Barrier film
The laminated barrier film with a polymer base, planarization, inorganic gas barrier, and organic-inorganic hybrid coating layers on both sides of a bonding layer addresses the poor barrier properties of polymer substrates, enhancing reliability and optical performance while maintaining inorganic gas barrier durability.
Patent Information
- Application Number
- PCT/KR2023/015242
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-11
- Filing Date
- 2023-10-04
- Publication Date
- 2024-11-14
AI Technical Summary
Conventional polymer-based flexible substrates for displays have poor moisture and oxygen barrier properties, which complicates their use in high-definition LCD or OLED displays, and the durability of inorganic gas barrier layers is compromised when applied externally, affecting the reliability of the barrier film.
A laminated barrier film structure is developed, featuring a polymer base layer, planarization layer, inorganic gas barrier layer, and organic-inorganic hybrid coating layer sequentially stacked on both sides of a bonding layer, with the inorganic gas barrier layer positioned inside to enhance durability and optical properties.
The proposed structure significantly improves the reliability, optical properties, and barrier performance against moisture and oxygen, maintaining the durability of the inorganic gas barrier layer while achieving high light transmittance and low water vapor permeability.
Smart Images

Figure KR2023015242_14112024_PF_FP_ABST
Abstract
Description
barrier film
[0001] The present invention relates to a barrier film.
[0002] More specifically, the present invention relates to a laminated barrier film having a structure in which a laminate including an inorganic gas barrier layer is arranged on both sides of a bonding layer.
[0003] This application claims priority from Korean Patent Application No. 10-2023-0060985, dated May 11, 2023, which is incorporated herein by reference.
[0004]
[0005] Materials such as displays, solar cells, and batteries are vulnerable to moisture and oxygen penetration, so they must be prevented from doing so.
[0006] Conventional display materials utilize glass substrates, which boast numerous advantages, including a small coefficient of linear expansion, excellent gas barrier properties, high light transmittance, superior surface flatness, superior heat resistance, and excellent chemical resistance, to prevent moisture and oxygen penetration. However, glass is susceptible to impact and shatters easily, and its high density makes it heavy. In particular, glass is not suitable for flexible displays, which are attracting attention as a key next-generation display. Therefore, active research is being conducted into polymer films that can replace glass.
[0007] Flexible displays are a key technology industry that has captured the attention of general consumers due to their low power, low cost, ultra-lightweight, large-area implementation, and portability, allowing easy access to information anytime, anywhere. Furthermore, flexible displays, which utilize polymer film as their substrate, can be produced using roll-to-roll methods. This industry is poised to emerge as a key player in the display market, driven by the commercialization of mass production technologies for small consumer devices such as mobile devices. Flexible substrates, in particular, are already a topic of intense research by numerous companies and research institutes.
[0008] Thermoplastic polymers such as polycarbonate (PC), polyimide (PI), polyethersulfone (PES), polyarylate (PAR), poly(ethylene naphthalate), poly(ethylene terephthalate) (PET), and cycloolefin copolymer, as well as polymers cured from curable resins such as acrylic resin, epoxy resin, and unsaturated polyester, have excellent optical properties and are used in flexible substrates.
[0009] However, flexible substrates containing only polymer transparent films manufactured from the aforementioned polymers have very poor barrier properties against moisture and oxygen penetration. Therefore, active experiments are underway to coat polymer transparent films with multilayer functional coatings that offer superior barrier properties against moisture and oxygen penetration. Currently, inorganic gas barrier layers and organic-inorganic hybrid coating layers are commonly used as functional coating layers.
[0010] However, the functional coating layer lacks superior optical properties compared to polymer transparent films. This makes it difficult to produce products that meet consumer demands when applied to high-definition LCD or OLED displays. Furthermore, if a functional coating layer, such as an inorganic gas barrier layer that blocks moisture and oxygen penetration, is positioned on the outside of the barrier film, the durability of the inorganic gas barrier layer can easily deteriorate after the barrier film is applied to the product, lowering the reliability of the barrier film.
[0011] Therefore, a barrier film with excellent reliability, optical properties, moisture and oxygen barrier properties is required.
[0012]
[0013] [Prior Art Literature]
[0014] [Patent Document]
[0015] Republic of Korea Publication Patent No. 10-2021-0156622
[0016]
[0017] The problem to be solved by the present invention is to provide a barrier film having excellent reliability, optical properties, and moisture and oxygen barrier properties.
[0018]
[0019] According to one embodiment of the present invention, a barrier film is provided in which a laminate in which a polymer substrate layer, a planarization layer, an inorganic gas barrier layer, and an organic-inorganic hybrid coating layer are sequentially laminated is disposed on both sides of a bonding layer.
[0020] In one embodiment, the bonding layer may have a thickness of 5 μm to 50 μm.
[0021] In one embodiment, the refractive index of the bonding layer may be less than the refractive index of the polymer substrate layer.
[0022] In one embodiment, the bonding layer may have an adhesion strength of greater than or equal to 2000 gf / 25 mm as measured according to ASTM D1876-08.
[0023] In one embodiment, the bonding layer may include an acrylic resin, an epoxy resin, a silicone resin, a fluorine resin, a styrene resin, a polyolefin resin, a thermoplastic elastomer, a polyoxyalkylene resin, a polyester resin, a polyvinyl chloride resin, a polycarbonate resin, a polyphenylene sulfide resin, a mixture of hydrocarbons, a polyamide resin, or a mixture thereof.
[0024] In one embodiment, the laminates disposed on both sides of the bonding layer may be arranged such that the organic / inorganic hybrid coating layer is positioned on the bonding layer side.
[0025] In one embodiment, the laminate disposed on one surface of the bonding layer may be disposed such that the polymer substrate layer is positioned toward the bonding layer, and the laminate disposed on the other surface of the bonding layer may be disposed such that the organic / inorganic hybrid coating layer is positioned toward the bonding layer.
[0026] In one embodiment, the laminates disposed on both sides of the bonding layer may be arranged such that the polymer substrate layer is positioned toward the bonding layer.
[0027] In one embodiment, the polymer substrate layer comprises a thermoplastic transparent base resin, and the thermoplastic transparent base resin may comprise at least one selected from the group consisting of polyethylene terephthalate, polyethersulfone, polycarbonate, polyimide, polyarylate, polyethylene naphthalate, polyethylene terephthalate glycol, polycyclohexylenedimethylene terephthalate glycol, and cycloolefin copolymer.
[0028] In one embodiment, the polymer substrate layer may have a coefficient of thermal expansion of 100 ppm / ℃ or less in a range of 100°C or more and 130°C or less.
[0029] In one embodiment, the polymer substrate layer may have a heat shrinkage rate in the MD (Machine Direction) direction of 0.5% or less and a heat shrinkage rate in the TD (Transverse Direction) direction of 0.3% or less, and the heat shrinkage rate may be calculated by the following mathematical equation 1.
[0030] [Mathematical Formula 1]
[0031] (Initial length of polymer substrate layer - length of polymer substrate layer after heat shrinkage treatment at 150℃ for 30 minutes / Initial length of polymer substrate layer) × 100
[0032]
[0033] In one embodiment, the planarization layer may have the same composition as the organic-inorganic hybrid coating layer.
[0034] In one embodiment, the planarization layer and the organic-inorganic hybrid coating layer may include a curable coating solution including a (meth)acrylate monomer, a (meth)acrylate oligomer having an epoxy group and a weight average molecular weight of 500 to 10,000, an initiator, silica particles, and a dispersion medium, and a curable sol solution including a metal alkoxide, a curing accelerator, an inorganic acid, and a solvent, and a curable resultant of the curable sol solution.
[0035] In one embodiment, the inorganic gas barrier layer may include an oxide, nitride, carbide, oxynitride, oxycarbide, nitride carbide, or oxynitride carbide containing one or more metals selected from the group consisting of Si, Al, In, Sn, Zn, Ti, Cu, Ce, and Ta.
[0036]
[0037] A barrier film according to one embodiment of the present invention has excellent reliability, optical properties, moisture and oxygen barrier properties.
[0038]
[0039] FIG. 1 is a drawing schematically showing the structure of a barrier film according to one embodiment of the present invention.
[0040] FIG. 2 is a drawing schematically showing the structure of a barrier film according to one embodiment of the present invention.
[0041] FIG. 3 is a drawing schematically showing the structure of a barrier film according to one embodiment of the present invention.
[0042] Figure 4 is a schematic drawing showing the structure of a laminate in which a polymer substrate layer, a planarization layer, an inorganic gas barrier layer, and an organic-inorganic hybrid coating layer are sequentially laminated.
[0043]
[0044] [Explanation of symbols]
[0045] 1: Polymer substrate layer
[0046] 2: Flattening layer
[0047] 3: Inorganic gas barrier layer
[0048] 4: Organic-inorganic hybrid coating layer
[0049] 5: Bonding layer
[0050]
[0051] According to one embodiment of the present invention, a barrier film is provided in which a laminate in which a polymer substrate layer, a planarization layer, an inorganic gas barrier layer, and an organic-inorganic hybrid coating layer are sequentially laminated is disposed on both sides of a bonding layer.
[0052]
[0053] The advantages and features of the present invention, and the methods for achieving them, will become clearer with reference to the embodiments described below, along with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below and may be implemented in various forms. These embodiments are provided solely to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the scope of the invention. The present invention is defined solely by the scope of the claims.
[0054] The size and thickness of each component shown in the drawing are arbitrarily shown for convenience of explanation, so the present invention is not necessarily limited to what is shown in the drawing, and the thickness is shown enlarged to clearly express various parts and areas.
[0055] The terms used in this invention have been selected from widely used, current terms, taking into account the functions of the invention. However, these terms may vary depending on the intentions of those skilled in the art, precedents, the emergence of new technologies, etc. Furthermore, in certain cases, the applicant may arbitrarily select terms, in which case their meanings will be described in detail in the description of the relevant invention. Therefore, the terms used in this invention should not be defined simply as names, but rather based on the meanings of the terms and the overall content of the invention.
[0056]
[0057] The terms used in this specification will be explained, and specific details for implementing the present invention will be described.
[0058] In this specification, terms such as "include" or "have" are intended to specify the presence of a feature, number, step, operation, component, part, or combination thereof described in the specification, but should be understood to not preclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof. In addition, when it is said that a part such as a layer, film, region, plate, or laminate is disposed "on" another part, this includes not only the case where it is disposed "directly above" the other part, but also the case where another part is disposed in between. Conversely, when it is said that a part such as a layer, film, region, plate, or laminate is disposed "under" another part, this includes not only the case where it is disposed "directly below" the other part, but also the case where another part is disposed in between. In addition, in this specification, being disposed "on" may include the case where it is disposed below as well as above.
[0059]
[0060] Below, specific details regarding the components included in the present invention are described.
[0061]
[0062] barrier film
[0063] Referring to FIGS. 1 to 3, a barrier film according to one embodiment of the present invention has a structure in which a polymer substrate layer (1), a planarization layer (2), an inorganic gas barrier layer (3), and an organic-inorganic hybrid coating layer (4) are sequentially laminated on both sides of a bonding layer (5), and thus has excellent reliability, optical properties, moisture and oxygen barrier properties.
[0064] Referring to FIG. 1, a barrier film according to one embodiment of the present invention may have a structure in which all laminates disposed on both sides of a bonding layer (5) have an organic-inorganic hybrid coating layer (4) positioned on the bonding layer (5). A barrier film according to one embodiment having such a structure may have superior reliability of the barrier film because the inorganic gas barrier layer (3) is positioned on the inner side of the barrier film.
[0065] Referring to FIG. 2, a barrier film according to an embodiment of the present invention may have a structure in which a laminate disposed on one surface of a bonding layer (5) has a polymer substrate layer (1) positioned toward the bonding layer (5) and a laminate disposed on the other surface of the bonding layer (5) has an organic / inorganic hybrid coating layer (4) positioned toward the bonding layer (5). FIG. 2 illustrates a barrier film having a structure in which a laminate disposed on a lower surface of the bonding layer (5) has a polymer substrate layer (1) positioned toward the bonding layer (5) and a laminate disposed on an upper surface of the bonding layer (5) has an organic / inorganic hybrid coating layer (4) positioned toward the bonding layer (5), but this is merely an example. That is, the laminates disposed on the upper and lower surfaces of the bonding layer (5) may be disposed with their positions exchanged. In a barrier film according to the same embodiment of the structure, the inorganic gas barrier layer (3) of the laminate disposed on one side of the bonding layer (5) is located on the inside of the barrier film, and the polymer substrate layer (1) of the laminate disposed on the other side is located on the bonding layer (5), so that the reliability and optical properties of the barrier film can be excellent.
[0066] Referring to FIG. 3, a barrier film according to one embodiment of the present invention may have a structure in which all laminates disposed on both sides of a bonding layer (5) have a polymer substrate layer (1) positioned on the bonding layer (5). A barrier film according to one embodiment having such a structure may have superior optical properties because a polymer substrate layer (1) having a refractive index similar to that of the bonding layer (5) is positioned on the bonding layer (5).
[0067] A barrier film according to one embodiment of the present invention has a structure in which identical laminates are arranged on both sides of a bonding layer (5), so that the manufacturing process is more economical and the manufacturing yield can be further improved.
[0068] A barrier film according to one embodiment of the present invention can have low water vapor permeability due to its multilayer structure.
[0069]
[0070] According to one embodiment, a barrier film may have a light transmittance (550 nm) of 85% to 95%. The light transmittance can be measured using a 3600D instrument from Minolta according to ASTM D1003.
[0071] According to one embodiment, a barrier film may have a water vapor permeability of 0.004 or less. The water vapor permeability can be measured using a Mocon PERMATRAN-W3 / 31 device at 37.8°C and 100% RH for 48 hours.
[0072] A barrier film according to one embodiment may have a haze of 1.00% or less. The haze can be measured using an NDH-5000 device from Nippon Denshoku according to ASTM D1003.
[0073]
[0074] Polymer substrate layer
[0075] In one embodiment, the polymer substrate layer may include a thermoplastic transparent base resin. Non-limiting examples of the thermoplastic transparent base resin include polyethylene terephthalate, polyethersulfone, polycarbonate, polyimide, polyarylate, polyethylene naphthalate, polyethylene terephthalate glycol, polycyclohexylenedimethylene terephthalate glycol, and cycloolefin copolymers.
[0076] In one embodiment, the thickness of the polymer substrate layer may be from 0.01 μm to 1000 μm. When the thickness of the polymer substrate layer increases or decreases by a certain value, the physical properties of the polymer substrate layer may also change.
[0077] In one embodiment, the polymer substrate layer may have a coefficient of thermal expansion of 100 ppm / ℃ or less in a temperature range of 100°C or more and 130°C or less, preferably 80 ppm / ℃ or less, and most preferably 50 ppm / ℃ or less. The temperature range of 100°C or more and 130°C or less may refer to a temperature range of 100°C or more and 130°C or less.
[0078] If the polymer substrate layer has a high coefficient of thermal expansion, significant shrinkage may occur upon returning to room temperature after high-temperature processing, potentially compromising the dimensional stability of the barrier film. Furthermore, differences in coefficients of thermal expansion compared to other layers can lead to cracking, delamination, or curling, reducing the durability and reliability of the barrier film.
[0079] The above thermal expansion coefficient can be measured by setting the pulling force to 0.01 N or more and 0.5 N or less, or 0.1 N or more and 0.3 N or less for a polymer substrate sample having a thickness of 10 ㎛ to 200 ㎛, and performing the first temperature increasing process at a temperature increasing rate of 1 ℃ / min or more and 10 ℃ / min or less, or 4 ℃ / min or more and 6 ℃ / min in a temperature range of 100 ℃ or more and 130 ℃ or less, and cooling at a cooling rate of 1 ℃ / min or more and 10 ℃ / min or less, or 4 ℃ / min or more and 6 ℃ / min or less in a temperature range of 130 ℃ or more and 100 ℃ or more. The thermal expansion change pattern can be measured using a TMA (TMA Q400 V20.7 Bulid 21) equipment manufactured by TA.
[0080] In one embodiment, the polymer substrate layer may have a heat shrinkage in the Machine Direction (MD) direction of 0.5% or less and a heat shrinkage in the Transverse Direction (TD) direction of 0.3% or less. The heat shrinkage can be calculated by the following Mathematical Formula 1. The MD direction may be a longitudinal direction or a transverse direction of the polymer substrate layer, and the TD direction may be a transverse direction or a vertical direction of the polymer substrate layer. When calculating the heat shrinkage in the MD direction, the "MD direction length" is substituted for the "length" in Mathematical Formula 1 below, and when calculating the heat shrinkage in the TD direction, the "TD direction length" is substituted for the "length" in Mathematical Formula 1 below.
[0081] [Mathematical Formula 1]
[0082] (Initial length of polymer substrate layer - length of polymer substrate layer after heat shrinkage treatment at 150℃ for 30 minutes / Initial length of polymer substrate layer) × 100
[0083]
[0084] If the thermal shrinkage of the polymer substrate layer is too high, the barrier film may not maintain dimensional stability. Furthermore, cracking, peeling, or curling may occur, reducing the durability and reliability of the barrier film.
[0085] In one embodiment, the refractive index of the polymer substrate layer may be 1.5 to 2.5, preferably 1.6 to 1.7, but is not limited thereto. In one embodiment, considering the optical properties of the barrier film, the refractive index of the polymer substrate layer is preferably greater than the refractive index of the bonding layer described later. The refractive index may refer to the refractive index for light with a wavelength in the range of 500 nm to 600 nm. The measurement wavelength of the refractive index may be, in other examples, 520 nm to 580 nm, 540 nm to 560 nm, or 545 nm to 555 nm.
[0086] In one embodiment, the polymer substrate layer may optionally include a glass fiber fabric, and the glass fiber fabric may be impregnated with a thermoplastic transparent polymer resin. In addition, the polymer substrate layer may optionally include an inorganic nanomaterial dispersed in the thermoplastic transparent polymer resin. The glass fiber fabric and the inorganic nanomaterial may be included in the polymer substrate layer to improve the mechanical properties or optical properties of the barrier film. A detailed description of the glass fiber fabric and the inorganic nanomaterial is omitted. However, in one embodiment of the present invention, the glass fiber fabric and the inorganic nanomaterial that can be included for the above purpose in the present technical field may be included in the polymer substrate layer.
[0087] In one embodiment, a plasma surface treatment layer may be disposed on the polymer substrate layer as needed. The plasma surface treatment layer may be disposed to improve the adhesion of the polymer substrate layer and the moisture and oxygen barrier properties of the barrier film. A detailed description of the plasma surface treatment layer is omitted. However, in the art, a plasma surface treatment layer that can be disposed for the above-described purpose may be disposed on the polymer substrate layer in one embodiment of the present invention.
[0088] Among the polymer substrate layer, planarization layer, inorganic gas barrier layer, and organic-inorganic hybrid coating layer of the laminate described below, the layer with the smallest refractive index difference with respect to the bonding layer may be the polymer substrate layer. Therefore, when the laminate is disposed on one surface of the bonding layer, the polymer substrate layer of the laminate should be disposed so as to be positioned toward the bonding layer, so that the optical properties of the barrier film can be improved.
[0089]
[0090] flattening layer
[0091] In one embodiment, the planarization layer may have the same composition as the organic-inorganic hybrid coating layer described below. The description of the planarization layer may be the same as the description of the organic-inorganic hybrid coating layer described below.
[0092] Even if the flattening layer and the organic-inorganic hybrid coating layer have the same composition, their positions within the laminate are different, and the functions or roles of each layer may be different.
[0093] The planarization layer can reduce stress at high temperatures caused by the difference in thermal expansion coefficient between the polymer substrate layer and the inorganic barrier layer, and can minimize defects that may occur during deposition by increasing the flatness of the polymer substrate layer.
[0094]
[0095] Inorganic gas barrier layer
[0096] In one embodiment, the inorganic gas barrier layer may include, but is not limited to, an oxide, nitride, carbide, oxynitride, oxycarbide, nitride-carbide, or oxynitride-carbide containing one or more metals selected from the group consisting of Si, Al, In, Sn, Zn, Ti, Cu, Ce, and Ta. More specifically, in one embodiment, the inorganic gas barrier layer may include, but is not limited to, silicon oxide, silicon nitride, aluminum oxide, or ITO (indium tin oxide).
[0097] In one embodiment, the thickness of the inorganic gas barrier layer may be from 10 nm to 200 nm, preferably from 20 nm to 150 nm, and most preferably from 30 nm to 100 nm.
[0098] When the thickness of the inorganic gas barrier layer satisfies this range, a uniform film can be formed, dispersion can be facilitated, excellent gas barrier properties can be exhibited, the interlayer stress reduction effect by the coating layer can be sufficiently expressed, and problems such as cracking or peeling can be prevented.
[0099] In a barrier film, the layer that contributes the most to moisture and oxygen blocking may be an inorganic gas barrier layer. Therefore, when a laminate in which a polymer substrate layer, a planarization layer, an inorganic gas barrier layer, and an organic-inorganic hybrid coating layer are sequentially laminated is disposed on one surface of a bonding layer to be described later, it may be advantageous for the reliability of the barrier film for the organic-inorganic hybrid coating layer of the laminate to be disposed so that it is positioned toward the bonding layer. This is because, when disposed as described above, the inorganic gas barrier layer can be positioned more internally within the barrier film that is ultimately manufactured, so that the durability of the inorganic gas barrier layer can be maintained excellently even after the barrier film is applied to a product.
[0100]
[0101] Organic-inorganic hybrid coating layer
[0102] In one embodiment, the organic-inorganic hybrid coating layer may include a curable coating solution including a (meth)acrylate monomer, a (meth)acrylate oligomer having an epoxy group and a weight average molecular weight of 500 to 10,000, an initiator, silica particles, and a dispersion medium, and a curable sol solution including a metal alkoxide, a curing accelerator, an inorganic acid, and a solvent, and a curable product of the curable sol solution.
[0103] The above curable sol solution may include a curable coating solution in which a (meth)acrylate monomer, a (meth)acrylate oligomer having an epoxy group and a weight average molecular weight of 500 to 10,000, and an initiator are dissolved in a solvent and silica particles are dispersed.
[0104] The above (meth)acrylate monomer functions to control the viscosity and curing density of the curable coating solution and to improve adhesion with the inorganic gas barrier layer. The (meth)acrylate monomer may be a monofunctional or polyfunctional monomer. Additionally, it may exist in an ethoxylated or propoxylated form. (Meth)acrylate monomers include 2(2-ethoxyethoxy)ethyl acrylate, 2-phenoxyethyl acrylate, 2-phenoxyethyl methacrylate, caprolactone acrylate, dicyclopentadienyl methacrylate, tetrahydrofurfuryl acrylate, tetrahydrofurfuryl methacrylate, 1,3-butylene glycol diacrylate, 1,4 butanediol dimethacrylate, diethylene glycol diacrylate, ethoxylated bisphenol A diacrylate, ethoxylated bisphenol A dimethacrylate, ethylene glycol dimethacrylate, ethoxylated trimethylolpropane triacrylate, pentaerythritol triacrylate, propoxylated glyceryl triacrylate, propoxylated trimethylolpropane triacrylate, Trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, tris(2-hydroxyethyl) isocyanurate triacrylate, etc. can be used alone or in combination of two or more thereof.
[0105] The (meth)acrylate oligomer having the above epoxy group and a weight average molecular weight of 500 to 10,000 is an oligomer having a (meth)acrylate group and an epoxy group, and contributes to good adhesion of an organic-inorganic hybrid coating layer on a polymer substrate layer or an inorganic gas barrier layer. In particular, it contributes to improving adhesion with a polymer substrate layer, and for example, bisphenol-A epoxy acrylate oligomer, flame-retardant epoxy acrylate oligomer, novolac-type epoxy acrylate oligomer, bisphenol-F epoxy acrylate oligomer, glycidyl amine-type epoxy acrylate oligomer, rubber-modified epoxy acrylate oligomer, etc. can be used alone or in combination of two or more thereof.
[0106] The above initiator can be any chemical compound capable of initiating polymerization of (meth)acrylate functional groups by actinic radiation. Examples of suitable photoinitiators include 1-hydroxy-cyclohexyl-phenyl-ketone, benzophenone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2-hydroxy-1-[4-(2-hydroxyethoxy)phenyl]-2-methyl-1-propanone, 2-benzyl-2-(dimethylamino)-1-[4-(4-morpholinyl)phenyl]-1-butanone, diphenyl(2,4,6-trimethylbenzoyl)phosphineoxide, and mixtures thereof. Photolatent base type photoinitiators, for example, 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone, can also be used as photoinitiators.
[0107] The dispersion medium used in the above curable coating liquid includes methanol, ethanol, propanol, isopropanol, butanol, isobutanol, secondary butanol, tertiary butanol, cyclohexanol, pentanol, octanol, decanol, di-n-butyl ether, ethylene glycol dimethyl ether, propylene glycol dimethyl ether, propylene glycol methyl ether, dipropylene glycol methyl ether, tripropylene glycol methyl ether, dipropylene glycol dimethyl ether, tripropylene glycol dimethyl ether, ethylene glycol butyl ether, diethylene glycol butyl ether, ethylene glycol dibutyl ether, ethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol dimethyl ether, ethylene glycol ethyl ether, ethylene glycol diethyl ether, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, butylene glycol, dibutylene glycol, tributylene glycol, It may include tetrahydrofuran, dioxane, acetone, diacetone alcohol, methyl ethyl ketone, cyclohexanone, methyl isobutyl ketone, ethyl acetate, n-propyl acetate, n-butyl acetate, t-butyl acetate, propylene glycol monomethyl ether acetate, dipropylene glycol methyl ether acetate, 1-methoxy-2-propanol, ethyl 3-ethoxypropionate, 2-propoxyethanol, ethylene glycol ethyl ether acetate, or mixtures thereof.
[0108] The silica particles dispersed in the curable coating solution preferably have an average particle size of about 100 nm or less, more preferably about 50 nm or less. The silica particles may be added to the coating solution in the form of a dry powder, a colloidal dispersion in a suitable liquid, or other forms. The silica particles may be present as is or may be chemically modified, such as by introducing an appropriate functional group to the surface to increase the miscibility of the particles with the curable coating solution.
[0109] Additionally, the curable coating solution may further include a silicon alkoxide having a (meth)acrylate group. In the present specification, (meth)acrylate means acrylate or methacrylate.
[0110] Examples of the silicon alkoxide having the above (meth)acrylate group include (3-acryloxypropyl)dimethylmethoxysilane, (3-acryloxypropyl)methyldimethoxysilane, (3-acryloxypropyl)trimethoxysilane, (methacryloxymethyl)dimethylethoxysilane, methacryloxymethyltriethoxysilane, methacryloxymethyltrimethoxysilane, methacryloxypropylmethyldiethoxysilane, methacryloxypropylmethyldimethoxysilane, (3-methacryloxypropyl)triethoxysilane, (3-methacryloxypropyl)trimethoxysilane, etc., each alone or a mixture of two or more thereof.
[0111] The relative amounts of each of the components constituting the curable coating solution for forming the above-mentioned organic-inorganic hybrid overcoating layer can be adjusted according to the properties of the desired film, and the weight ratio of the (meth)acrylate monomer, the (meth)acrylate oligomer having an epoxy group and a weight average molecular weight of 500 to 10,000, and the silica particles contained in the curable coating solution is preferably 1 to 40 : 1 to 40 : 1 to 25, or preferably 10 to 30 : 10 to 30 : 1 to 10, or more preferably 15 to 25 : 15 to 25 : 1 to 7.
[0112] Then, a sol solution containing metal alkoxide, curing accelerator, inorganic acid, and water dissolved in a solvent is mixed with the curable coating solution.
[0113] As the metal alkoxide included in the sol solution, it is preferable to use one selected from the metal alkoxides represented by the following chemical formulas 1 to 3 or a mixture of two or more thereof.
[0114] <Chemical Formula 1>
[0115] R 1x M 1 (OR 2 ) 4-x
[0116] <Chemical Formula 2>
[0117] R 1y M 2 (OR 2 ) 3-y
[0118] <Chemical Formula 3>
[0119] R 1 z Nb(OR 2 ) 5-z
[0120] In the above chemical formulas 1 to 3, R1 is any one selected from the group consisting of an alkyl group, a vinyl group, an allyl group, a (meth)acryloxy group, an epoxide group, and an amino group having 1 to 4 carbon atoms, R2 is an alkyl group having 1 to 4 carbon atoms, M1 is a metal selected from the group consisting of Si, Ti, Zr, Ge, and Sn, M2 is a metal selected from the group consisting of Al, In, and Sb, x is 0, 1, 2, or 3, y is 0, 1, or 2, and z is 0, 1, 2, 3, or 4.
[0121] These metal alkoxides include aluminum acrylate, aluminum ethoxide, aluminum isopropoxide, aluminum methacrylate, antimony III n-butoxide, antimony III ethoxide, antimony III methoxide, germanium n-butoxide, germanium ethoxide, germanium isopropoxide, germanium methoxide, methacryloxytriethylgermane, indium methoxyethoxide, niobium V n-butoxide, niobium V ethoxide, tin II ethoxide, tin II methoxide, di-n-butyl tin diacrylate, di-n-butyl tin dimethacrylate, titanium n-butoxide, titanium ethoxide, titanium isobutoxide, titanium isopropoxide, titanium methacrylate triisopropoxide, titanium methacryloxyethyl acetoacetate triisopropoxide, titanium Examples thereof include n-propoxide zirconium n-butoxide, zirconium t-butoxide, zirconium dimethacrylate dibutoxide, zirconium ethoxide, zirconium isopropoxide, zirconium methacrylate, zirconium methacryloxyethyl acetoacetate tri-n-butoxide, zirconyl dimethacrylate, methyl trimethoxysilane, methyltriethoxysilane, tetraethoxysilane (tetraethyl orthosilicate, TEOS), tetramethoxysilane, etc., and these may be used alone or in combination of two or more.
[0122] Meanwhile, the curing accelerator included in the sol solution is preferably an organic acid curing accelerator, which enables a condensation reaction even at a relatively low temperature, thereby contributing to the application of the roll-to-roll method. Such curing accelerators may be anhydrides, carboxylic acids, or mixtures thereof. Suitable examples of anhydrides include acetic anhydride, acrylic anhydride, cyclic anhydrides, hexahydrophthalic anhydride, methacrylic anhydride, propionic anhydride, or mixtures thereof. Possible carboxylic acid components include acetic acid, acrylic acid, formic acid, fumaric acid, itaconic acid, maleic acid, methacrylic acid, propionic acid, methylene succinic acid, or mixtures thereof. These may be used alone or in combination of two or more.
[0123] The above-mentioned inorganic acid may be any inorganic acid capable of catalyzing a sol-gel hydrolysis reaction. Suitable inorganic acids include hydrochloric acid, nitric acid, sulfuric acid, hydrofluoric acid, and mixtures thereof.
[0124] The solvents include methanol, ethanol, propanol, isopropanol, butanol, isobutanol, secondary butanol, tertiary butanol, cyclohexanol, pentanol, octanol, decanol, di-n-butyl ether, ethylene glycol dimethyl ether, propylene glycol dimethyl ether, propylene glycol methyl ether, dipropylene glycol methyl ether, tripropylene glycol methyl ether, dipropylene glycol dimethyl ether, tripropylene glycol dimethyl ether, ethylene glycol butyl ether, diethylene glycol butyl ether, ethylene glycol dibutyl ether, ethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol dimethyl ether, ethylene glycol ethyl ether, ethylene glycol diethyl ether, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, butylene glycol, dibutylene glycol, tributylene glycol, tetrahydrofuran, dioxane, Examples thereof include acetone, diacetone alcohol, methyl ethyl ketone, cyclohexanone, methyl isobutyl ketone, ethyl acetate, n-propyl acetate, n-butyl acetate, t-butyl acetate, propylene glycol monomethyl ether acetate, dipropylene glycol methyl ether acetate, 1-methoxy-2-propanol, ethyl 3-ethoxypropionate, 2-propoxyethanol, ethylene glycol ethyl ether acetate, etc., and these may be used alone or in combination of two or more.
[0125] The relative amounts of each component constituting the sol solution for forming the aforementioned organic-inorganic hybrid coating layer can be appropriately adjusted depending on the properties of the desired film, and the thickness of the hybrid coating layer is preferably 0.1 to 10 ㎛.
[0126] The organic-inorganic hybrid coating layer can protect the aforementioned inorganic gas barrier layer.
[0127]
[0128] laminate
[0129] The structure of the laminate is explained with reference to Fig. 4.
[0130] In one embodiment, the laminate may have a structure in which a polymer substrate layer (1), a planarization layer (2), an inorganic gas barrier layer (3), and an organic-inorganic hybrid coating layer (4) are sequentially laminated.
[0131] Here, the structure in which a polymer substrate layer, a planarization layer, an inorganic gas barrier layer, and an organic-inorganic hybrid coating layer are sequentially laminated means a structure in which a planarization layer is laminated on a polymer substrate layer, an inorganic gas barrier layer is laminated on the planarization layer, and an organic-inorganic hybrid coating layer is laminated on an inorganic gas barrier layer.
[0132]
[0133] Below, the manufacturing method of the laminate is described. However, the description below is only an example, and it is of course possible to vary the lamination order of each layer.
[0134] The planarization layer can be formed by applying the above-described curable sol solution on the polymer substrate layer and UV curing or thermal curing. UV curing is not particularly limited as long as it can cause a radical reaction by a UV light source, but a mercury or metal halide lamp can be used alone or in combination. For example, UV curing can be performed at an energy of 160 mJ / cm. 2 1600 mJ / cm 2 The curing can be performed for 1 second to several minutes, for example, less than 1 minute. Meanwhile, the heat curing can be performed for 1 minute to several hours, for example, less than 1 hour, or 2 to 10 minutes, at a temperature of, for example, 100°C to 200°C.
[0135] The inorganic gas barrier layer can be formed by depositing and coating on the planarization layer using a physical or chemical method.
[0136] The organic-inorganic hybrid coating layer can be formed through methods such as bar coating, spin coating, dip coating, and spray coating.
[0137] The organic-inorganic hybrid coating layer can be formed by applying the above-described curable sol solution onto an inorganic gas barrier layer and curing it by UV or heat. UV curing is not particularly limited as long as it can cause a radical reaction by a UV light source, but a mercury or metal halide lamp can be used alone or in combination. For example, UV curing can be performed at an energy of 160 mJ / cm. 2 1600 mJ / cm 2 The curing can be performed for 1 second to several minutes, for example, less than 1 minute. Meanwhile, the heat curing can be performed for 1 minute to several hours, for example, less than 1 hour, or 2 to 10 minutes, at a temperature of, for example, 100°C to 200°C.
[0138]
[0139] bonding layer
[0140] In one embodiment, the bonding layer can be a pressure sensitive adhesive (PSA), an optical clear adhesive (OCA), or an optical clear resin (OCR).
[0141] In one embodiment, the bonding layer may include an adhesive component or adhesive ingredients. As used herein, the term "adhesive component" may refer to a component that is viscous at room temperature, can be bonded by applying pressure without being activated by heat, water, or solvents, exhibits strong holding power after bonding, and has cohesiveness and elasticity. As used herein, the term "adhesive component" may refer to a component that, unlike the adhesive component, can provide permanent bonding rather than temporary bonding, and may refer to a composition that is typically applied for bonding in a liquid form, exhibits adhesive power upon solidification, cooling, or curing, and can cause physical destruction when the bonded objects are separated after bonding. That is, when the bonding layer includes an adhesive component, an adhesive layer can be implemented, and when the resin layer includes an adhesive component, an adhesive layer can be implemented.
[0142] In one embodiment, the bonding layer may include an acrylic resin, an epoxy resin, a silicone resin, a fluorine resin, a styrenic resin, a polyolefin resin, a thermoplastic elastomer, a polyoxyalkylene resin, a polyester resin, a polyvinyl chloride resin, a polycarbonate resin, a polyphenylene sulfide resin, a mixture of hydrocarbons, a polyamide resin, or a mixture thereof. In addition, the listed resins may include one or more functional groups or moieties that can be cured by heat, such as a glycidyl group, an isocyanate group, a hydroxyl group, a carboxyl group, or an amide group, so as to be cured and exhibit adhesive properties, or one or more functional groups or moieties that can be cured by irradiation with an active energy ray, such as an epoxide group, a cyclic ether group, a sulfide group, an acetal group, or a lactone group.
[0143] In one embodiment, the thickness of the bonding layer may be 5 μm to 50 μm. If the thickness of the bonding layer is too thick, the optical properties of the barrier film may be negatively affected, and if the thickness of the bonding layer is too thin, the adhesive strength between the laminates may be insufficient, which may reduce the reliability of the barrier film.
[0144] In one embodiment, the refractive index of the bonding layer may be less than the refractive index of the polymer substrate layer. If the refractive index of the bonding layer is greater than the refractive index of the polymer substrate layer, the optical properties of the barrier film may be degraded.
[0145] In one embodiment, the refractive index of the bonding layer may be greater than or equal to 1.45, and preferably may be from 1.47 to 1.50. The refractive index may refer to a refractive index for light having a wavelength ranging from 500 nm to 600 nm. In other examples, the wavelength at which the refractive index is measured may be from 520 nm to 580 nm, from 540 nm to 560 nm, or from 545 nm to 555 nm.
[0146] In one embodiment, the adhesion of the bonding layer may be greater than or equal to 2000 gf / 25 mm, and preferably greater than or equal to 2500 gf / 25 mm. The adhesion may be measured in accordance with ASTM D1876-08 "Standard Test Method for Peel Resistance of Adhesives (T-Peel Test)".
[0147]
[0148] Hereinafter, the contents for carrying out the present invention will be described in more detail through comparative examples and practical examples, but the examples are only examples, and the present invention is not limited thereto.
[0149] Comparative Example 1 (Laminate, Fig. 4)
[0150] A polyethylene terephthalate film (V5410) manufactured by SKC was prepared as a polymer substrate layer. The film had a thickness of 50 ㎛, a coefficient of thermal expansion of 70.65 ppm / ℃ in the range of 100°C to 130°C, a heat shrinkage in the MD direction of 0.4% and a heat shrinkage in the TD direction of 0.2% calculated by the above-described mathematical formula 1, and a refractive index of 1.65.
[0151]
[0152] To form a flattening layer and an organic-inorganic hybrid coating layer, a curable sol solution was prepared as follows.
[0153] First, 238.1 g of ethanol, 120.7 g of tetraethyl orthosilicate (TEOS), 3.2 g of 36 wt% hydrochloric acid, and 41.1 g of water were stirred at room temperature at 200 rpm for 1 hour. Then, 562.5 g of ethanol was added to form a primary mixture. Then, 0.55 g of hexahydrophthalic anhydride (HHPA) (Lonza Chemicals), 1.4 g of water, and 32 g of ethyl alcohol were stirred at room temperature at 250 rpm for 1 hour, added to the primary mixture, stirred at room temperature at approximately 200 rpm for 4 hours, and then filtered through a 0.2 μm filter to prepare a sol solution.
[0154] Approximately 31 g of a 30 wt% colloidal silica solution (Nissan Chemicals, catalog no. IPA-ST) based on isopropyl alcohol as a solvent was prepared by ultrasonication at room temperature for 60 minutes. Then, 52.7 g of ethoxylated trimethylolpropane triacrylate (Sartomer, catalog number SR-454), 59.8 g of bisphenol-A epoxy acrylate oligomer having a molecular weight of about 4,700 (Sartomer, catalog number CN120), 2.84 g of photoinitiator 1-hydroxy-cyclohexyl-phenyl-ketone (Ciba, catalog number Irgacure 184), and 1.17 g of photolatent base 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone (Ciba, catalog number 907) were mixed and stirred at about 200 rpm for 5 minutes. After this, 110 g of ethyl acetate and 305 g of 1-methoxy-2-2-propanol prepared above were added and stirred at 250 rpm for 30 minutes at room temperature. The mixture thus formed, the prepared silica solution, and 438 g of isopropanol were mixed again and stirred at 250 rpm for 1 hour at room temperature to prepare a curable coating solution.
[0155] The sol solution was added to the above curable coating solution while stirring at 200 rpm, stirred for 1 hour, and then filtered through a 1 μm filter to prepare a curable sol solution.
[0156]
[0157] The above curable sol solution was bar-coated on the polymer substrate layer, dried at 100°C for 30 seconds, and then UV-cured with an energy of 1,000 mJ / cm2 to form a planarization layer on the polymer substrate layer. At this time, the thickness of the planarization layer was 2 μm.
[0158]
[0159] To form an inorganic gas barrier layer on the above-mentioned flattening layer, a reactive sputtering method was used as follows.
[0160] A dual magnetron sputtering device using a mid-frequency (MF) power source was used, and power was applied to a silicon target with a purity of 99.999%. At this time, the power density was adjusted to 7.3 watts / cm2. At the same time, 200 sccm of argon (Ar) gas and 50 sccm of oxygen gas were injected, and plasma was formed under a pressure of 3 mtorr to perform sputtering, and a silicon oxide thin film was deposited while transporting the substrate film at a speed of 1 M / min.
[0161]
[0162] The curable sol solution was bar-coated on the inorganic gas barrier layer, dried at 100°C for 30 seconds, and then UV-cured with an energy of 1,000 mJ / cm2 to form an organic-inorganic hybrid coating layer. At this time, the thickness of the organic-inorganic hybrid coating layer was 2 μm.
[0163]
[0164] In this way, a laminate was manufactured in which a polymer substrate layer, a planarization layer, an inorganic gas barrier layer, and an organic-inorganic hybrid coating layer were sequentially laminated. The structure of the laminate according to Comparative Example 1 is as shown in Fig. 4.
[0165]
[0166] Example 1 (barrier film, Fig. 1)
[0167] Two laminates were prepared according to Comparative Example 1.
[0168] An acrylic OCA was prepared as a bonding layer. At this time, the thickness of the acrylic OCA was 25 ㎛ and the refractive index was 1.49.
[0169] Two laminates according to Comparative Example 1 were bonded using an acrylic OCA. At this time, the organic / inorganic hybrid coating layers of the two laminates according to Comparative Example 1 were both positioned on the acrylic OCA side. The structure of the barrier film according to Example 1 is as shown in Fig. 1.
[0170]
[0171] Example 2 (barrier film, Fig. 2)
[0172] Two laminates were prepared according to Comparative Example 1.
[0173] An acrylic OCA was prepared as a bonding layer. At this time, the thickness of the acrylic OCA was 25 ㎛ and the refractive index was 1.49.
[0174] Two laminates according to Comparative Example 1 were bonded using an acrylic OCA. At this time, one of the two laminates according to Comparative Example 1 had the polymer substrate layer positioned on the acrylic OCA side, and the other had the organic / inorganic hybrid coating layer positioned on the acrylic OCA side. The structure of the barrier film according to Example 2 is as shown in Fig. 2.
[0175]
[0176] Example 3 (barrier film, Fig. 3)
[0177] Two laminates were prepared according to Comparative Example 1.
[0178] An acrylic OCA was prepared as a bonding layer. At this time, the thickness of the acrylic OCA was 25 ㎛ and the refractive index was 1.49.
[0179] Two laminates according to Comparative Example 1 were bonded using an acrylic OCA. At this time, the polymer substrate layers of the two laminates according to Comparative Example 1 were both positioned on the acrylic OCA side. The structure of the barrier film according to Example 3 is as shown in Fig. 3.
[0180]
[0181] Experimental Example 1
[0182] The adhesive strength of the bonding layer of the barrier film according to Examples 1 to 3 was measured by ASTM D1876-08 "Standard Test Method for Peel Resistance of Adhesives (T-Peel Test)," and the results are shown in Table 1.
[0183]
[0184] Experimental Example 2
[0185] The light transmittance (550 nm), water vapor transmittance, and Haze of Comparative Example 1 and Examples 1 to 3 were measured by the following methods, and the results are shown in Table 1.
[0186] 1) Light transmittance (550 nm): Measured using Minolta's CM-3600d equipment according to ASTM D1003.
[0187] 2) Water vapor permeability: Measured using Mocon PERMATRAN-W3 / 31 equipment at 37.8 ℃ and RH 100% for 48 hours.
[0188] 3) Haze: Measured using Nippon Denshoku's NDH-5000 equipment according to ASTM D1003.
[0189]
[0190] Comparative Example 1 Example 1 Example 2 Example 3 Light transmittance (%) 91.38 8.18 9.15 91.65 Water vapor transmittance (g / m 2 / day)0.0050.0010.0010.001Haze(%)0.450.960.620.84Adhesion strength of bonding layer(gf / 25 mm)-250020002200
[0191] The above description is merely an illustrative description of the technical idea of the present invention, and those skilled in the art will appreciate that various modifications and variations can be made without departing from the essential characteristics of the present invention. The drawings disclosed in this specification are not intended to limit the technical idea of the present invention, but rather to illustrate it, and the scope of the technical idea of the present invention is not limited by these drawings. The scope of protection of the present invention should be interpreted by the claims, and all technical ideas within a scope equivalent thereto should be interpreted as being included in the scope of the rights of the present invention.
Claims
1. A barrier film in which a polymer substrate layer, a planarization layer, an inorganic gas barrier layer, and an organic-inorganic hybrid coating layer are sequentially laminated on both sides of a bonding layer.
2. In paragraph 1, The above bonding layer is a barrier film having a thickness of 5 ㎛ to 50 ㎛.
3. In paragraph 1, A barrier film having a refractive index of the above bonding layer lower than the refractive index of the above polymer substrate layer.
4. In paragraph 1, The above bonding layer is a barrier film having an adhesive strength of 2000 gf / 25 mm or more as measured according to ASTM D1876-08.
5. In paragraph 1, The above bonding layer is a barrier film comprising an acrylic resin, an epoxy resin, a silicone resin, a fluorine resin, a styrene resin, a polyolefin resin, a thermoplastic elastomer, a polyoxyalkylene resin, a polyester resin, a polyvinyl chloride resin, a polycarbonate resin, a polyphenylene sulfide resin, a mixture of hydrocarbons, a polyamide resin, or a mixture thereof.
6. In paragraph 1, A barrier film in which all laminates arranged on both sides of the bonding layer are arranged so that the organic / inorganic hybrid coating layer is located on the bonding layer side.
7. In paragraph 1, A barrier film in which a laminate disposed on one surface of a bonding layer is disposed such that a polymer substrate layer is positioned toward the bonding layer, and a laminate disposed on the other surface of the bonding layer is disposed such that an organic / inorganic hybrid coating layer is positioned toward the bonding layer.
8. In paragraph 1, A barrier film in which all laminates arranged on both sides of the bonding layer are arranged so that the polymer substrate layer is located on the bonding layer side.
9. In paragraph 1, The above polymer substrate layer comprises a thermoplastic transparent base resin, A barrier film comprising the thermoplastic transparent base resin, wherein the thermoplastic transparent base resin comprises at least one selected from the group consisting of polyethylene terephthalate, polyethersulfone, polycarbonate, polyimide, polyarylate, polyethylene naphthalate, polyethylene terephthalate glycol, polycyclohexylenedimethylene terephthalate glycol, and cycloolefin copolymer.
10. In paragraph 9, The above polymer substrate layer is a barrier film having a thermal expansion coefficient of 100 ppm / ℃ or less in the range of 100 ℃ or more and 130 ℃ or less.
11. In paragraph 9, The above polymer substrate layer is a barrier film having a heat shrinkage in the MD (Machine Direction) direction of 0.5% or less and a heat shrinkage in the TD (Transverse Direction) direction of 0.3% or less, and the heat shrinkage is calculated by the following mathematical formula 1. [Mathematical Formula 1] (Initial length of polymer substrate layer - length of polymer substrate layer after heat shrinkage treatment at 150℃ for 30 minutes / Initial length of polymer substrate layer) × 100 12. In paragraph 1, The above-mentioned flattening layer is a barrier film having the same composition as the above-mentioned organic-inorganic hybrid coating layer.
13. In paragraph 12, The above-mentioned planarization layer and the above-mentioned organic-inorganic hybrid coating layer are a barrier film including a curable coating solution including a (meth)acrylate monomer, a (meth)acrylate oligomer having an epoxy group and a weight average molecular weight of 500 to 10,000, an initiator, silica particles, and a dispersion medium, and a curable sol solution including a metal alkoxide, a curing accelerator, an inorganic acid, and a solvent, and a curable resultant of the curable sol solution.
14. In paragraph 1, The above inorganic gas barrier layer is a barrier film comprising an oxide, nitride, carbide, oxynitride, oxycarbide, nitride carbide, or oxynitride carbide containing at least one metal selected from the group consisting of Si, Al, In, Sn, Zn, Ti, Cu, Ce, and Ta.
Citation Information
Patent Citations
A plastic substrate having structure of multi-layerand method for preparing the same
KR100646252B1
A manufacturing method of plastic film for display substrate
KR1020130074624A
Full die and partial die tape outs from common design
KR1020230029541A
Hybrid tilt measuring apparatus
KR102490250B1
Barrier film or sheet and laminated packaging material comprising the film or sheet and packaging container made therefrom
WO2017072122A1