Chemicals column coating agent for aerosol fire extinguishant, and coating method

By using silicone oil, inorganic flame retardant and platinum catalyst coating agent, the problems of aerosol fire extinguishing agent columns are easily fired, explosive and easy to damage, improving earthquake resistance and stability, ensuring orderly combustion and reducing It is a safety hazard and is suitable for the column coating method of aerosol fire extinguishing agent.

WO2024234426A1PCT designated stage expired Publication Date: 2024-11-21HUBEI JIANDUN FIRE TECH CO LTD

Patent Information

Application Number
PCT/CN2023/098888
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2023-06-07
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

The aerosol fire extinguishing agent column is prone to fire and explosive ignition, and is easily damaged during storage and transportation, affecting the fire extinguishing effect and safety. The prior art cannot effectively solve these problems by improving the structure of the fire extinguishing device.

Method used

A multifunctional coating agent composed of silicone oil, inorganic flame retardant and platinum catalyst is used to improve the shock resistance and stability of the drug column through the coating method, avoid fire and explosion, and reduce safety hazards caused by high temperatures.

Benefits of technology

It effectively improves the earthquake resistance and stability of the medicine column, ensures orderly combustion, reduces safety hazards caused by fire jumps and explosions, and reduces the heat insulation requirements for fire extinguishing devices, and improves the fire extinguishing effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023098888_21112024_PF_FP_ABST
    Figure CN2023098888_21112024_PF_FP_ABST
Patent Text Reader

Abstract

A chemicals column coating agent for an aerosol fire extinguishant, and a coating method. The chemicals column coating agent is prepared by mixing high-temperature-resistant silicone oil, an inorganic flame retardant, and a platinum-containing catalyst. The surface of a chemicals column of the aerosol fire extinguishant is tightly coated with the chemicals column coating agent, so that the shock resistance of the chemicals column is enhanced, and the damage rate caused by storage and transportation is reduced. Moreover, the chemicals column coating agent can also block combustion heat, reduce the risks of flame spurting and deflagration of the chemicals column, reduce the heat insulation requirement for a fire extinguishing apparatus, and improve the safety of operators. Additionally, the ordered combustion of the chemicals column can be guaranteed, fire extinguishing aerosol is continuously generated for fire extinguishing, explosion accidents caused by pressure as a result of the fire extinguishing apparatus failing to resist a large amount of gas generated by deflagration are avoided, and the fire extinguishing safety is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Aerosol fire extinguishing agent powder coating agent and coating method Technical Field

[0001] The invention belongs to the technical field of aerosol fire extinguishing agent packaging materials, and particularly relates to a powder column coating agent and a coating method for an aerosol fire extinguishing agent. Background Art

[0002] Thermal aerosol fire extinguishing agents are pyrotechnic agents composed of an oxidizing agent, a reducing agent, and a binder. The combustion reaction that occurs when releasing the thermal aerosol fire extinguishing agent is highly exothermic and gas-generating, with combustion temperatures exceeding 1000°C. It also produces large amounts of gases such as N2, CO2, and water vapor. Therefore, fire extinguishing equipment must not only have excellent thermal insulation properties but also withstand a certain level of pressure. However, once the aerosol fire extinguishing agent charge ignites, the fire will quickly spread to the charge surface, causing flashover and deflagration. This generates a large amount of heat and gas in a short period of time, rapidly increasing the temperature on the charge surface and within the device, which can easily cause burns or scalds. The large amount of gas produced in a short period of time also poses the risk of device explosion, seriously compromising the safety of the fire extinguishing device.

[0003] Based on the above technical problems, two strategies are generally adopted at present. One is to put a coolant inside the device to absorb the heat of combustion, and the other is to set a heat insulation layer inside the device to improve the heat resistance of the device. For example, Chinese patent CN107998560A discloses a handheld fire extinguisher and a fire extinguishing method. By setting a rubber sheath in the fire extinguisher and filling a coolant in the sleeve, the risk of burns caused by heat is avoided. At the same time, the coolant is used to cover the powder column to ensure that the aerosol spraying temperature is low. Chinese patent CN202366360U discloses a hot aerosol fire extinguishing device, which reduces the temperature of the device by setting an insulation tube inside the device, wherein the insulation tube includes an insulation block, a cooling material layer, a lower insulation block, and a coolant layer. Chinese patent CN2519680Y discloses an aerosol fire extinguishing and fire-blocking cooling device, in which the heat-reduction block inside the box cools the high-temperature aerosol, thereby reducing the safety hazards caused by high temperature.

[0004] While improvements to fire extinguishing devices can reduce device temperatures and prevent burns to operators, they do not address the inherent flammability and deflagration characteristics of the aerosol. Furthermore, prolonged vibration during storage and transportation of the aerosol, or after loading into the fire extinguishing device, can damage the aerosol, compromising the safety and stability of the aerosol fire extinguishing agent and severely impacting the fire extinguishing effect. Therefore, improvements to the fire extinguishing device structure alone cannot address the safety, stability, shock resistance, and thermal insulation issues of aerosol fire extinguishing agents.

[0005] Summary of the Invention

[0006] In response to the above technical problems, the present invention provides a coating agent and coating method for aerosol fire extinguishing agent powder column. By preparing a multifunctional coating agent, the shock resistance and stability of the aerosol fire extinguishing agent powder column are improved. At the same time, the powder column is ensured to burn in an orderly manner during spraying, avoiding the occurrence of fire and deflagration. At the same time, the coating agent also has a certain heat insulation effect, which reduces the requirements for heat insulation of the fire extinguishing device and reduces the safety hazards caused by high temperature.

[0007] In order to achieve the above object, the present invention provides a powder column coating agent suitable for an aerosol fire extinguishing agent, which is composed of 80-95 parts of silicone oil, 10-40 parts of an inorganic flame retardant and 0.1-0.5 parts of a catalyst.

[0008] Preferably, the silicone oil is any one of vinyl-terminated silicone oil, methyl silicone oil, ethyl silicone oil, phenyl silicone oil, methyl hydrogen silicone oil, methylphenyl silicone oil, methylchlorophenyl silicone oil, methylethoxy silicone oil, methyltrifluoropropyl silicone oil, methylvinyl silicone oil, methylhydroxy silicone oil, ethyl hydrogen silicone oil or hydroxy hydrogen silicone oil.

[0009] Preferably, the inorganic flame retardant is any one of Al(OH)3, Mg(OH)2, Zn(OH)2, Fe(OH)3, Cu(OH)2, MgCO3, CaCO3 or ammonium polyphosphate.

[0010] Preferably, the catalyst is any one of chloroplatinic acid, potassium chloroplatinate or platinum acetylacetonate.

[0011] Preferably, the catalyst is prepared into an ethanol solution before use, wherein the mass fraction of platinum in the catalyst ethanol solution is 0.1%.

[0012] The present invention also provides a method for coating an aerosol fire extinguishing agent charge with a coating agent, which specifically comprises the following steps:

[0013] (1) Weighing an appropriate amount of catalyst and dissolving it in anhydrous ethanol to prepare a catalyst solution with a platinum mass fraction of 0.1%;

[0014] (2) Weighing silicone oil and inorganic flame retardant, adding them to the catalyst solution, and stirring evenly to obtain a coating agent liquid;

[0015] (3) Fix the formed pellets on a custom mold coated with a release agent and fix the coated paper tube on the base;

[0016] (4) Add coating agent liquid to the coating paper tube, solidify and shape it at room temperature, and then remove the customized mold to complete the coating of the drug column.

[0017] Preferably, the customized mold described in step (3) and step (4) is composed of a base (1), a paper tube fixing seat (2) and a medicine column supporting seat (3) stacked in sequence and fixedly connected.

[0018] Preferably, the release agent in step (3) is vaseline.

[0019] Preferably, the mass ratio of the drug column and the coating agent in step (4) is 1:1.

[0020] The beneficial effects of the present invention are as follows: a powder column coating agent suitable for hot aerosol fire extinguishing agents is prepared by using silicone oil, an inorganic flame retardant and a platinum-containing catalyst, which can coat the powder column in multiple aspects, thereby improving the shock resistance of the powder column, reducing the sensitivity of the powder column to vibration during storage and transportation alone or after being loaded into a fire extinguishing device for storage and transportation, reducing the incidence of breakage, and thus ensuring the fire extinguishing effect.

[0021] The present invention selects high-temperature resistant silicone oil as raw material and adds an inorganic flame retardant, so that the prepared powder column coating agent can withstand the high temperature generated when the aerosol fire extinguishing agent burns, plays a heat insulating role, reduces the heat insulation requirements for the fire extinguishing device, thereby reducing the difficulty of the preparation process of the fire extinguishing device and enabling it to be widely promoted.

[0022] The powder column coating agent is tightly wrapped on the surface of the powder column, and inorganic flame retardants are added thereto. This can prevent the disorderly movement of the flame, make the powder column burn in an orderly manner, avoid the occurrence of fire and deflagration, thereby ensuring that the aerosol fire extinguishing agent produces fire extinguishing gas in an orderly manner for continuous fire extinguishing, avoid pulse combustion that brings greater pressure to the fire extinguishing device, and reduce safety hazards such as explosion of the fire extinguishing device. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is a schematic diagram of the structure of the customized mold.

[0024] FIG2 is a schematic diagram of the coating of the drug column according to the present invention.

[0025] In the figure, 1 is the base, 2 is the paper tube fixing seat, 3 is the medicine column support seat, 4 is the coating paper tube, 5 is the coating agent, and 6 is the medicine column. DETAILED DESCRIPTION

[0026] The technical solutions of the present invention are further explained below with reference to the accompanying drawings and specific embodiments. It is worth noting that the following embodiments are only preferred embodiments of the present invention and should not be construed as limiting the present invention. The scope of protection of the present invention shall be determined by the claims. Any modifications or substitutions made to the technical solutions of the present invention by those skilled in the art without creative effort shall fall within the scope of protection of the present invention.

[0027] The following examples use a K-type aerosol fire extinguishing agent, the diameter of the powder column is 32 mm, and the mass is 50 g.

[0028] Example 1

[0029] For an aerosol fire extinguishing agent charge with a diameter of 32 mm and a mass of 50 g, a custom mold as shown in Figure 1 is designed. The top of the base 1 is fixedly connected to the paper tube fixing seat 2, and a charge support seat is fixed to the top of the paper tube fixing seat 2. The cross-sections of the paper tube fixing seat 2 and the charge support seat 3 are both trapezoidal, and the top cross-sectional diameter of the charge support seat 3 is slightly smaller than the diameter of the charge.

[0030] During use, vaseline is applied to the contact surface of the custom mold with the coating agent. The object is then demolded later. The drug column is then placed on the drug column support 3 and the coating paper tube 4 is placed on the paper tube holder 2. During installation, care is taken to fit the coating paper tube to the lowest end of the paper tube holder 2 to secure the coating paper tube. This allows the coating agent to be contained and maintain its shape during solidification. In the embodiment shown, the base 1 has a diameter of 50 mm and a height of 20 mm; the paper tube holder 2 has a diameter of 40 mm and a height of 10 mm; and the drug column support 3 has a diameter of 32 mm and a height of 35 mm.

[0031] Example 2

[0032] (1) Weigh chloroplatinic acid and dissolve it in anhydrous ethanol to prepare a chloroplatinic acid ethanol solution with a platinum mass fraction of 0.1%;

[0033] (2) Weigh 80 parts of ethyl-terminated silicone oil, 19.8 parts of Al(OH)3, and 0.2 parts of chloroplatinic acid ethanol solution, mix and stir evenly to obtain a coating agent liquid;

[0034] (3) Apply a layer of vaseline on the surfaces of the custom mold that are in contact with the coating agent, and place the aerosol fire extinguishing agent column 6 on the column support seat 3 of the custom mold, and then put the coating paper tube 4 on the paper tube fixing seat 2. When putting the tube, be sure to put the paper tube to the bottom end of the paper tube fixing seat 2;

[0035] (4) Pour the coating liquid obtained in step (2) into the paper tube, and place the cast mold and the drug column at room temperature to solidify for more than 12 hours until the coating is completely solidified (Figure 2). Remove the customized mold and complete the coating.

[0036] Example 3

[0037] (1) Weigh potassium chloroplatinate and dissolve it in anhydrous ethanol to prepare a potassium chloroplatinate ethanol solution with a platinum mass fraction of 0.1%;

[0038] (2) Weigh 80 parts of methyl silicone oil, 19.8 parts of Mg(OH)2, and 0.2 parts of potassium chloroplatinate ethanol solution, mix and stir evenly to obtain a coating agent liquid;

[0039] (3) Coating was performed according to the method and steps described in Example 2.

[0040] Example 4

[0041] (1) Weighing platinum acetylacetonate, dissolving it in anhydrous ethanol to prepare a platinum acetylacetonate ethanol solution with a mass fraction of platinum of 0.1%;

[0042] (2) Weigh 80 parts of vinyl silicone oil, 19.8 parts of Zn(OH)2, and 0.2 parts of acetylacetonate platinum ethanol solution, mix and stir evenly to obtain a coating agent liquid;

[0043] (3) Coating was performed according to the method and steps described in Example 2.

[0044] Example 5

[0045] (1) Weigh chloroplatinic acid and dissolve it in anhydrous ethanol to prepare a chloroplatinic acid ethanol solution with a platinum mass fraction of 0.1%;

[0046] (2) Weigh 80 parts of phenyl silicone oil, 19.8 parts of Fe(OH)3, and 0.2 parts of chloroplatinic acid ethanol solution, mix and stir evenly to obtain a coating agent liquid;

[0047] (3) Coating was performed according to the method and steps described in Example 2.

[0048] Example 6

[0049] (1) Weigh potassium chloroplatinate and dissolve it in anhydrous ethanol to prepare a potassium chloroplatinate ethanol solution with a platinum mass fraction of 0.1%;

[0050] (2) Weigh 80 parts of methyl hydrogen silicone oil, 19.8 parts of Cu(OH)2, and 0.2 parts of potassium chloroplatinate ethanol solution, mix and stir evenly to obtain a coating agent liquid;

[0051] (3) Coating was performed according to the method and steps described in Example 2.

[0052] Example 7

[0053] (1) Weighing platinum acetylacetonate, dissolving it in anhydrous ethanol to prepare a platinum acetylacetonate ethanol solution with a mass fraction of platinum of 0.1%;

[0054] (2) Weigh 80 parts of methylphenyl silicone oil, 19.8 parts of MgCO3, and 0.2 parts of acetylacetonate platinum ethanol solution, mix and stir evenly to obtain a coating agent liquid;

[0055] (3) Coating was performed according to the method and steps described in Example 2.

[0056] Example 8

[0057] (1) Weigh chloroplatinic acid and dissolve it in anhydrous ethanol to prepare a chloroplatinic acid ethanol solution with a platinum mass fraction of 0.1%;

[0058] (2) Weigh 80 parts of methylchlorophenyl silicone oil, 19.8 parts of CaCO3, and 0.2 parts of chloroplatinic acid ethanol solution, mix and stir evenly to obtain a coating agent liquid;

[0059] (3) Coating was performed according to the method and steps described in Example 2.

[0060] Example 9

[0061] (1) Weighing platinum acetylacetonate, dissolving it in anhydrous ethanol to prepare a platinum acetylacetonate ethanol solution with a mass fraction of platinum of 0.1%;

[0062] (2) Weigh 80 parts of methyl trifluoropropyl silicone oil, 19.8 parts of ammonium polyphosphate, and 0.2 parts of acetylacetonate platinum ethanol solution, mix and stir evenly to obtain a coating agent liquid;

[0063] (3) Coating was performed according to the method and steps described in Example 2.

[0064] Example 10

[0065] (1) Weigh chloroplatinic acid and dissolve it in anhydrous ethanol to prepare a chloroplatinic acid ethanol solution with a platinum mass fraction of 0.1%;

[0066] (2) Weigh 85 parts of methyl vinyl silicone oil, 14.9 parts of Zn(OH)2, and 0.1 parts of chloroplatinic acid ethanol solution, mix and stir evenly to obtain a coating agent liquid;

[0067] (3) Coating was performed according to the method and steps described in Example 2.

[0068] Example 11

[0069] (1) Weigh potassium chloroplatinate and dissolve it in anhydrous ethanol to prepare a potassium chloroplatinate ethanol solution with a platinum mass fraction of 0.1%;

[0070] (2) Weigh 90 parts of methylhydroxy silicone oil, 9.7 parts of Fe(OH)3, and 0.3 parts of potassium chloroplatinate ethanol solution, mix and stir evenly to obtain a coating agent liquid;

[0071] (3) Coating was performed according to the method and steps described in Example 2.

[0072] Example 12

[0073] (1) Weighing platinum acetylacetonate, dissolving it in anhydrous ethanol to prepare a platinum acetylacetonate ethanol solution with a mass fraction of platinum of 0.1%;

[0074] (2) Weigh 95 parts of methylethoxy silicone oil, 4.5 parts of Fe(OH)3, and 0.5 parts of acetylacetonate platinum ethanol solution, mix and stir evenly to obtain a coating agent liquid;

[0075] (3) Coating was performed according to the method and steps described in Example 2.

[0076] Comparative Example 1

[0077] A layer of aluminum foil is wrapped around the outside of the K-type aerosol fire extinguishing agent column. The aluminum foil is purchased from Shenzhen Mileqi Tape Co., Ltd. and has a thickness of 0.1 mm.

[0078] Comparative Example 2

[0079] Weigh 80 parts of methyl silicone oil and 20 parts of Al(OH)3, mix and stir evenly to obtain a coating agent liquid, and then perform coating according to the method and steps described in Example 2.

[0080] Comparative Example 3

[0081] (1) Weighing platinum acetylacetonate and dissolving it in anhydrous ethanol to prepare a platinum acetylacetonate ethanol solution with a mass fraction of 0.1% of platinum;

[0082] (2) Weigh 60 parts of methyl silicone oil, 39.97 parts of Al(OH)3 and 0.03 parts of acetylacetonate platinum ethanol solution, mix and stir evenly to obtain a coating agent liquid;

[0083] (3) Coating was performed according to the method and steps described in Example 2.

[0084] Comparative Example 4

[0085] (1) Weighing platinum acetylacetonate and dissolving it in anhydrous ethanol to prepare a platinum acetylacetonate ethanol solution with a mass fraction of 0.1% of platinum;

[0086] (2) Weigh 75 parts of methyl silicone oil, 24 parts of Al(OH)3 and 1 part of acetylacetonate platinum ethanol solution, mix and stir evenly to obtain a coating agent liquid;

[0087] (3) Coating was performed according to the method and steps described in Example 2.

[0088] Comparative Example 5

[0089] (1) Weighing platinum acetylacetonate and dissolving it in anhydrous ethanol to prepare a platinum acetylacetonate ethanol solution with a mass fraction of platinum of 1%;

[0090] (2) Weigh 80 parts of methyl silicone oil, 19.8 parts of Al(OH)3 and 0.2 parts of acetylacetonate platinum ethanol solution, mix and stir evenly to obtain a coating agent liquid;

[0091] (3) Coating was performed according to the method and steps described in Example 2.

[0092] Results: The coated aerosol fire extinguishing agent columns and the bare aerosol fire extinguishing agent columns in Examples 2-12 and Comparative Examples 1-5 were respectively assembled into fire extinguishing devices with 70g ceramic balls. Then, a spraying experiment was carried out to test the surface temperature and spraying time of the device, and the combustion of the columns was observed. The results are shown in the following table.

[0093] The results show that, compared with the bare explosive and the aluminum foil coating in Comparative Example 1, the coating with the coating agent used in Examples 2-12 can effectively reduce the surface temperature of the spraying device, thereby reducing the thermal insulation requirements for the fire extinguishing device; at the same time, it can also extend the spraying time of the aerosol fire extinguishing agent, ensure the orderly combustion of the explosive, and reduce the incidence of safety hazards caused by the explosive due to fire and deflagration.

Claims

1. A powder column coating agent for an aerosol fire extinguishing agent, characterized in that: The composition comprises 80-95 parts of silicone oil, 10-40 parts of inorganic flame retardant and 0.1-0.5 parts of catalyst.

2. The coating agent for an aerosol fire extinguishing agent column according to claim 1, characterized in that: The silicone oil is any one of vinyl-terminated silicone oil, methyl silicone oil, ethyl silicone oil, phenyl silicone oil, methyl hydrogen-containing silicone oil, methylphenyl silicone oil, methylchlorophenyl silicone oil, methylethoxy silicone oil, methyltrifluoropropyl silicone oil, methylvinyl silicone oil, methylhydroxy silicone oil, ethyl hydrogen-containing silicone oil or hydroxy hydrogen-containing silicone oil.

3. The coating agent for an aerosol fire extinguishing agent column according to claim 1, characterized in that: The inorganic flame retardant is any one of Al(OH)3, Mg(OH)2, Zn(OH)2, Fe(OH)3, Cu(OH)2, MgCO3, CaCO3 or ammonium polyphosphate.

4. The coating agent for an aerosol fire extinguishing agent column according to claim 1, characterized in that: The catalyst is any one of chloroplatinic acid, potassium chloroplatinate or platinum acetylacetonate.

5. The coating agent for aerosol fire extinguishing agent column according to claim 4, characterized in that: The catalyst is prepared into an ethanol solution before use, wherein the mass fraction of platinum in the catalyst ethanol solution is 0.1%.

6. A method for coating the coating agent of the aerosol fire extinguishing agent column as claimed in claims 1 to 5, characterized in that: The following steps are involved: (1) weighing an appropriate amount of catalyst and dissolving it in anhydrous ethanol to prepare a catalyst solution with a platinum mass fraction of 0.1%; (2) Weighing silicone oil and inorganic flame retardant, adding them to the catalyst solution, and stirring evenly to obtain a coating agent liquid; (3) Fix the formed drug column on a custom mold coated with a release agent, and fix the coated paper tube on the base; (4) Add coating agent liquid to the coating paper tube, solidify and shape it at room temperature, and then remove the customized mold to complete the coating of the drug column.

7. The coating method according to claim 6, characterized in that: The customized mold described in step (3) and step (4) is composed of a base (1), a paper tube fixing seat (2) and a medicine column supporting seat (3) which are stacked in sequence and fixedly connected.

8. The coating method according to claim 6, characterized in that: The release agent described in step (3) is vaseline.

9. The coating method according to claim 6, characterized in that: The mass ratio of the drug column and the coating agent described in step (4) is 1:1.

Citation Information

Patent Citations

  • Hot aerosol fire extinguisher with thermostable ablative-insulative layer and manufacture method

    CN101700427A

  • Polymorphic preparation method of novel bionic nanocapsule fire extinguisher and fire extinguishing patch

    CN111068234A

  • Flame-retardant waterproof and fireproof insulating sealant and preparation method thereof

    CN113214781A

  • Aerosol fire-extinguishing agent composition

    JP2019097691A

Cited By

  • Low-toxicity high-efficiency aerosol fire extinguishing agent composition and preparation method thereof

    CN122297965A