Strontium compound, method for producing same, and method for forming thin film using same
A novel strontium compound with a tetradentate aminoethenolate ligand structure addresses the limitations of existing materials by providing high thermal stability and volatility, enabling the production of high-quality, high-dielectric thin films for advanced DRAM devices.
Patent Information
- Application Number
- PCT/KR2024/005498
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-11
- Filing Date
- 2024-04-24
- Publication Date
- 2024-11-14
AI Technical Summary
Current materials used in DRAM capacitor manufacturing have limitations in achieving high dielectric constants and volatility, leading to challenges in reducing thin film thickness and increasing surface area, which are necessary for more integrated DRAM devices, and existing strontium precursors face issues like rapid growth, low volatility, and contamination risks.
A novel strontium compound with a tetradentate aminoethenolate ligand structure is developed, providing excellent thermal stability and volatility, suitable for use as a precursor for strontium-containing thin films, which can be deposited using chemical vapor deposition or atomic layer deposition to form high-quality, high-dielectric thin films.
The new strontium compound enables the production of high-density, high-purity thin films with excellent physical and electrical properties, improving deposition efficiency and equipment longevity by avoiding contamination and rapid growth issues.
Smart Images

Figure KR2024005498_14112024_PF_FP_ABST
Abstract
Description
Strontium compound, method for producing same, and method for forming thin film using same
[0001] The present invention relates to a novel strontium compound, a method for producing the same, and a method for forming a strontium-containing thin film using the same.
[0002] The capacitance of a capacitor in a DRAM (Dynamic Random Access Memory) device is proportional to the surface area of the capacitor and the dielectric constant, and inversely proportional to the thickness of the dielectric film. To produce more integrated DRAM devices in the future, the thickness of the dielectric film used must be reduced or the effective surface area of the capacitor must be increased. While the surface area has been increased by using a three-dimensional structure, further reduction in the dielectric film thickness is essential for achieving this. However, this is difficult to achieve with currently available materials. Therefore, the development of materials with a higher permittivity than commercially available materials is required.
[0003] Strontium titanium oxide (STO (SrTiO3)) is emerging as a high-k material that can be used for this purpose, and since the permittivity of STO is much higher than that of materials currently used in semiconductor processes, it is expected that it will be used in DRAM capacitors in the future.
[0004] In the case of strontium, due to its large ion size and low ionic valence (+2), it often forms compounds larger than dimers, which presents the problem of low volatility. In other words, it is very difficult to develop a strontium precursor that is both highly volatile and monomolecular.
[0005] Currently used Sr( iCyclopentadienyl (Cp) precursors such as Pr3Cp)2 have various problems such as rapid initial growth of thin films, and thus, development of new strontium precursors is necessary to solve these problems.
[0006] The existing precursor, Sr( i Unlike Pr3Cp)2, a new strontium precursor, [Sr(demamp)(tmhd)]2 precursor, which hardly experiences initial rapid growth, has been reported (KR 10-1399552, US 9790238, Chem. Mater. 2015, 27, 3881). However, this strontium precursor has the problem of low volatility as a dimer, which limits its use as a deposition precursor.
[0007] Meanwhile, a Sr(amak)2 precursor having a fluorinated amino alcohol ligand has been reported (J. Chem. Soc., Dalton Trans., 2001, 2462-2466). However, although the precursor Sr(amak)2 is a single molecule, it contains the halogen element F, which can cause contamination of the thin film and corrosion of the thin film and equipment during deposition. This can have negative effects such as lowering the quality of the deposited thin film and shortening the life of the deposition equipment. In addition, there are disadvantages such as a slow deposition rate and a low yield of the deposition precursor, which reduces the efficiency of the deposition process.
[0008] Therefore, there is a need for the development of a new structural strontium precursor that has a high dielectric constant and excellent vapor pressure and thermal stability to enable the production of high-quality thin films.
[0009] The present invention aims to provide a deposition precursor that overcomes the above-described problems, has excellent stability, improves the quality of a deposited thin film, and extends the life of equipment.
[0010] Accordingly, the present invention aims to provide a novel strontium compound having a high dielectric constant, thermal stability, and high volatility, which is useful as a precursor for thin film deposition.
[0011] In addition, the present invention aims to provide a method for producing the above strontium compound.
[0012] In addition, the present invention aims to provide a method for producing a high-quality strontium-containing thin film using the above strontium compound.
[0013] To achieve the above purpose, the present invention provides a strontium compound represented by the following chemical formula 1 as a novel strontium precursor.
[0014] [Chemical Formula 1]
[0015]
[0016] In the above chemical formula 1,
[0017] A and B are each independently C1-C10 alkoxy or diC1-C10 alkylamino;
[0018] R 1 is C1-C10 alkyl or diC1-C10 alkylamino;
[0019] L 1 and L 2 are each independently C1-C10 alkylene.
[0020] According to one embodiment, the L 1 and L 2 Each of them can independently be C2-C10 alkylene.
[0021] According to one embodiment, the strontium compound may be represented by the following chemical formula 2:
[0022] [Chemical Formula 2]
[0023]
[0024] In the above chemical formula 2, A, B and R 1 is the same as the definition in the above chemical formula 1;
[0025] n is an integer from 1 to 5.
[0026] In one embodiment, A and B are each independently C1-C4 alkoxy or diC1-C4 alkylamino; R 1 is C1-C4 alkyl; n can be an integer from 1 to 3.
[0027] In one embodiment, A and B are each independently C1-C4alkoxy and diC1-C4alkylamino; R 1 is diC1-C4alkylamino; n can be an integer from 1 to 3.
[0028] In one embodiment, the strontium compound may be selected from the following structures, but is not limited thereto.
[0029]
[0030]
[0031]
[0032]
[0033] In addition, the present invention provides a method for producing a strontium compound of the following chemical formula 1 by reacting a compound of the following chemical formula 3 with a compound of the following chemical formula 4.
[0034] [Chemical Formula 1]
[0035]
[0036] [Chemical Formula 3]
[0037]
[0038] [Chemical Formula 4]
[0039]
[0040] In the above chemical formulas 1, 3 and 4,
[0041] A and B are each independently C1-C10 alkoxy or diC1-C10 alkylamino;
[0042] R 1 is C1-C10 alkyl or diC1-C10 alkylamino;
[0043] L 1 and L 2 are each independently C1-C10 alkylene;
[0044] R a1 Inland R a3 , R' and R'' are each independently C1-C10 alkyl.
[0045] In addition, the present invention provides a method for manufacturing a strontium-containing thin film using the strontium compound of the above chemical formula 1. In this case, the manufacturing method may be performed by a chemical vapor deposition method or an atomic layer deposition method.
[0046] The strontium compound of the present invention has a novel structure comprising a ligand without steric hindrance to an alkoxycarbon, i.e., a tetradentate aminoethenolate ligand, and has excellent thermal stability and volatility, making it very useful as a precursor for a strontium-containing thin film and further enabling the production of a strontium-containing thin film of higher quality. In addition, the strontium compound according to the present invention exists as a solid at room temperature, thus providing good handleability. Furthermore, when the strontium compound according to the present invention is employed as a deposition precursor, it is possible to produce a high-k thin film having high density and purity and excellent physical and electrical properties.
[0047] With these characteristics, the strontium compound according to the present invention can be applied to various thin film deposition methods, has a high volatility, a fast and easy deposition speed, and has excellent cohesion and excellent step coverage, allowing a high-dielectric thin film to be formed with a uniform thickness on various types of substrates.
[0048] Figure 1 shows a TGA graph of Sr(ONO1)2 (Example 1).
[0049] Hereinafter, the present invention will be described in more detail. Unless otherwise defined, the technical and scientific terms used herein have the meanings commonly understood by those of ordinary skill in the art to which this invention pertains. In the following description, descriptions of well-known functions and configurations that may unnecessarily obscure the gist of the present invention will be omitted.
[0050] The term "alkyl" as used herein refers to a monovalent substituent, including both linear and branched forms.
[0051] Additionally, the term "includes" in this specification is an open-ended description having an equivalent meaning to expressions such as "comprises," "contains," "has," or "characterizes," and does not exclude additional elements, materials, or processes not listed.
[0052] In addition, the term "substantially identical" in this specification means that the compound before and after a specific treatment does not cause changes in the state and structure of the compound, i.e., the compound before and after a specific treatment can fall into the category of identity.
[0053] Additionally, the singular forms used herein may be intended to include the plural forms as well, unless the context specifically indicates otherwise.
[0054] In addition, units used in this specification without special mention are based on weight, and for example, units of % or ratio mean weight% or weight ratio.
[0055] In addition, the term "strontium compound" in this specification can be represented by chemical formula 1 and has an equivalent meaning to expressions such as "strontium precursor" or "strontium precursor compound".
[0056] The present invention provides a novel strontium precursor capable of producing a strontium-containing thin film, which is a strontium compound represented by the following chemical formula 1.
[0057] [Chemical Formula 1]
[0058]
[0059] In the above chemical formula 1,
[0060] A and B are each independently C1-C10 alkoxy or diC1-C10 alkylamino;
[0061] R 1 is C1-C10 alkyl or diC1-C10 alkylamino;
[0062] L 1 and L 2 are each independently C1-C10 alkylene.
[0063] The strontium compound of the present invention is a novel structural compound comprising a ligand without steric hindrance to the alkoxy carbon, i.e., a four-dentate aminoethenolate ligand, and can be usefully used as a precursor for producing a strontium-containing thin film. The strontium compound according to one embodiment may include all structural isomeric forms of the ligand, including the cis-trans form and the EZ form.
[0064] Furthermore, the strontium compound of the present invention has good thermal stability and excellent volatility, making it very useful as a precursor for a strontium-containing thin film and further enabling the production of a higher quality strontium-containing thin film.
[0065] In addition, the strontium compound of the present invention can be deposited using various deposition methods due to its good thermal stability, high volatility, and excellent reactivity, and it is possible to manufacture a high-density, high-purity strontium-containing thin film with a high deposition rate.
[0066] In one embodiment, in the chemical formula 1, preferably L 1 and L 2 Each of them can independently be C2-C10 alkylene.
[0067] In a preferred aspect for having improved properties as a thin film precursor, the strontium compound may be represented by the following chemical formula 2.
[0068] [Chemical Formula 2]
[0069]
[0070] In the above chemical formula 2, A, B and R 1 is the same as the definition in the above chemical formula 1;
[0071] n is an integer from 1 to 5.
[0072] In the chemical formula 2 according to one embodiment, A and B are each independently C1-C4 alkoxy or diC1-C4 alkylamino; R 1 is C1-C4 alkyl or diC1-C4 alkylamino; n can be an integer from 1 to 3.
[0073] In one embodiment, in the chemical formula 2, preferably, A is C1-C4 alkoxy or diC1-C4 alkylamino; B is diC1-C4 alkylamino; R 1 is C1 to C4 alkyl; n can be an integer from 1 to 3.
[0074] In the chemical formula 2 according to one embodiment, preferably, A and B are each independently C1-C4 alkoxy; R 1 is C1-C4 alkyl or diC1-C4 alkylamino; n can be an integer from 1 to 3.
[0075] According to one specific example, in the above chemical formula 2, A and B are each independently methoxy, ethoxy, n-propoxy, i-propoxy, n-butoxy, i-butyl, t-butoxy, dimethylamino or diethylamino; R 1 is methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, t-butyl, dimethylamino, diethylamino or ethylmethylamino; n can be an integer of 1 or 2.
[0076] More specifically, A is methoxy, ethoxy, dimethylamino or diethylamino; B is dimethylamino or diethylamino; R 1is methyl, ethyl, t-butyl, dimethylamino, diethylamino or ethylmethylamino; n can be an integer of 1 or 2.
[0077] More specifically, A and B are each independently methoxy or ethoxy; R 1 is methyl, ethyl, t-butyl, dimethylamino, diethylamino or ethylmethylamino; n can be an integer of 1 or 2.
[0078] According to one embodiment, the strontium compound may be selected from the following structures, but is not limited thereto.
[0079]
[0080]
[0081]
[0082]
[0083] In addition, the present invention provides a method for producing a strontium compound of the above chemical formula 1.
[0084] The strontium compound of the above chemical formula 1 can be prepared by reacting the compound of the following chemical formula 3 with the compound of the following chemical formula 4.
[0085] [Chemical Formula 3]
[0086]
[0087] [Chemical Formula 4]
[0088]
[0089] In the above chemical formulas 3 and 4, A, B, L 1 , L 2 and R 1 is the same as the definition in the above chemical formula 1;
[0090] R a1 Inland R a3 , R' and R'' are each independently C1-C10 alkyl.
[0091] In one embodiment, the reaction can be carried out at 20 to 30°C for 12 to 36 hours.
[0092] In the above reaction, for 1 mole of the compound of the chemical formula 3, 1.5 to 3 moles, preferably 1.8 to 2.2 moles, of the compound of the chemical formula 4 can be used.
[0093] According to one embodiment, the reaction can be carried out in an organic solvent, and the usable organic solvent is not limited, but an organic solvent having high solubility for the reactants can be used, and specifically, one or more mixed organic solvents selected from hexane, diethyl ether, toluene, tetrahydrofuran, etc. can be used.
[0094] In one embodiment, the reaction can be performed under an inert gas atmosphere such as nitrogen or argon.
[0095] In one specific example, the reaction can be carried out by reacting the compound of Chemical Formula 3 and the compound of Chemical Formula 4 in the presence of hexane, toluene, or a mixed organic solvent thereof at 20 to 30°C for 12 to 36 hours to obtain the strontium compound of Chemical Formula 1 in a good yield. At this time, after the reaction, if necessary, the purity can be maximized by purification through filtration, extraction, recrystallization, distillation, sublimation, chromatography, etc.
[0096] The strontium compound manufactured above is a stable solid at room temperature, is thermally stable and has good volatility, and thus can be used to manufacture a high-quality strontium-containing thin film.
[0097] In addition, the present invention provides a method for manufacturing a strontium-containing thin film using the strontium compound or a composition for deposition of a strontium-containing thin film containing the same.
[0098] According to one embodiment, the strontium-containing thin film deposition composition includes the strontium compound according to one embodiment, and the amount of the strontium compound used in the composition of the present invention may be included within a range that can be recognized by a person skilled in the art in consideration of the film formation conditions of the thin film or the thickness and characteristics of the thin film.
[0099] According to one embodiment, the method for manufacturing the strontium-containing thin film can provide the strontium-containing thin film on a substrate through a known deposition method. Specifically, the deposition method can be a solution process or vacuum deposition, and the vacuum deposition can specifically be chemical vapor deposition (CVD), plasma-enhanced chemical vapor deposition (PECVD), atomic layer deposition (ALD), low-pressure vapor deposition, plasma-enhanced atomic layer deposition, etc.
[0100] According to one embodiment, the manufacturing method may include a) a step of heating a substrate mounted in a chamber; b) a step of injecting a strontium compound according to one embodiment or a strontium-containing thin film deposition composition including the same into the chamber and adsorbing the strontium compound onto the substrate; and c) a step of injecting a reaction gas to produce a thin film on the substrate; and steps b) and c) may be repeated several times depending on the thickness of the strontium-containing thin film.
[0101] In a manufacturing method according to one embodiment, deposition conditions can be controlled according to the structure or thermal characteristics of the target thin film, and the deposition conditions may include, but are not limited to, the input flow rate of the strontium compound or the strontium-containing thin film deposition composition including the same, the input flow rate of the reaction gas, the input flow rate of the carrier gas, the pressure, the RF power, the substrate temperature, etc. of the strontium compound or the strontium-containing thin film deposition composition including the same, and the non-limiting examples of such deposition conditions include, but are not limited to, the input flow rate of the strontium-containing thin film formation composition being 10 to 1000 cc / min, the carrier gas being 10 to 1000 cc / min, the reaction gas being 1 to 1000 cc / min, the pressure being 0.5 to 10 torr, the RF power being 200 to 1000 W, and the substrate temperature being 80 to 400°C, preferably 200 to 400°C.
[0102] The above reaction gas is not limited, but one or more mixed gases selected from oxygen (O2), ozone (O3), water vapor (H2O), hydrogen peroxide (H2O2), nitrogen monoxide (NO), nitrous oxide (N2O), nitrogen dioxide (NO2), ammonia (NH3), nitrogen (N2), hydrazine (N2H4), amine, diamine, hydrogen (H2), argon (Ar), and helium (He) can be used, and the carrier gas is not limited as long as it is a common gas that does not react with the strontium compound of the present invention, and a non-limiting example thereof may be one or more mixed gases selected from nitrogen, helium, neon, argon, krypton, xenon, radon, etc.
[0103] The above substrate is not limited to a conventional substrate, and non-limiting examples thereof include a substrate including one or more semiconductor materials selected from Ru, TiN, Si, Ge, SiGe, GaP, GaAs, SiC, SiGeC, InAs, and InP, a rigid substrate such as a silicon on insulator (SOI) substrate, a quartz substrate, or a glass substrate for a display, or a flexible plastic substrate such as polyimide, polyethylene terephthalate (PET, PolyEthylene Terephthalate), polyethylene naphthalate (PEN, PolyEthylene Naphthalate), polymethyl methacrylate (PMMA, Poly Methyl MethAcrylate), polycarbonate (PC, PolyCarbonate), polyethersulfone (PES), and polyester.
[0104] According to one embodiment, the strontium-containing thin film manufactured according to the method for manufacturing the strontium-containing thin film is a high-dielectric thin film material having a high density and high permittivity. That is, according to the method for manufacturing the strontium-containing thin film according to the present invention, by using a strontium compound having a specific ligand introduced therein as a precursor, a high-quality thin film having excellent physical, electrical, and chemical properties, a high permittivity, and excellent vapor pressure and thermal stability can be manufactured.
[0105] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.
[0106] Hereinafter, the synthesis of the strontium compound according to the present invention was performed under an inert argon or nitrogen atmosphere using a glove box or a Schlenk line. 1The structure of the obtained strontium compound was analyzed by H NMR spectrum and elemental analysis.
[0107] [Example 1] Preparation of strontium compound Sr(ONO1)2
[0108]
[0109] Step 1: Synthesis of ONO1 (1-(bis(2-methoxyethyl)amino)-3,3-dimethylbutan-2-one) ligand
[0110] After equipping a stirrer and a thermometer, Bis(2-methoxyethyl)amine (20 g, 0.15 mol), 1-chloro-3,3-dimethylbutan-2-one (20.19 g, 0.15 mol), and Triethylamine (23.445 g, 0.18 mol) were added to a 450 mL pressure bottle. Then, the solution was stirred and reacted for one day while maintaining the solution temperature at 120 °C. After completion of the reaction, a saturated NaOH aqueous solution was added to the resulting solution, stirred for 30 minutes, and the organic layer was extracted with DCM (15 mL x 3). The combined organic fractions were dried over anhydrous MgSO4 and filtered. After concentrating the solvent under reduced pressure, distillation was performed at 60 to 90°C (750 mTorr) to obtain ONO1 (1-(bis(2-methoxyethyl)amino)-3,3-dimethylbutan-2-one) ligand as a pale yellow oil (31.2 g, 89.9% yield).
[0111] 1 H NMR (C6D6, 500 MHz): δ 3.68 (s, 2H, NCH2C), 3.38 (t, 4H, NCH2), 3.10 (s, 6H, OCH3), 2.96 (t, 4H, NCH2CH2OCH3), 0.98 (s, 9H, C(CH3)3)
[0112] Step 2: Synthesis of Sr(ONO1)2(strontium (Z)-1-(bis(2-methoxyethyl)amino)-3,3-dimethylbut-1-en-2-olate)
[0113] In a 250 mL round bottom flask equipped with a stirrer under an argon atmosphere, ONO1 ligand (4.16 g, 18 mmol) was slowly added to hexane (100 mL) containing Sr(btsa)2(DME)2 (5.89 g, 10 mmol). The mixture was stirred at room temperature for one day to allow the reaction to proceed. After completion of the reaction, the solvent was concentrated under reduced pressure and then sublimed at 70 °C (750 mTorr) to obtain Sr(ONO1)2 as a pale orange solid (3 g, 55.3% yield).
[0114] 1 H NMR (C6D6, 500 MHz): δ 3.86 (m, 4H, CH2), 3.70 (s, 2H, NCHC), 3.39 (s, 12H, OCH3), 2.98 (m. 4H, CH2), 2.67 (m, 4H, CH2), 1.96 (m, 4H, CH2), 1.49(s, 18H, C(CH3)3); Anal. Calc for C 24 H 48 N2O6Sr: C, 52.58; H, 8.82; N, 5.11%. Found: C, 52.70; H, 8.87; N, 4.75%.
[0115] [Example 2] Preparation of strontium compound Sr(ONO2)2
[0116]
[0117] Step 1: Synthesis of ONO2 (1-(bis(2-ethoxyethyl)amino)-3,3-dimethylbutan-2-one) ligand
[0118] After equipping a stirrer and a thermometer, Bis(2-ethoxyethyl)amine (5 g, 0.031 mol), 1-chloro-3,3-dimethylbutan-2-one (4.17 g, 0.031 mol), Triethylamine (8.08 g, 0.062 mol), and acetone 100 mL were added to a 500 mL round bottom flask. Then, the mixture was stirred and refluxed for 4 hours to react. After completion of the reaction, the resulting solution was concentrated under reduced pressure, and the organic layer was extracted with DCM (15 mL x 3). The combined organic fractions were dried over anhydrous MgSO4 and filtered. After concentrating the solvent under reduced pressure, distillation was performed at 55 to 65°C (750 mTorr) to obtain ONO2 (1-(bis(2-ethoxyethyl)amino)-3,3-dimethylbutan-2-one) ligand as a pale yellow oil (5.6 g, 69% yield).
[0119] 1 H NMR (C6D6, 500 MHz): δ 3.72 (s, 2H, NCH2C), 3.47 (t, 4H, NCH2), 3.29 (m, 4H, OCH2CH3), 2.98 (t, 4H, NCH2CH2OC), 1.09 (t, 6H, OCH2CH3), 1.00(s, 9H, C(CH3)3)
[0120] Step 2: Synthesis of Sr(ONO2)2(strontium (Z)-1-(bis(2-ethoxyethyl)amino)-3,3-dimethylbut-1-en-2-olate)
[0121] In a 100 mL round bottom flask equipped with a stirrer, under an argon atmosphere, ONO2 ligand (0.52 g, 2 mmol) was slowly added to hexane (30 mL) containing Sr(btsa)2(DME)2 (0.59 g, 1 mmol). The mixture was stirred at room temperature for one day to allow the reaction to proceed. After completion of the reaction, the solvent was concentrated under reduced pressure to obtain Sr(ONO2)2 as a pale orange solid (0.5 g, 83% yield).
[0122] 1 H NMR (C6D6, 500 MHz): δ 3.93 (m, 8H, CH2), 3.81 (m, 4H, CH2), 3.75 (s, 2H, NCHC), 3.02 (m, 4H, CH2), 2.71 (m. 4H, CH2), 2.07 (m, 4H, CH2), 1.49(s, 18H, C(CH3)3), 1.18(t, 12H, OCH2CH3).
[0123] [Example 3] Preparation of strontium compound Sr(ONO3)2
[0124]
[0125] Step 1: Synthesis of ONO3 (Bis(2-methoxyethyl)aminoacetone) ligand
[0126] After equipping a stirrer and a thermometer, Bis(2-methoxyethyl)amine (20 g, 0.15 mol), Chloroacetone (14 g, 0.15 mol), Triethylamine (39 g, 0.30 mol), and acetone 100 mL were added to a 500 mL round bottom flask. Then, the mixture was stirred and refluxed for 4 hours to react. After completion of the reaction, a saturated NaOH aqueous solution was added to the resulting solution, stirred for 30 minutes, and the organic layer was extracted with DCM (15 mL x 3). The combined organic fractions were dried over anhydrous MgSO4 and filtered. The solvent was concentrated under reduced pressure, and distilled at 60 to 65 °C (750 mTorr) to obtain ONO3 (Bis(2-methoxyethyl)aminoacetone) ligand as a pale yellow oil (31.2 g, 89.9% yield).
[0127] 1 H NMR (C6D6, 500 MHz): δ 3.26(t, 4H, CH2), 3.19(s, 2H, NCH2C), 3.05(s, 6H, OCH3), 2.71(t, 4H, CH2), 1.85(s, 3H, CCH3)
[0128] Step 2: Synthesis of Sr(ONO3)2(strontium (Z)-1-(bis(2-methoxyethyl)amino)-prop-1-en-2-olate)
[0129] In a 250 mL round bottom flask equipped with a stirrer under an argon atmosphere, ONO3 ligand (0.38 g, 2 mmol) was slowly added to toluene (100 mL) in which Sr(btsa)2(DME)2 (0.59 g, 1 mmol) was dissolved. The mixture was stirred at room temperature for one day to allow the reaction to proceed. After completion of the reaction, the solvent was concentrated under reduced pressure to obtain Sr(ONO3)2 as an orange solid (0.4 g, 87% yield).
[0130] 1H NMR (C6D6, 500 MHz): δ 3.85 (m, 2H), 3.41 (m, 2H), 3.39 (s, 2H), 2.10 (s, 3H)
[0131] [Example 4] Preparation of strontium compound Sr(ONN)2
[0132]
[0133] Step 1: Synthesis of N1-(2-methoxyethyl)-N2,N2-dimethylethane-1,2-diamine
[0134] After equipping a stirrer and a thermometer, 1-chloro-2-methoxyethane (6.1 g, 0.063 mol) was added to a 450 mL pressure bottle, and N1,N1-dimethylethane-1,2-diamine (19.4 g, 0.21 mol) was slowly added dropwise while maintaining the solution temperature at 0 ℃. Then, the reaction was carried out by stirring for one day while maintaining the solution temperature at 120 ℃. After completion of the reaction, the resulting solution was concentrated under reduced pressure, and the organic layer was extracted with DCM (15 mL x 3), and the combined organic fractions were dried over anhydrous MgSO4 and filtered. The solvent was concentrated under reduced pressure to obtain N1-(2-methoxyethyl)-N2,N2-dimethylethane-1,2-diamine as a colorless and transparent oil (4.3 g, 46.7% yield).
[0135] 1 H NMR (C6D6, 500 MHz): δ 4.28(s, 1H, NH), 3.36(t, 2H, CH2), 3.09(s, 3H, OCH3), 2.76(t, 2H, CH2), 2.65(t, 2H, CH2), 2.33(t, 2H, CH2), 2.05(s, 6H, N(CH3)2)
[0136] Step 2: Synthesis of ONN (1-((2-(dimethylamino)ethyl)(2-methoxyethyl)amino)-3,3-dimethylbutan-2-one) ligand
[0137] After equipping a stirrer and a thermometer, N1-(2-methoxyethyl)-N2,N2-dimethylethane-1,2-diamine (15.3 g, 0.11 mol), 1-chloro-3,3-dimethylbutan-2-one (14.1 g, 0.11 mol), Triethylamine (34.1 g, 0.26 mol), and THF (100 mL) were added to a 450 mL pressure bottle. Then, the mixture was stirred and reacted for one day while maintaining the solution temperature at 120 °C. After completion of the reaction, the resulting solution was concentrated under reduced pressure, and the organic layer was extracted with DCM (15 mL x 3). The combined organic fractions were dried over anhydrous MgSO4 and filtered. After concentrating the solvent under reduced pressure, distillation was performed at 70 to 105°C (750 mTorr) to obtain ONN (1-((2-(dimethylamino)ethyl)(2-methoxyethyl)amino)-3,3-dimethylbutan-2-one) ligand as a light yellow oil (10.6 g, 41.3% yield).
[0138] 1 H NMR (CDCl3, 500 MHz): δ 3.67(s, 2H, NCH2C), 3.40(t, 2H, CH2), 3.10(s, 3H, OCH3), 2.95(t, 2H, CH2), 2.91(t, 2H, CH2), 2.39(t, 2H, CH2), 2.10(s, 6H, N(CH3)2), 0.99(s, 9H, C(CH3)3)
[0139] Step 3: Synthesis of Sr(ONN)2(strontium (Z)-1-((2-(dimethylamino)ethyl)(2-methoxyethyl)amino)-3,3-dimethylbut-1-en-2-olate)
[0140] In a 100 mL round bottom flask equipped with a stirrer under an argon atmosphere, ONN ligand (0.44 g, 1.8 mmol) was slowly added to hexane (30 mL) containing Sr(btsa)2(DME)2 (0.59 g, 1 mmol). The mixture was stirred at room temperature for one day to allow the reaction to proceed. After completion of the reaction, the solvent was concentrated under reduced pressure to obtain Sr(ONN)2 as a pale orange solid (0.48 g, 92.3% yield).
[0141] 1 H NMR (C6D6, 500 MHz): δ 4.22 (s, 2H, NCHC), 3.25 (s, 6H, OCH3), 2.73 (m, 4H, CH2), 2.43 (s, 12H, N(CH3)2), 1.76 (m, 4H, CH2), 1.56 (m, 4H, CH2), 1.44(s, 18H, C(CH3)3)
[0142] [Example 5] Preparation of strontium compound Sr(NNN)2
[0143]
[0144] Step 1: Synthesis of Bis-(2-(dimethylamino)ethyl)amine
[0145] After equipping a stirrer and a thermometer, bis-(2-chloroethyl)amine hydrochloride (20 g, 0.11 mol) was added to a 450 mL pressure bottle, and dimethylamine (75.8 g, 1.7 mol) was slowly added dropwise while maintaining the solution temperature at 0 ℃. Then, the reaction was carried out by stirring for one day while maintaining the solution temperature at 120 ℃. After completion of the reaction, a saturated NaOH aqueous solution was added to the resulting solution, and after stirring for 30 minutes, the organic layer was extracted with DCM (15 mL x 3), and the combined organic fractions were dried over anhydrous MgSO4 and filtered. After concentrating the solvent under reduced pressure, Bis-(2-(dimethylamino)ethyl)amine was obtained as a colorless and transparent oil (4.8 g, 26.9% yield).
[0146] 1 H NMR (C6D6, 500 MHz): δ 5.29(s, 1H, NH), 2.70(t, 4H, NCH2CH2N(CH3)2), 2.40(t, 4H, CH2N(CH3)2), 2.21(s, 12H, N(CH3)2)
[0147] Step 2: Synthesis of NNN (1-(bis(2-(dimethylamino)ethyl)amino)-3,3-dimethylbutan-2-one) ligand
[0148] After equipping a stirrer and a thermometer, Bis-(2-(dimethylamino)ethyl)amine (4.8 g, 0.030 mol), 1-chloro-3,3-dimethylbutan-2-one (4.056 g, 0.030 mol), Triethylamine (3.64 g, 0.036 mol) and THF (100 mL) were added to a 450 mL pressure bottle. Then, the mixture was stirred and refluxed for 4 hours to react. After completion of the reaction, the resulting solution was concentrated under reduced pressure, and the organic layer was extracted with DCM (15 mL x 3). The combined organic fractions were dried over anhydrous MgSO4 and filtered. After concentrating the solvent under reduced pressure, distillation was performed at 75 to 90°C (750 mTorr) to obtain NNN (1-(bis(2-(dimethylamino)ethyl)amino)-3,3-dimethylbutan-2-one) ligand as a pale yellow oil (1.0 g, 12.9% yield).
[0149] 1 H NMR (C6D6, 500 MHz): δ 3.70(s, 2H, NCH2C), 2.90(t, 4H, NCH2CH2N(CH3)2), 2.40(t, 4H, CH2N(CH3)2), 2.10(s, 12H, N(CH3)2), 1.00(s, 9H, C(CH3)3)
[0150] Step 3: Synthesis of Sr(NNN)2(strontium (Z)-1-(bis(2-(dimethylamino)ethyl)amino)-3,3-dimethylbut-1-en-2-olate)
[0151] In a 100 mL round bottom flask equipped with a stirrer under an argon atmosphere, NNN ligand (0.46 g, 1.8 mmol) was slowly added to hexane (30 mL) containing Sr(btsa)2(DME)2 (0.59 g, 1 mmol). The mixture was stirred at room temperature for one day to allow the reaction to proceed. After completion of the reaction, the solvent was concentrated under reduced pressure to obtain Sr(NNN)2 as a pale orange solid (0.5 g, 92.6% yield).
[0152] 1 H NMR (C6D6, 500 MHz): δ 4.13 (s, 2H, NCHC), 2.25 (s, 12H, N(CH3)2), 1.44 (s, 18H, C(CH3)3)
[0153] [Example 6] Preparation of strontium compound Sr(NNN2)2
[0154]
[0155] Step 1: Synthesis of NNN2 (1-(bis(3-(dimethylamino)propyl)amino)-3,3-dimethylbutan-2-one) ligand
[0156] After equipping a stirrer and a thermometer, N1-(3-(dimethylamino)propyl)-N3,N3-dimethylpropane-1,3-diamine (6.9 g, 0.037 mol), 1-chloro-3,3-dimethylbutan-2-one (5 g, 0.037 mol), Triethylamine (4.5 g, 0.044 mol) and THF (100 mL) were added to a 500 mL 450 mL pressure bottle. Then, the solution was stirred and reacted for one day while maintaining the solution temperature at 120 °C. After completion of the reaction, a saturated NaOH aqueous solution was added to the resulting solution, stirred for 30 minutes, and the organic layer was extracted with DCM (15 mL x 3). The combined organic fractions were dried over anhydrous MgSO4 and filtered. After concentrating the solvent under reduced pressure, distillation was performed at 85 to 130°C (750 mTorr) to obtain NNN2 (1-(bis(3-(dimethylamino)propyl)amino)-3,3-dimethylbutan-2-one) ligand as a pale yellow oil (21.2 g, 75% yield).
[0157] 1 H NMR (C6D6, 500 MHz): δ 3.41(s, 2H, NCH2C), 2.72(t, 4H, CH2), 2.30(t, 4H, CH2) 2.11(s, 12H, N(CH3)2), 1.65(t, 4H, CH2), 0.99(s, 9H, C(CH3)3)
[0158] Step 2: Synthesis of Sr(NNN2)2(strontium (Z)-1-(bis(3-(dimethylamino)propyl)amino)-3,3-dimethylbut-1-en-2-olate)
[0159] In a 100 mL round bottom flask equipped with a stirrer under an argon atmosphere, NNN2 ligand (0.57 g, 2 mmol) was slowly added to hexane (30 mL) containing Sr(btsa)2(DME)2 (0.59 g, 1 mmol). The mixture was stirred at room temperature for one day to allow the reaction to proceed. After completion of the reaction, the solvent was concentrated under reduced pressure to obtain Sr(NNN2)2 as an orange solid (0.6 g, 91% yield).
[0160] 1 H NMR (C6D6, 500 MHz): δ 4.25(s, 1H), 2.25(m, 16H), 2.16(s, 4H), 2.10(s, 12H), 1.30(s, 9H)
[0161] [Example 7] Preparation of strontium compound Sr(ONO4)2
[0162]
[0163] Step 1: Synthesis of ONO4 (2-(bis(2-methoxyethyl)amino)-N,N-dimethylacetamide) ligand
[0164] After equipping a stirrer and a thermometer, Bis(2-methoxyethyl)amine (11 g, 0.082 mol), 2-Chloro-N,N-dimethylacetamide (10 g, 0.082 mol), Triethylamine (12.9 g, 0.099 mol), and acetone 100 mL were added to a 450 mL pressure bottle. The mixture was stirred and reacted for one day while maintaining the solution temperature at 120 °C. After completion of the reaction, the resulting solution was concentrated under reduced pressure, and the organic layer was extracted with DCM (15 mL x 3). The combined organic fractions were dried over anhydrous MgSO4 and filtered. After concentrating the solvent under reduced pressure, distillation was performed at 50 to 70°C (750 mTorr) to obtain ONO4 (2-(bis(2-methoxyethyl)amino)-N,N-dimethylacetamide) ligand as a pale yellow oil (14.5 g, 81% yield).
[0165] 1 H NMR (CDCl3, 500 MHz): δ 3.37(s, 2H, NCH2C), 3.36(t, 4H, CH2), 3.09(s, 6H, OCH3), 2.91(t, 4H, CH2), 2.67(s, 3H, NCH3), 2.52(s, 3H, NCH3)
[0166] Step 2: Synthesis of Sr(ONO4)2(strontium (Z)-2-(bis(2-methoxyethyl)amino)-1-(dimethylamino)ethen-1-olate)
[0167] In a 100 mL round bottom flask equipped with a stirrer under an argon atmosphere, ONO4 ligand (2.51 g, 11.5 mmol) was slowly added to hexane (30 mL) containing Sr(btsa)2(DME)2 (3.38 g, 5.7 mmol). The mixture was stirred at room temperature for one day to allow the reaction to proceed. After completion of the reaction, the solvent was concentrated under reduced pressure to obtain Sr(ONO4)2 as a pale orange solid (2.8 g, 93.3% yield).
[0168] 1 H NMR (C6D6, 500 MHz): δ 4.06(m, 4H, CH2), 3.38(s, 12H, OCH3), 3.22(s, 2H, NCHC), 2.97(s, 12H, N(CH3)2), 2.97(m, 4H, CH2), 2.73(m, 4H, CH2), 2.12(m, 4H, CH2)
[0169] Experimental Example 1: Material Analysis of Strontium Compounds
[0170] In order to determine the thermal stability, volatility, and decomposition temperature of the strontium compound, Sr(ONO1)2, synthesized in Example 1, thermogravimetric analysis (TGA) was used. TGA analysis was performed by heating Sr(ONO1)2 (Example 1) to 600°C at a rate of 10°C / min in an argon atmosphere, while injecting argon gas at a pressure of 1.5 bar / min.
[0171] As shown in Fig. 1, the strontium compound of Example 1, Sr(ONO1)2, exhibited a rapid mass loss in the range of 95 to 295°C, showing a total mass loss of 94%.
[0172] From the above TGA analysis, it was confirmed that the strontium compound of the present invention has excellent thermal stability.
[0173] While the embodiments of the present invention have been described in detail above, those skilled in the art will appreciate that various modifications and variations can be made to the present invention without departing from the spirit and scope of the invention as defined in the appended claims. Therefore, modifications to future embodiments of the present invention will not depart from the scope of the invention.
Claims
1. A strontium compound represented by the following chemical formula 1: [Chemical Formula 1] In the above chemical formula 1, A and B are each independently C1-C10 alkoxy or diC1-C10 alkylamino; R 1 is C1-C10 alkyl or diC1-C10 alkylamino; L 1 and L 2 are each independently C1-C10 alkylene.
2. In paragraph 1, Above L 1 and L 2 A strontium compound, each independently a C2-C10 alkylene.
3. In paragraph 1, The above strontium compound is a strontium compound represented by the following chemical formula 2: [Chemical Formula 2] In the above chemical formula 2, A, B and R 1 is the same as the definition in claim 1; n is an integer from 1 to 5.
4. In paragraph 3, The above A and B are each independently C1-C4 alkoxy or diC1-C4 alkylamino; R 1 A strontium compound, wherein is C1-C4 alkyl; and n is an integer from 1 to 3.
5. In paragraph 3, The above A and B are each independently C1-C4 alkoxy and diC1-C4 alkylamino; R 1 A strontium compound wherein is diC1-C4 alkylamino; and n is an integer from 1 to 3.
6. In paragraph 1, The above strontium compound is selected from the following structures:
7. A method for producing a strontium compound of the following chemical formula 1 by reacting a compound of the following chemical formula 3 with a compound of the following chemical formula 4. [Chemical Formula 1] [Chemical Formula 3] [Chemical Formula 4] In the above chemical formulas 1, 3 and 4, A and B are each independently C1-C10 alkoxy or diC1-C10 alkylamino; R 1 is C1-C10 alkyl or diC1-C10 alkylamino; L 1 and L 2 are each independently C1-C10 alkylene; R a1 Inland R a3 , R' and R'' are each independently C1-C10 alkyl.
8. A method for producing a strontium-containing thin film using a strontium compound according to any one of claims 1 to 6.
9. In paragraph 8, A method for manufacturing a strontium-containing thin film, the method being performed by chemical vapor deposition or atomic layer deposition.
Citation Information
Patent Citations
Barium or strontium-based complex