High-speed wire online heat treatment device and process based on energy recycling
Through the online heat treatment equipment and waste heat recovery system, combined with molten salt energy storage power generation technology, the problems of insufficient cooling capacity of high-speed wires and waste heat recovery are solved, efficient production and energy recycling are achieved, and the strength and uniformity of wires are improved.
Patent Information
- Application Number
- PCT/CN2023/111182
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2023-08-04
- Publication Date
- 2024-11-21
AI Technical Summary
The existing high-speed wire cooling methods have problems such as insufficient cooling capacity, poor uniformity of the same circle, complex process, high energy consumption, and environmental pollution, which are difficult to meet the requirements of high strength and high toughness, and lack the technology of post-rolling waste heat recovery and energy recycling.
Using online heat treatment equipment based on energy recycling, combined with waste heat recovery system and molten salt energy storage power generation system, rapid cooling and isothermal treatment is performed through fast cooling tanks and isothermal tanks, and molten salt is used for heat recovery and energy storage peak power generation, realizing Highly efficient surface desalination and tissue uniformity control.
The production efficiency, strength, plasticity and mechanical properties of high-speed wires are improved, and the recovery of waste heat after rolling and energy recycling are achieved, achieving the green and low-carbon production target.
Smart Images

Figure CN2023111182_21112024_PF_FP_ABST
Abstract
Description
A high-speed wire online heat treatment equipment and process based on energy recycling Technical Field
[0001] The present invention relates to a high-speed wire online heat treatment device and process based on energy recycling, belonging to the technical field of metal wire manufacturing and material heat treatment, and power generation using waste heat from steel production. Background Art
[0002] At present, conventional high-speed wire rods produced both domestically and internationally are cooled on a Stelmor line after spinning to control microstructural transformation. With the continuous development of my country's economy, the automotive and transportation sectors are developing rapidly, and lightweighting requirements are gradually increasing, placing higher demands on the strength and plasticity of high-speed wire rods. High-speed wire rods on the Stelmor cooling line often adjust parameters such as the air-cooling line length, fan air volume, roller speed, and insulation cover to control the microstructure, mechanical properties, and uniformity of performance within the same coil. Due to the insufficient cooling capacity of the Stelmor cooling line, hypereutectoid steel and hypoeutectoid steel wire rods will remain in the secondary network carbide and tertiary cementite precipitation temperature ranges, respectively, for a long time on the air-cooling rollers. At the same time, due to the insufficient cooling capacity, the uniformity of performance within the same coil is poor, making it difficult to produce high-speed wire rods with higher strength and toughness requirements, such as steel for bridge cables with a rating of 1960MPa or above and ultra-high-strength steel strands with a rating of 2200MPa or above.
[0003] Specifically, existing high-speed wire cooling methods include the following: (square / round billet sizes vary, 220mm×220mm is used as an example):
[0004] 1. Offline salt bath in steel mill: billet → rolling → spinning → cooling on Stelmor cooling line (air cooling) → coiling → single / multi-wire pay-off → straightening → descaling → heating → salt bath → cleaning → coiling.
[0005] 2. Offline salt bath in wire drawing plant (downstream of steel plant): ① Billet → Rolling → Wire laying → Cooling on Stelmor cooling line → Coiling, ② After arriving at the wire drawing plant: Single / Multi-wire pay-off → Descaling / Pickling → Heating → Salt bath → Cleaning → Wire drawing → Winding.
[0006] 3. Online salt bath in wire drawing plant: ① Billet → Rolling → Wire laying (such as 15mm diameter wire rod) → Cooling on Stelmor cooling line (air cooling) → Coiling → Single / Multi-wire pay-off → Descaling → Heating → Salt bath → Cleaning → Coiling, ② After arriving at the wire drawing plant: Single / Multi-wire pay-off → Straightening → Descaling / Pickling → Heating → Salt bath → Cleaning → Wire drawing → Winding.
[0007] Chinese patent 202210328695.0 discloses 2200MPa grade steel wire wire rod and its manufacturing method. However, the patent adopts high-speed wire rolling, Stelmor cooling, and salt bath preparation. The process is air-cooled wire rod and then salt bath, that is, offline salt bath production, which also has the problem of many complex processes.
[0008] Domestic Xingcheng Special Steel and Anshan Iron and Steel use online water bath treatment, which to a certain extent makes up for the shortcomings of the air cooling line. However, when the wire rod enters the water online, an air film is quickly formed on the surface, which hinders the convection with the water, resulting in an extremely unstable cooling rate of the wire rod. The process is extremely difficult to control, and it is still impossible to achieve isothermal sorbite phase transformation control of the wire rod, and the material properties fluctuate greatly.
[0009] The offline lead bath requires the wire rod to be reheated, which is a cumbersome process with high energy consumption and carbon emissions. The discharge and treatment costs of residual lead on the wire surface and waste lead liquid are high. At the same time, the lead smoke, lead dust and volatile vapors generated during the production process are toxic and harmful to the human body and the environment. It was explicitly eliminated in the 2005 National Development and Reform Commission's Document No. 40, "Guiding Catalogue for Industrial Structure Adjustment (2005)".
[0010] Molten salt, with its high specific heat capacity, high heat transfer capacity, and excellent stability, is a promising cooling / heat transfer medium to replace air and water cooling. Internationally, Nippon Steel DLP and domestically, including Qinggang, Baosteel, Shagang, and Jiyuan, all use molten salt as a cooling medium for online or offline salt bath treatments. Offline salt baths require repackaging, descaling, pay-off, reheat treatment, and wind-up of the air-cooled wire rod, resulting in low production efficiency, low yield, and high costs.
[0011] In terms of energy utilization, only 30% to 50% of the energy in the steelmaking process is effectively utilized, leaving the remaining energy as waste heat, which has enormous potential for recovery. Waste heat recovery technology is already in use in ironmaking, steelmaking, and sintering processes. However, waste heat recovery technology for bar cooling beds is still immature, and waste heat recovery after wire rolling has not yet been implemented.
[0012] There is no mature, applied technology for waste heat recovery from rolling mills, either domestically or internationally. Conventional post-rolling air-cooling lines have an unstable heat source. The wire rods are cooled by fans, making wind energy collection difficult, heat dispersion, and low temperatures. This leads to large waste heat fluctuations and difficulties in achieving a heat-water balance. Furthermore, the energy efficiency of heat recovered at low temperatures is extremely low, limiting the development of post-rolling waste heat recovery. For example, Sweden's Avest Steel Plant utilizes an energy recovery system for slab heat on a slab cooling bed. The circulating water supplied by the boiler is heated to approximately 85°C by slab heat radiation through the cooling bed's lined pipes. This type of heat recovery system only produces low-temperature steam, resulting in extremely low energy efficiency.
[0013] At the same time, in existing technologies, molten salt energy storage technology is mainly used in solar thermal power stations and has not been used in the steel industry.
[0014] In addition, in the prior art, residual salt on the surface of wire rods or drawn wires after the salt bath cannot be completely removed. Molten salt is hygroscopic and corrosive. Failure to completely remove residual salt from the overlapped joints will exacerbate corrosion, which will lead to increased wire breakage in the downstream silk-making process. In other words, incomplete removal of residual salt from the surface will exacerbate corrosion. Currently known methods for surface desalination all rely on air blowing and high-pressure water spraying. Molten salt solidifies after being sprayed with water, making spray desalination more difficult. Furthermore, the wire rods have overlapped joints, and the air blowing and high-pressure water spraying method cannot remove residual salt from the overlapped joints.
[0015] Currently, after steel mills conduct offline salt bath on wire rods, they straighten the wire rods or steel wires during surface desalting to facilitate the removal of residual salt on the straight wires. However, there is a problem that the surface of the wire rods or steel wires is easily scratched.
[0016] In the prior art, after the wire rod is subjected to an offline salt bath, only air blowing is used to remove salt from the surface. However, the air blowing cannot completely remove salt, resulting in severe corrosion of the wire rod after half a year.
[0017] The existing technology uses air blowing + high-pressure water spraying to remove salt from the surface. The surface has light red rust formed by water stains. If it cannot be blown away, the rust will be aggravated. In addition, the residual salt at the overlap will aggravate the corrosion.
[0018] At present, there is a lack of an integrated equipment with high production efficiency, stable liquid level and high temperature uniformity, efficient surface desalination, high heat exchange efficiency, post-rolling waste heat recovery, green and low-carbon, energy recycling, molten salt energy storage and peak-shaving power generation. It can not only effectively improve the microstructure, mechanical properties and uniformity of the same-circle performance of high-speed wire through online heat treatment, but also realize waste heat recovery for energy recycling and energy storage and peak-shaving power generation.
[0019] In view of the current problems such as insufficient cooling capacity of the Stelmor wire, large fluctuations in the cooling speed of the water bath treatment, environmental protection restrictions on the offline lead bath, low production efficiency of the offline salt bath, low yield, high cost, and incomplete surface desalination, the present invention proposes an online heat treatment equipment and process for high-speed wire rods based on energy recycling. The purpose is to suppress the precipitation of secondary network carbides of hypereutectoid steel and tertiary cementite of hypoeutectoid steel by performing online rapid cooling quenching-isothermal-controlled cooling-cleaning on the wire rods, thereby achieving troostite / bainite treatment of the wire rods, which not only achieves the goals of high online production efficiency of high-speed wire rods, good surface quality, high strength, good plasticity, good toughness, and good uniformity of mechanical properties in the same circle, but also realizes the recovery of waste heat after rolling for molten salt energy storage and peak-shaving power generation, thereby achieving the goals of green, low-carbon and energy recycling.
[0020] Summary of the Invention
[0021] The problem to be solved by the present invention is to provide an online heat treatment equipment for high-speed wire rod based on energy recycling, which is composed of a coupling of online heat treatment equipment, a waste heat recovery system, and a molten salt energy storage and power generation system. When the above equipment is used, the wire rod enters the online heat treatment equipment after spinning for online rapid cooling quenching-isothermal-controlled cooling-cleaning, which can effectively inhibit the precipitation of secondary network carbides of hypereutectoid steel and tertiary cementite of hypoeutectoid steel, and realize the sorbite / bainite treatment, organizational uniformity and surface quality control of the wire rod; after heating, the molten salt used in the salt bath passes through the waste heat recovery system to realize the recovery of waste heat after rolling; the heat recovered by the waste heat recovery system is stored and released by the molten salt energy storage and power generation system, realizing molten salt energy storage and peak-shaving power generation.
[0022] At the same time, the present invention provides a process for online heat treatment of high-speed wire based on energy recycling, which has the advantages of low cost, green and low carbon, and energy recycling. It not only achieves the purpose of high online production efficiency of high-speed wire, good surface quality, high strength, good plasticity, good toughness, and good uniformity of mechanical properties in the same circle, but also realizes the recovery of waste heat after rolling for molten salt energy storage and peak-shaving power generation, thereby achieving the purpose of green and low carbon and energy recycling.
[0023] At the same time, the present invention provides a wire rod obtained by a process of high-speed wire online heat treatment based on energy recycling.
[0024] At the same time, the present invention provides the application of the above-mentioned wire rod in bainite cold heading steel, spring steel, tool steel, bearing steel, bridge cables, steel strands, tire bead cords, cutting wires, and diamond wires.
[0025] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0026] A high-speed wire rod online heat treatment equipment and process based on energy recycling is used for online heat treatment of wire rods on a high-speed wire rod rolling production line, and the waste heat after rolling is recovered and peak-shaving power generation is performed through molten salt energy storage, thereby realizing energy recycling.
[0027] An online heat treatment equipment for high-speed wire rod based on energy recycling, comprising online heat treatment equipment, a waste heat recovery system and a molten salt energy storage and peak-shaving power generation system; the online heat treatment equipment comprises molten salt, a conveyor roller, a rapid cooling tank, an isothermal tank, an air-cooling and cooling control device, a cleaning system, a flue gas collection system and a brine separation system, the molten salt is placed in the rapid cooling tank and the isothermal tank, the flue gas collection system pipeline is located above the rapid cooling tank, the isothermal tank, the air-cooling and cooling control device and the cleaning system, and the brine separation system is connected to the cleaning system; the waste heat recovery system comprises molten salt and a salt-salt heat exchanger; the molten salt energy storage and power generation system comprises molten salt, a low-temperature storage tank, a waste heat boiler, an intermediate storage tank, a molten salt furnace, a high-temperature storage tank, a superheater, an evaporator and a preheater.
[0028] Specifically, the online heat treatment equipment includes a quick cooling tank, an isothermal tank, an air cooling and controlled cooling device, a cleaning system and a drying device that pass through the wire rod from left to right;
[0029] The rapid cooling tank and the isothermal tank are both filled with molten salt;
[0030] A lower tank body I for circulating molten salt with the quick cooling tank is provided below the quick cooling tank; a lower tank body II for circulating molten salt with the isothermal tank is provided below the isothermal tank;
[0031] The waste heat recovery system includes a salt-salt heat exchanger for exchanging heat with the molten salt in the lower tank body I and the lower tank body II;
[0032] The molten salt after heat exchange in the salt-salt heat exchanger flows to the molten salt energy storage peak-shaving power generation system.
[0033] A fume collection system is installed above the quick cooling tank, isothermal tank, air cooling control equipment and cleaning system.
[0034] The brine separation system is connected to the cleaning system; the cleaning system includes a cleaning nozzle I, an annular air knife III, a stepped water tank, annular air knife IV, a cleaning nozzle II and annular air knife V arranged from left to right; the air-cooled cooling control equipment includes annular air knife I and annular air knife II located between the isothermal tank and the cleaning system.
[0035] The molten salt energy storage and peak-shaving power generation system includes an intermediate storage tank for storing the molten salt heated in the salt-salt heat exchanger. The intermediate storage tank is connected to the high-temperature storage tank. The molten salt in the high-temperature storage tank provides heat for the power generation equipment, and the heated molten salt is stored in the low-temperature storage tank; the molten salt in the low-temperature storage tank flows back to the shell side of the salt-salt heat exchanger and the intermediate storage tank.
[0036] The molten salt temperature of the rapid cooling tank is 250-600°C, and the cooling rate of the rapid cooling tank is at least 30°C / s; the molten salt temperature of the isothermal tank is 400-585°C.
[0037] A roller conveyor is provided inside the stepped water tank, and the roller conveyor is provided with 2 to 7 drop sections. The horizontal projection overlapping distance between the tail of the previous drop section and the head of the next drop section is 100mm to 1500mm. Each drop section forms a step shape. Each drop section includes 3 to 20 rollers arranged from left to right and extending upward, with a drop height of 100mm to 500mm, an inclination angle of 10° to 60°, and a roller spacing of 50mm to 400mm; an ultrasonic vibration device is provided in the stepped water tank.
[0038] An online heat treatment process for high-speed wire rods based on energy recycling comprises the following steps:
[0039] S01, salt bath rapid cooling: after spinning, the wire rod temperature is 800-1050℃, and enters the rapid cooling tank with 250-600℃ molten salt for rapid cooling and quenching, and the quenching time is 4-40s;
[0040] S02, salt bath isothermal: the rapidly cooled quenched wire rod is placed in an isothermal bath with molten salt at 400-585°C for isothermal transformation, with an isothermal time of 30-400s;
[0041] S03, controlled cooling: After the wire rod comes out of the isothermal tank, it is purged with hot air at 200-550℃ in the annular air knife I for 5-20 seconds, and then purged with compressed air in the annular air knife II for 5-30 seconds;
[0042] S04, cleaning: After controlled cooling, the wire rod enters the cleaning system, and the residual salt on the surface is removed by the cleaning nozzle I, and then it is purged by the annular air knife III, and then enters the stepped water tank in sequence to remove the residual salt on the wire rod surface, and then the surface salt water is removed by the annular air knife IV and the cleaning nozzle II, and then the residual salt water is removed by the annular air knife V;
[0043] S05, Drying: The cleaned wire rod enters the drying equipment for drying and is rolled up to obtain the finished product;
[0044] S06, the molten salt for the salt bath is discharged through the salt-salt heat exchanger tubes: the molten salt heated to 430-610°C in the rapid cooling tank and the isothermal tank first overflows into the lower tank body I and the lower tank body II, then enters the salt-salt heat exchanger through the pipeline, discharges heat through the salt-salt heat exchanger tubes, and then circulates to the lower tank body I and the lower tank body II;
[0045] S07, waste heat recovery system absorbs heat: 230-350°C cooling salt enters the shell side of the salt-salt heat exchanger from the low-temperature storage tank of the molten salt energy storage peak-shaving power generation system. The shell side cooling salt of the salt-salt heat exchanger absorbs the heat of the high-temperature molten salt in the tube side of the salt-salt heat exchanger. After the shell side cooling salt of the salt-salt heat exchanger absorbs heat and the temperature rises to 400-585°C, it returns to the molten salt energy storage peak-shaving power generation system to complete heat recovery;
[0046] S08, molten salt energy storage peak-shaving power generation process:
[0047] Heat storage during off-peak hours: The shell-side cooling salt of the salt-salt heat exchanger absorbs heat and rises to a temperature of 400-585°C before returning to the intermediate storage tank of the molten salt energy storage peak-shaving power generation system. The molten salt in the intermediate storage tank enters the molten salt furnace and is heated to 550-600°C before entering the high-temperature storage tank to store heat.
[0048] Heat release during peak power period: During peak power period, the heat in the 550-600℃ molten salt in the high-temperature storage tank is converted into high-temperature steam and enters the power generation equipment to generate electricity. After the molten salt temperature drops to 230-350℃, it enters the low-temperature storage tank for circulation, playing the role of peak power generation.
[0049] The molten salt is a cooling medium / heat transfer medium composed of two or more of potassium nitrate, sodium nitrate, lithium nitrate, calcium nitrate, silver nitrate, potassium nitrite, and sodium nitrite, and the water content in the molten salt for the salt bath does not exceed 1wt.%.
[0050] The wire rod is obtained by the process of the present invention.
[0051] The wire rod of the present invention is used in bainite cold heading steel, spring steel, tool steel, bearing steel, bridge cables, steel strands, bead cords, cutting wires and diamond wires.
[0052] The raw material wire rods of the present invention are 92Si, 97Si, Y10B21 and 55SiCrA, and their compositions are shown in Table 1 below. The remainder in Table 1 is Fe.
[0053] Table 1 Wire rod composition
[0054] The structure of the wire rod after salt bath of the present invention (taking the troostite structure as an example) is shown in Table 2 below.
[0055] Table 2 Tissue after salt bath
[0056] The mechanical properties of the wire rod after salt bath of the present invention (taking the sorbite structure as an example) are shown in Table 3 below.
[0057] Table 3 Mechanical properties of wire rod after salt bath
[0058] The present invention has the following technical effects or advantages:
[0059] The present invention discloses an online heat treatment device and process for high-speed wire rods based on energy recycling, which is used for online heat treatment of wire rods on a high-speed wire rod rolling production line, recovers the waste heat after rolling and performs peak-shaving power generation through molten salt energy storage, thereby realizing energy recycling.
[0060] The online salt bath process of the present invention is: continuous casting billet (220mm×220mm square billet) → rolling → spinning (15mm diameter wire rod) → salt bath → cleaning → coiling. It has high production efficiency and short process, and can omit multiple processes such as wire pay-off, shot blasting and dephosphorization, reheating, and wire winding, truly realizing green, low-carbon, and efficient production.
[0061] The high-speed wire online heat treatment equipment based on energy recycling of the present invention can realize the bainite / bainite treatment of wire rods, improve the bainite / bainite structure ratio, weaken or eliminate the risk of abnormal structure, and is used to produce bainite cold heading steel, spring steel, tool steel, bearing steel, bridge cables, steel strands, tire bead cords, cutting wires, diamond wires and other purposes. It utilizes the heat concentration of rapid cooling tanks and isothermal tanks and the advantages of salt-salt efficient heat exchange to realize post-rolling waste heat recovery. The heat recovered from the waste heat is stored in the molten salt energy storage peak-shaving power generation system during the valley period and released during the peak period for peak-shaving power generation. It not only achieves the goals of high online production efficiency of high-speed wire rods, good surface quality, high strength, good plasticity, good toughness, and good uniformity of mechanical properties in the same circle, but also realizes the recovery of post-rolling waste heat for molten salt energy storage peak-shaving power generation, thereby achieving the goals of green, low-carbon and energy recycling.
[0062] The present invention adopts air knife + flushing + stepped water tank + ultrasonic vibration washing to clean the wire rod, ensuring that the overlapping parts of the wire rod can also be cleaned.
[0063] The present invention is suitable for direct salt bath treatment after wire rod spinning, post-rolling waste heat recovery and molten salt energy storage and peak-shaving power generation. The overall structural design is reasonable, and the parameters such as molten salt circulation, flow rate, liquid level, temperature, and flow field of the online heat treatment continuous equipment are adjustable, which effectively ensures the liquid level stability, temperature uniformity and accuracy of the cooling medium / heat transfer medium in the salt bath rapid cooling tank and the salt bath isothermal tank. The air-cooled cooling control equipment effectively ensures the wire rod control cooling capacity, and the cleaning equipment effectively ensures the surface quality of the wire rod. The salt bath rapid cooling tank and the salt bath isothermal tank have concentrated heat, which effectively ensures waste heat recovery. Molten salt is used to store and release heat, which effectively ensures waste heat recovery for energy storage and peak-shaving power generation.
[0064] The salt bath rapid cooling of the present invention can effectively control the precipitation of secondary network carbides of hypereutectoid steel and tertiary cementite of hypoeutectoid steel, and effectively control the transformation of austenite of hypereutectoid steel and hypoeutectoid steel wire rods to sorbite / bainite. The salt bath isothermal process can effectively control the transformation of untransformed austenite of hypereutectoid steel and hypoeutectoid steel to sorbite / bainite. The air cooling control equipment can effectively control the uniformity of the structure of hypereutectoid steel and hypoeutectoid steel after phase transformation. Finally, the wire rod is cleaned to remove surface molten salt and dried to achieve the purpose of effectively regulating the surface quality and uniformity of the structure and performance of the wire rod.
[0065] The existing conventional air-cooled wire rod structure is (taking the sorbite structure as an example): the lamellar spacing is ~120μm, the sorbite rate is 80-90%, and the performance uniformity in the same circle is ~80MPa. The microstructure diagram of the wire rod after heat treatment of the present invention shows that the lamellar spacing is ~80μm, the sorbite rate is ≥95%, and the performance uniformity in the same circle is ~30MPa.
[0066] The mechanical properties of existing conventional air-cooled wire rods (taking sorbite structure as an example) are as follows: the tensile strength of conventional air-cooled wire rods is 1400 MPa, the surface shrinkage is 30%, and the tensile strength can reach 1960 MPa or below after downstream silk making; while the tensile strength of the wire rods after heat treatment of the present invention is 1512 MPa, the surface shrinkage is 35%, and the tensile strength can reach 2200 MPa or above after downstream silk making. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] FIG1 is a schematic structural diagram of a high-speed wire rod online heat treatment device based on energy recycling of the present invention;
[0068] FIG2 is a microstructure diagram of tempered troostite + tempered martensite + retained austenite obtained in Example 1 of the present invention;
[0069] FIG3 is a diagram of the bainite structure obtained in Example 2 of the present invention;
[0070] FIG4 is a diagram of the bainite structure obtained in Example 3 of the present invention;
[0071] FIG5 is a diagram of the structure of the troostite obtained in Example 4 of the present invention;
[0072] FIG6 is a process diagram of online heat treatment of high-speed wire rods based on energy recycling according to the present invention;
[0073] FIG7 is a schematic structural diagram of the device according to embodiment 2 of the present invention. DETAILED DESCRIPTION
[0074] The present invention will be further described in detail below with reference to the accompanying drawings and specific examples. The following examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.
[0075] Example 1
[0076] As shown in Figures 1 and 7, an online heat treatment device for high-speed wire rods based on energy recycling includes online heat treatment equipment, a waste heat recovery system, and a molten salt energy storage peak-shaving power generation system;
[0077] The online heat treatment equipment includes, from left to right, a quick cooling tank 1 through which the wire rod passes, an isothermal tank 3, an air cooling and controlled cooling device, a cleaning system, and a drying device 14;
[0078] The rapid cooling tank 1 and the isothermal tank 3 are both filled with molten salt;
[0079] A lower tank body I2 for circulating molten salt with the quick cooling tank 1 is provided below the quick cooling tank 1; a lower tank body II4 for circulating molten salt with the isothermal tank 3 is provided below the isothermal tank 3;
[0080] The waste heat recovery system includes a salt-salt heat exchanger 15 for exchanging heat with the molten salt in the lower tank body I2 and the lower tank body II4;
[0081] The molten salt after heat exchange in the salt-salt heat exchanger 15 flows to the molten salt energy storage peak-shaving power generation system.
[0082] A fume collection system 5 is provided above the rapid cooling tank 1, the isothermal tank 3, the air-cooling control equipment and the cleaning system.
[0083] The brine separation system 24 is connected to the cleaning system; the cleaning system includes a cleaning nozzle I8, an annular air knife III9, a stepped water tank 10, an annular air knife IV11, a cleaning nozzle II12 and an annular air knife V13 arranged from left to right; the air-cooled cooling control equipment includes an annular air knife I6 and an annular air knife II7 located between the isothermal tank 3 and the cleaning system.
[0084] The molten salt energy storage and peak-shaving power generation system includes an intermediate storage tank 16 for storing the molten salt heated in the salt-salt heat exchanger 15. The intermediate storage tank 16 is connected to the high-temperature storage tank 18. The molten salt in the high-temperature storage tank 18 provides heat for the power generation equipment, and the heated molten salt is stored in the low-temperature storage tank 22; the molten salt in the low-temperature storage tank 22 flows back to the shell side of the salt-salt heat exchanger 15 and the intermediate storage tank 16.
[0085] The cooling rate of the rapid cooling tank 1 is 30°C / s.
[0086] A roller conveyor is provided inside the stepped water trough 10, and the roller conveyor is provided with two drop sections. The horizontal projection overlapping distance between the tail of the previous drop section and the head of the next drop section is 100 mm. Each drop section forms a step shape. Each drop section includes three rollers arranged from left to right and extending upward, with a drop height of 100 mm, an inclination angle of 60°, and a roller spacing of 50 mm; an ultrasonic vibration device is provided inside the stepped water trough 10.
[0087] An online heat treatment process for high-speed wire rods based on energy recycling comprises the following steps:
[0088] e. After spinning, the wire rod is heated with molten salt: after spinning, the wire rod temperature is 800°C, and enters the 250°C molten salt in the rapid cooling tank 1 for rapid cooling. The quenching time is 4 seconds. The wire rod heats the molten salt, and the molten salt temperature rises by 180°C.
[0089] f. Isothermal section wire rod heating molten salt: The rapidly cooled quenched wire rod enters the 400°C molten salt in the isothermal tank 3 for isothermal transformation. The isothermal time is 30 seconds. The wire rod heats the molten salt in this section, and the molten salt temperature rises by 210°C.
[0090] g, controlled cooling: after the wire rod comes out of the isothermal bath 3, it is purged with 200°C hot air from the annular air knife I6 for 5 seconds, and then purged with compressed air from the annular air knife II7 for 5 seconds;
[0091] h. Cleaning: After controlled cooling, the wire rod enters the cleaning system, and the residual salt on the surface is removed by the cleaning nozzle I8, and then it is purged by the annular air knife III9, and then enters the stepped water tank 10 to remove the residual salt on the wire rod surface, and then the surface salt water is removed by the annular air knife IV11 and the cleaning nozzle II12, and then the residual salt water is removed by the annular air knife V13;
[0092] i. Drying: After cleaning, the wire rod enters the drying equipment 14 for drying and is rolled up to obtain the finished product;
[0093] j. The molten salt for salt bath releases heat through the salt-salt heat exchanger 15 tube pass: the molten salt heated to 430°C and 610°C in the quick cooling tank 1 and the isothermal tank 3 respectively overflows into the lower tank body I2 and the lower tank body II4, then enters the salt-salt heat exchanger 15 through the pipeline, releases heat through the salt-salt heat exchanger 15 tube pass, and then circulates to the lower tank body I2 and the lower tank body II4;
[0094] k. Heat absorption by the waste heat recovery system: 230°C cooling salt enters the shell side of the salt-salt heat exchanger 15 from the low-temperature storage tank 22 of the molten salt energy storage peak-shaving power generation system. The shell side cooling salt of the salt-salt heat exchanger 15 absorbs the heat of the high-temperature molten salt in the tube side of the salt-salt heat exchanger 15. After the shell side cooling salt of the salt-salt heat exchanger 15 absorbs heat and the temperature rises to 400°C, it returns to the molten salt energy storage peak-shaving power generation system to complete heat recovery.
[0095] l. Molten salt energy storage peak-shaving power generation process: Heat storage during off-peak hours: The shell-side cooling salt of the salt-salt heat exchanger 15 absorbs heat and its temperature rises to 400°C before returning to the intermediate storage tank 16 of the molten salt energy storage peak-shaving power generation system. The molten salt in the intermediate storage tank 16 enters the molten salt furnace 17, is heated to 550°C, and then enters the high-temperature storage tank 18 to store heat;
[0096] Heat release during peak power period: During peak power period, the heat in the 550℃ molten salt in the high-temperature storage tank 18 is converted into high-temperature steam and enters the power generation equipment to generate electricity. After the molten salt temperature drops to 230℃, it enters the low-temperature storage tank 22 for circulation, playing the role of peak power generation.
[0097] The process of this embodiment is a quenching-tempering process. The molten salt temperature of the rapid cooling tank 1 is 250°C, and the molten salt temperature of the isothermal tank 3 is 400°C. This embodiment is designed to have an annual capacity of 350,000 tons, a steel output of approximately 120 tons / h, and an annual operation time of approximately 2,640 hours. When the wire rod is cooled, it undergoes isothermal heat treatment in the salt bath section to produce high-strength steel, and at the same time generates sensible heat of 2.59×10 7 kJ / h heat, based on 70% heat recovery, the initial estimate is that 1.81×10 7 kJ / h of heat, and generate electricity by coupling the molten salt heat storage system.
[0098] The molten salt is a cooling medium / heat transfer medium composed of two or more of potassium nitrate, sodium nitrate, lithium nitrate, calcium nitrate, silver nitrate, potassium nitrite, and sodium nitrite. The water content in the molten salt for the salt bath is 1 wt.%.
[0099] As shown in Figures 2 and 6, the process used in this embodiment is a quenching-tempering process, resulting in a microstructure of tempered troostite + tempered martensite + retained austenite. A microstructure photograph is shown in Figure 2. The raw material is 55SiCrA, and the performance uniformity within the same circle is approximately 50 MPa. The tensile strength is 1989 MPa, and the reduction of area is 47%.
[0100] The wire rod of this embodiment is used in spring steel, tool steel, bearing steel, bridge cables, steel strands, tire bead cords, cutting wires, and diamond wires.
[0101] Example 2:
[0102] As shown in Figure 7, an online heat treatment equipment for high-speed wire rod based on energy recycling includes a rapid cooling tank 1, a lower tank body I2, an isothermal tank 3, a lower tank body II4, a flue gas collection system 5, an annular air knife I6, an annular air knife II7, a cleaning nozzle I8, an annular air knife III9, a stepped water tank 10, an annular air knife IV11, a cleaning nozzle II12, an annular air knife V13, a drying equipment 14, a salt-salt heat exchanger 15, an intermediate storage tank 16, a molten salt furnace 17, a high-temperature storage tank 18, a superheater 19, an evaporator 20, a preheater 21, a low-temperature storage tank 22, a steam drum 23 and a brine separation system 24.
[0103] The embodiment of the present invention provides an online heat treatment device for high-speed wire rods based on energy recycling, including an online heat treatment device, a waste heat recovery system, and a molten salt energy storage peak-shaving power generation system.
[0104] The online heat treatment equipment includes, from left to right, a quick cooling tank 1, an isothermal tank 3, annular air knife I6, annular air knife II7, a cleaning nozzle I8, annular air knife III9, a stepped water tank 10, annular air knife IV11, a cleaning nozzle II12, annular air knife V13, and a drying device 14, which pass through the wire rod in sequence;
[0105] The rapid cooling tank 1 and the isothermal tank 3 are both filled with molten salt;
[0106] A lower tank body I2 for circulating molten salt with the quick cooling tank 1 is provided below the quick cooling tank 1; a lower tank body II4 for circulating molten salt with the isothermal tank 3 is provided below the isothermal tank 3;
[0107] The waste heat recovery system includes a salt-salt heat exchanger 15 for exchanging heat with the molten salt in the lower tank body I2 and the lower tank body II4. The salt-salt heat exchanger 15 includes a tube side for the molten salt used for the salt bath to release heat and a shell side for containing cooling salt. The heated molten salt in the lower tank body I2 and the lower tank body II4 passes through the salt-salt heat exchanger 15 tube side to release heat. The cooling salt in the shell side of the salt-salt heat exchanger 15 absorbs the heat of the high-temperature molten salt in the salt-salt heat exchanger 15 tube side. The cooling salt in the shell side of the salt-salt heat exchanger 15 absorbs heat and then the temperature rises before returning to the molten salt energy storage peak-shaving power generation system to complete heat recovery.
[0108] A fume collection system 5 is provided above the rapid cooling tank 1 and the isothermal tank 3 .
[0109] The brine separation system 24 is located below the stepped water tank 10 and is connected to the stepped water tank 10 .
[0110] The molten salt energy storage and peak-shaving power generation system includes an intermediate storage tank 16 for storing the molten salt after the shell side of the salt-salt heat exchanger 15 is heated. The intermediate storage tank 16 is connected to the molten salt furnace 17. The molten salt in the intermediate storage tank 16 is heated by the molten salt furnace 17 and enters the high-temperature storage tank 18. After the molten salt in the high-temperature storage tank 18 passes through the superheater 19 and the evaporator 20, the water absorbs heat and becomes high-temperature steam and enters the steam drum 23 to directly generate electricity. A steam drum 23 is provided between the superheater 19 and the evaporator 20. The molten salt after heating is stored in the low-temperature storage tank 22 through the preheater 21; the molten salt in the low-temperature storage tank 22 flows back to the shell side of the salt-salt heat exchanger 15 and the intermediate storage tank 16.
[0111] The molten salt temperature of the rapid cooling tank 1 is 400°C, and the cooling rate of the rapid cooling tank 1 is 50°C / s; the molten salt temperature of the isothermal tank 3 is 585°C.
[0112] As shown in Figure 7, a roller conveyor is provided inside the stepped water tank 10, and the roller conveyor is provided with 7 drop sections to form a stepped shape; the horizontal projection overlapping distance between the tail of the previous drop section and the head of the next drop section is 1500mm, and each drop section forms a step shape. Each drop section includes 20 rollers arranged from left to right and extending upward, with a drop height of 500mm, an inclination angle of 30°, and a roller spacing of 400mm; an ultrasonic vibration device is provided in the stepped water tank 10.
[0113] Preferably, the salt bath rapid cooling roller, salt bath isothermal roller, air-cooled controlled cooling roller, and cleaning roller are all made of 316L stainless steel, with a roller length of 1540 mm, a roller diameter of 120 mm, and a roller spacing of 253 mm.
[0114] Preferably, the salt bath rapid cooling roller, the salt bath isothermal roller, the air cooling controlled cooling roller, and the cleaning roller are all speed-adjustable, and the roller speed is 0.01 m / s.
[0115] Preferably, the rapid cooling tank 1, the lower tank body I2, the isothermal tank 3, the lower tank body II4 and the molten salt contact parts are all made of 316L and 347H materials with a thickness of 5 mm.
[0116] Preferably, the molten salt pump in the salt bath rapid cooling tank is used to regulate parameters such as the molten salt circulation, flow rate, liquid level, temperature, and flow field of the rapid cooling tank 1 and the lower tank body 12.
[0117] Preferably, the molten salt pump in the salt bath isothermal tank is used to regulate parameters such as the molten salt circulation, flow rate, liquid level, temperature, and flow field of the isothermal tank 3 and the lower tank body II4.
[0118] Preferably, the amount of molten salt used in the salt bath is 100t.
[0119] Preferably, the air-cooled controlled cooling equipment can realize slow cooling control after the wire rod leaves the salt tank, with a cooling rate of 3°C / s.
[0120] Preferably, the cleaning system can remove residual salt from the wire rod and recycle the brine.
[0121] Preferably, the flue gas collection system 5 can realize the recycling of salt mist condensation, and the salt water enters the cleaning system for recycling.
[0122] Preferably, the brine separation system 24 utilizes high-temperature waste heat to achieve salt crystallization and reuse and discharge water vapor into the cleaning system for recycling.
[0123] Preferably, the heat exchange area of the salt-salt heat exchanger 15 is 100m 2 .
[0124] Preferably, a filter is provided in the pipes at the connection between the salt-salt heat exchanger 15 and the lower tank body I2 and the lower tank body II4, which can mechanically filter the oxidized iron scale and realize the centralized collection of the oxidized iron scale.
[0125] Preferably, the molten salt energy storage peak-shaving power generation system can use coal gas for heating and energy storage, thereby improving the peak-shaving power generation regulation capability of the molten salt energy storage system.
[0126] Preferably, the amount of molten salt used in the molten salt energy storage peak-shaving power generation system is 500t.
[0127] Preferably, the high-temperature storage tank 18, the intermediate storage tank 16 and the molten salt contact parts are all made of 347H material with a thickness of 5 mm.
[0128] An online heat treatment process for high-speed wire rods based on energy recycling comprises the following steps:
[0129] e. After spinning, the wire rod is heated to molten salt: after spinning, the wire rod temperature is 1050°C, and enters the 400°C molten salt in the rapid cooling tank 1 for rapid cooling. The quenching time is 40s. The wire rod is heated to molten salt, and the molten salt temperature rises by 200°C.
[0130] f. Isothermal section wire rod heating molten salt: The rapidly cooled quenched wire rod enters the 585°C molten salt in isothermal tank 3 for isothermal transformation. The isothermal time is 400s. The wire rod heats this section of molten salt, and the molten salt temperature rises by 10°C.
[0131] g, controlled cooling: after the wire rod comes out of the isothermal bath 3, it is purged with 550°C hot air from the annular air knife I6 for 20 seconds, and then purged with compressed air from the annular air knife II7 for 30 seconds;
[0132] h. Cleaning: After controlled cooling, the wire rod enters the cleaning system, and the residual salt on the surface is removed by the cleaning nozzle I8, and then it is purged by the annular air knife III9, and then enters the stepped water tank 10 to remove the residual salt on the wire rod surface, and then the surface salt water is removed by the annular air knife IV11 and the cleaning nozzle II12, and then the residual salt water is removed by the annular air knife V13;
[0133] i. Drying: After cleaning, the wire rod enters the drying equipment 14 for drying and is rolled up to obtain the finished product;
[0134] j. The molten salt for the salt bath is discharged through the salt-salt heat exchanger 15 tube pass: the molten salt heated to 600°C and 595°C in the rapid cooling tank 1 and the isothermal tank 3 respectively first overflows into the lower tank body I2 and the lower tank body II4, then enters the salt-salt heat exchanger 15 through the pipeline, and discharges heat through the salt-salt heat exchanger 15 tube pass. After heat discharge, it circulates to the lower tank body I2 and the lower tank body II4;
[0135] k. Heat absorption by the waste heat recovery system: 350°C cooling salt enters the shell side of the salt-salt heat exchanger 15 from the low-temperature storage tank 22 of the molten salt energy storage peak-shaving power generation system. The shell side cooling salt of the salt-salt heat exchanger 15 absorbs the heat of the high-temperature molten salt in the tube side of the salt-salt heat exchanger 15. After the shell side cooling salt of the salt-salt heat exchanger 15 absorbs heat and the temperature rises to 585°C, it returns to the molten salt energy storage peak-shaving power generation system to complete heat recovery.
[0136] l. Molten salt energy storage peak-shaving power generation process: Heat storage during off-peak hours: The shell-side cooling salt of the salt-salt heat exchanger 15 absorbs heat and its temperature rises to 585°C before returning to the intermediate storage tank 16 of the molten salt energy storage peak-shaving power generation system. The molten salt in the intermediate storage tank 16 enters the molten salt furnace 17, is heated to 600°C, and then enters the high-temperature storage tank 18 to store heat.
[0137] Heat release during peak power period: During peak power period, the heat in the 600℃ molten salt in the high-temperature storage tank 18 is converted into high-temperature steam and enters the power generation equipment to generate electricity. After the molten salt temperature drops to 350℃, it enters the low-temperature storage tank 22 for circulation, playing the role of peak power generation.
[0138] The molten salt is a cooling medium / heat transfer medium composed of two or more of potassium nitrate, sodium nitrate, lithium nitrate, calcium nitrate, silver nitrate, potassium nitrite, and sodium nitrite. The water content in the molten salt for the salt bath is 0.5 wt.%.
[0139] The process of this embodiment is a bainite process, and the obtained structure is bainite. The structure photo is shown in Figure 3. The raw material is Y10B21, the temperature of the rapid cooling tank 1 is 400°C, and the temperature of the isothermal tank 3 is 585°C. The wire rod of this embodiment is used in bainite cold heading steel.
[0140] Example 3:
[0141] The device of this embodiment differs from the device of embodiment 2 only in that:
[0142] A roller conveyor is provided inside the stepped water trough 10, and the roller conveyor is provided with 5 drop sections. The horizontal projection overlapping distance between the tail of the previous drop section and the head of the next drop section is 500mm. Each drop section forms a step shape. Each drop section includes 10 rollers arranged from left to right and extending upward at an angle, with a drop height of 300mm, an inclination angle of 10°, and a roller spacing of 60mm.
[0143] The molten salt temperature of the rapid cooling tank 1 is 405°C, and the molten salt temperature of the isothermal tank 3 is 400°C.
[0144] The salt bath fast cooling roller, salt bath isothermal roller, air cooling controlled cooling roller and cleaning roller can all be adjusted at variable speeds, with the roller speed being 1m / s.
[0145] The quick cooling tank 1, the lower tank body I2, the isothermal tank 3, the lower tank body II4 and the parts in contact with the molten salt are all made of 316L and 347H materials with a thickness of 20 mm.
[0146] The amount of molten salt used in the salt bath is 500t.
[0147] The air-cooled controlled cooling equipment can realize slow cooling control after the wire rod leaves the salt tank, with a cooling rate of 15℃ / s.
[0148] The heat exchange area of the salt-salt heat exchanger 15 is 500m 2 .
[0149] The amount of molten salt used in the molten salt energy storage peak-shaving power generation system is 3,000t.
[0150] The high-temperature storage tank 18, the intermediate storage tank 16 and the parts in contact with the molten salt are all made of 347H material with a thickness of 20 mm.
[0151] An online heat treatment process for high-speed wire rods based on energy recycling comprises the following steps:
[0152] e. After spinning, the wire rod is heated with molten salt: after spinning, the wire rod temperature is 1000℃, and enters the 405℃ molten salt in the rapid cooling tank 1 for rapid cooling. The quenching time is 10s. The wire rod is heated with molten salt, and the molten salt temperature rises by 150℃.
[0153] f. Isothermal section wire rod heating molten salt: The rapidly cooled quenched wire rod enters the 400°C molten salt in the isothermal tank 3 for isothermal transformation. The isothermal time is 100s. The wire rod heats this section of molten salt, and the molten salt temperature rises by 100°C.
[0154] g, controlled cooling: after the wire rod comes out of the isothermal bath 3, it is purged with 300°C hot air from the annular air knife I6 for 10 seconds, and then purged with compressed air from the annular air knife II7 for 10 seconds;
[0155] h. Cleaning: After controlled cooling, the wire rod enters the cleaning system, and the residual salt on the surface is removed by the cleaning nozzle I8, and then it is purged by the annular air knife III9, and then enters the stepped water tank 10 to remove the residual salt on the wire rod surface, and then the surface salt water is removed by the annular air knife IV11 and the cleaning nozzle II12, and then the residual salt water is removed by the annular air knife V13;
[0156] i. Drying: After cleaning, the wire rod enters the drying equipment 14 for drying and is rolled up to obtain the finished product;
[0157] j. The molten salt for the salt bath is discharged through the salt-salt heat exchanger 15 tube pass: the molten salt heated to 555°C and 500°C in the rapid cooling tank 1 and the isothermal tank 3 respectively first overflows into the lower tank body I2 and the lower tank body II4, then enters the salt-salt heat exchanger 15 through the pipeline, and discharges heat through the salt-salt heat exchanger 15 tube pass. After heat discharge, it circulates to the lower tank body I2 and the lower tank body II4;
[0158] k. Heat absorption by the waste heat recovery system: 300°C cooling salt enters the shell side of the salt-salt heat exchanger 15 from the low-temperature storage tank 22 of the molten salt energy storage peak-shaving power generation system. The shell side cooling salt of the salt-salt heat exchanger 15 absorbs the heat of the high-temperature molten salt in the tube side of the salt-salt heat exchanger 15. After the shell side cooling salt of the salt-salt heat exchanger 15 absorbs heat and the temperature rises to 500°C, it returns to the molten salt energy storage peak-shaving power generation system to complete heat recovery;
[0159] l. Molten salt energy storage peak-shaving power generation process: Heat storage during off-peak hours: The shell-side cooling salt of the salt-salt heat exchanger 15 absorbs heat and its temperature rises to 500°C before returning to the intermediate storage tank 16 of the molten salt energy storage peak-shaving power generation system. The molten salt in the intermediate storage tank 16 enters the molten salt furnace 17, is heated to 580°C, and then enters the high-temperature storage tank 18 to store heat;
[0160] Heat release during peak power period: During peak power period, the heat in the 580℃ molten salt in the high-temperature storage tank 18 is converted into high-temperature steam and enters the power generation equipment to generate electricity. After the molten salt temperature drops to 300℃, it enters the low-temperature storage tank 22 for circulation, playing the role of peak power generation.
[0161] The molten salt is a cooling medium / heat transfer medium composed of two or more of potassium nitrate, sodium nitrate, lithium nitrate, calcium nitrate, silver nitrate, potassium nitrite, and sodium nitrite. The water content in the molten salt for the salt bath is 0.3 wt.%.
[0162] The process of this embodiment is a bainite process, and the obtained structure is bainite. The structure photo is shown in Figure 4. The raw material is Y10B21, the temperature of the rapid cooling tank 1 is 405°C, and the temperature of the isothermal tank 3 is 400°C. The wire rod of this embodiment is used in bainite cold heading steel.
[0163] Example 4:
[0164] The only difference between this embodiment and embodiment 3 is that:
[0165] An online heat treatment process for high-speed wire rods based on energy recycling comprises the following steps:
[0166] e. After spinning, the wire rod is heated with molten salt: after spinning, the wire rod temperature is 900°C, and enters the 600°C molten salt in the rapid cooling tank 1 for rapid cooling. The quenching time is 15s, and the wire rod is heated with molten salt, and the molten salt temperature rises by 10°C.
[0167] f. Isothermal section wire rod heating molten salt: The rapidly cooled quenched wire rod enters the 545°C molten salt in the isothermal tank 3 for isothermal transformation. The isothermal time is 50 seconds. The wire rod heats the molten salt in this section, and the molten salt temperature rises by 10°C.
[0168] g, controlled cooling: after the wire rod comes out of the isothermal bath 3, it is purged with 400°C hot air from the annular air knife I6 for 15 seconds, and then purged with compressed air from the annular air knife II7 for 20 seconds;
[0169] h. Cleaning: After controlled cooling, the wire rod enters the cleaning system, and the residual salt on the surface is removed by the cleaning nozzle I8, and then it is purged by the annular air knife III9, and then enters the stepped water tank 10 to remove the residual salt on the wire rod surface, and then the surface salt water is removed by the annular air knife IV11 and the cleaning nozzle II12, and then the residual salt water is removed by the annular air knife V13;
[0170] i. Drying: After cleaning, the wire rod enters the drying equipment 14 for drying and is rolled up to obtain the finished product;
[0171] j. The molten salt for the salt bath is discharged through the salt-salt heat exchanger 15 tube pass: the molten salt heated to 610°C and 555°C in the quick cooling tank 1 and the isothermal tank 3 respectively first overflows into the lower tank body I2 and the lower tank body II4, then enters the salt-salt heat exchanger 15 through the pipeline, and discharges heat through the salt-salt heat exchanger 15 tube pass. After heat discharge, it circulates to the lower tank body I2 and the lower tank body II4;
[0172] k, waste heat recovery system absorbs heat: 300°C cooling salt enters the shell side of the salt-salt heat exchanger 15 from the low-temperature storage tank 22 of the molten salt energy storage peak-shaving power generation system. The shell side cooling salt of the salt-salt heat exchanger 15 absorbs the heat of the high-temperature molten salt in the tube side of the salt-salt heat exchanger 15. After the shell side cooling salt of the salt-salt heat exchanger 15 absorbs heat and the temperature rises to 585°C, it returns to the molten salt energy storage peak-shaving power generation system to complete heat recovery;
[0173] l. Molten salt energy storage peak-shaving power generation process: Heat storage during off-peak hours: The shell-side cooling salt of the salt-salt heat exchanger 15 absorbs heat and its temperature rises to 585°C before returning to the intermediate storage tank 16 of the molten salt energy storage peak-shaving power generation system. The molten salt in the intermediate storage tank 16 enters the molten salt furnace 17, is heated to 600°C, and then enters the high-temperature storage tank 18 to store heat.
[0174] Heat release during peak power period: During peak power period, the heat in the 600℃ molten salt in the high-temperature storage tank 18 is converted into high-temperature steam and enters the power generation equipment to generate electricity. After the molten salt temperature drops to 300℃, it enters the low-temperature storage tank 22 for circulation, playing the role of peak power generation.
[0175] The molten salt is a cooling medium / heat transfer medium composed of two or more of potassium nitrate, sodium nitrate, lithium nitrate, calcium nitrate, silver nitrate, potassium nitrite, and sodium nitrite. The water content in the molten salt for the salt bath is 0.6 wt.%.
[0176] The process of this embodiment is a troostite process, and the resulting structure is a troostite structure. Figure 5 shows a corresponding microstructure photograph. The troostite ratio is 95%, the interlamellar spacing is 75nm, the network carbide is grade 1.0, the same-turn performance uniformity is approximately 30MPa, the tensile strength is 1512MPa, and the area reduction is 35%. After downstream wire making, the wire rod can reach 2200MPa or above. The raw material is 92Si, the temperature of the rapid cooling tank 1 is 600°C, and the temperature of the isothermal tank 3 is 545°C. The wire rod of this embodiment is used in spring steel, tool steel, bearing steel, bridge cables, steel strand, bead cord, cutting wire, and diamond wire.
[0177] Example 5:
[0178] The only difference between this embodiment and embodiment 4 is that the raw material is 97Si, the sorbitization rate is 96%, the interlamellar spacing is 79nm, the network carbide is level 1.0, the uniformity of the same-circle performance is about 30MPa, the tensile strength is 1585MPa, and the area shrinkage is 31%; after downstream silk making, it can reach 2300MPa level or above.
[0179] Table 4 below is a table of wire rod structures after salt bath obtained in Examples 1 to 5 of the present invention.
[0180] Table 4 Wire rod structure after salt bath obtained in Example 1 to Example 5
[0181] Table 5 below is a table showing the mechanical properties of the wire rods after salt bath obtained in Examples 1 to 5 of the present invention.
[0182] Table 5 Mechanical properties of wire rods after salt bath obtained in Examples 1 to 5
[0183] Test method for the same-turn mechanical fluctuation range: Take 2 turns of wire rod 5m away from the end of the coil, and divide each turn of wire rod into 8 equal sections with the overlap area as the base point. Take 1 tensile specimen on each section. The extreme difference in strength of the tensile specimen after tensile testing is the same-turn difference of the wire rod. The tensile test is carried out in accordance with GB-T 228.1-2021 Tensile test of metallic materials Part 1: Room temperature test method.
[0184] The tensile strength and reduction of area were obtained from the above tensile tests.
[0185] The wire rods obtained in Examples 1 to 5 of the present invention after salt bathing can also achieve efficient surface desalination at the overlaps, and no surface corrosion occurs on the treated wire rods.
[0186] Example 6:
[0187] The only difference between this embodiment and embodiment 1 is that the water tank is an existing water tank without a drop section; the residual salt at the overlap of the wire rod obtained in this embodiment cannot be completely removed, and corrosion is aggravated after half a year.
[0188] It should be understood that in order to streamline the present disclosure and aid understanding of one or more of the various inventive aspects, in the above description of exemplary embodiments of the invention, various features of the invention are sometimes grouped together into a single embodiment, figure, or description thereof. However, this disclosed method should not be interpreted as reflecting an intention that the claimed invention requires more features than are expressly recited in each claim. Rather, as reflected in the claims, inventive aspects lie in less than all of the features of the previously disclosed embodiments. Accordingly, the claims that follow the detailed description are hereby expressly incorporated into this detailed description, with each claim standing on its own as a separate embodiment of the invention.
[0189] Although the present invention has been described with respect to a limited number of embodiments, it will be apparent to those skilled in the art, having benefit of the foregoing description, that other embodiments are contemplated within the scope of the invention thus described. Furthermore, it should be noted that the language used in this specification has been selected primarily for readability and didactic purposes, rather than for the purpose of explaining or limiting the subject matter of the present invention. Consequently, many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the appended claims. The disclosure of the present invention is intended to be illustrative rather than restrictive of the scope of the invention, which is defined by the appended claims.
[0190] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A high-speed wire online heat treatment equipment based on energy recycling, characterized in that: Including online heat treatment equipment, waste heat recovery system and molten salt energy storage peak-shaving power generation system; The online heat treatment equipment includes, from left to right, a quick cooling tank (1) through which the wire rod passes, an isothermal tank (3), an air cooling and controlled cooling device, a cleaning system and a drying device (14); The rapid cooling tank (1) and the isothermal tank (3) are both filled with molten salt; A lower tank body I (2) for circulating molten salt with the quick cooling tank (1) is provided below the quick cooling tank (1); a lower tank body II (4) for circulating molten salt with the isothermal tank (3) is provided below the isothermal tank (3); The waste heat recovery system includes a salt-salt heat exchanger (15) for exchanging heat with the molten salt in the lower tank body I (2) and the lower tank body II (4); The molten salt after heat exchange in the salt-salt heat exchanger (15) flows to the molten salt energy storage peak-shaving power generation system; The cleaning system is connected to the brine separation system (24); the cleaning system comprises a cleaning nozzle I (8), an annular air knife III (9), a stepped water tank (10), an annular air knife IV (11), a cleaning nozzle II (12) and an annular air knife V (13) which are arranged in sequence from left to right; the air-cooled cooling device comprises an annular air knife I (6) and annular air knife II (7) which are located between the isothermal tank (3) and the cleaning system; A roller conveyor is arranged inside the stepped water tank (10), and the roller conveyor is provided with 2 to 7 drop sections, the horizontal projection overlap distance between the tail of the previous drop section and the head of the next drop section is 100 mm to 1500 mm, each drop section forms a step shape, and each drop section includes 3 to 20 rollers arranged in sequence from left to right and extending obliquely upward, with a drop height of 100 mm to 500 mm, an inclination angle of 10° to 60°, and a roller spacing of 50 mm to 400 mm; an ultrasonic vibration device is arranged inside the stepped water tank (10); The molten salt energy storage peak-shaving power generation system comprises an intermediate storage tank (16) for storing the molten salt after the temperature is increased in the salt-salt heat exchanger (15); the intermediate storage tank (16) is connected to the high-temperature storage tank (18); the molten salt in the high-temperature storage tank (18) provides heat for the power generation equipment; the molten salt after the heat is stored in the low-temperature storage tank (22); the molten salt in the low-temperature storage tank (22) flows back to the shell side of the salt-salt heat exchanger (15) and the intermediate storage tank (16).
2. The device according to claim 1, characterized in that A fume collection system (5) is arranged above the quick cooling tank (1), the isothermal tank (3), the air cooling control equipment and the cleaning system.
3. The device according to claim 1, characterized in that The molten salt temperature of the rapid cooling tank (1) is 250-600°C, and the cooling rate of the rapid cooling tank (1) is at least 30°C / s; the molten salt temperature of the isothermal tank (3) is 400-585°C.
4. A process for high-speed wire online heat treatment equipment based on energy recycling according to any one of claims 1 to 3, characterized in that: The following steps are involved: S01, salt bath rapid cooling: after spinning, the wire rod temperature is 800-1050°C, and enters the rapid cooling tank (1) for rapid cooling and quenching in molten salt at 250-600°C, with a quenching time of 4-40s; S02, salt bath isothermal: the rapidly cooled quenched wire rod is placed in an isothermal bath (3) with molten salt at 400-585°C for isothermal transformation, with an isothermal time of 30-400s; S03, controlled cooling: after the wire rod comes out of the isothermal tank (3), it is purged with hot air at 200-550°C through the annular air knife I (6) for 5-20 seconds, and then purged with compressed air through the annular air knife II (7) for 5-30 seconds; S04, cleaning: After controlled cooling, the wire rod enters the cleaning system, and the residual salt on the surface is removed by the cleaning nozzle I (8), and then it is purged by the annular air knife III (9), and then enters the stepped water tank (10) in sequence to remove the residual salt on the surface of the wire rod, and then the surface salt water is removed by the annular air knife IV (11) and the cleaning nozzle II (12), and then the residual salt water is removed by the annular air knife V (13); S05, drying: the cleaned wire rod enters the drying equipment (14) for drying, and then is rolled up to obtain the finished product; S06, the molten salt for salt bath is discharged through the tube side of the salt-salt heat exchanger (15): the molten salt heated to 430-610°C in the quick cooling tank (1) and the isothermal tank (3) first overflows into the lower tank body I (2) and the lower tank body II (4), then enters the salt-salt heat exchanger (15) through the pipeline, and discharges heat through the tube side of the salt-salt heat exchanger (15), and then circulates to the lower tank body I (2) and the lower tank body II (4); S07, waste heat recovery system absorbs heat: cooling salt at 230-350°C enters the shell side of the salt-salt heat exchanger (15) from the low-temperature storage tank (22) of the molten salt energy storage peak-shaving power generation system, and the shell side cooling salt of the salt-salt heat exchanger (15) absorbs the heat of the high-temperature molten salt of the tube side of the salt-salt heat exchanger (15). After the shell side cooling salt of the salt-salt heat exchanger (15) absorbs heat and the temperature rises to 400-585°C, it returns to the molten salt energy storage peak-shaving power generation system to complete heat recovery; S08, molten salt energy storage peak-shaving power generation process: Heat storage during off-peak hours: The shell cooling salt of the salt-salt heat exchanger (15) absorbs heat and rises to 400-585°C before returning to the intermediate storage tank (16) of the molten salt energy storage peak-shaving power generation system. The molten salt in the intermediate storage tank (16) enters the molten salt storage system. The salt furnace (17) is heated to 550-600°C and then enters the high-temperature storage tank (18) to store heat; Heat release during peak power period: During peak power period, the heat in the 550-600°C molten salt in the high-temperature storage tank (18) is converted into high-temperature steam and enters the power generation equipment to generate electricity. After the molten salt temperature drops to 230-350°C, it enters the low-temperature storage tank (22) for circulation, playing the role of peak power generation; The molten salt is a cooling medium / heat transfer medium composed of two or more of potassium nitrate, sodium nitrate, lithium nitrate, calcium nitrate, silver nitrate, potassium nitrite, and sodium nitrite, and the water content in the molten salt for salt bath does not exceed 1wt.%.
5. Wire rod obtained by the process according to claim 4.
6. Application of the wire rod according to claim 5 in bainite cold heading steel, spring steel, tool steel, bearing steel, bridge cables, steel strands, tire bead cords, cutting wires, and diamond wires.
Citation Information
Patent Citations
Photovoltaic power generation system equipped with electric heating energy storage and operation method
CN113187680A
Process method for isothermal treatment and waste heat recovery after strip steel rolling
CN114833207A
Diamond wire brass wire salt bath isothermal quenching heat treatment process method
CN114836602A
Waste heat recycling system of heat treatment furnace
CN115950275A
High-speed wire online heat treatment equipment and process based on energy cyclic utilization