Hollow fiber membrane for humidifier, manufacturing method thereof, and humidifier including hollow fiber membrane
The integration of antioxidants in the hollow fiber membrane for fuel cell humidifiers addresses the issue of radical-induced deterioration, enhancing durability and performance by capturing and decomposing peroxide or hydroxyl radicals, thus maintaining efficient moisture and gas exchange in fuel cell systems.
Patent Information
- Application Number
- PCT/KR2024/006409
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-11
- Filing Date
- 2024-05-10
- Publication Date
- 2024-11-14
AI Technical Summary
In fuel cell systems, incomplete reactions produce peroxide or hydroxyl radicals that cause oxidation and deterioration of the organic hollow fiber membranes in humidifiers, leading to reduced efficiency and durability, as these radicals flow back from the fuel cell stack to the membrane humidifier.
A hollow fiber membrane for humidifiers is developed with a polymer and an antioxidant, where the antioxidant is dispersed within the polymer, typically in amounts of 0.01 to 5 parts by weight, to capture and decompose peroxide or hydroxyl radicals, thereby enhancing the membrane's chemical durability.
The incorporation of antioxidants in the hollow fiber membrane effectively suppresses decomposition from peroxide or hydroxyl radicals, improving the membrane's durability and maintaining sufficient moisture exchange and gas permeability, ensuring efficient operation in fuel cell systems.
Smart Images

Figure KR2024006409_14112024_PF_FP_ABST
Abstract
Description
Hollow fiber membrane for humidifier, method for manufacturing same, and humidifier including the hollow fiber membrane
[0001] The present invention relates to a hollow fiber membrane for a humidifier having a novel composition, a method for manufacturing the same, and a humidifier including the hollow fiber membrane.
[0002] Fuel cells are power-generating cells that convert the chemical energy of hydrogen and oxygen into electrical energy through an electrochemical reaction. Unlike conventional chemical cells like batteries or accumulators, fuel cells can continuously produce electricity as long as hydrogen and oxygen are supplied. They also have the advantage of no heat loss, making them more than twice as efficient as internal combustion engines.
[0003] Furthermore, fuel cells are environmentally friendly energy generators that generate no pollutants, as they use hydrogen and oxygen as raw materials and produce water as a product. Therefore, fuel cells are not only environmentally friendly but also offer the advantage of reducing concerns about resource depletion due to increased energy consumption.
[0004] Fuel cells can be classified into polymer electrolyte membrane fuel cells (PEMFC), phosphoric acid fuel cells (PAFC), molten carbonate fuel cells (MCFC), solid oxide fuel cells (SOFC), and alkaline fuel cells (AFC).
[0005] Among these, polymer electrolyte fuel cells are known to be suitable for use in transportation systems because they can operate at lower temperatures and have a higher power density than other fuel cells.
[0006] Meanwhile, polymer electrolyte fuel cells generally form water by reacting 2 moles of hydrogen and 1 mole of oxygen in the fuel cell stack during operation. However, if the reaction is incomplete, peroxide or hydroxide radicals may be formed as byproducts.
[0007] There is a problem in that when the peroxide or hydroxyl radicals generated in this way flow from the fuel cell stack to the membrane humidifier, they cause oxidation of the organic hollow fiber membrane within the membrane humidifier, resulting in decomposition and deterioration of the hollow fiber membrane.
[0008] Decomposition and deterioration of the hollow fiber membrane impede the delivery of sufficiently moist air to the fuel cell stack, thereby reducing the efficiency of the fuel cell stack and the entire fuel cell.
[0009] Accordingly, there is an industrial demand for hollow fiber membranes that are resistant to decomposition by peroxide or hydroxyl radicals.
[0010] In order to solve the above-mentioned problems, a hollow fiber membrane for a humidifier, which is inhibited from decomposition by peroxide or hydroxyl radicals, a method for manufacturing the same, and a humidifier including the hollow fiber membrane are provided.
[0011] According to one aspect, a hollow fiber membrane for a humidifier is provided, which comprises a polymer and an antioxidant, and comprises 0.01 to 5 parts by weight of the antioxidant per 100 parts by weight of the hollow fiber membrane.
[0012] According to another aspect, a method for manufacturing a hollow fiber membrane for a humidifier is provided, comprising: a step of obtaining a spinning solution by mixing an antioxidant in an amount of 0.01 to 5 parts by weight based on 100 parts by weight of a spinning solution; a step of spinning the spinning solution into a coagulation tank through a nozzle; and a step of coagulating the spinning solution in the coagulation tank.
[0013] According to another aspect, a humidifier including the above hollow fiber membrane is provided.
[0014] A hollow fiber membrane for a humidifier according to one aspect comprises a polymer and an antioxidant, and by including 0.01 to 5 parts by weight of the antioxidant per 100 parts by weight of the hollow fiber membrane, the hollow fiber membrane is prevented from being decomposed by peroxide or hydroxyl radicals by capturing and / or decomposing peroxide or hydroxyl radicals flowing into the humidifier from a fuel cell stack, thereby improving the chemical durability of the hollow fiber membrane.
[0015] Figures 1 and 2 are exploded perspective views of a fuel cell humidifier according to one embodiment.
[0016] The present inventive concept described below is capable of various modifications and embodiments. Specific embodiments are illustrated in the drawings and described in detail in the detailed description. However, this is not intended to limit the present inventive concept to specific embodiments, but should be understood to encompass all modifications, equivalents, or alternatives within the technical scope of the present inventive concept.
[0017] The terminology used below is only used to describe specific embodiments and is not intended to limit the present invention. Singular expressions include plural expressions unless the context clearly indicates otherwise. Hereinafter, it should be understood that terms such as "comprises" or "has" indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, but do not exclude in advance the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof.
[0018] When a component is referred to as being "connected, coupled" to another component, it should be understood that while the component may be directly connected or coupled to the other component, there may also be a new component between the component and the other component. Conversely, when a component is referred to as being "directly connected" or "directly coupled" to another component, it should be understood that no new component exists between the component and the other component.
[0019] Throughout the specification, when an element, such as a layer, film, region, or plate, is referred to as being "on" or "above" another element, this includes not only instances where the element is directly above the other element, but also instances where there are other elements intervening between them. Terms such as first, second, etc. may be used throughout the specification to describe various components, but the components themselves should not be limited by these terms. These terms are used solely to distinguish one element from another.
[0020] The term "polymer" as used throughout the specification means a polymer formed by polymerization of one or more monomer units, and has a meaning encompassing polymer resins and polymer macromolecules.
[0021] The embodiments described below are merely exemplary, and various modifications are possible from these embodiments.
[0022] A hollow fiber membrane for a humidifier according to one aspect includes a polymer and an antioxidant, and may include 0.01 to 5 parts by weight of the antioxidant per 100 parts by weight of the hollow fiber membrane.
[0023] According to one embodiment, the antioxidant may be included in an amount of 0.1 to 5 parts by weight, for example, the antioxidant may be included in an amount of 1 to 3 parts by weight, or 2 to 4 parts by weight, and a range defined by any two values of the aforementioned numerical ranges may be included.
[0024] If the antioxidant is contained in the hollow fiber membrane in an amount of less than 0.01 parts by weight, it is not sufficient to prevent deterioration of the hollow fiber membrane due to peroxide or hydroxyl radicals generated in the fuel cell reaction, and if it exceeds 5 parts by weight, the pores of the hollow fiber membrane are closed, resulting in a decrease in moisture exchange performance and gas permeability, making it impossible to perform the essential function of the membrane humidifier.
[0025] According to one embodiment, the antioxidant may be dispersed within the polymer. For example, the antioxidant may have a particle shape and may be dispersed and present in a structure embedded within the polymer. Here, "dispersed" means that the antioxidant exists within the space formed by the polymer backbone.
[0026] According to one embodiment, the antioxidant may be randomly or uniformly dispersed within the polymer. For example, the antioxidant may be uniformly dispersed within the polymer.
[0027] In one embodiment, at least a portion of the antioxidant may be exposed to the surface of the polymer. For example, a portion of the antioxidant exposed to the surface of the polymer may be embedded in the polymer, and only a portion thereof may be exposed to the outside.
[0028] According to one embodiment, the hollow fiber membrane may include a concentration gradient region in which the concentration of the antioxidant within the hollow fiber membrane varies. For example, the concentration of the antioxidant may increase from the inner surface of the hollow fiber membrane toward the outer surface.
[0029] By configuring the outer surface of the hollow fiber membrane to have more antioxidants, it is possible to effectively capture and decompose hydrogen peroxide or hydroxyl radicals flowing into the humidifier together with high-humidity air from the fuel cell stack.
[0030] According to one embodiment, the antioxidant may include an organic antioxidant, a metal antioxidant, an organo-metallic antioxidant, a HALS (Hindered amine Light stabilizer), a sulfur-based antioxidant, a phosphorus-based antioxidant, or a combination thereof.
[0031] For example, the organic antioxidant may include Coumaric acid, Dopamine, Hydroquinone, Phenolphthalein, Phthalic acid, Acetylsalicylic acid, Phenolic antioxidants, Naiacin, Luminol, Urine, Phytic acid, Glyoxal, or any mixture thereof.
[0032] For example, the metal-based antioxidant may include a salt of Ce metal such as Ce(NO3)3, CeCl3, Ce2(SO4)3, etc., a salt of Mn metal such as Mn(NO3), etc., a metal oxide such as CeO2, CeSiO2, MnO2, TiO2, etc., or any mixture thereof.
[0033] For example, the organometallic complex may include a Ce-crown complex, a Ce-phosphoric acid complex, a Ce-Bypyridine, or any mixture thereof.
[0034] According to one embodiment, the polymer may be selected from known polymers suitable for forming a hollow fiber membrane, and may include, for example, a polyvinylidene fluoride (PVDF) polymer, a polysulfone polymer, a sulfonated polysulfone, cellulose acetate, cellulose triacetate, polymethyl methacrylate, Nafion, a polystyrene (PS) polymer, a polytetrafluoroethylene (PTFE) polymer, a perfluorosulfonic acid (PFSA) polymer, a polyphenylsulfone polymer, a polyethersulfone (PES) polymer, a polyacrylonitrile (PAN) polymer, a polyetherimide (PEI) polymer, a polyimide (PI) polymer, or any combination of the above-mentioned polymers.
[0035] For example, the polymer may include a polystyrene-based polymer.
[0036] According to one embodiment, the polymer may be included in an amount of 10 to 35 parts by weight per 100 parts by weight of the hollow fiber membrane. For example, the polymer may be included in an amount of 15 to 30 parts by weight per 100 parts by weight of the hollow fiber membrane.
[0037] According to one embodiment, the thickness of the hollow fiber membrane may be 60 um to 300 um. For example, the thickness of the hollow fiber membrane may be 80 um to 120 um, 100 um to 140 um, but is not limited thereto, and may have any arbitrary thickness range included in the above range.
[0038] According to one embodiment, the hollow fiber membrane may further include additives such as surfactants, hydrophilic organic compounds, or hydrophilic polymers. These additives may be selected and added in an appropriate amount so long as they do not impair the inherent physical properties of the hollow fiber membrane. It will be apparent to those skilled in the art that other materials commonly used in the manufacture of hollow fiber membranes may also be used.
[0039] According to one embodiment, the hollow fiber membrane may have an antioxidant randomly or uniformly dispersed in the polymer.
[0040] For example, the hollow fiber membrane can achieve improved durability against peroxide and hydroxyl radicals without significantly impairing the porosity of the hollow fiber membrane by uniformly dispersing an antioxidant in the polymer.
[0041] According to one embodiment, the hollow fiber membrane has a cavity inside and may include a plurality of pores that connect the inner surface and the outer surface to each other through gas.
[0042] According to one implementation example, the hollow fiber membrane has a water vapor permeability of 0.1 g / s / m measured under the conditions of a shell-side dew point of 75°C, a pressure of 0.8 barg, and a flow rate of 1000 slpm. 2 It can be ideal, for example, a water vapor permeability of 0.13 g / s / m 2 If the water vapor permeability satisfies the above range, sufficient moisture exchange performance of the hollow fiber membrane can be expected.
[0043] According to one implementation example, the hollow fiber membrane has a nitrogen permeability of 100 cc / min / cm under a pressure condition of 0.5 bar. 2 It may be less than, for example, the nitrogen permeability is 80 cc / min / cm 2 It could be.
[0044] According to one embodiment, the hollow fiber membrane has an oxygen permeability of 100 cc / min / cm under a pressure condition of 0.5 bar. 2It may be less than, for example, the oxygen permeability is 80 cc / min / cm 2 It could be.
[0045] The above hollow fiber membrane has the aforementioned water vapor permeability, nitrogen permeability and oxygen permeability, and is suitable for use in a humidifier of a fuel cell with improved durability by having sufficient moisture exchange and gas permeability even when an antioxidant is introduced to improve durability.
[0046]
[0047] A method for manufacturing a hollow fiber membrane for a humidifier according to one aspect may include the steps of: mixing a polymer and an antioxidant in an organic solvent, wherein the antioxidant is mixed in an amount of 0.01 to 5 parts by weight relative to 100 parts by weight of a spinning solution to obtain a spinning solution; spinning the spinning solution into a coagulation tank through a nozzle; and solidifying the spinning solution in the coagulation tank.
[0048] For the overlapping components of the manufacturing method of the above hollow fiber membrane with the above-described ones, refer to the above.
[0049] According to one embodiment, the step of obtaining the radiation source may include a step of mixing the antioxidant and the polymer in a solvent.
[0050] The solvent may include at least one of a first solvent, a second solvent, and a third solvent. For example, the solvent may be a mixed solvent including two types of solvents among the first solvent, the second solvent, and the third solvent.
[0051] The first solvent is a solvent that cannot dissolve the polymer at room temperature (e.g., 23 to 25°C) but can dissolve the polymer at high temperatures (e.g., 80°C or higher), and may include butanol, isobutanol, octanol, pentanol, isopentanol, dimethyl phthalate, diethyl phthalate, dibutyl phthalate, dioctyl phthalate, polyoxylethylene octylphenyl ether, or a combination thereof.
[0052] The second solvent is a solvent that cannot dissolve the polymer, and may include water, methanol, ethanol, isopropanol, acetone, hexane, pentane, benzene, toluene, carbon tetrachloride, o-dichlorobenzene, polyethylene glycol, or a combination thereof.
[0053] The third solvent is a solvent that can dissolve the polymer even at room temperature, and may include N-methyl-2-pyrrolidone, dimethyl sulfoxide, dimethyl acetamide, dimethyl formamide, methyl ethyl ketone, tetrahydrofuran, tetramethyl urea, or trimethyl phosphate.
[0054] A person skilled in the art can use one or a mixture of two or more of the first solvent, the second solvent, and the third solvent, taking into account the characteristics of the polymer and the production of a hollow fiber membrane having desired properties.
[0055] According to one embodiment, when the solvent is a mixed solvent of two or more solvents, the mixing ratio of the solvents may be 1:9 to 9:1 by weight, but is not limited thereto, and a person skilled in the art may select an appropriate range by considering the content of the polymer and antioxidant, the viscosity of the spinning solution, and the physical properties of the final hollow fiber membrane.
[0056] According to one embodiment, the content of the polymer contained in the above-described radiation source may be 10 to 35 wt%. For example, the content of the polymer may be 15 to 30 wt%, but is not limited thereto, and a person skilled in the art may select an appropriate content range by considering the physical properties, gas permeability, etc. of the final hollow fiber membrane.
[0057] According to one embodiment, the content of the antioxidant included in the radiation source may be 0.01 to 5 parts by weight. For example, the content of the antioxidant may be 1 to 5 parts by weight, or 2 to 4 parts by weight, but is not limited thereto, and a person skilled in the art may select an appropriate content range by considering the physical properties, gas permeability, etc. of the final hollow fiber membrane.
[0058] According to one embodiment, the temperature at which the polymer, antioxidant, and solvent are mixed in the step of obtaining the above-described radiation source may be 10 to 130°C, for example, 50 to 90°C, or 60 to 80°C.
[0059] According to one embodiment, the time for mixing the above-mentioned radiation source may be 2 to 24 hours, for example, 5 to 22 hours, or 6 to 20 hours, but is not limited thereto, and mixing may be performed for a time period until the radiation source is uniformly mixed within the above-mentioned time range.
[0060] According to one embodiment, the viscosity of the spinning solution may be 5000 cps to 30000 cps at 50°C. When the viscosity of the spinning solution satisfies the above range, smooth discharge of the hollow fiber membrane spinning solution is facilitated.
[0061] The above-mentioned radiation dope can be discharged from the outer tube of the multi-shaped radiation nozzle, and at the same time, the core liquid can be discharged together from the inner tube.
[0062] The core liquid serves to form the hollow fiber membrane, and may be a mixed solution comprising any one solvent selected from the group consisting of water, polyvinylpyrrolidone, N,N-dimethyl acetamide (DMAc), N,N-dimethyl formamide (DMF), N-methyl-2-pyrrolidone (NMP), dimethyl sulfoxide (DMSO), methyl ethyl ketone (MEK), gamma butyrolactone, sulfolane, 1,3-dimethyl-2-imidazolidinone, and mixtures thereof, and an additive selected from the group consisting of ethanol, sorbitol, polyethylene glycol, ethylene glycol, polypropylene glycol, propylene glycol, diethylene glycol, glycerin, lithium chloride, lithium bromide, and mixtures thereof.
[0063] The core solution may have a mixed weight ratio of the solvent and the additive of 70:30 to 40:60. When the weight ratio of the additive is less than 30, finger-shaped macropores may be formed throughout the hollow fiber membrane, and when the weight ratio of the additive exceeds 60, the phase transition speed may be slow, resulting in a hollow fiber membrane having a closed internal structure.
[0064] According to one embodiment, the step of irradiating the above-mentioned radiation source into the coagulation tank may include a step of irradiating the discharge liquid using a multi-tubular radiation device, for example, a double-tubular radiation device or a triple-tubular radiation device, but is not limited to such a multi-tubular type, and any discharge method capable of forming a hollow shape may be used without limitation.
[0065] According to one embodiment, in the step of radiating the above-mentioned radiation source into the coagulation tank, the radiation temperature may be 25 to 100°C, for example, 30 to 50°C.
[0066] According to one embodiment, in the step of irradiating the above-mentioned radiation source into the coagulation tank, the discharge speed may be 6 to 25 g / min, for example, 6 to 23 g / min, or 8 to 20 g / min. If the discharge speed exceeds 25 g / min, it is difficult to obtain a uniform thickness and porosity of the hollow fiber membrane, and if it is less than 6 g / min, the nozzle may become clogged.
[0067] After the above-mentioned radiation source is irradiated into the coagulation tank, the radiation source is coagulated by the coagulation solution.
[0068] According to one embodiment, the coagulation tank may be configured as a single tank, but is not limited thereto, and may be configured such that two or more coagulation tanks are arranged in series. When there are two or more coagulation tanks, the coagulant used in each coagulation tank may be the same or different.
[0069] According to one embodiment, the coagulant provided to the coagulation tank serves to coagulate the discharged liquid through the detention into the form of a hollow fiber membrane, and the coagulant used at this time can be appropriately selected and used by a person skilled in the art from known coagulants.
[0070] For example, the coagulant may be selected from acidic solutions, water, ethanol, sorbitol, polyethylene glycol, ethylene glycol, polypropylene glycol, propylene glycol, diethylene glycol, glycerin, lithium chloride, lithium bromide, and mixtures thereof.
[0071] In this case, when a mixed solution of two types of solutions is used as the coagulant, the first solution and the second solution may be mixed in a volume ratio of 1:9 to 9:1, for example, 2:8 to 8:2, 3:7 to 7:3, 4:6 to 6:4, or 5:5. The type and concentration of the coagulant may be appropriately selected by a person skilled in the art in consideration of the type of dope solution and core solution of the hollow fiber membrane, the physical properties of the hollow fiber membrane, etc.
[0072] According to one embodiment, the hollow fiber membrane obtained through the above coagulation tank may undergo a post-processing step.
[0073] According to one embodiment, the post-treatment step may include chemical treatment and / or physical treatment.
[0074] For example, the chemical treatment among the above post-treatment steps is performed to remove and dry the coagulant contained within the pores after the hollow fiber membrane is formed, and may include water washing, washing, hot water treatment, etc.
[0075] For example, the physical treatment during the above post-processing step may include stretching, shrinking, etc. to control the size and shape of the pores inside the hollow fiber membrane to improve the strength and durability of the hollow fiber membrane.
[0076]
[0077] A humidifier according to one aspect may include the aforementioned hollow fiber membrane for a humidifier.
[0078] For the hollow fiber desert, please refer to the above, and below, the humidifier will be described with reference to FIGS. 1 and 2.
[0079] Figures 1 and 2 are perspective views of a fuel cell humidifier (100) according to one embodiment of the present invention.
[0080] As shown in FIGS. 1 and 2, the fuel cell humidifier (100) of the present invention includes a middle case (110), a cap case (120), a fixing part (130), and a hollow fiber membrane bundle (200).
[0081] The middle case (110) is combined with the cap case (120) to form the outer shape of the membrane humidifier (100). The middle case (110) and the cap case (120) may be made of a hard plastic such as polycarbonate or a metal. The middle case (110) and the cap case (120) may have a circular cross-sectional shape in the width direction, as shown in FIG. 1, or may have a polygonal cross-sectional shape in the width direction, as shown in FIG. 2. The polygon may be a rectangle, a square, a trapezoid, a parallelogram, a pentagon, a hexagon, etc., and the polygon may have rounded corners. In addition, the circle may be an oval.
[0082] In the middle case (110), a second fluid inlet (112) through which the second fluid is supplied and a second fluid outlet (113) through which the second fluid is discharged are formed.
[0083] In FIGS. 1 and 2, a plurality of hollow fiber membranes (210) are arranged in the middle case (110) in the form of a single hollow fiber membrane bundle (200), but the hollow fiber membranes (210) may also be arranged in the middle case (110) in a state of being divided and accommodated in two or more cartridges.
[0084] A fluid inlet (121) is formed in the cap case (120). The fluid inlet (121) formed in one of the cap cases (120) respectively connected to both ends of the middle case (110) becomes a first fluid inlet, and the fluid inlet (121) formed in the other one becomes a first fluid outlet. The first fluid introduced through the fluid inlet (121) functioning as the first fluid inlet passes through the internal conduits (i.e., lumens) of the hollow fiber membranes (210) accommodated inside the middle case (110) and then exits through the fluid inlet (121) functioning as the first fluid outlet.
[0085] The ends of the hollow fiber membranes (210) are potted in the fixing member (130). The fixing member (130) binds the hollow fiber membranes (210) and fills the gap between the hollow fiber membranes (210) and the gap between the hollow fiber membranes (210) and the middle case (110). As a result, each of the two ends of the middle case (110) is blocked by the fixing member (130), and a flow path through which a second fluid passes is formed therein. The material of the fixing member (130) is known in the art, and a detailed description thereof is omitted herein.
[0086]
[0087] Hereinafter, an embodiment of the present invention will be described through examples and comparative examples, and the scope of the present invention is not intended to be limited to the examples.
[0088]
[0089] (Example)
[0090] Example 1
[0091] A dope stock solution was prepared by mixing 20 wt% of polystyrene (PS), 6 wt% of polyvinylpyrrolidone (PVP), and 32 wt% of antioxidant Ce(NO3) in 72 wt% of solvent N-methylpyrrolidone (NMP), and a core solution was prepared by mixing N-methylpyrrolidone (NMP) and ethanol in a volume ratio of 6:4. The dope stock solution was discharged through the outer tube of a double tubular nozzle, and the core solution was discharged through the inner tube, thereby immersing the radiant material in a coagulation tank containing a coagulation solution. The radiant material was formed into a hollow fiber membrane by contact with the coagulation solution in the coagulation tank. At this time, the coagulation solution used was water and PEG in a ratio of 1:1 (v / v), and the temperature was adjusted to 40°C. The hollow fiber membrane passing through the coagulation tank was washed with water at 40°C in a washing tank and then dried to obtain a hollow membrane. At this time, the thickness of the hollow fiber membrane was 100 μm.
[0092] The antioxidant used in Example 1 was Ce(NO3)3, but when other antioxidants such as Ethylene bis (oxyethylene) bis[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate] or Benzenamine were used, similar effects to Example 1 were confirmed.
[0093]
[0094] Example 2
[0095] A hollow fiber membrane was manufactured in the same manner as in Example 1, except that the content of the antioxidant was changed to 3 wt% and the solvent was changed to 71 wt%.
[0096]
[0097] Example 3
[0098] A hollow fiber membrane was manufactured in the same manner as in Example 1, except that the content of the antioxidant was changed to 5 wt% and the solvent was changed to 69 wt%.
[0099]
[0100] Example 4
[0101] A hollow fiber membrane was manufactured in the same manner as in Example 1, except that the content of the antioxidant was changed to 0.1 wt% and the solvent was changed to 73.9 wt%.
[0102]
[0103] Comparative Example 1
[0104] A hollow fiber membrane was manufactured in the same manner as in Example 1, except that the solvent was changed to 74 wt% without adding an antioxidant.
[0105]
[0106] Comparative Example 2
[0107] A hollow fiber membrane was manufactured in the same manner as in Example 1, except that the content of the antioxidant was changed to 6 wt% and the solvent was changed to 68 wt%.
[0108]
[0109] Evaluation Example 1: Evaluation of Deterioration / Decomposition of Humidifying Film
[0110] The humidifying films manufactured in Examples 1 to 4 and Comparative Examples 1 and 2 were immersed in Fenton reagent (3% H2O2, 1 ppm FeSO4) at 80°C for 24 hours, and then the molecular weight was analyzed to measure the change in molecular weight of the humidifying film after immersion compared to the humidifying film before immersion, and the results are shown in Table 1 below.
[0111]
[0112] Molecular weight reduction ratio Example 15% Example 23% Example 31% Example 410% Comparative example 130% Comparative example 21%
[0113] Molecular weight reduction ratio = [(initial humidifying film molecular weight - humidifying film molecular weight after immersion) / initial humidifying film molecular weight] x 100 As shown in Table 1 above, when Ce(NO3)3 was added as an antioxidant to the humidifying film composition, and when its content was increased, the effect of preventing deterioration and decomposition by peroxide and hydroxyl radicals was confirmed.
[0114]
[0115] Evaluation Example 2: Performance Evaluation of Humidifying Film
[0116] (Evaluation method)
[0117] Water vapor permeability: Water vapor permeability is measured by passing dry air through the cavity and moist air through the shell, and the amount of water vapor transferred to the dry air passing through the cavity. After making a sample for measuring water vapor permeability, connect it to the evaluation device and apply 70℃, 20 slpm, 0.1 barg to the dry air side and 75℃, 0.8 barg, and 20 slpm of dew point to the shell side, and measure the dew point of the part that escapes through the cavity to calculate the water vapor permeability.
[0118] Tensile strength: Tensile strength is measured using a general UTM (universal testing machine), holding the moisture barrier with both ends of the grip and pulling it at a speed of 50 mm / min to measure the strength at the moment of breaking.
[0119] Nitrogen permeability: Nitrogen permeability is measured using a CFP device. Nitrogen at 0.5 bar pressure is blown into one cavity while the other cavity is sealed with polyurethane. The flow rate of nitrogen flowing out toward the shell is measured.
[0120] Oxygen permeability: Evaluated in the same way as the nitrogen permeability above, only the gas used is converted to air.
[0121]
[0122] The water vapor permeability, tensile strength, nitrogen permeability, and oxygen permeability of the hollow fiber membranes manufactured in Examples 1 to 4 and Comparative Examples 1 and 2 were measured using the aforementioned method to confirm whether they had properties applicable to a fuel cell humidifier. The results are shown in Fig. 2 below.
[0123] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Water vapor permeability (g / s.m2) 0.18 0.18 0.17 0.18 0.18 0.09 Tensile strength (g / fiber) 396 396 395 398 400 346 Nitrogen permeability (cc / min.cm2) 5 15 45 35 15 231 Oxygen permeability (cc / min.cm2) 5 15 45 35 15 231
[0124] The hollow fiber membranes to which the antioxidants of Examples 1 to 4 were applied exhibited water vapor permeability similar to that of Comparative Example 1 to which no antioxidant was applied, which confirmed that the antioxidant dispersed within the polymer did not significantly affect the formation and porosity of the hollow fiber membrane and that it is suitable for use in a membrane humidifier for a fuel cell.
[0125] However, when the antioxidant was added in an amount exceeding 5 wt% to 6 wt% as in Comparative Example 2, the porous structure of the polymer was not sufficiently formed during the hollow fiber membrane formation process, so the water vapor permeability decreased to less than 0.1, making it unsuitable for use as a membrane humidifier hollow fiber membrane. That is, the hollow fiber membrane of Comparative Example 2 showed a water vapor permeability that was not suitable for use in a membrane humidifier for a fuel cell. In addition, in Comparative Example 2, the nitrogen and oxygen permeabilities were also reduced, and it is thought that this is because the porous structure of the polymer was not sufficiently formed due to the excessive presence of the antioxidant in the polymer.
[0126] Based on these results, when an antioxidant is used in an amount of 0.01 to 5 parts by weight, it can be used as a hollow fiber membrane for use in a fuel cell humidifier while preventing deterioration of the hollow fiber membrane from oxidizing substances.
Claims
1. A hollow fiber membrane for a humidifier, comprising a polymer and an antioxidant, and containing 0.01 to 5 parts by weight of an antioxidant per 100 parts by weight of the hollow fiber membrane.
2. In paragraph 1, A hollow fiber membrane for a humidifier, wherein the above antioxidant is dispersed in a polymer.
3. In paragraph 1, A hollow fiber membrane for a humidifier, wherein at least a portion of the above antioxidant is exposed on the surface of the polymer.
4. In paragraph 1, A hollow fiber membrane for a humidifier, wherein the concentration of an antioxidant increases from the inner surface to the outer surface of the hollow fiber membrane.
5. In paragraph 1, A hollow fiber membrane for a humidifier, wherein the antioxidant comprises an organic antioxidant, a metal antioxidant, an organo-metallic antioxidant, a HALS (hindered amine light) antioxidant, a sulfur antioxidant, a phosphorus antioxidant, or a combination thereof.
6. In paragraph 5, A hollow fiber membrane for a humidifier, wherein the antioxidant comprises a metal-based antioxidant.
7. In paragraph 1, A hollow fiber membrane for a humidifier, comprising 0.1 to 5 parts by weight of the above antioxidant.
8. In paragraph 1, A hollow fiber membrane for a humidifier, wherein the polymer comprises a polyvinylidene fluoride (PVDF) polymer, a polysulfone polymer, a sulfonated polysulfone, cellulose acetate, cellulose triacetate, polymethyl methacrylate, Nafion, a polystyrene (PS) polymer, a polytetrafluoroethylene (PTFE) polymer, a perfluorosulfonic acid (PFSA) polymer, a polyphenylsulfone polymer, a polyethersulfone (PES) polymer, a polyacrylonitrile (PAN) polymer, a polyetherimide (PEI) polymer, a polyimide (PI) polymer, or a combination thereof.
9. In paragraph 8, The above polymer is a hollow fiber membrane for a humidifier, comprising a polystyrene-based polymer.
10. In paragraph 1, A hollow fiber membrane for a humidifier, wherein the polymer is included in an amount of 10 to 35 parts by weight per 100 parts by weight of the dope concentrate.
11. In paragraph 1, A hollow fiber membrane for a humidifier, wherein the thickness of the hollow fiber membrane is 60 to 300 um.
12. In paragraph 1, The above hollow fiber membrane is a hollow fiber membrane for a humidifier, having a water vapor permeability of 0.1 g / s / m2 or more measured under conditions of 1 bar pressure and 80 ℃ temperature.
13. In paragraph 1, The above hollow fiber membrane has a nitrogen permeability of 100 cc / min / cm under a pressure condition of 0.5 bar. 2 Lee Ha-in, hollow fiber membrane for humidifier.
14. In paragraph 1, The above hollow fiber membrane has an oxygen permeability of 100 cc / min / cm under a pressure condition of 0.5 barg. 2 The following is a hollow fiber membrane for a humidifier.
15. A method for manufacturing a hollow fiber membrane for a humidifier, comprising: a step of obtaining a spinning solution by mixing an antioxidant in an amount of 0.01 to 5 parts by weight based on 100 parts by weight of the spinning solution; a step of spinning the spinning solution into a coagulation tank through a nozzle; and a step of coagulating the spinning solution in the coagulation tank.
16. In paragraph 15, The step of obtaining the above-mentioned radiation source includes a step of mixing the above-mentioned antioxidant and the above-mentioned polymer in a solvent, A method for manufacturing a hollow fiber membrane for a humidifier, wherein the solvent comprises at least two types of solvents among a first solvent, a second solvent, and a third solvent.
17. In paragraph 16, The first solvent comprises butanol, isobutanol, octanol, pentanol, isopentanol, dimethyl phthalate, diethyl phthalate, dibutyl phthalate, dioctyl phthalate, polyoxyethylene octylphenyl ether, or a combination thereof, The second solvent comprises water, methanol, ethanol, isopropanol, acetone, hexane, pentane, benzene, toluene, carbon tetrachloride, o-dichlorobenzene, polyethylene glycol, or a combination thereof, A method for producing a hollow fiber membrane for a humidifier, wherein the third solvent comprises N-methyl-2-pyrrolidone, dimethyl sulfoxide, dimethyl acetamide, dimethyl formamide, methyl ethyl ketone, tetrahydrofuran, tetramethyl urea, or trimethyl phosphate.
18. In paragraph 15, A method for manufacturing a hollow fiber membrane for a humidifier, further comprising a post-treatment step after the step of coagulating the above-mentioned radiation source.
19. In paragraph 18, A method for manufacturing a hollow fiber membrane for a humidifier, wherein the above post-treatment step includes chemical treatment and / or physical treatment.
20. A humidifier comprising a hollow fiber membrane for a humidifier according to any one of claims 1 to 14.
Citation Information
Patent Citations
Hollow fiber and humidifier for fuel battery
JP2007162176A
Humidifier for fuel cell, and fuel cell system
JP2007242523A
Porous membrane and its manufacturing method
JP2009142799A
Hollow fiber membrane for humidification, and hollow fiber membrane module for humidification using the same
JP2020151699A
Sorting apparatus for foreign material with air
KR102417994B1