Method for producing activated carbon with a high specific capacitance from raw materials of organic origin
Patent Information
- Application Number
- PCT/PL2023/050033
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-14
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
[0001] METHOD FOR PRODUCING ACTIVATED CARBON WITH A HIGH SPECIFIC CAPACITANCE FROM RAW MATERIALS OF ORGANIC ORIGIN
[0002] Field of the invention
[0003] The invention relates to a method for producing active carbon with a high porosity and specific capacitance from materials of organic origin, for use in supercapacitors, devices that smooth out voltage collapses and peak overloads of low- and high-power power grids, and in powerenhancing components for solar cells and chemical power sources.
[0004] State of the art
[0005] Supercapacitors are devices with a large electrical capacity, far exceeding the capacity of ordinary capacitors. A supercapacitor contains two porous electrodes, an electrolyte and a separator. Its special properties are achieved through the use of active carbon structures, which are the main building blocks of the electrodes in the capacitor. The properties of a supercapacitor are therefore dependent on the properties of the electrodes used, and in particular on the specific carbon structures. A key factor to achieve the best possible parameters for capacitor capacitance is to obtain carbon structures with optimum porosity and the right surface chemistry, which are influenced by the type of raw material and the preparation conditions. Carbon structures are obtained from various carbon-containing source materials, such as, e.g., bamboo, coconutshells, willow peat, wood, coconut fibre, lignite and petroleum tar. Methods for obtaining active carbon structures for use in supercapacitors are known in the art.
[0006] One of these is a method for the pyrolytic formation of carbon nanostructures for use in supercapacitors, described in CN103539118B. The method relates to the preparation of active carbon, involving pre-treatment of the rice husk raw material, charring, pre-treatment of the charred material, activation and post treatment. Pre-treatment of the raw material includes treatment with alkaline reagents, mixed reagents and pre-treatment by water infiltration. The sources of rice husk raw material used are large, which helps to reduce costs. Carbon obtained by this method has potential for use as an electrode material in super capacitors.
[0007] In addition, CN102826549A describes a method for preparing active carbon for use in supercapacitors, involving the following steps: crushing of petroleum coke, milling, screening and carbonisation of the coke under a nitrogen atmosphere, treatment of the carbonised petroleum coke with HNO3 solution at 30-50°C for 4h, filtering and washing until neutralised, drying at 50°C, expanding at 130-160°C, mixing the expanded petroleum coke with KOH in a weight ratio of 1:3, activating the coke by heating its mixture with KOH at 800-850°C under a nitrogen atmosphere for 2-3 hours, boiling the product in an aqueous HC1 solution for 5 minutes, washing with deionised water until neutralised, thus obtaining activated carbon. This treatment allows the distance between layers of petroleum coke graphite microcrystals to be increased and the thickness of these microcrystals to be reduced, which facilitates the activation of petroleum coke and improves such properties of activated carbon as specific surface area and specific volume.
[0008] EP3445712B1 discloses the production of active carbons characterised by a BET specific surface area between 1000 m2 / g and 3500 m2 / g, with the described method comprising the following steps: mixing the carbon precursor with a first component containing one salt (potassium carbonate, potassium bicarbonate or potassium chloride) and one or more other components containing at least one second salt, which is phosphate; preheating the said mixture to a first temperature of 150°C to 600°C and soaking for 10 min to 10 h in an inert medium, and activating the said mixture in an inert medium by increasing the temperature to a second, higher temperature of 600°C to 1000°C and soaking for 10 min to 20 h. The method is carried out without using any strong acids or bases. Petroleum tar, coconut shell powder, brown coal, municipal waste, industrial by-products, asphaltenes, biowaste, organic waste, biomass, agricultural waste, wood by-products, fruit shells, nut shells, carbon fibres, synthetic polymers, carbohydrates, resins, and combinations of these can be used as carbon precursors in the method.
[0009] KR101982987B1 describes a method for producing active carbon for high-power energy storage, including: a step of impregnating and pulverising cellulose-based biomass; a step of loading the impregnated and pulverised biomass into an oven; a step of activating the biomass; a step of cooling the activated biomass; and a step of cleaning the cooled biomass with a cleaning solution to produce active carbon, with either active gas or inert gas being supplied to the oven.
[0010] However, there is a continuing need to provide a method for obtaining carbon structures for use as electrode materials in supercapacitors, which structures would be characterised by increased values of specific capacitance. There is also a need to develop methods for obtaining such materials with the use of renewable raw materials, especially cheap organic waste. Summary of the invention
[0011] The objective of the present invention was to provide a method for obtaining carbon structures for use as electrode materials in supercapacitors, that allows improved specific capacitance values to be obtained in supercapacitors built with these structures. Unexpectedly, it turned out that the combination of a cheap organic raw material, a sequence of steps and process parameters set out below allowed this objective to be met.
[0012] In its first aspect, the present invention relates to a method for producing active carbon with a high specific capacitance from raw materials of organic origin, comprising the following steps: a) preparing an organic raw material, b) burning the organic raw material, b) treating the biochar with an alkaline reagent solution and drying the biochar, d) activating the biochar; e) purifying the biochar.
[0013] In the method according to the invention, the organic raw material is selected from maize stalks and cereal straw, preferably wheat straw, or mixtures thereof. In step a), the processed organic material is separated from other waste and subjected to fragmentation, preferably in a crushing- milling-sifting sequence. In step b), the organic raw material is subjected to carbonisation at a temperature of 350 to 550°C, preferably 400°C fora period of 1 to 3 h, preferably 1.5 h. In step c), a solution of alkaline reagent at a mass concentration of 25 to 35%, preferably 30%, is used, which is mixed with the biochar over a period of 22 to 26 h, preferably 24 h, in a ratio of biochar : alkaline reagent of 1 :2.5 to 1 :3.5, preferably 1:3. In step d), additional activation of the biochar is carried out by supplying the reaction medium with an aqueous aerosol in a shielding gas. Preferably, argon is used as the shielding gas. Preferably, the pressure in step a) is IkPa.
[0014] Preferably, in step b), the gaseous products are removed by a stream of shielding gas delivered at a rate of 2-5 1 / min.
[0015] Preferably, in step d), the biochar is dried at a temperature of 100-110°C. Preferably in step d), the activation of the biochar is carried out at a temperature of 700°C for 90 minutes in the flowing shielding gas at a pressure of 1 kPa with simultaneous removal of the gaseous reaction products by a stream of shielding gas delivered at a rate of 1-2 1 / min.
[0016] Preferably in step d), the aerosol used in the additional activation contains droplets of 5-20 pm.
[0017] Preferably in step e), the biochar is washed with water until the pH of the washing water reaches a value below 8.5-9 and then dried at a temperature of 100-110°C.
[0018] In its second aspect, the present invention relates to the use of active carbon obtained by the method according to the invention defined above as an electrode material in supercapacitors.
[0019] Advantages of the invention
[0020] The method for producing active carbon according to the invention leads to an optimum carbon structure with pores adapted to the electrolytes used in supercapacitors and to the energy topology of defects in the solid. The highly porous active carbon thus formed provides a high specific capacitance value of more than 220 F / g which ultimately increases the energy density of the supercapacitor. Specific capacitance measured by galvanostatic charging and discharging method.
[0021] Detailed description of the invention
[0022] Below, in the description of the present invention, the following terminology is adopted:
[0023] In the context of the present invention, the term "organic raw material" means maize stalks, cereal straw, preferably wheat straw, or mixtures thereof. These materials belong to organic waste. The term "raw material" is used interchangeably in this description.
[0024] In the context of the present invention, the term "biochar" means the residue after carbonisation of an organic raw material, while the term "carbonisation" means a thermal process leading to an increase in the carbon content of the processed raw material.
[0025] In the context of the present invention, the term "shielding gas" means an inert gas, in particular a noble gas, with which the reactor volume is filled. "Reactor" in the context of the present invention means any process apparatus capable of maintaining stable reaction conditions, including in particular pressure and temperature. As indicated above, the object of the invention is a method for producing active carbon with a high specific capacitance.
[0026] The method is adapted to the processing of raw materials of organic origin, including in particular organic waste, especially maize stalks or cereal straw, especially wheat straw.
[0027] The method for producing active carbon according to the invention comprises five steps, which will be described in detail below.
[0028] The first step is the preparation of the raw materials. The raw material of organic origin used, selected from maize stalks and cereal straw, preferably wheat straw, or mixtures thereof, is separated from other waste materials and crushed to an average size of about 10-20 mm, and then subjected to milling and sifting.
[0029] The second step is the burning of the organic raw material. For this purpose, the crushed raw material is placed in the thermal reactor, and then a vacuum is created and shielding gases are fed. Any inert gas, in particular a noble gas, and preferably argon, can be used as a shielding gas. The shielding gas fills the reactor volume and is then pressurised to a value of 0.5 to 2 kPa above atmospheric pressure. The contents of the reactor are subjected to carbonisation at a temperature in the range of 300-500°C, preferably at 400°C for 1-3 h, preferably for 90 minutes.
[0030] Gaseous reaction products should be removed when carrying out this step. They are removed by a stream of shielding gas, preferably argon, flowing through the reactor. Preferably, there is an excess of shielding gas maintained in the reactor at about 1 kPa above atmospheric pressure. Once carbonisation is complete, the oven cools spontaneously.
[0031] In the third step, after cooling, the biochar is withdrawn from the reactor and mixed with an alkaline reagent solution having a mass concentration of 25 to 35%, preferably 30%. The solution is added to the biochar, respecting a mass ratio of biochar : alkaline reagent of 1:2.5 to 1:3.5, preferably 1:3. The treatment of the biochar with the alkaline reagent solution with simultaneous stirring is carried out over a period of 22 to 26 h, preferably 24 h. Any substance of an alkaline nature, preferably an alkali metal or alkaline earth metal hydroxide, e.g. potassium hydroxide (KOH), can be used as the alkaline reagent. After this period, the biochar together with the remaining solution is placed back in the oven and dried at a temperature higher than room temperature, preferably in the range of 100-110°C. In the fourth step, the dried biochar is placed in the thermal reactor, where its activation is carried out at a temperature of 600 to 800°C, preferably 700°C for a period of 75 to 105 minutes, preferably 90 minutes, in the flowing shielding gas. During the activation of the biochar, the gaseous products are removed along with the fed stream of shielding gas that flows through the reactor. In this step, an additional activation of the biochar is also carried out by delivering an aqueous aerosol with a water droplet size of 5-20 pm into the shielding gas atmosphere, directly from an ultrasonic aerosol generator to the reactor. At the end of this step, the reactor contents are spontaneously cooled.
[0032] In the fifth step, the activated carbon is washed with water to remove the alkaline reagent. Rinsing is carried out until the rinse water reaches a pH value of less than 8.5-9. The carbon is then dried at a temperature in the range of 100-110°C.
[0033] Exemplary embodiment
[0034] The method for producing active carbon was carried out as follows:
[0035] 1) Wheat straw was separated from other waste and crushed to an average size of about 10-20 mm. The milling was carried out using a mechanical mill and the milling product was sifted through a sieve.
[0036] 2) The crushed raw material was placed in the thermal reactor for burning. A vacuum was created in the reactor and the shielding gas, argon, was introduced. The reactor volume was filled with argon to equalize the pressure, and then the pressure was increased to a level of about 1 kPa above atmospheric pressure. Carbonisation of the raw material in such a protective atmosphere was carried out at a temperature of 400°C for 90 minutes. The gaseous reaction products were removed by a stream of argon, which was delivered at a rate of 2-5 1 / min, through a hydrovalve in a controlled manner. The excess pressure of argon was maintained in the reactor at a level of about 1 kPa. Once this step was completed, the reactor was switched off and cooled spontaneously.
[0037] 3) After cooling to room temperature, the biochar was withdrawn from the reactor and placed in a KOH solution with a mass concentration of 30% while maintaining a mass ratio of biochar : KOH = 1:3. The biochar was then kept in the KOH solution for 24 hours with simultaneous stirring. After this period, the biochar together with the remaining solution was moved to the oven and dried at a constant temperature in the range of 100-110°C. 4) In the next step, the dried biochar was placed in the thermal reactor, where its activation was carried out at a constant temperature of 700°C for 90 minutes in the flowing argon. The gaseous reaction products were removed with a stream of argon gas through the hydrovalve, in a controlled manner, at a flow rate of 1-2 1 / min. The excess pressure of argon was maintained in the reactor at a level of about 1 kPa. An additional activation was carried out by delivering an aqueous aerosol into the argon atmosphere, directly from an ultrasonic aerosol generator to the reactor. The size of water droplets is 5-20 pm, the efficiency of the generator is 3.0±0.5 cm3 / min., the frequency of the ultrasound emitter is 2.64 MHz. Once this step was completed, the oven was switched off and cooled spontaneously. The additional activation of the biochar increases the value of the specific capacitance of the biochar by about 100% compared to the biochar obtained without this step.
[0038] 5) After the oven had cooled to room temperature, the activated carbon was withdrawn from the reactor and washed with water to remove traces of the activator (KOH). At the end of the washing process, the pH of the rinse water was below 8.5. The carbon was then dried in the oven at a temperature in the range of 100-110°C until a constant mass was obtained.
[0039] After the activation process, the dried carbon exhibited a specific surface area of more than 1200 m2, a total pore volume of 0.8-0.85 cm3g-1, a micro pore volume of 0.6-0.65 cm3g-1and an average pore diameter of 2.3-2.5 nm. These data were obtained using BET analysis of nitrogen adsorption isotherms, which were obtained with a Nova Touch LX2 porometer.
Claims
Claims1. A method for producing active carbon with a high specific capacitance from raw materials of organic origin, comprising the following steps: a) preparing an organic raw material, b) burning the organic raw material, b) treating the biochar with an alkaline reagent solution and drying the biochar, d) activating the biochar; e) purifying the biochar, characterised in that the organic raw material is selected from maize stalks and cereal straw, preferably wheat straw, or mixtures thereof, wherein in step a), the processed organic material is separated from other waste and subjected to fragmentation, preferably in a crushing-milling-sifting sequence; wherein in step b), the organic raw material is subjected to carbonisation at a temperature of 350 to 550°C for a period of 1 to 3 h, wherein in step c), a solution of alkaline reagent at a mass concentration of 25 to 35% is used, which is mixed with the biochar over a period of 22 to 26 h in a ratio of biochar : alkaline reagent of 1:2.5 to 1 :3.5, wherein in step d), additional activation of the biochar is carried out by supplying the reaction medium with an aqueous aerosol in a shielding gas.2 The method according to claim 1, wherein argon is used as the shielding gas.3 The method according to claim 1 or 2, wherein the pressure in step a) is IkPa.4 The method according to one of claims 1-3, wherein in step b), the gaseous products are removed by a stream of shielding gas delivered at a rate of 2-5 1 / min.5 The method according to one of claims 1-4, wherein in step d), the biochar is dried at a temperature of 100-110°C.The method according to one of claims 1-5, wherein in step d), the activation of the biochar is carried out at a temperature of 700°C for 90 minutes in the flowing shielding gas at a pressure of 1 kPa with simultaneous removal of the gaseous reaction products by a stream of shielding gas delivered at a rate of 1-2 1 / min. The method according to one of claims 1-6, wherein in step d), the aerosol used in the additional activation contains droplets of 5-20 pm. The method according to one of claims 1-6, wherein in step e), the biochar is washed with water until the pH of the washing water reaches a value below 8.5-9 and then dried at a temperature of 100-110°C. Use of active carbon obtained by the method according to one of claims 1-8 as an electrode material in super capacitors.