and a resistance portion that generates a pressure of 1 MPa or more at the downstream end of the single-flight flight and at a position 1D upstream from the downstream end of the single-flight flight, or (D) a double-flight flight having a clearance between the cylinder and the single-flight flight of 1.3% or more of the cylinder diameter and a resistance portion that generates a pressure of 1 MPa or more at the downstream end of the double-flight flight and at a position 1D upstream from the downstream end of the single-flight flight. [2] The method for producing a resin composition according to [1], wherein the clearance between the cylinder and the single-flight flight or the double-flight flight is 2.0% or more of the cylinder diameter.[3] The method for producing a resin composition according to [1], wherein the second kneading zone has: (a) a single flight having a clearance between the cylinder and the flight member of at least 1.3% of the cylinder diameter and a resistance portion downstream of the single flight that generates a pressure of at least 4 MPa, (b) a double flight having a clearance between the cylinder and the flight member of at least 1.3% of the cylinder diameter and a resistance portion downstream of the double flight that generates a pressure of at least 4 MPa, (c) a single flight and a resistance portion downstream of the single flight that generates a pressure of at least 2 MPa at the downstream end of the single flight and at a position 2D upstream from the downstream end of the single flight, or (d) a double flight having a clearance between the cylinder and the flight member of at least 1.3% of the cylinder diameter and a resistance portion downstream of the double flight that generates a pressure of at least 2 MPa at the downstream end of the double flight and at a position 2D upstream from the downstream end of the single flight. [4] The method for producing a resin composition according to any of [1] to [3], wherein the length of the single flight or the double flight is at least 3D. [5] A method for producing a resin composition according to any one of claims [1] to [4], wherein the fibrous filler is a fiber bundle. [6] A method for producing a resin composition according to any one of [1] to [5], wherein the fibrous filler is glass fiber or carbon fiber. [7] A method for producing a resin composition according to any one of [1] to [6], wherein the thermoplastic resin comprises at least one selected from the group consisting of polypropylene, polyester, polyamide, polycarbonate, polystyrene, polyphenylene ether, ABS resin, AS resin, PPS resin, and liquid crystal polymer. [8] A resin composition obtainable by the method for producing a resin composition according to any one of [1] to [7], wherein the thermoplastic resin comprises at least one selected from the group consisting of polypropylene, polyester, polyamide, polycarbonate, polystyrene, polyphenylene ether, ABS resin, AS resin, PPS resin, and liquid crystal polymer.
[0017] According to the present invention, there is provided a method for producing a resin composition that can reduce the rate of remaining undefibrated fiber bundles.
[0018] It is a schematic diagram showing an example of a twin-screw kneading extruder according to the present embodiment. It is a diagram explaining the clearance between a single flight and a cylinder. It is a diagram explaining the clearance between a double flight and a cylinder. It is a perspective view showing an example of a notched segment. It is a diagram showing the resin pressure in Example 3.
[0019] Hereinafter, several embodiments of the present invention will be described in detail, but the present invention is not limited to the following embodiments.
[0020] The method for producing a resin composition of this embodiment is a method for producing a resin composition by melt-kneading a thermoplastic resin and a fibrous filler using a twin-screw kneading extruder, the twin-screw kneading extruder having, in order from upstream as viewed in a flow direction of the materials to be melt-kneaded, a first supply port, a first kneading zone, a second supply port, and a second kneading zone, the thermoplastic resin and the fibrous filler are supplied to the twin-screw kneading extruder from the first supply port and the second supply port, respectively, in the first kneading zone, 50 mass % or more of the thermoplastic resin supplied from the first supply port is melted, the second kneading zone has (A) a single flight and a pressure of 2 MPa or more on the downstream side of the single flight, (B) a double flight having a clearance between the cylinder of 1.3% or more of the cylinder diameter and a resistance portion downstream of the double flight that generates a pressure of 2 MPa or more; (C) a single flight and a resistance portion that generates a pressure of 1 MPa or more at the downstream end of the single flight and at a position 1D upstream from the downstream end of the single flight; or (D) a double flight having a clearance between the cylinder of 1.3% or more of the cylinder diameter and a resistance portion that generates a pressure of 1 MPa or more at the downstream end of the double flight and at a position 1D upstream from the downstream end of the single flight. According to this method, the residual rate of undefibrated fiber bundles can be reduced. This method also has excellent productivity for the resin composition. Furthermore, according to this method, the remaining fiber length in the resin composition can be maintained long.
[0021] Single- and double-row flights are usually used as conveying segments, and the kneading zone of a twin-screw kneading extruder generally uses a combination of screw segments commonly used as kneading segments, such as forward kneading discs, reverse kneading discs, neutral kneading discs, rotors, etc. In contrast, the method according to this embodiment uses single- and double-row flights in the second kneading zone. This method makes it possible to achieve dispersion and mixing of a fibrous filler with excellent productivity.
[0022] D usually refers to the approximate value of the diameter of the cylinder. In other words, "a position 1D upstream from the downstream end of the single flight" means a position approximately "1 x D" upstream from the "downstream end of the single flight." Furthermore, the term "2D" described below indicates a length "approximately twice D," and the term "3D" indicates a length "approximately three times D." The same applies to other similar terms such as "4D."
[0023] In this specification, 1D is defined as the range of −7.0% to +7.0% of the cylinder diameter. In other words, if the cylinder diameter is defined as D', 1D means "0.93×D' to 1.07×D'". Similarly, "2D" means "0.93×2×D' to 1.07×2×D'", and "3D" means "0.93×3×D' to 1.07×3×D'".
[0024] Fig. 1 is a schematic diagram showing an example of a twin-screw kneading extruder according to this embodiment. This twin-screw kneading extruder includes a cylinder (not shown), a screw 2 disposed in the cylinder, and a die (not shown) provided at the downstream end of the cylinder. The twin-screw kneading extruder may be configured with screws that rotate and intermesh with each other. Examples of twin-screw kneading extruders include co-rotating twin-screw kneading extruders and co-intermeshing twin-screw kneading extruders.
[0025] The twin-screw kneading extruder includes, in order from upstream as viewed in the flow direction of the materials to be melt-kneaded, a supply zone 20, a first kneading zone 21, a conveying zone 22, a second kneading zone 23, and a conveying zone 24. A first supply port 1a and a second supply port 1b are provided in the supply zone 20 and the conveying zone 22, respectively, and a vent port 5 is provided in the conveying zone 24. That is, the twin-screw kneading extruder includes, in order from upstream as viewed in the flow direction of the materials to be melt-kneaded, a first supply port 1a, a first kneading zone 21, a second supply port 1b, and a second kneading zone 23. For example, hoppers (not shown) are connected to the first supply port 1a and the second supply port 1b.
[0026] The second kneading zone 23 has a mixing / dispersion section 23a on the upstream side and a resistance section 23b on the downstream side, viewed from the direction of flow of the melt-kneaded material. The provision of the resistance section 23b in the second kneading zone 23 is thought to facilitate the mixture of molten thermoplastic resin and fibrous filler filling the gap between the flight and the cylinder, improving the mixing effect. The resistance section has the highest pressure at the upstream end of the resistance section 23b and decreases toward the downstream side. The mixing / dispersion section 23a is a region configured with screw segments where the pressure decreases from the downstream end (the upstream end of the resistance section 23b) toward the upstream side.
[0027] The screw segments used in the mixing and dispersing section 23a include, for example, conveying segments having forward flights. Specific examples of the screw segments include single- and double-flighted segments.
[0028] The mixing / dispersing section 23a is composed of a single flight or a double flight with a clearance between the cylinder and the flight being 1.3% or more of the cylinder diameter. The resistance section 23b is a resistance section that generates a pressure of 2 MPa or more. Preferably, the resistance section 23b is a resistance section that generates a pressure of 4 MPa or more.
[0029] Fig. 2 is a diagram illustrating the clearance between a single flight and a cylinder, in which a represents the clearance, b represents the cylinder, c represents the flight width, and dx represents the cylinder diameter.
[0030] When a single flight is used, the flight width is preferably 20% or more of the lead length of the flight, and more preferably about 30%. By widening the flight width, dispersion and mixing effects in the gap between the screw and the flight tend to be more easily achieved.
[0031] Figure 3 is a diagram illustrating the clearance between the two flights and the cylinder. In Figure 3, "a" represents the clearance, "b" represents the cylinder, and "dx" represents the cylinder diameter. That is, when the mixing / dispersing section 23a is composed of two flights, "a" in Figure 3 is 1.3% or more of the cylinder diameter dx.
[0032] When using double flights, it is usually difficult to increase the flight width, but it is preferable to increase the clearance between the flights and the cylinder. This increases the passage rate through the gap between the flights and the cylinder, which tends to make it easier to achieve dispersion and mixing effects. The clearance between the flights and the cylinder may be, for example, 2% or more of the cylinder diameter. From the viewpoint of maintaining a relatively high shear rate in the clearance area, the clearance between the flights and the cylinder may be, for example, less than 10% of the cylinder diameter.
[0033] The length of the single flight or the double flight that constitutes the mixed dispersion section 23a may be, for example, 2D or more, or 3D or more, from the viewpoint of providing a sufficient area filled with the mixture of fibrous filler and thermoplastic resin.
[0034] The resistance portion 23b may be, for example, a screw segment such as a reverse flight, a seal ring, a neutral kneading disk, a reverse kneading disk, or a notched segment (a flight or ring with a notch), or a combination thereof. From the viewpoint of facilitating filling with the mixture of the molten thermoplastic resin and the fibrous filler, the resistance portion 23b may be formed, for example, by adjusting the combination and length of the screw segments so that the conveying force to the downstream side is lower than the discharge rate under the operating conditions of the twin-screw kneading extruder.
[0035] The resistor portion 23b preferably includes a cutout segment. A cutout segment is a segment having a cutout portion. An example of a cutout segment is shown in Fig. 4. The cutout segment 10 shown in Fig. 4 is a cutout segment having a plurality of cutout portions.
[0036] A method for producing a resin composition using the twin-screw kneading extruder is described below. In this method, a thermoplastic resin and a fibrous filler are melt-kneaded using the twin-screw kneading extruder to produce a resin composition. The resulting resin composition is, for example, a fibrous filler-reinforced thermoplastic resin composition pellet.
[0037] First, a thermoplastic resin is supplied from a first supply port 1a to a supply zone 20. The thermoplastic resin supplied from the first supply port 1a to the supply zone 20 is transported to a first kneading zone 21. In the first kneading zone 21, 50 mass% or more of the thermoplastic resin supplied from the first supply port 1a is melted. The thermoplastic resin leaving the first kneading zone 21 is transported to a conveying zone 22, where it joins with a fibrous filler.
[0038] The fibrous filler is fed from the feed port 1b to the conveying zone 22, where it meets with the thermoplastic resin.
[0039] The thermoplastic resin and fibrous filler that have left the conveying zone 22 are kneaded in the second kneading zone 23. This disperses the fibrous filler in the thermoplastic resin. The resistance portion described above is formed in the second kneading zone 23.
[0040] The thermoplastic resin and fibrous filler that have left the second kneading zone 23 pass through the conveying zone 24 and are discharged from the die to the outside of the twin-screw kneading extruder. This allows a fiber-filler-reinforced thermoplastic resin composition to be obtained. The obtained fiber-filler-reinforced thermoplastic resin composition may be pelletized as necessary.
[0041] The manufacturing method of this embodiment may include, for example, a plasticization step in which a thermoplastic resin is supplied to the extruder and plasticized by heating and kneading; a kneading / dispersion step in which, after the plasticization step, one or more bundles of fibrous filler are supplied to the extruder and the defibrated fibrous filler and the plasticized thermoplastic resin are kneaded with a screw while defibrating the fibrous filler bundles; a devolatilization step in which volatile components are removed as necessary; an extrusion step in which the mixture obtained in the mixing / dispersion step is extruded from a die to the outside of the twin-screw kneading extruder; and a pelletization step in which the mixture extruded from the die is pelletized.
[0042] [Plasticization Step] The plasticization step is carried out, for example, in the feeding zone 20 and the first kneading zone 21 .
[0043] In the plasticizing step, the thermoplastic resin (for example, resin pellets) supplied from the supply port 1a is transported and melted.
[0044] Examples of the screw segments used in the supply zone 20 include conveying segments made of flights. Examples of the screw segments used in the first kneading zone 21 include screw segments such as reverse flights, seal rings, forward kneading discs, reverse kneading discs, and combinations thereof.
[0045] For example, resin pellets are transported in the supply zone 20. The supply zone 20 functions to transport the resin pellets from the supply port 1a side toward the die.
[0046] Preheating with an external heater may be carried out as a preparation step for plasticization.
[0047] Because the thermoplastic resin is sandwiched between the rotating screw 2 and the cylinder, frictional force is applied to the thermoplastic resin, generating frictional heat. The preheating and frictional heat may cause the thermoplastic resin to begin to melt. In some cases, the groove depth of the screw 2 and the preheating temperature may be adjusted by a conventionally known method in the supply zone 20 so that the thermoplastic resin is transported smoothly.
[0048] In the first kneading zone 21, pressure is applied to the thermoplastic resin transferred from the supply zone 20 to melt the thermoplastic resin. In the first kneading zone 21, shear stress is applied to the thermoplastic resin, and as a result, the thermoplastic resin is transferred further forward (towards the conveying zone 22) while being melted.
[0049] As described above, 50% by mass or more of the thermoplastic resin is melted in the first kneading zone 21. This tends to reduce breakage of the fibrous filler. It is believed that the reduction in the resin viscosity in the first kneading zone 21 reduces breakage of the fibrous filler.
[0050] The first kneading zone 21 may be provided with an open vent or a vacuum vent for removing excess volatile components after plasticizing and melting the thermoplastic resin.
[0051] The thermoplastic resin (melt) melted in the plasticizing step joins with the fibrous filler in the conveying zone 22 and is then subjected to a kneading and dispersing step in the second kneading zone 23. The fibrous filler is supplied to the extruder from the second supply port 1b. The number of fibrous fillers supplied to the extruder is, for example, one or more bundles.
[0052] [Kneading and Dispersing Step] In the kneading and dispersing step, the fibrous filler and the molten thermoplastic resin are kneaded together, whereby the fiber bundles of the fibrous filler are defibrated and dispersed in the thermoplastic resin.
[0053] The kneading and dispersing step is carried out in the mixing and dispersing section 23a of the second kneading zone 23 and in the resistance section 23b downstream thereof.
[0054] [Post-process] After the kneading and dispersion process, an open vent or a vacuum vent may be provided to remove volatile components contained in the raw resin, decomposition products of the surface treatment agent for the fibrous filler, and the sizing agent, as well as reaction residues. From the viewpoint of suppressing oxidation and deterioration of the resin, it is preferable to provide a vacuum vent.
[0055] There are no limitations on the fibrous filler and thermoplastic resin used in the method according to this embodiment, but specific examples are shown below.
[0056] [Fiber-based filler] The fiber-based filler is, for example, a fiber bundle formed by bundling a plurality of monofilaments with a sizing agent or the like. Fiber bundles bound with a sizing agent or the like are easy to handle during kneading. There are no particular restrictions on the number of monofilaments constituting the fiber bundle, but it may be, for example, 300 to 3,000, or 1,100 to 2,200. The fiber-based filler may be formed by continuously feeding a bundle of monofilaments as rovings to a twin-screw kneading extruder, or may be fed to a twin-screw kneading extruder in the form of chopped strands obtained by cutting the rovings. Chopped strands are preferred as the fiber-based filler from the viewpoints of transportation and handling.
[0057] Examples of fibrous fillers include glass fiber, carbon fiber, aramid fiber, and basalt fiber. One type of fibrous filler may be used alone, or two or more types may be used in combination.
[0058] (Glass Fiber) The fiber diameter of the monofilaments forming the glass fiber bundle is not particularly limited, but is preferably in the range of, for example, 6 to 20 μm, and those with diameters of 6 μm, 10 μm, and 13 μm are commonly available on the market.
[0059] The fiber diameter can be determined, for example, by cutting the fibers perpendicular to the fiber direction, measuring the diameters of the cross sections by observing them under a microscope, and calculating the number average of the diameters of 100 or more fibers.
[0060] (Carbon fiber) The type of carbon fiber is not particularly limited, but examples thereof include PAN (polyacrylonitrile)-based carbon fiber, which is mainly made of acrylonitrile, pitch-based carbon fiber, which is mainly made of tar pitch, and rayon-based carbon fiber. For example, PAN-based carbon fiber is preferred from the viewpoint of composition purity and uniformity. The method for producing the carbon fiber is not particularly limited.
[0061] The fiber diameter of the monofilaments forming the carbon fiber bundle may be, for example, more than 2 μm and not more than 15 μm, 3 to 12 μm, or 4 to 10 μm. If the fiber diameter is 2 μm or less, the rigidity of the fiber tends to decrease. If the fiber diameter exceeds 15 μm, the aspect ratio of the fiber (the ratio of length (L) to thickness (D): L / D) decreases, and the rigidity, heat resistance, etc. may decrease.
[0062] As the PAN-based carbon fiber, for example, "Pyrofil" manufactured by Mitsubishi Rayon Co., Ltd., "Torayca" manufactured by Toray Industries, Inc., or "Besfight" manufactured by Toho Tenax Co., Ltd. can be used.
[0063] As the pitch-based carbon fiber, for example, "Dialead" manufactured by Mitsubishi Plastics, Inc., "DonaCarbo" manufactured by Osaka Gas Chemicals, or "Kureka" manufactured by Kureha Chemical Industry Co., Ltd. can be used.
[0064] (Aramid Fiber) The aramid constituting the aramid fiber is preferably meta-aramid, para-aramid, or copolymerized para-aramid, more preferably para-aramid or copolymerized para-aramid, and even more preferably copolymerized para-aramid. Here, the para-aramid refers to an aramid having a structure in which each benzene ring is linearly linked via an amide group (CONH).
[0065] Specific examples of aramid fibers include meta-aramid fibers such as NOMEX, a trade name of DuPont, TEIJINCONEX, a trade name of Teijin Limited, Japan, METASTAR, a trade name of Yantai Co., Ltd., China, and X-FIPER, a trade name of SRO Group, China, as well as TWARON, a trade name of Teijin Limited, KEVLAR, a trade name of DuPont, KERMEL TECH, a trade name of Kermel, and HERACRON, a trade name of Kolon Industries.
[0066] The fiber diameter of the monofilaments forming the aramid fiber bundle may be, for example, 1 to 50 μm, 3 to 30 μm, or 5 to 15 μm, from the viewpoint of increasing the bending strength and impact resistance of the resulting resin composition.
[0067] (Basalt fiber) Basalt fiber is made by melting the mineral basalt in a melting furnace and spinning it into fibers, and is usually made of only basalt. Basalt fiber is usually made of silicon oxide (SiO 2 ) in an amount of 55 to 65 mass % and aluminum oxide (Al 2 O 3 ) 15 to 20 mass % and iron oxide (FeO, Fe 2 O 3 ) etc. Because recrystallization occurs during melt spinning, it tends to have a more homogeneous crystalline structure than other rock wools.
[0068] The fiber diameter of the monofilaments forming the basalt fiber bundle may be, for example, 2 to 15 μm, 6 to 13 μm, or 9 to 13 μm.
[0069] The fibrous filler is preferably glass fiber or carbon fiber.
[0070] In order to improve dispersibility, the fibrous filler may be surface-treated with a surface treatment agent such as an organic silane coupling agent, a titanate coupling agent, an aluminate coupling agent, a zirconate coupling agent, a silicone compound, a higher fatty acid, a fatty acid metal salt, or a fatty acid ester.
[0071] There are no limitations on the binder used to bind the fibrous filler, but for example, when the fibrous filler is an organic fiber, a polar resin or the like is preferably used.
[0072] Examples of polar resins include thermosetting resins such as unsaturated polyesters, vinyl ester resins, epoxy resins, phenolic (e.g., resol) resins, urea-melamine resins, polyimides, urethane resins, copolymers and modified products thereof; and thermoplastic resins such as saturated polyesters, polyamides, acrylic resins, copolymers and modified products thereof, and acid-modified polyolefins.
[0073] [Thermoplastic Resin] Examples of thermoplastic resins include polycarbonate, polybutylene terephthalate, polyethylene terephthalate, polyethylene naphthalate, various polyamides (PA6, PA66, PA46, PA12, semi-aromatic PA, etc.), acrylonitrile-butadiene-styrene (ABS) resin, acrylonitrile-styrene (AS) resin, methyl methacrylate-styrene (MS) resin, polyethylene, polypropylene, polyacetal, polyamideimide, polyethersulfone, polyimide, polyphenylene oxide, polyphenylene sulfide (PPS resin), polyphenylsulfone, polyetheretherketone, polystyrene, syndiotactic polystyrene, liquid crystalline polyester (liquid crystal polymer), thermoplastic polyurethane, polyvinyl chloride, fluororesin, and mixtures thereof. These may be used alone or in combination of two or more. The thermoplastic resin may be appropriately selected from the properties required for the intended use, such as heat resistance, chemical resistance, and moldability.
[0074] The thermoplastic resin preferably contains at least one selected from the group consisting of polypropylene, polyester, polyamide, polycarbonate, polystyrene, polyphenylene ether, ABS resin, AS resin, PPS resin, and liquid crystal polymer.
[0075] Although an example of the method for producing the resin composition according to the present embodiment has been described above, the method is not limited to this.
[0076] For example, the above describes an embodiment in which the second kneading zone 23 has (A) a single-loop flight and a resistance portion that generates a pressure of 2 MPa or more downstream of the single-loop flight, or (B) a double-loop flight with a clearance between the cylinder and the double-loop flight of 1.3% or more of the cylinder diameter and a resistance portion that generates a pressure of 2 MPa or more downstream of the double-loop flight, but this second kneading zone 23 may be replaced with one that has (C) a single-loop flight and resistance portions that generate a pressure of 1 MPa or more at the downstream end of the single-loop flight and at a position 1D upstream from the downstream end of the single-loop flight. In this case, it is more preferable that the second kneading zone 23 has (c) a single-loop flight and resistance portions that generate a pressure of 2 MPa or more at the downstream end of the single-loop flight and at a position 2D upstream from the downstream end of the single-loop flight.
[0077] Similarly, the second kneading zone 23 may be replaced with (D) a zone having a double flight whose clearance with the cylinder is 1.3% or more of the cylinder diameter, and resistance portions that generate a pressure of 1 MPa or more at the downstream end of the double flight and at a position 1D upstream from the downstream end of the single flight. In this case, it is more preferable that the zone have (d) a double flight whose clearance with the cylinder is 1.3% or more of the cylinder diameter, and resistance portions that generate a pressure of 2 MPa or more at the downstream end of the double flight and at a position 2D upstream from the downstream end of the single flight.
[0078] Also, the vent may or may not be provided.
[0079] The method for producing a resin composition described above is a method for producing a resin composition in which a thermoplastic resin and a fibrous filler are melt-kneaded using a twin-screw kneading extruder, and the twin-screw kneading extruder is provided with, in order from upstream as viewed in a flow direction of the materials to be melt-kneaded, a first supply port, a first kneading zone, a second supply port, and a second kneading zone, and the thermoplastic resin and the fibrous filler are supplied to the twin-screw kneading extruder from the first supply port and the second supply port, respectively, and in the first kneading zone, 50 mass % or more of the thermoplastic resin supplied from the first supply port is melted, and the second kneading zone has (A) a single flight and a pressure of 2 MPa or more downstream of the single flight. (B) having two flights whose clearance with the cylinder is 1.3% or more of the cylinder diameter and a resistance section which generates a pressure of 2 MPa or more downstream of the two flights, (C) having a single flight and a resistance section which generates a pressure of 1 MPa or more at the downstream end of the single flight and at a position 1D upstream from the downstream end of the single flight, or (D) having two flights whose clearance with the cylinder is 1.3% or more of the cylinder diameter and a resistance section which generates a pressure of 1 MPa or more at the downstream end of the two flights and at a position 1D upstream from the downstream end of the single flight. According to this method, the residual rate of undefibrated fiber bundles can be reduced.
[0080] In the above method, the clearance between the single-start flight or the double-start flight and the cylinder may be 2.0% or more of the cylinder diameter.
[0081] In the above method, the second kneading zone may have (a) a single-loop flight having a clearance between it and the cylinder of 1.3% or more of the cylinder diameter, and a resistance section that generates a pressure of 4 MPa or more downstream of the single-loop flight, (b) a double-loop flight having a clearance between it and the cylinder of 1.3% or more of the cylinder diameter, and a resistance section that generates a pressure of 4 MPa or more downstream of the double-loop flight, (c) a single-loop flight and resistance sections that generate a pressure of 2 MPa or more at the downstream end of the single-loop flight and at a position 2D upstream from the downstream end of the single-loop flight, or (d) a double-loop flight having a clearance between it and the cylinder of 1.3% or more of the cylinder diameter, and resistance sections that generate a pressure of 2 MPa or more at the downstream end of the double-loop flight and at a position 2D upstream from the downstream end of the single-loop flight.
[0082] In the above method, the length of the single flight or the double flight may be 3D or more.
[0083] [Resin Composition] According to the method for producing a resin composition according to this embodiment, a resin composition can be obtained in which the residual rate of undefibrated fiber bundles is reduced. The resin composition (fiber-based filler reinforced thermoplastic resin composition) obtained by this method maintains the inherent performance of the thermoplastic resin composition while improving its mechanical strength due to the fiber-based filler. The resin composition can be subjected to various molding methods such as injection molding, extrusion molding, compression molding, blow molding, and injection-compression molding. In particular, it is suitable for use in injection molding. The resin composition is suitable for use in, for example, plastic parts that require mechanical strength. The resin composition is particularly suitable for use in automobile parts, building materials, electrical appliance parts, etc.
[0084] The present invention will be described below using examples and comparative examples, but the present invention is not limited to these examples.
[0085] (Materials) The materials used in the examples and comparative examples are shown below.
[0086] [Thermoplastic resins] AS resin: Cevian N050SF (melt index (MI) 32 g / 10 min) manufactured by Daicel Miraize Co., Ltd. PA6 resin: A1020BRL (melt index (MI) 34 g / 10 min) manufactured by Unitika Ltd. PP resin: Noblen R101 (melt index (MI) 20 g / 10 min) manufactured by Sumitomo Chemical Co., Ltd. to which 1.5% maleic anhydride-modified PP has been added.
[0087] [Glass fiber bundle] GF (1): ECS03 T-351 manufactured by Nippon Electronic Glass Co., Ltd. (chopped strands of 3 mm length made by bundling monofilaments of 13 μm diameter) GF (2): ECS03 T-249H manufactured by Nippon Electronic Glass Co., Ltd. (chopped strands of 3 mm length made by bundling monofilaments of 10.5 μm diameter) GF (3): ECS03 T-480H manufactured by Nippon Electronic Glass Co., Ltd. (chopped strands of 3 mm length made by bundling monofilaments of 10.5 μm diameter)
[0088] The materials were used so that the resin composition would contain 70% by weight of thermoplastic resin and 30% by weight of glass fiber bundles.
[0089] (Configuration and conditions of extruder) A twin-screw kneading extruder was used, which was equipped with, from upstream to downstream in the flow direction of the melt-kneaded materials, a first feed port, a first kneading zone, a second feed port, and a second kneading zone. The thermoplastic resin and fibrous filler were fed into the twin-screw kneading extruder from the first feed port and the second feed port, respectively, and 50% by mass or more of the thermoplastic resin fed from the first feed port was melted in the first kneading zone. The configuration and conditions of the extruder used are shown below. Extruder: Co-rotating twin-screw kneading extruder TEM-26SX (manufactured by Shibaura Machine Co., Ltd.) Cylinder diameter: 26.6 mm Extrusion conditions: Cylinder temperature 250°C, discharge rate 100 kg / hour Pressure sensors: Installed at the upstream end of the resistance section (i.e., the downstream end of the flight), and at positions 65.0 mm upstream (equivalent to 2.40 D upstream) and 105.0 mm upstream (equivalent to 4.00 D upstream) from the upstream end of the resistance section (i.e., the downstream end of the flight).
[0090] [Screw Segment] (1) Screw segment used in the resistance part Notched segment: A screw segment in which a ring having 12 notches on the circumference is combined with four pairs of 1D segments alternately on the left and right.
[0091] (2) Screw segments used in the mixing and dispersion section Double-row flight a: A double-row flight having a flight lead length of 1D and a cylinder clearance of 0.66% of the cylinder diameter. Double-row flight b: A double-row flight having a flight lead length of 1D and a cylinder clearance of 1.62% of the cylinder diameter. Double-row flight c: A double-row flight having a flight lead length of 1D and a cylinder clearance of 3.25% of the cylinder diameter. Single-row flight a: A single-row flight having a flight lead length of 1D and a cylinder clearance of 0.66% of the cylinder diameter and a flight width of 30% of the cylinder diameter. Single-row flight b: A single-row flight having a flight lead length of 1D and a cylinder clearance of 3.25% of the cylinder diameter and a flight width of 33% of the cylinder diameter. Single-row flight c: A single-row flight having a flight lead length of 1D and a cylinder clearance of 0.66% of the cylinder diameter and a flight width of 23% of the cylinder diameter. Forward kneading discs: Seven discs are arranged in 1D, shifted by 30° in the same direction as the screw rotation.
[0092] [Examples 1 to 7 and Comparative Examples 1 to 3] 70% by weight of AS resin and 30% by weight of GF (ECS03 T-351) were melt-kneaded using a co-rotating twin-screw kneading extruder TEM-26SX to obtain a resin composition. The screw configurations of the resistance section and the mixing / dispersion section of the twin-screw kneading extruder, as well as the screw rotation speed, are shown in Table 1. Table 2 also shows the resin pressure at the upstream end of the resistance section (i.e., the downstream end of the flight), as well as the resin pressure at positions 65.0 mm upstream (corresponding to 2.40 D upstream) and 105.0 mm upstream (corresponding to 4.00 D upstream) from the upstream end of the resistance section (i.e., the downstream end of the flight).
[0093] (Evaluation of Resin Composition) The obtained resin composition was evaluated by the following procedure.
[0094] The obtained thermoplastic resin composition was dried at 120°C for 4 hours, and then molded into test specimens using an injection molding machine IS80EPN-2A manufactured by Shibaura Machine Co., Ltd. at a cylinder temperature of 240°C and a mold temperature of 60°C.
[0095] [Number of Undefibrated Fibers] Thirty test pieces were visually observed, and the number of undefibrated fibers was counted.
[0096] [Flexural Modulus] The flexural modulus of the test piece was measured using a Tensilon universal testing machine RTC-1310A manufactured by A&D Corporation.
[0097] The number of unfibrillated fibers and the flexural modulus of the test specimen are shown in Table 2.
[0098] In the table, the notation "Notch: 2D" indicates that the notch segment has a length of 2D. The same applies to similar notations such as "2-flight a: 4D."
[0099]
[0100] For Example 3, the resin pressure at the upstream end of the resistance section (i.e., the downstream end of the mixing-dispersion section), and the resin pressure at positions 65.0 mm upstream (corresponding to 2.40 D upstream) and 105.0 mm upstream (corresponding to 4.00 D upstream) from the upstream end of the resistance section (i.e., the downstream end of the mixing-dispersion section) are shown in Figure 5. As is clear from Figure 5, in Example 3, the pressure is highest at the upstream end of the resistance section and decreases toward the downstream side, and the mixing-dispersion section has a region configured with screw segments in which the pressure decreases from the downstream end (upstream end of the resistance section) toward the upstream side.
[0101] Examples 8 to 10: 70% by weight of PA6 resin and 30% by weight of GF (ECS03 T-249H) were melt-kneaded using a co-rotating twin-screw kneading extruder TEM-26SX to obtain a resin composition. The screw configurations of the resistance section and the mixing / dispersion section of the twin-screw kneading extruder, as well as the screw rotation speed, are shown in Table 3. Table 4 also shows the resin pressure at the upstream end of the resistance section (i.e., the downstream end of the flight), as well as the resin pressure at positions 65.0 mm upstream (corresponding to 2.40 D upstream) and 105.0 mm upstream (corresponding to 4.00 D upstream) from the upstream end of the resistance section (i.e., the downstream end of the flight).
[0102] (Evaluation of Resin Composition) The obtained resin composition was evaluated by the following procedure.
[0103] The obtained thermoplastic resin composition was vacuum dried at 80°C for 24 hours, and then molded into test specimens using an injection molding machine IS80EPN-2A manufactured by Shibaura Machine Co., Ltd. at a cylinder temperature of 240°C and a mold temperature of 60°C.
[0104] [Number of Undefibrated Fibers] Thirty test pieces were visually observed, and the number of undefibrated fibers was counted.
[0105] [Flexural Modulus] The flexural modulus of the test piece was measured using a Tensilon universal testing machine RTC-1310A manufactured by A&D Corporation.
[0106] The number of unfibrillated fibers and the flexural modulus of the test specimen are shown in Table 4.
[0107]
[0108]
[0109] [Examples 11 to 13 and Comparative Example 4] 70% by weight of PP resin and 30% by weight of GF (ECS03 T-480H) were melt-kneaded using a co-rotating twin-screw kneading extruder TEM-26SX to obtain a resin composition. The screw configurations of the resistance section and the mixing / dispersion section of the twin-screw kneading extruder, as well as the screw rotation speed, are shown in Table 5. Table 6 also shows the resin pressure at the upstream end of the resistance section (i.e., the downstream end of the flight), and the resin pressures at positions 65.0 mm upstream (corresponding to 2.40 D upstream) and 105.0 mm upstream (corresponding to 4.00 D upstream) from the upstream end of the resistance section (i.e., the downstream end of the flight).
[0110] (Evaluation of Resin Composition) The obtained resin composition was evaluated by the following procedure.
[0111] The obtained thermoplastic resin composition was dried at 120°C for 4 hours, and then molded into test specimens using an injection molding machine IS80EPN-2A manufactured by Shibaura Machine Co., Ltd. at a cylinder temperature of 240°C and a mold temperature of 60°C.
[0112] [Number of Undefibrated Fibers] Thirty test pieces were visually observed, and the number of undefibrated fibers was counted.
[0113] [Flexural Modulus] The flexural modulus of the test piece was measured using a Tensilon universal testing machine RTC-1310A manufactured by A&D Corporation.
[0114] The number of unfibrillated fibers and the flexural modulus of the test specimens are shown in Table 6.
[0115]
[0116]
[0117] It can be seen that the methods according to the Examples can reduce the residual rate of undefibrated fiber bundles compared to the methods according to the Comparative Examples. In other words, it can be seen that the methods according to the Examples can produce resin compositions with a low residual rate of undefibrated fiber bundles.
[0118] 1a, 1b...supply ports, 5...vent port, 10...notched segment, 20...supply zone, 21...first kneading zone, 22, 24...conveying zone, 23...second kneading zone, 23b...resistance section, 23a...mixing and dispersing section.
Claims
1. A method for producing a resin composition in which a thermoplastic resin and a fibrous filler are melt-kneaded using a twin-screw kneading extruder, the twin-screw kneading extruder having, in order from upstream as viewed in the flow direction of the materials to be melt-kneaded, a first supply port, a first kneading zone, a second supply port, and a second kneading zone, the thermoplastic resin and the fibrous filler are supplied to the twin-screw kneading extruder from the first supply port and the second supply port, respectively, and in the first kneading zone, 50 mass% or more of the thermoplastic resin supplied from the first supply port is melted, and the second kneading zone has: (A) a single flight and a resistance portion that generates a pressure of 2 MPa or more downstream of the single flight; (B) a double flight having a clearance between the cylinder and the double flight of 1.3% or more of the cylinder diameter, and a resistance portion that generates a pressure of 2 MPa or more downstream of the double flight. (C) a single-flight and a resistance portion that generates a pressure of 1 MPa or more at a downstream end of the single-flight and at a position 1D upstream from the downstream end of the single-flight, or (D) a double-flight having a clearance between the cylinder of 1.3% or more of a cylinder diameter and a resistance portion that generates a pressure of 1 MPa or more at the downstream end of the double-flight and at a position 1D upstream from the downstream end of the single-flight.
2. The method for producing a resin composition according to claim 1, wherein the clearance between the single-row flight or the double-row flight and the cylinder is 2.0% or more of the cylinder diameter.
3. A method for producing a resin composition according to claim 1, wherein the second kneading zone (a) has a single-rod flight having a clearance between the cylinder of 1.3% or more of the cylinder diameter and a resistance section downstream of the single-rod flight that generates a pressure of 4 MPa or more; (b) has a double-rod flight having a clearance between the cylinder of 1.3% or more of the cylinder diameter and a resistance section downstream of the double-rod flight that generates a pressure of 4 MPa or more; (c) has a single-rod flight and a resistance section that generates a pressure of 2 MPa or more at the downstream end of the single-rod flight and at a position 2D upstream from the downstream end of the single-rod flight; or (d) has a double-rod flight having a clearance between the cylinder of 1.3% or more of the cylinder diameter and a resistance section that generates a pressure of 2 MPa or more at the downstream end of the double-rod flight and at a position 2D upstream from the downstream end of the single-rod flight.
4. A method for producing a resin composition according to any one of claims 1 to 3, wherein the length of the single flight or the double flight is 3D or more.
5. A method for producing a resin composition according to any one of claims 1 to 3, wherein the fibrous filler is a fiber bundle.
6. A method for producing a resin composition according to any one of claims 1 to 3, wherein the fibrous filler is glass fiber or carbon fiber.
7. A method for producing a resin composition according to any one of claims 1 to 3, wherein the thermoplastic resin comprises at least one selected from the group consisting of polypropylene, polyester, polyamide, polycarbonate, polystyrene, polyphenylene ether, ABS resin, AS resin, PPS resin and liquid crystal polymer.
8. A resin composition obtainable by the method for producing a resin composition according to any one of claims 1 to 3, wherein the thermoplastic resin comprises at least one selected from the group consisting of polypropylene, polyester, polyamide, polycarbonate, polystyrene, polyphenylene ether, ABS resin, AS resin, PPS resin and liquid crystal polymer.
Citation Information
Patent Citations
Raw material for electromagnetic wave-shielding material and its production
JP1997235382A
Method for kneading easily deteriorative material to be kneaded and twin-screw extruder fitted thereto
JP2003205519A