Dielectric composition with high-temperature stability
The dielectric composition, combining barium titanate with specific oxides and carbonates, addresses the challenge of temperature stability and capacitance retention in multilayer ceramic capacitors, achieving a high dielectric constant and low loss coefficient to meet the X7R standard, ensuring reliable performance in automotive applications.
Patent Information
- Application Number
- PCT/KR2024/006306
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-05-10
- Publication Date
- 2024-11-14
AI Technical Summary
Multilayer ceramic capacitors used in automotive applications face challenges in maintaining capacitance stability at high temperatures, as existing compositions with COG characteristics have low dielectric constants and are inadequate for high-capacity requirements, while compositions with excessive rare earth materials have improved dielectric constants but struggle to meet X7R standards for temperature stability.
A dielectric composition based on a barium titanate (BaTiO3) main component, supplemented with specific oxides and carbonates of Yb, Sc, Lu, Zr, Mg, V, Mn, Cr, Fe, Ni, Co, Cu, Zn, and Si, which provides a high dielectric constant, low loss coefficient, and excellent electrostrictive properties, meeting the X7R standard by optimizing the content of these components to ensure stability and capacitance retention across a wide temperature range.
The composition achieves a high dielectric constant, low loss coefficient, and excellent temperature stability, satisfying the X7R standard, thereby ensuring reliable performance of multilayer ceramic capacitors in automotive applications by maintaining capacitance within ±15% from -55°C to 125°C.
Smart Images

Figure KR2024006306_14112024_PF_FP_ABST
Abstract
Description
Dielectric composition with high temperature stability
[0001] The present invention relates to a ceramic composition having high temperature stability, and more particularly, to a dielectric composition satisfying X7R characteristics.
[0002] Multilayer ceramic chip capacitors have high capacity and high reliability, but are relatively small in size, so they are widely used in fields such as automobiles and motors that require precision and stability.
[0003] There are various requirements for multilayer ceramic capacitors, such as capacity, temperature stability, and voltage stability. In particular, multilayer ceramic capacitors for automotive electronics must not change their capacity (capacitance) even at high temperatures because they operate at high temperatures. In this regard, the Electronic Industries Association (EIA) of the United States stipulates that a multilayer ceramic capacitor satisfies the X7R characteristic when the change in capacitance at temperatures between -55 and 125 degrees Celsius is within ±15% of the reference capacitance at 25 degrees Celsius.
[0004] The present invention provides a dielectric composition that satisfies the X7R standard.
[0005] According to embodiments of the present invention, a dielectric composition includes a barium titanate-based base material main component and a secondary component, wherein the secondary component comprises a first secondary component including at least one selected from the group consisting of oxides and carbonates of at least one element selected from Yb, Sc, Lu, and Tm, a second secondary component including at least one selected from the group consisting of oxides and carbonates of at least one element selected from Dy, Y, Ho, Tb, Gd, Eu, and Er, a third secondary component including at least one selected from the group consisting of oxides of Ba and Zr, a fourth secondary component including at least one selected from the group consisting of oxides and carbonates of a valence-fixed acceptor element including Mg, a fifth secondary component including at least one selected from the group consisting of oxides and carbonates of a valence-variable acceptor element including at least one selected from the group consisting of V, Mn, Cr, Fe, Ni, Co, Cu, and Zn, and a sixth secondary component including at least one selected from the group consisting of oxides, carbonates, and glasses of Si. It comprises at least one subcomponent, and at least one subcomponent comprises a first subcomponent, a second subcomponent and a third subcomponent, the content of one or more elements included in the first subcomponent is 0.2 to 6 molar parts with respect to 100 molar parts of the parent material main component, the content of one or more elements included in the second subcomponent is 0.2 to 6 molar parts with respect to 100 molar parts of the parent material main component, and the content of the third subcomponent is 4 to 6 molar parts with respect to 100 molar parts of the parent material main component.
[0006] The dielectric composition of the present invention satisfies the X7R characteristics of the EIA standard.
[0007] FIG. 1 is a perspective view showing a laminated ceramic capacitor according to an embodiment of the present invention.
[0008] FIG. 2 is a perspective view showing a plurality of electrode units of a laminated ceramic capacitor according to an embodiment of the present invention.
[0009] Hereinafter, in order to explain the technical idea of the present invention in detail to an extent that a person of ordinary skill in the art to which the present invention pertains can easily put it into practice, the most preferred embodiment of the present invention will be described with reference to the accompanying drawings. First, when adding reference numerals to components in each drawing, it should be noted that the same components are given the same numerals as much as possible even if they are shown in different drawings. In addition, when describing the present invention, if it is determined that a specific description of a related well-known structure or function may obscure the gist of the present invention, the detailed description thereof will be omitted.
[0010] The present invention relates to a dielectric composition, and electronic components including the dielectric composition include capacitors, inductors, piezoelectric elements, varistors, thermistors, etc., and below, a multilayer ceramic capacitor (MLCC) will be described as an example of the dielectric composition and electronic components.
[0011] Multilayer ceramic capacitors
[0012] FIG. 1 is a perspective view showing a multilayer ceramic capacitor according to an embodiment of the present invention, and FIG. 2 is a perspective view showing a plurality of electrode units of a multilayer ceramic capacitor according to an embodiment of the present invention.
[0013] Referring to FIG. 1, a multilayer ceramic capacitor according to an embodiment of the present invention is configured to include a dielectric (100), a first external electrode (220), and a second external electrode (240).
[0014] The dielectric (100) is composed of a rectangular parallelepiped having a top surface, a bottom surface, a first side surface, a second side surface opposite the first side surface, a third side surface, and a fourth side surface opposite the third side surface. As an example, the first side surface is the left side in the drawing, the second side surface is the right side in the drawing, the third side surface is the front side in the drawing, and the fourth side surface is the back side in the drawing.
[0015] The dielectric (100) may include a plurality of dielectric sheets. The plurality of dielectric sheets may be laminated. Each dielectric sheet may include a dielectric composition and may be formed by sintering the dielectric composition.
[0016] The first external electrode (220) is an electrode disposed on the first side of the dielectric (100). The first external electrode (220) may be formed to extend from the first side of the dielectric (100) to the upper surface, lower surface, third side, and fourth side of the dielectric (100). The second external electrode (240) is an electrode disposed on the second side of the dielectric (100). The second external electrode (240) may be formed to extend from the second side of the dielectric (100) to the upper surface, lower surface, third side, and fourth side of the dielectric (100). The first external electrode (220) and the second external electrode (240) may be formed to face each other at a predetermined distance from each other on the upper surface, lower surface, third side, and fourth side of the dielectric (100).
[0017] Referring to FIG. 2, a laminated ceramic capacitor according to an embodiment of the present invention may further include a plurality of electrode units (300). At this time, the plurality of electrode units (300) are laminated to form a laminate, and this laminate is disposed inside a dielectric (100).
[0018] A plurality of electrode units (300) are stacked vertically in the drawing and placed inside the dielectric (100). Each electrode unit (300) includes a first electrode set (320) and a second electrode set (340), and the first electrode set (320) and the second electrode set (340) are alternately stacked.
[0019] The first electrode set (320) is composed of a plate-shaped conductor formed in a rectangular shape. The first electrode set (320) is arranged inside the dielectric (100) so as to be offset from the first side of the dielectric (100). The first end of the first electrode set (320) is connected to the first external electrode (220) at the first side of the dielectric (100).
[0020] The second electrode set (340) is composed of a plate-shaped conductor formed in a rectangular shape. The second electrode set (340) is arranged inside the dielectric (100) so as to be offset from the second side of the dielectric (100). The first end of the second electrode set (340) is connected to the second external electrode (240) at the second side of the dielectric (100).
[0021] The first electrode set (320) and the second electrode set (340) are respectively distributed and arranged on two adjacent dielectric sheets among the dielectric sheets included in the dielectric (100). The first electrode set (320) and the second electrode set (340) may partially overlap with the dielectric sheets interposed therebetween.
[0022] Dielectric composition and method for producing the same
[0023] Hereinafter, a dielectric composition and a manufacturing method thereof according to embodiments of the present invention will be described in detail. The dielectric composition can form the above-described dielectric (100). However, to avoid redundant description, any content that overlaps with the above-described content will be omitted.
[0024] The dielectric composition according to embodiments of the present invention may include a parent material main component including a rare earth element. The parent material main component may be a barium titanate compound including Ba and Ti, and preferably, BaTiO3. In addition, the dielectric composition according to embodiments of the present invention may additionally include an auxiliary component, and the auxiliary component may include the first to sixth auxiliary components.
[0025] The dielectric composition according to embodiments of the present invention may include the auxiliary components of Table 1 per 100 moles of the base material BaTiO3.
[0026] First component, second component, third component, fourth component, fifth component, sixth component, Yb2O3Dy2O3Y2O3BaZrO3MgCO3V2O5MnO2Cr2O3Ba 0.6 Ca 0.4 SiO30.1-3.000.1-3.000-3.004.00-6.000.1-3.000.03-2.000.03-2.000.03-2.000.1-5.00
[0027] The dielectric material of multilayer ceramic capacitors for AC circuits is mainly composed of a composition with C0G characteristics. The composition with COG characteristics uses (CaSr)(TiZr)O3, a low-k material, as its main raw material. This composition with C0G characteristics has excellent electrostriction characteristics as a paraelectric, a loss factor (DF) of 0.004, a sintering temperature of 1260℃, and very little change in capacity depending on temperature. However, it is difficult to implement capacity because the permittivity is low at about 30. Therefore, when higher capacity is required, a composition with a lower Curie temperature by adding BaZrO3 and rare earth materials (such as Gd2O3) in excess to BaTiO3 is used, and such a composition has a cubic structure at room temperature.
[0028] In this way, the composition in which BaZrO3 and rare earth materials (such as Gd2O3) are excessively added to BaTiO3 has a dielectric constant of 800, a loss factor (DF) of 0.02, and a sintering temperature of 1200°C. Compared to the existing C0G characteristic composition, the composition has a relatively high dielectric constant and excellent electrostriction characteristics, but compared to the general X7R characteristic composition, the dielectric constant is significantly lower, making it difficult to implement a high capacity likewise.
[0029] To solve this problem, the dielectric composition according to embodiments of the present invention is characterized in that it satisfies the X7R standard that must change within the range of 15% to -15% by adding the first to third auxiliary components described below to BaTiO3, and has a high permittivity and a low loss factor of less than 0.01 compared to the existing C0G characteristic composition and the composition in which BaZrO3 and a rare earth material (Gd2O3, etc.) are excessively added to BaTiO3, thereby providing a dielectric composition suitable for an AC circuit. The dielectric composition according to embodiments of the present invention has a relatively high permittivity, which is advantageous for implementing capacity, and has excellent electrostriction characteristics and a low loss factor compared to the existing composition having X7R characteristics, making it suitable for an AC circuit.
[0030]
[0031] Hereinafter, each component of the dielectric composition according to embodiments of the present invention will be described in more detail.
[0032] Main ingredient of the parent material
[0033] The dielectric composition according to embodiments of the present invention may include a base material component including Ba and Ti. According to embodiments, the base material component is BaTiO3.
[0034] The above-mentioned parent material main component may be included in a dielectric composition in powder form. The average particle diameter of the parent material main component powder is not particularly limited, but may be 1000 nm or less. Preferably, the average particle diameter of the parent material main component powder may be 200 nm to 350 nm, and more preferably, 250 nm.
[0035] First component
[0036] The dielectric composition according to embodiments of the present invention may include, as a first auxiliary component, at least one selected from the group consisting of oxides and carbonates of at least one element selected from Yb, Sc, Lu, and Tm. The first auxiliary component is preferably at least one selected from the group consisting of oxides and carbonates of the Yb element, but is not limited thereto. Alternatively, the first auxiliary component may include at least one selected from the group consisting of oxides and carbonates of at least one element selected from Sc, Lu, and Tm, which are other rare earth elements, instead of the Yb element.
[0037] The first auxiliary component may be included in an amount of 0.2 to 6 mol parts per 100 mol parts of the parent material main component. The content of the first auxiliary component may be based on the content of one or more elements included in the first auxiliary component, regardless of the addition form such as oxide or carbonate. For example, the total content of the elements included in the first auxiliary component may be 0.2 to 6 mol parts per 100 mol parts of the parent material main component. For example, when the first auxiliary component is Yb2O3, assuming that 2 mol parts of Yb2O3 exist per 100 mol parts of BaTiO3, 4 mol parts of Yb, a metal included in the first auxiliary component, exist. Therefore, in this case, 4 mol parts of Yb are included per 100 mol parts of BaTiO3.
[0038] The first subcomponent may have the effect of shifting the Curie temperature toward a higher temperature and improving the stability of capacitance according to temperature changes. In other words, the first subcomponent serves to prevent a decrease in the reliability of a multilayer ceramic capacitor formed using a dielectric composition according to embodiments of the present invention.
[0039] If the content of the Yb element included in the first auxiliary component is less than 0.2 mol parts with respect to 100 mol parts of the main component of the parent material, the effect of improving the temperature coefficient of capacitance (TCC) in the high temperature section may not be significantly exhibited, and if the content of the Yb element included in the first auxiliary component exceeds 6 mol parts with respect to 100 mol parts of the main component of the parent material, the characteristics related to sintering may be deteriorated.
[0040] Second component
[0041] The dielectric composition according to embodiments of the present invention may include at least one selected from the group consisting of oxides and carbonates of at least one element among Dy, Y, Ho, Tb, Gd, Eu, and Er as a second auxiliary component. The second auxiliary component may be Dy2O3 and It may be at least one selected from the group consisting of Y2O3, wherein the total content of Dy2O3 and Y2O3 may be from 0.2 to 6 molar parts. Alternatively, the second auxiliary component may include at least one selected from the group consisting of oxides and carbonates of at least one element selected from among Ho, Tb, Gd, Eu, and Er, which are other rare earth elements, instead of Dy and Y.
[0042] The second auxiliary component may be contained in an amount of 0.2 to 6 molar parts based on 100 molar parts of the parent material main component. The content of the second auxiliary component may be based on the content of one or more elements contained in the second auxiliary component, regardless of the addition form such as oxide or carbonate. For example, the total content of elements contained in the second auxiliary component may be 0.2 to 6 molar parts based on 100 molar parts of the parent material main component. For example, the second auxiliary component may be Dy2O3 and When Y2O3 is included, assuming that Dy2O3 is present in 1 molar part and Y2O3 is present in 0.5 molar part for 100 molar parts of BaTiO3, Dy, a metal included in the second auxiliary component, is present in 2 molar parts and Y is present in 1 molar part. Therefore, in this case, the total content of elements included in the second auxiliary component is 3 molar parts for 100 molar parts of BaTiO3.
[0043] The second auxiliary component can help improve the high-temperature TCC and prevent the deterioration of the reliability of the multilayer ceramic capacitor formed from the dielectric composition. If the content of the element contained in the second auxiliary component is less than 0.2 mol parts or more than 6 mol parts per 100 mol parts of the main component of the parent material, this effect may be insufficient.
[0044] Third component
[0045] The dielectric composition according to embodiments of the present invention may include at least one selected from the group consisting of oxides containing Ba and Zr as a third auxiliary component. The third auxiliary component is preferably BaZrO3 or a mixture of BaO and ZrO2, but is not limited thereto. In the case of BaZrO3, the ratio of Ba and Zr is not particularly limited, and the molar ratio of Ba to Zr (Ba / Zr) may be 0.5 to 1.5, and preferably, 0.9 to 1.1.
[0046] When a third auxiliary component is added, the overall permittivity may decrease, and the permittivity change according to temperature may become flat. The third auxiliary component may be included in an amount of 4 to 6 parts by mole per 100 parts by mole of the main component of the base material. If the content of the third auxiliary component is less than 4 parts by mole per 100 parts by mole of the main component of the base material, the high-temperature TCC improvement effect may not be significantly exhibited, and if the content of the second auxiliary component exceeds 6 parts by mole per 100 parts by mole of the main component of the base material, the high-temperature withstand voltage characteristics may deteriorate.
[0047] 4th subsidiary component
[0048] The dielectric composition according to embodiments of the present invention may include at least one of an oxide and a carbonate of a fixed-valence acceptor element including Mg as a fourth component.
[0049] The fourth auxiliary component may be included in an amount of 0.1 to 3 molar parts or less with respect to 100 molar parts of the main component of the parent material. The content of the fourth auxiliary component may be based on the content of the Mg element included in the fourth auxiliary component, regardless of the addition form such as oxide or carbonate. For example, the content of the Mg element included in the fourth auxiliary component may be 0.1 to 3 molar parts or less with respect to 100 molar parts of the main component of the parent material.
[0050] If the content of the fourth component is less than 0.1 mol parts or more than 3 mol parts with respect to 100 mol parts of the main component of the dielectric base material, the dielectric constant may decrease and the high-temperature withstand voltage characteristics may decrease, which is not desirable.
[0051] 5th subsidiary component
[0052] The dielectric composition according to embodiments of the present invention may include at least one selected from the group consisting of oxides and carbonates of atomic variable acceptor elements including at least one of V, Mn, Cr, Fe, Ni, Co, Cu, and Zn as a fifth auxiliary component. The fifth auxiliary component may include V2O5, MnO2, and It is preferable that at least one selected from the group consisting of Cr2O3, but is not limited thereto.
[0053] The fifth auxiliary component may be included in an amount of 0.03 to 4 molar parts per 100 molar parts of the parent material main component. The content of the fifth auxiliary component may be based on the content of the elements included in the fifth auxiliary component, regardless of the addition form, such as oxide or carbonate. For example, the total content of the elements included in the fifth auxiliary component may be 0.03 to 4 molar parts per 100 molar parts of the parent material main component.
[0054] The fifth auxiliary component can improve the high-temperature withstand voltage characteristics by improving the reduction resistance of the dielectric composition. If the content of the fifth auxiliary component is less than 0.03 parts by mole, the high-temperature withstand voltage may be reduced, and if it exceeds 4 parts by mole, the reliability of the dielectric magnetic composition may be reduced (e.g., a decrease in permittivity, etc.).
[0055] 6th component
[0056] The dielectric composition according to embodiments of the present invention may include, as a sixth auxiliary component, at least one selected from the group consisting of an oxide of Si element, a carbonate of Si element, and a glass containing Si element. Preferably, the sixth auxiliary component is Ba. x Ca 1-x It may include a complex oxide represented by SiO3 (wherein x is 0.3 to 0.8). The x value of the complex oxide may be 0.3 to 0.8. Here, if the x value is too small, the dielectric properties may deteriorate due to a reaction between SiO2 and the main component BaTiO3. Conversely, if the x value is too large, the melting point may increase, which may deteriorate the properties related to plasticity.
[0057] The sixth auxiliary component may be included in an amount of 0.1 to 5 mol parts based on 100 mol parts of the main component of the above-mentioned parent material. If the content of the sixth auxiliary component is less than 0.1 mol parts, the rate of change in capacitance depending on temperature may increase. Conversely, if the content of the sixth auxiliary component exceeds 5 mol parts, problems such as reduced sinterability and density, and formation of secondary phases may occur, which is not preferable.
[0058] Experimental example
[0059] BaTiO3 mixed solid solution powder, which is a base powder containing the main component, was manufactured by applying the solid-state method as follows.
[0060] The starting materials are BaCO3 and TiO2. These starting material powders were mixed in a ball mill and calcined at 900-1000℃ to prepare the main component base material powder. After mixing the auxiliary component additive powders with the main component base material powder in the ingredient ratios shown in Table 2, the raw material powder containing the main and auxiliary components was ball milled for a predetermined time (e.g., 20 hours) using zirconia balls as a mixing / dispersing medium and mixing ethanol / toluene with a dispersant and binder.
[0061] The manufactured slurry was molded into a 10㎛ thick sheet using a doctor blade type coater, and Ni internal electrodes were printed on the molded sheet. The upper and lower covers were manufactured by laminating 25 layers of cover sheets, and 21 layers of printed active sheets were pressed and laminated to manufacture a press bar. The press bar was cut into chips of size 3225 (length Х width Х thickness 3.2 mm Х 2.5 mm Х 2.5 mm) using a cutter.
[0062] After the manufactured chip was calcined, it was fired at a temperature of 1210°C to 1320°C for more than 1 hour in a reducing atmosphere (0.1% H2 / 99.9% N2, H2O / H2 / N2 atmosphere), and then heat-treated by reoxidation in a nitrogen (N2) atmosphere at a temperature of 1000°C for more than 2 hours.
[0063] The external electrode was completed by performing a termination process and electrode firing using copper paste on the fired chip.
[0064] For the laminated ceramic capacitor specimens completed as described above, the capacitance (dielectric constant), sintering temperature and dissipation factor (DF), and temperature-dependent capacitance change (TCC) were measured and evaluated. In addition, room temperature insulation resistance and high temperature accelerated life were evaluated, but are not described.
[0065] The room temperature capacitance was measured using an LCR meter under conditions of 1 kHz and AC 0.2 V / ㎛. The permittivity of the multilayer ceramic capacitor (MLCC) chip was calculated from the capacitance, dielectric thickness, internal electrode area, and number of layers of the multilayer ceramic capacitor (MLCC) chip.
[0066] Dissipation factor (DF) was measured at 1 kHz and 1 Vrms using a capacitance meter (Keysight, E4981A).
[0067] The change in capacitance according to temperature was measured in the temperature range of -55℃ to 125℃. In this temperature range, the change in capacitance was measured under the conditions of 1kHz and 1Vrms using an LCR-meter. At this time, the change rate (%) of the capacitance at each temperature was measured compared to the capacitance at 25℃. In this specification, the change in capacitance at 125℃ is described. If the change rate of capacitance (Temperature Coefficient of Capacitance, TCC) at 125℃ was within ±15%, it was judged as good, and otherwise, it was judged as bad.
[0068] Sample material main ingredient moles per 100 moles of main ingredient 1,2 total amount of main ingredient 123456Yb2O3+Dy2O3Yb2O3Dy2O3Y2O3BaZrO3MgCO3V2O5MnO2Cr2O3Ba 0.6 Ca 0.4SiO3101.00052.500.120.110.173.551.0020.101.00052.500.120.110.173.551.1 031.221.00052.500.120.110.173.552.2241.501.00052.500.120.110.173.552.5 052.001.00052.500.120.110.173.553.0062.501.00052.500.120.110.173.553.5073.001.00052.500.120.110.173.554.0083.501.00052.500.120.110.173.554.50
[0069] Sample Dielectric constantDissipation factor(DF)Sintering temperature(℃)High temperatureTCC(125℃)X7RCharacteristics judgment119000.0121210-19.4X219000.0111220-14.80319000.0091225-13.00418000.0071230-11.10515000.0061230-9.50615000.0071240-8.90714500.0081280-7.750814000.0121300-19.8X
[0070] Table 2 shows samples in which the content of the first subcomponent Yb was changed while the content of the second subcomponent Dy was fixed at 2 mol, the content of the third subcomponent at 5 mol, the content of the fourth subcomponent Mg at 2.5 mol, the content of the sum of the fifth subcomponent (V, Mn, Cr) at 0.69 mol, and the content of the sixth subcomponent at 3.55 mol. Table 3 shows the characteristics of samples corresponding to Samples 1 to 8 of Table 2.
[0071] When the content of the first auxiliary component Yb was 0 mol (Sample 1), the high temperature TCC (125℃) was outside the range of ±15% and was vulnerable to temperature changes. In addition, when the content of the first auxiliary component Yb exceeded 6 mol (Sample 8), the problem of being vulnerable to temperature changes occurred because the high temperature TCC (125℃) was outside the range of ±15%. On the other hand, in the range where the content of the first auxiliary component Yb exceeded 0 mol (e.g., 0.2 mol or more) and 6 mol or less (Samples 2 to 7), the high temperature TCC was within ±15%, satisfying the X7R standard. Therefore, the appropriate content range of the first auxiliary component can be said to be 0.2 to 6 mol parts or less with respect to 100 mol parts of the main component of the base material.
[0072] Meanwhile, as the content of the first auxiliary component Yb increases, the capacity change rate decreases, but the sintering temperature tends to increase. That is, when the content of Yb is 7 mol or more, a sintering temperature of 1300°C or more is required, and if the sintering temperature is too high, problems such as damage to the Ni internal electrode may occur. To solve this, the dielectric composition according to the embodiments of the present invention is characterized in that all of the first to third auxiliary components are added to BaTiO3. As shown in the table above, when the dielectric composition includes all of the first to third auxiliary components, the X7R standard can be satisfied even if the content of the first auxiliary component Yb is not increased to 7 mol or more. In this way, since the content of Yb added to the dielectric composition can be lowered to satisfy the X7R standard, there is an effect of suppressing an increase in the sintering temperature.
[0073] In addition, when the total content of the first and second subcomponents is within the range of 2 to 4 molar parts (samples 3 to 7), the loss factor (DF) was found to be less than 0.01. Therefore, when the total content of the first and second subcomponents is within the range of 2 to 4 molar parts (samples 3 to 7), it can be said to be a composition suitable for an AC circuit because it satisfies the X7R standard, has a high dielectric constant of 1400 or higher, and has a loss factor (DF) of less than 0.01.
[0074] Sample material main ingredient moles per 100 moles of main ingredient 1,2 total amount of main ingredient 123456Yb2O3+Dy2O3Yb2O3Dy2O3Y2O3BaZrO3MgCO3V2O5MnO2Cr2O3Ba 0.6 Ca 0.4 SiO392.000052.500.120.110.173.552.00102.000.10052.500.120.110.173.552.10 112.001.22052.500.120.110.173.553.22122.001.50052.500.120.110.173.553.50 132.002.00052.500.120.110.173.554.00142.002.50052.500.120.110.173.554.50152.003.00052.500.120.110.173.555.00162.003.50052.500.120.110.173.555.50
[0075] Sample Dielectric constantDissipation factor(DF)Sintering temperature(℃)High temperatureTCC(125℃)X7RCharacteristics judgment919000.0091220-19.0X1019000.0081225-14.901118000.0081235-9.301215000.0081240-8.901314500.0081280-7.601414500.0121300-6.501514000.0121310-6.001614000.0131315-19.5X
[0076] Table 4 shows samples in which the content of the second auxiliary component Dy was changed while the content of the first auxiliary component Yb was fixed at 4 mol, the content of the third auxiliary component was fixed at 5 mol, the content of the fourth auxiliary component Mg was fixed at 2.5 mol, the content of the sum of the fifth auxiliary component (V, Mn, Cr) was fixed at 0.69 mol, and the content of the sixth auxiliary component was fixed at 3.55 mol. Table 5 shows the characteristics of samples corresponding to samples 9 to 16 of Table 4.
[0077] When the content of the second auxiliary component Dy is 0 mol (Sample 9), there is a problem that the high temperature TCC (125℃) is outside the range of ±15% and is vulnerable to temperature changes. In addition, when the content of the second auxiliary component Dy exceeds 6 mol (Sample 16), there was also a problem that the high temperature TCC (125℃) was outside the range of ±15% and was vulnerable to temperature changes. On the other hand, in the range where the content of the second auxiliary component Dy exceeds 0 mol (e.g., 0.2 mol or more) and is 6 mol or less (Samples 10 to 15), the high temperature TCC was within ±15%, satisfying the X7R standard. Therefore, the appropriate content range of the second auxiliary component Dy can be said to be 0.2 to 6 mol parts in element ratio with respect to 100 mol parts of the main component of the base material.
[0078] In addition, when the total content of the first and second subcomponents is within the range of 2 to 4 molar parts (samples 10 to 13), the loss factor (DF) was found to be less than 0.01. Therefore, when the total content of the first and second subcomponents is within the range of 2 to 4 molar parts (samples 10 to 13), it can be said to be a composition suitable for an AC circuit because it satisfies the standard of X7R, has a high dielectric constant of 1400 or higher, and has a loss factor (DF) of less than 0.01.
[0079] Sample material main ingredient moles per 100 moles Total amount of auxiliary ingredients 1,2 Yb2O3+Dy2O3+Y2O3Yb2O3Dy2O3Y2O3BaZrO3MgCO3V2O5MnO2Cr2O3Ba 0.6 Ca 0.4SiO3172.0000.1052.500.120.110.173.552.10182.000.500.5052.500.120.110.173.553.00192.001.001.0052.500.120.110.173.55 4.00202.001.002.0052.500.120.110.173.555.00212.0003.0052.500.120.110.173.555.00222.0003.5052.500.120.110.173.555.50
[0080] Sample Dielectric constantDissipation factor(DF)Sintering temperature(℃)High temperatureTCC(125℃)X7RCharacteristic judgment1719000.0091220-14.501815000.0061230-9.701914500.0081280-8.502014000.0121300-6.202114000.0131315-6.002214000.0131320-19.4X
[0081] Table 6 shows samples in which the total contents of the second subcomponents Dy and Y were changed while the content of the first subcomponent Yb was fixed at 4 mol, the content of the third subcomponent at 5 mol, the content of the fourth subcomponent Mg at 2.5 mol, the content of the sum of the fifth subcomponent (V, Mn, Cr) at 0.69 mol, and the content of the sixth subcomponent at 3.55 mol. Table 7 shows the characteristics of samples corresponding to samples 17 to 22 in Table 6.
[0082] When the total content of the second auxiliary components Dy and Y exceeded 6 mol (Sample 22), the high temperature TCC (125℃) exceeded ±15%, showing vulnerability to temperature changes. On the other hand, when the total content of the second auxiliary components Dy and Y was in the range of 0.2 mol to 6 mol (Samples 17 to 21), the high temperature TCC (125℃) was within ±15%, satisfying the X7R standard.
[0083] In addition, for Samples 17 and 21, although the second auxiliary component contained Y as a substitute element for Dy, the high-temperature TCC was found to be within ±15%, satisfying the X7R specification. In this way, it can be seen that the second auxiliary component satisfies the X7R specification even though it contains Y as a substitute element for Dy. However, it can be seen that the X7R specification is satisfied only when the total content of the elements included in the second auxiliary component is 0.2 to 6 molar parts (Samples 17 to 21), and when the total content of the elements exceeds 6 molar parts (Sample 22), the high-temperature TCC (125℃) is outside ±15%.
[0084] Meanwhile, when the total content of the first and second subcomponents is within the range of 2 to 4 molar parts (samples 17 to 19), the loss factor (DF) was found to be less than 0.01. Therefore, when the total content of the first and second subcomponents is within the range of 2 to 4 molar parts (samples 17 to 19), it can be said to be a composition suitable for an AC circuit because it satisfies the X7R standard, has a high dielectric constant of 1400 or higher, and has a loss factor (DF) of less than 0.01.
[0085] Sample material main ingredient moles per 100 moles Total amount of auxiliary ingredients 1,2 Yb2O3+Dy2O3+Y2O3Yb2O3Dy2O3Y2O3BaZrO3MgCO3V2O5MnO2Cr2O3Ba 0.6 Ca 0.4SiO3232.001.000.5032.500.120.110.173.553.50242.001.000.5052.500.120.110.173.553. 50252.001.000.507.52.500.120.110.173.553.50262.001.000.50102.500.120.110.173.553. 50272.001.000.50132.500.120.110.173.553.50282.001.000.50172.500.120.110.173.553.50292.001.000.50252.500.120.110.173.553.50302.001.000.50302.500.120.110.173.553.50
[0086] Sample Dielectric ConstantDissipation Factor(DF)High TemperatureTCC(125℃)X7RCharacteristicsJudgment2317000.012-2.9602415000.006-9.5002515000.012-16.10X2614500.015-24.31X2714500.018-43.20X2814000.020-62.10X2914000.025-58.41X3014000.027-53.76X
[0087] Table 8 shows samples in which the content of the third subcomponent was changed while the content of the first subcomponent Yb was fixed at 4 mol, the content of the sum of the second subcomponent (Dy, Y) was fixed at 3 mol, the content of the fourth subcomponent Mg was fixed at 2.5 mol, the content of the sum of the fifth subcomponent (V, Mn, Cr) was fixed at 0.69 mol, and the content of the sixth subcomponent was fixed at 3.55 mol. Table 9 shows the characteristics of samples corresponding to samples 23 to 30 of Table 8.
[0088] When the content of the third auxiliary ingredient exceeded 6 mol (samples 25-30), the high temperature TCC (125℃) exceeded ±15% and was vulnerable to temperature changes. On the other hand, in the range where the content of the third auxiliary ingredient was 6 mol or less (samples 23-24), the high temperature TCC was within ±15%, satisfying the X7R standard. In addition, when the content of the third auxiliary ingredient was less than 4 mol (sample 23), the loss factor (DF) exceeded 0.01, but when the content of the third auxiliary ingredient was 4 mol or more (sample 24), the loss factor (DF) was less than 0.01. Therefore, when the content of the third component is within 4 to 6 mol parts per 100 mol parts of the main component of the parent material (Sample 24), it can be said to be a composition suitable for an AC circuit because it satisfies the standard of X7R, has a high dielectric constant of 1400 or more, and has a loss factor (DF) of less than 0.01.
[0089] The present invention is not limited to the embodiments described above and the accompanying drawings, but is defined by the appended claims. Therefore, it will be apparent to those skilled in the art that various substitutions, modifications, and alterations are possible within the scope of the technical spirit of the present invention as defined in the claims, and such modifications also fall within the scope of the appended claims.
Claims
1. In a dielectric composition containing a main component and a secondary component of a barium titanate-based material, The above auxiliary ingredients are, A first subcomponent comprising at least one selected from the group consisting of oxides and carbonates of at least one element selected from the group consisting of Yb, Sc, Lu and Tm; A second secondary component comprising at least one selected from the group consisting of oxides and carbonates of at least one element selected from Dy, Y, Ho, Tb, Gd, Eu and Er; A third component comprising at least one selected from the group consisting of oxides comprising Ba and Zr; A fourth minor component comprising at least one of an oxide and a carbonate of an atomic fixed acceptor element including Mg; A fifth secondary component comprising at least one selected from the group consisting of oxides and carbonates of variable acceptor elements, wherein the atomic number comprises at least one of V, Mn, Cr, Fe, Ni, Co, Cu, and Zn; and A sixth auxiliary component comprising at least one selected from the group consisting of oxides, carbonates and glasses of the Si element; comprising at least one auxiliary component; The at least one subcomponent includes the first subcomponent, the second subcomponent, and the third subcomponent, The content of one or more elements included in the first auxiliary component is 0.2 to 6 molar parts per 100 molar parts of the main component of the parent material, The content of one or more elements included in the second auxiliary component is 0.2 to 6 molar parts per 100 molar parts of the main component of the parent material, The content of the third auxiliary component is 4 to 6 molar parts per 100 molar parts of the main component of the parent material. Genetic composition.
2. In paragraph 1, The above first subcomponent includes the Yb element, Genetic composition.
3. In paragraph 1, The total content of the first and second auxiliary components is 2 to 4 moles, Genetic composition.
4. In paragraph 1, The above second component includes Dy2O3 and Y2O3, The total content of Dy and Y included in the above second component is 0.2 to 6 molar parts, Genetic composition.
5. In paragraph 1, wherein said at least one subcomponent further comprises said fourth subcomponent, The content of the Mg element included in the fourth auxiliary component is 0.1 to 3 mol parts per 100 mol parts of the main component of the parent material. Genetic composition.
6. In paragraph 1, wherein said at least one subcomponent further comprises said fifth subcomponent, The content of the variable valence acceptor element included in the fifth auxiliary component is 0.03 to 4 mol parts per 100 mol parts of the parent material main component. Genetic composition.
7. In paragraph 1, wherein said at least one subcomponent further comprises said sixth subcomponent, The content of the above sixth auxiliary component is 0.1 to 5 mol parts per 100 mol parts of the main component of the above-mentioned parent material. Genetic composition.
8. In paragraph 7, The above sixth component is Ba x Ca 1-x Comprising a complex oxide represented by SiO3 (wherein x is 0.3 to 0.8), Genetic composition.
9. In a method for producing a genetic composition, Step for preparing the main component of barium titanate-based base material; A step of preparing at least one subcomponent including the first subcomponent, the second subcomponent and the third subcomponent among a first subcomponent including at least one selected from the group consisting of oxides and carbonates of at least one element selected from Yb, Sc, Lu and Tm, a second subcomponent including at least one selected from the group consisting of oxides and carbonates of at least one element selected from Dy, Y, Ho, Tb, Gd, Eu and Er, a third subcomponent including at least one selected from the group consisting of oxides of Ba and Zr, a fourth subcomponent including at least one selected from the group consisting of oxides and carbonates of a valence-fixed acceptor element including Mg, a fifth subcomponent including at least one selected from the group consisting of oxides and carbonates of a valence-variable acceptor element including at least one selected from the group consisting of oxides and carbonates of at least one element selected from V, Mn, Cr, Fe, Ni, Co, Cu, and Zn, and a sixth subcomponent including at least one selected from the group consisting of oxides, carbonates and glasses of the element Si; A step of preparing a mixture comprising the above main component and at least one auxiliary component; and Comprising a step of calcining the above mixture, The content of one or more elements included in the first auxiliary component is 0.2 to 6 molar parts per 100 molar parts of the main component of the parent material, The content of one or more elements included in the second auxiliary component is 0.2 to 6 molar parts with respect to 100 molar parts of the main component of the parent material, The content of the third auxiliary component is 4 to 6 molar parts per 100 molar parts of the main component of the parent material. Method for producing a dielectric composition.
10. In paragraph 9, The sintering temperature of the above mixture is 1210℃ or higher. Method for producing a dielectric composition.
Citation Information
Patent Citations
Dielectric porcelain and laminated ceramic capacitor using the same and preparation thereof
JP1991112861A
Dielectric ceramic composition and ceramic electronic part
JP2011201761A
Method for producing dielectric ceramic composition and electronic part
JP2012206885A
Agricultural waterway pipe with smooth water supply
KR1020220100123A
High-torque fastening device for directional propellant using hydraulic cylinder as power source