Preparation method for carbon-coated aluminum foil current collector for lithium battery
By de-oiling and etching the surface of aluminum foil, combining carbon nanotubes and conductive carbon black and other materials, modified polyaniline and fluorinated polyaniline are prepared, which solves the problem of uneven interface resistance and coating of aluminum foil current collector in lithium-ion batteries. , improves the conductivity and adhesion of lithium batteries, and ensures the electrochemical performance and safety of batteries.
Patent Information
- Application Number
- PCT/CN2023/141368
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2023-12-25
- Publication Date
- 2024-11-21
AI Technical Summary
Traditional aluminum foil or copper foil current collectors have problems with large interface resistance and uneven coating in lithium-ion batteries, which affect electrochemical performance and safety, and the residual rolling oil on the surface of the foil affects the adhesion ability of the carbon coated layer.
By performing surface oil removal and chemical etching treatment on aluminum foil, conductive paste is prepared using materials such as carbon nanotubes and conductive carbon black, and materials such as end amino tree macromolecules and epoxy resins are used to improve the binding force and conductivity of the binder. Properties, the modified polyaniline and fluorinated polyaniline are formed to enhance the conductivity and adhesion of the carbon coated current collector.
The conductivity and adhesion of the carbon-coated current collector of lithium batteries is improved, the electrical and safety performance of the battery is ensured, the coating is removed, and the stability and energy storage performance of lithium batteries are enhanced.
Smart Images

Figure PCTCN2023141368-FTAPPB-I100001 
Figure PCTCN2023141368-FTAPPB-I100002
Abstract
Description
Preparation method of aluminum foil coated carbon current collector for lithium battery Technical Field
[0001] The present application relates to the technical field of carbon-coated current collectors for lithium batteries, and specifically to a method for preparing a carbon-coated aluminum foil current collector for lithium batteries. Background Art
[0002] Lithium-ion batteries are widely used in many fields, including automobiles and mobile phones, due to their high energy density. Lithium batteries are primarily composed of positive and negative electrode active materials, electrolytes, separators, and positive and negative electrode current collectors. Currently, aluminum foil, copper foil, composite aluminum foil, composite copper foil, and carbon-coated aluminum foil, carbon-coated copper foil, composite carbon-coated aluminum foil, and composite carbon-coated copper foil with improved surface carbon coating are the primary materials used to transmit electrons. Traditional aluminum or copper foil current collectors suffer from high interfacial resistance, while carbon-coated current collectors can change the interfacial resistance and improve battery charging and discharging. However, the carbon coating is significantly affected by the raw material aluminum foil during the preparation process, which can easily lead to uneven coating and pose potential risks to the electrochemical performance and safety of lithium-ion batteries. To improve the stability of carbon-coated current collectors in power lithium-ion batteries, lithium-ion carbon-coated current collectors must consider reducing the impact of residual rolling oil on the foil surface on the carbon coating layer. The cleanliness of the foil surface can be a key factor to improve. The sodium borate used in aluminum foil treatment will leave a small amount of borate ions on the surface of the aluminum foil, thereby improving the corrosion resistance of the aluminum foil during battery use; and the rolling oil on the surface of the aluminum foil will affect the adhesion of the carbon coating and the positive electrode material to the current collector, seriously affecting the safety, charging and discharging and energy storage performance of the lithium battery.
[0003] Summary of the Invention
[0004] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0005] The purpose of this application is to provide a method for preparing an aluminum foil-coated carbon current collector for lithium batteries to solve the problems raised in the above background technology.
[0006] In order to solve the above technical problems, this application provides the following technical solutions:
[0007] Step 1: Degrease the surface of the aluminum foil and chemically etch both sides of the aluminum foil using an etching solution; then wash and dry the etched aluminum foil to obtain a current collector;
[0008] Step 2: mixing carbon nanotubes with sulfur powder, introducing nitrogen, and reacting at high temperature to obtain thiol-modified carbon nanotubes; dispersing the amino-terminated dendrimers and thiol-modified carbon nanotubes in pure water to obtain a mixed dispersion, ultrasonically treating the mixture, and coating the mixture on both sides of an aluminum foil current collector under vacuum conditions, followed by drying to obtain a pretreated aluminum foil current collector;
[0009] Step 3: Aniline, ammonium persulfate, and citric acid solution are mixed and stirred to react to obtain doped polyaniline; the doped polyaniline is crushed and dispersed in pure water, sodium hydroxide and 2-chloroethylamine hydrochloride are added, the temperature is increased to react, washed, and dried to obtain modified polyaniline; the modified polyaniline is dispersed in anhydrous ethanol, tridecafluorooctyltrimethoxysilane is added, ultrasonicated, washed, and dried to obtain fluorinated polyaniline;
[0010] Step 4: Mix and stir conductive carbon black, fluorinated polyaniline, epoxy resin, nanosilver particles, polyvinyl pyrrolidone, water, and ethylene glycol to obtain a conductive slurry; apply the conductive slurry to both sides of the pretreated aluminum foil current collector, and bake to obtain an aluminum foil-coated carbon current collector for lithium batteries.
[0011] Optionally, in step 1, the specific method for degreasing the surface of the aluminum foil is: electrolytic degreasing at a speed of 20 to 100 m / min and a corona power of 6 to 30 kW.
[0012] Optionally, in step 1, the etching solution comprises, by weight, 69-95% deionized water, 0.5-10% sodium hydroxide, 0.1-20% sodium borate, and 0.03-1% sodium gluconate.
[0013] Optionally, in step 2, the specific preparation method of the thiolated carbon nanotubes is: by weight, 0.5 to 1 parts of carbon nanotubes and 2 to 4 parts of sulfur powder are mixed, nitrogen is introduced, and the mixture is reacted at 170 to 190° C. for 12 to 16 hours.
[0014] Optionally, in step 2, the mixed dispersion comprises, by weight, 9 to 12 parts of amino-terminated dendrimers, 4 to 6 parts of thiol-modified carbon nanotubes, and 100 to 120 parts of pure water.
[0015] Optionally, in step 3, the specific preparation method of the doped polyaniline is: by weight, 9 to 12 parts of aniline, 18 to 20 parts of ammonium persulfate, and 20 to 30 parts of citric acid solution are stirred and reacted for 20 to 24 hours.
[0016] Optionally, in step 3, the specific preparation method of the modified polyaniline is as follows: by weight, 3 to 5 parts of doped polyaniline are crushed and dispersed in pure water, sodium hydroxide is added to adjust the pH value to 9 to 10, 1 to 2 parts of 2-chloroethylamine hydrochloride are added, the temperature is raised to 60 to 70° C., the reaction is carried out for 16 to 24 hours, and the modified polyaniline is obtained by washing and drying.
[0017] Optionally, in step 3, the specific preparation method of the fluorinated polyaniline is: taking 6 to 10 parts by weight of modified polyaniline and dispersing them in anhydrous ethanol, adding 3 to 4 parts of tridecafluorooctyltrimethoxysilane, ultrasonicating for 4 to 6 hours, washing, and drying.
[0018] Optionally, in step 4, the contents of the components in the conductive paste are, by weight, 15 to 20 parts of conductive carbon black, 8 to 10 parts of fluorinated polyaniline, 4 to 6 parts of epoxy resin, 2 to 3 parts of nanosilver particles, 6 to 8 parts of polyvinyl pyrrolidone, 30 to 38 parts of water, and 6 to 12 parts of ethylene glycol.
[0019] Compared with the prior art, the beneficial effects achieved by the present application are as follows: the present application first degreases and etches the surface of the aluminum foil to obtain an aluminum foil current collector. In order to improve the bonding strength between the conductive paste and the aluminum foil current collector, the binder in the conductive paste is selected from epoxy resin, and the current collector is pretreated with amino-terminated dendrimers. The amino-terminated dendrimers carry multiple amino groups and can self-assemble into films. On the one hand, the etching solution contains sodium hydroxide, and the surface of the aluminum foil current collector treated with the etching solution is rich in hydroxyl groups, which can generate hydrogen bonds with amino groups, thereby improving the bonding strength of the amino-terminated dendrimer film on the aluminum foil surface; on the other hand, the amino groups can promote the curing of the epoxy resin, thereby improving the bonding effect. The thiol-modified carbon nanotubes have good dispersibility and can coordinate with metals to achieve stable loading. Mixing with amino-terminated dendrimers can improve the conductive properties. When preparing the conductive paste, conductive carbon black is selected as the conductive material, and polyaniline and nano-silver particles are added as conductive auxiliary materials. Doped polyaniline is prepared by doping with citric acid, introducing hydroxyl and carboxyl groups, introducing amino groups using 2-chloroethylamine hydrochloride, and modifying it with tridecafluorooctyltrimethoxysilane to obtain fluorinated polyaniline. The amino group can promote the curing of epoxy resin and improve the dispersibility of polyaniline in epoxy resin. The introduction of fluorine not only improves the bonding strength of epoxy resin, but also improves heat resistance and mechanical strength. The carbon-coated current collector prepared by the process of this application has better conductivity and is not easy to fall off. The adhesive has strong bonding with the conductive powder and aluminum foil current collector and is not easy to fall off, thereby ensuring the electrical performance and safety performance of the lithium battery.
[0020] Still other aspects will become apparent upon reading and understanding the detailed description. DETAILED DESCRIPTION
[0021] The following is a clear and complete description of the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of them. Based on the embodiments of this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.
[0022] The main materials and their sources in the following examples are: amino-terminated dendrimers are from Chenyuan New Materials, brand CYD-110, with a molecular formula of C 62 H 128 N 26 O 12, the number of terminal amino groups is 8; aluminum foil comes from Dingsheng New Materials; sodium hydroxide (CAS No.: 1310-73-2), sodium borate (CAS No.: 1303-96-4), sodium gluconate (CAS No.: 527-07-1), ammonium persulfate (CAS No.: 7727-54-0), citric acid (CAS No.: 77-92-9), 2-chloroethylamine hydrochloride (CAS No.: 870-24-6), tridecafluorooctyltrimethoxysilane ( The raw materials used in the study were: polyvinyl pyrrolidone K30 (CAS No.: 9003-39-8), ethylene glycol (CAS No.: 107-21-1), aniline (CAS No.: 62-53-3), and sulfur powder from McLean; carbon nanotubes brand XFM01 and conductive carbon black brand XFI15 from Xianfeng Nano; epoxy resin from Dow 662E epoxy resin; and nanosilver particles from Zhongke Keyou, with a particle size of 10 nm.
[0023] Example 1
[0024] Step 1: Degrease the surface of a 13 μm aluminum foil at a speed of 20 m / min and a corona power of 6 kW, chemically etch both sides of the foil using an etching solution, rinse with water, and dry to obtain an etched aluminum foil current collector; wherein the etching solution comprises 69% deionized water, 10% sodium hydroxide, 20% sodium borate, and 1% sodium gluconate;
[0025] Step 2: 0.5 g of carbon nanotubes and 2 g of sulfur powder were mixed, nitrogen was introduced, and the mixture was reacted at 170° C. for 12 h to obtain thiolated carbon nanotubes; 9 g of amino-terminated dendrimers and 4 g of thiolated carbon nanotubes were dispersed in 100 g of pure water to obtain a mixed dispersion. After ultrasonic treatment for 30 min, the mixed dispersion was double-sided coated on an aluminum foil current collector under vacuum conditions and dried to obtain a pretreated aluminum foil current collector;
[0026] Step 3: 9 g of aniline, 18 g of ammonium persulfate, and 20 g of citric acid were stirred and reacted for 20 h to obtain doped polyaniline; 3 g of doped polyaniline was crushed and dispersed in pure water, sodium hydroxide was added to adjust the pH to 9, 1 g of 2-chloroethylamine hydrochloride was added, the temperature was raised to 60° C. and reacted for 16 h, washed, and dried to obtain modified polyaniline; 6 g of modified polyaniline was dispersed in anhydrous ethanol, 3 g of tridecafluorooctyltrimethoxysilane was added and ultrasonicated for 4 h, washed, and dried to obtain fluorinated polyaniline;
[0027] Step 4: Mix 15g of conductive carbon black, 8g of fluorinated polyaniline, 4g of epoxy resin, 2g of nanosilver particles, 6g of polyvinyl pyrrolidone, 30g of water, and 6g of ethylene glycol and stir for 3h to obtain a conductive slurry; use the conductive slurry to coat both sides of the pretreated aluminum foil current collector with a carbon coating layer thickness of 1μm, and bake at 90°C to obtain an aluminum foil carbon-coated current collector for lithium batteries.
[0028] Example 2
[0029] Step 1: Degrease the surface of a 13 μm aluminum foil at a speed of 40 m / min and a corona power of 10 kW, chemically etch both sides of the foil using an etching solution, rinse with water, and dry to obtain an etched aluminum foil current collector; wherein the etching solution comprises 70% deionized water, 9% sodium hydroxide, 19.97% sodium borate, and 1.03% sodium gluconate;
[0030] Step 2: 0.6 g of carbon nanotubes and 2.2 g of sulfur powder were mixed and then nitrogen was introduced, and the mixture was reacted at 175° C. for 12.5 h to obtain thiolated carbon nanotubes; 9.5 g of amino-terminated dendrimers and 4.3 g of thiolated carbon nanotubes were dispersed in 105 g of pure water to obtain a mixed dispersion, which was ultrasonically treated for 30 min. The mixed dispersion was then coated on both sides of an aluminum foil current collector under vacuum conditions and dried to obtain a pretreated aluminum foil current collector;
[0031] Step 3: 9.5 g of aniline, 18.3 g of ammonium persulfate, and 22 g of citric acid were stirred and reacted for 20 h to obtain doped polyaniline; 3.3 g of doped polyaniline was crushed and dispersed in pure water, sodium hydroxide was added to adjust the pH to 9.5, 1.2 g of 2-chloroethylamine hydrochloride was added, the temperature was raised to 65° C. and the reaction was carried out for 20 h, followed by washing and drying to obtain modified polyaniline; 6.8 g of modified polyaniline was dispersed in anhydrous ethanol, 3.2 g of tridecafluorooctyltrimethoxysilane was added and ultrasonicated for 5 h, followed by washing and drying to obtain fluorinated polyaniline;
[0032] Step 4: Mix 16g of conductive carbon black, 8g of fluorinated polyaniline, 4.8g of epoxy resin, 2.2g of nanosilver particles, 6.3g of polyvinyl pyrrolidone, 32g of water, and 7.2g of ethylene glycol and stir for 4h to obtain a conductive slurry; use the conductive slurry to coat both sides of the pretreated aluminum foil current collector with a carbon coating thickness of 1μm, and bake at 90°C for 1min to obtain an aluminum foil carbon-coated current collector for lithium batteries.
[0033] Example 3
[0034] Step 1: Degrease the surface of a 13 μm aluminum foil at a speed of 40 m / min and a corona power of 10 kW, chemically etch both sides of the foil with an etching solution, rinse with water, and dry to obtain an etched aluminum foil current collector; wherein the etching solution comprises 89% deionized water, 10% sodium hydroxide, 0.5% sodium borate, and 0.5% sodium gluconate;
[0035] Step 2: 0.65 g of carbon nanotubes and 2.5 g of sulfur powder were mixed, nitrogen was introduced, and the mixture was reacted at 180° C. for 15 h to obtain thiolated carbon nanotubes; 10 g of amino-terminated dendrimers and 4.7 g of thiolated carbon nanotubes were dispersed in 106 g of pure water to obtain a mixed dispersion, which was ultrasonically treated for 30 min. The mixed dispersion was then coated on both sides of an aluminum foil current collector under vacuum conditions and dried to obtain a pretreated aluminum foil current collector;
[0036] Step 3: 10 g of aniline, 18.3 g of ammonium persulfate, and 23 g of citric acid were stirred and reacted for 22 h to obtain doped polyaniline; 4 g of doped polyaniline was crushed and dispersed in pure water, sodium hydroxide was added to adjust the pH to 9.5, 1.3 g of 2-chloroethylamine hydrochloride was added, the temperature was raised to 70° C. and reacted for 24 h, washed, and dried to obtain modified polyaniline; 8 g of modified polyaniline was dispersed in anhydrous ethanol, 3.4 g of tridecafluorooctyltrimethoxysilane was added and ultrasonicated for 6 h, washed, and dried to obtain fluorinated polyaniline;
[0037] Step 4: Mix 18g of conductive carbon black, 9g of fluorinated polyaniline, 5.2g of epoxy resin, 2.4g of nanosilver particles, 7g of polyvinyl pyrrolidone, 34g of water, and 8g of ethylene glycol and stir for 3h to obtain a conductive slurry; use the conductive slurry to coat both sides of the pretreated aluminum foil current collector with a carbon coating thickness of 1μm, and bake at 90°C for 1min to obtain an aluminum foil carbon-coated current collector for lithium batteries.
[0038] Example 4
[0039] Step 1: Degrease the surface of a 13 μm aluminum foil at a speed of 50 m / min and a corona power of 18 kW, chemically etch both sides of the foil using an etching solution, rinse with water, and dry to obtain an etched aluminum foil current collector; wherein the etching solution comprises 92% deionized water, 0.5% sodium hydroxide, 6.5% sodium borate, and 1% sodium gluconate;
[0040] Step 2: 0.8 g of carbon nanotubes and 3.3 g of sulfur powder were mixed, nitrogen was introduced, and the mixture was reacted at 180° C. for 12 h to obtain thiolated carbon nanotubes; 10.3 g of amino-terminated dendrimers and 4.9 g of thiolated carbon nanotubes were dispersed in 110 g of pure water to obtain a mixed dispersion. After ultrasonic treatment for 30 min, the mixed dispersion was double-sided coated on an aluminum foil current collector under vacuum conditions and dried to obtain a pretreated aluminum foil current collector;
[0041] Step 3: 10 g of aniline, 20 g of ammonium persulfate, and 25 g of citric acid were stirred and reacted for 22 h to obtain doped polyaniline; 4.3 g of doped polyaniline was crushed and dispersed in pure water, sodium hydroxide was added to adjust the pH to 10, 1.8 g of 2-chloroethylamine hydrochloride was added, the temperature was raised to 65° C. and reacted for 20 h, washed, and dried to obtain modified polyaniline; 8.3 g of modified polyaniline was dispersed in anhydrous ethanol, 3.7 g of tridecafluorooctyltrimethoxysilane was added and ultrasonicated for 6 h, washed, and dried to obtain fluorinated polyaniline;
[0042] Step 4: Mix 20g of conductive carbon black, 8g of fluorinated polyaniline, 5g of epoxy resin, 2.7g of nanosilver particles, 7.4g of polyvinyl pyrrolidone, 35g of water, and 10g of ethylene glycol and stir for 4h to obtain a conductive slurry; use the conductive slurry to coat both sides of the pretreated aluminum foil current collector with a carbon coating thickness of 1μm, and bake at 90°C for 1min to obtain an aluminum foil carbon-coated current collector for lithium batteries.
[0043] Example 5
[0044] Step 1: Degrease the surface of a 13 μm aluminum foil at a speed of 60 m / min and a corona power of 22 kW, chemically etch both sides of the foil using an etching solution, rinse with water, and dry to obtain an etched aluminum foil current collector; wherein the etching solution comprises 75% deionized water, 10% sodium hydroxide, 14.4% sodium borate, and 0.6% sodium gluconate;
[0045] Step 2: 0.8 g of carbon nanotubes and 3.2 g of sulfur powder were mixed, nitrogen was introduced, and the mixture was reacted at 180° C. for 14 h to obtain thiolated carbon nanotubes; 10.6 g of amino-terminated dendrimers and 5.2 g of thiolated carbon nanotubes were dispersed in 115 g of pure water to obtain a mixed dispersion. After ultrasonic treatment for 30 min, the mixed dispersion was double-sided coated on an aluminum foil current collector under vacuum conditions and dried to obtain a pretreated aluminum foil current collector;
[0046] Step 3: 11 g of aniline, 19 g of ammonium persulfate, and 30 g of citric acid were stirred and reacted for 20 h to obtain doped polyaniline; 3 g of doped polyaniline was crushed and dispersed in pure water, sodium hydroxide was added to adjust the pH to 9, 2 g of 2-chloroethylamine hydrochloride was added, the temperature was raised to 70° C. and reacted for 24 h, washed, and dried to obtain modified polyaniline; 9 g of modified polyaniline was dispersed in anhydrous ethanol, 3.3 g of tridecafluorooctyltrimethoxysilane was added and ultrasonicated for 5 h, washed, and dried to obtain fluorinated polyaniline;
[0047] Step 4: Mix 18g of conductive carbon black, 10g of fluorinated polyaniline, 6g of epoxy resin, 2g of nanosilver particles, 6g of polyvinyl pyrrolidone, 30g of water, and 10g of ethylene glycol and stir for 3.5h to obtain a conductive slurry; use the conductive slurry to coat both sides of the pretreated aluminum foil current collector with a carbon coating thickness of 1μm, and bake at 90°C for 1min to obtain an aluminum foil carbon-coated current collector for lithium batteries.
[0048] Example 6
[0049] Step 1: Degreasing the surface of a 13 μm aluminum foil at a speed of 100 m / min and a corona power of 30 kW, chemically etching both sides of the foil with an etching solution, washing with water, and drying the foil to obtain an etched aluminum foil current collector; wherein the etching solution comprises 92% deionized water, 0.9% sodium hydroxide, 7% sodium borate, and 0.1% sodium gluconate;
[0050] Step 2: 1g of carbon nanotubes and 4g of sulfur powder were mixed, nitrogen was introduced, and the mixture was reacted at 190°C for 16h to obtain thiolated carbon nanotubes; 12g of amino-terminated dendrimers and 6g of thiolated carbon nanotubes were dispersed in 120g of pure water to obtain a mixed dispersion. After ultrasonic treatment for 30min, the mixed dispersion was double-sided coated on an aluminum foil current collector under vacuum conditions and dried to obtain a pretreated aluminum foil current collector;
[0051] Step 3: 12 g of aniline, 20 g of ammonium persulfate, and 30 g of citric acid solution were stirred and reacted for 24 h to obtain doped polyaniline; 5 g of doped polyaniline was crushed and dispersed in pure water, sodium hydroxide was added to adjust the pH to 10, 2 g of 2-chloroethylamine hydrochloride was added, the temperature was raised to 70° C. and reacted for 24 h, washed, and dried to obtain modified polyaniline; 10 g of modified polyaniline was dispersed in anhydrous ethanol, 4 g of tridecafluorooctyltrimethoxysilane was added and ultrasonicated for 6 h, washed, and dried to obtain fluorinated polyaniline;
[0052] Step 4: Mix 20g of conductive carbon black, 10g of fluorinated polyaniline, 6g of epoxy resin, 3g of nanosilver particles, 8g of polyvinyl pyrrolidone, 38g of water, and 12g of ethylene glycol and stir for 4h to obtain a conductive slurry; use the conductive slurry to coat both sides of the pretreated aluminum foil current collector with a carbon coating thickness of 1μm, and bake at 90°C for 1min to obtain an aluminum foil carbon-coated current collector for lithium batteries.
[0053] Comparative Example 1
[0054] Aluminum foil coated carbon current collector for lithium batteries was prepared using conventional technology.
[0055] Step 1: Degrease the surface of a 13 μm aluminum foil at a speed of 20 m / min and a corona power of 6 kW, chemically etch both sides of the foil using an etching solution, rinse with water, and dry to obtain an etched aluminum foil current collector; wherein the etching solution comprises 69% deionized water, 10% sodium hydroxide, 20% sodium borate, and 1% sodium gluconate;
[0056] Step 2: Mix 15g of conductive carbon black, 4g of epoxy resin, 2g of nanosilver particles, 6g of polyvinyl pyrrolidone, 30g of water, and 6g of ethylene glycol and stir for 3h to obtain a conductive slurry; use the conductive slurry to coat both sides of the pretreated aluminum foil current collector with a carbon coating thickness of 1μm, and bake at 90°C to obtain an aluminum foil carbon-coated current collector for lithium batteries.
[0057] Comparative Example 2
[0058] The surface of the aluminum foil current collector is not pretreated by using amino-terminated dendrimers or thiol-modified carbon nanotube dispersion.
[0059] Step 1: Degrease the surface of a 13 μm aluminum foil at a speed of 40 m / min and a corona power of 10 kW, chemically etch both sides of the foil using an etching solution, rinse with water, and dry to obtain an etched aluminum foil current collector; wherein the etching solution comprises 70% deionized water, 9% sodium hydroxide, 19.97% sodium borate, and 1.03% sodium gluconate;
[0060] Step 2: 9.5 g of aniline, 18.3 g of ammonium persulfate, and 22 g of citric acid were stirred and reacted for 20 h to obtain doped polyaniline; 3.3 g of doped polyaniline was crushed and dispersed in pure water, sodium hydroxide was added to adjust the pH to 9.5, 1.2 g of 2-chloroethylamine hydrochloride was added, the temperature was raised to 65° C. and reacted for 20 h, washed, and dried to obtain modified polyaniline; 6.8 g of modified polyaniline was dispersed in anhydrous ethanol, 3.2 g of tridecafluorooctyltrimethoxysilane was added and ultrasonicated for 5 h, washed, and dried to obtain fluorinated polyaniline;
[0061] Step 3: Mix 16g of conductive carbon black, 8g of fluorinated polyaniline, 4.8g of epoxy resin, 2.2g of nanosilver particles, 6.3g of polyvinyl pyrrolidone, 32g of water, and 7.2g of ethylene glycol and stir for 4h to obtain a conductive slurry; use the conductive slurry to coat both sides of the pretreated aluminum foil current collector with a carbon coating thickness of 1μm, and bake at 90°C for 1min to obtain an aluminum foil carbon-coated current collector for lithium batteries.
[0062] Comparative Example 3
[0063] The surface of the aluminum foil current collector is pretreated using amino-terminated dendrimers and carbon nanotube dispersions.
[0064] Step 1: Degrease the surface of a 13 μm aluminum foil at a speed of 40 m / min and a corona power of 10 kW, chemically etch both sides of the foil with an etching solution, rinse with water, and dry to obtain an etched aluminum foil current collector; wherein the etching solution comprises 89% deionized water, 10% sodium hydroxide, 0.5% sodium borate, and 0.5% sodium gluconate;
[0065] Step 2: Disperse 10 g of amino-terminated dendrimers and 4.7 g of carbon nanotubes in 106 g of pure water to obtain a mixed dispersion. After ultrasonic treatment for 30 min, the mixed dispersion was double-sided coated on an aluminum foil current collector under vacuum conditions and dried to obtain a pretreated aluminum foil current collector.
[0066] Step 3: 10 g of aniline, 18.3 g of ammonium persulfate, and 23 g of citric acid were stirred and reacted for 22 h to obtain doped polyaniline; 4 g of doped polyaniline was crushed and dispersed in pure water, sodium hydroxide was added to adjust the pH to 9.5, 1.3 g of 2-chloroethylamine hydrochloride was added, the temperature was raised to 70°C, the reaction was continued for 24 h, and the modified polyaniline was obtained by washing and drying; 8 g of the modified polyaniline was dispersed in anhydrous ethanol, 3.4 g of tridecafluorooctyltrimethoxysilane was added, and the mixture was ultrasonically reacted for 6 h, washed, and dried to obtain fluorinated polyaniline;
[0067] Step 4: Mix 18g of conductive carbon black, 9g of fluorinated polyaniline, 5.2g of epoxy resin, 2.4g of nanosilver particles, 7g of polyvinyl pyrrolidone, 34g of water, and 8g of ethylene glycol and stir for 3h to obtain a conductive slurry; use the conductive slurry to coat both sides of the pretreated aluminum foil current collector with a carbon coating thickness of 1μm, and bake at 90°C for 1min to obtain an aluminum foil carbon-coated current collector for lithium batteries.
[0068] Comparative Example 4
[0069] Polyaniline was used to prepare the conductive paste.
[0070] Step 1: Degrease the surface of a 13 μm aluminum foil at a speed of 50 m / min and a corona power of 18 kW, chemically etch both sides of the foil using an etching solution, rinse with water, and dry to obtain an etched aluminum foil current collector; wherein the etching solution comprises 92% deionized water, 0.5% sodium hydroxide, 6.5% sodium borate, and 1% sodium gluconate;
[0071] Step 2: 0.8 g of carbon nanotubes and 3.3 g of sulfur powder were mixed, nitrogen was introduced, and the mixture was reacted at 180° C. for 12 h to obtain thiolated carbon nanotubes; 10.3 g of amino-terminated dendrimers and 4.9 g of thiolated carbon nanotubes were dispersed in 110 g of pure water to obtain a mixed dispersion. After ultrasonic treatment for 30 min, the mixed dispersion was double-sided coated on an aluminum foil current collector under vacuum conditions and dried to obtain a pretreated aluminum foil current collector;
[0072] Step 3: Mix 20g of conductive carbon black, 8g of polyaniline, 5g of epoxy resin, 2.7g of nanosilver particles, 7.4g of polyvinyl pyrrolidone, 35g of water, and 10g of ethylene glycol and stir for 4h to obtain a conductive slurry; use the conductive slurry to coat both sides of the pretreated aluminum foil current collector with a carbon coating thickness of 1μm, and bake at 90°C for 1min to obtain an aluminum foil carbon-coated current collector for lithium batteries.
[0073] Comparative Example 5
[0074] The doped polyaniline was first modified with tridecafluorooctyltrimethoxysilane and then further modified with 2-chloroethylamine hydrochloride.
[0075] Step 1: Degrease the surface of a 13 μm aluminum foil at a speed of 60 m / min and a corona power of 22 kW, chemically etch both sides of the foil using an etching solution, rinse with water, and dry to obtain an etched aluminum foil current collector; wherein the etching solution comprises 75% deionized water, 10% sodium hydroxide, 14.4% sodium borate, and 0.6% sodium gluconate;
[0076] Step 2: 0.8 g of carbon nanotubes and 3.2 g of sulfur powder were mixed, nitrogen was introduced, and the mixture was reacted at 180° C. for 14 h to obtain thiolated carbon nanotubes; 10.6 g of amino-terminated dendrimers and 5.2 g of thiolated carbon nanotubes were dispersed in 115 g of pure water to obtain a mixed dispersion. After ultrasonic treatment for 30 min, the mixed dispersion was double-sided coated on an aluminum foil current collector under vacuum conditions and dried to obtain a pretreated aluminum foil current collector;
[0077] Step 3: 11 g of aniline, 19 g of ammonium persulfate, and 30 g of citric acid were stirred and reacted for 20 h to obtain doped polyaniline; 9 g of doped polyaniline was dispersed in anhydrous ethanol, 3.3 g of tridecafluorooctyltrimethoxysilane was added, ultrasonicated for 5 h, washed, and dried to obtain fluorinated polyaniline; 3 g of fluorinated polyaniline was crushed and dispersed in pure water, sodium hydroxide was added to adjust the pH to 9, 2 g of 2-chloroethylamine hydrochloride was added, the temperature was raised to 70° C., the reaction was carried out for 24 h, washed, and dried to obtain modified polyaniline;
[0078] Step 4: Mix 18g of conductive carbon black, 10g of modified polyaniline, 6g of epoxy resin, 2g of nanosilver particles, 6g of polyvinyl pyrrolidone, 30g of water, and 10g of ethylene glycol and stir for 3.5h to obtain a conductive slurry; use the conductive slurry to coat both sides of the pretreated aluminum foil current collector with a carbon coating thickness of 1μm, and bake at 90°C for 1min to obtain an aluminum foil carbon-coated current collector for lithium batteries.
[0079] Comparative Example 6
[0080] The conductive paste was prepared by modifying polyaniline with 2-chloroethylamine hydrochloride.
[0081] Step 1: Degrease the surface of a 13 μm aluminum foil at a speed of 100 m / min and a corona power of 30 kW, then chemically etch both sides of the foil using an etching solution, rinse with water, and dry to obtain an etched aluminum foil current collector. The etching solution comprises 92% deionized water, 0.9% sodium hydroxide, 7% sodium borate, and 0.1% sodium gluconate.
[0082] Step 2: 1g of carbon nanotubes and 4g of sulfur powder were mixed, nitrogen was introduced, and the mixture was reacted at 190°C for 16h to obtain thiolated carbon nanotubes; 12g of amino-terminated dendrimers and 6g of thiolated carbon nanotubes were dispersed in 120g of pure water to obtain a mixed dispersion, which was ultrasonically treated for 30min and then coated on both sides of an aluminum foil current collector under vacuum conditions. After drying, a pretreated aluminum foil current collector was obtained;
[0083] Step 3: 12 g of aniline, 20 g of ammonium persulfate, and 30 g of citric acid solution were stirred and reacted for 24 h to obtain doped polyaniline; 5 g of doped polyaniline was crushed and dispersed in pure water, sodium hydroxide was added to adjust the pH value to 10, 2 g of 2-chloroethylamine hydrochloride was added, the temperature was raised to 70° C. and the reaction was carried out for 24 h, followed by washing and drying to obtain modified polyaniline;
[0084] Step 4: Mix 20g of conductive carbon black, 10g of modified polyaniline, 6g of epoxy resin, 3g of nanosilver particles, 8g of polyvinyl pyrrolidone, 38g of water, and 12g of ethylene glycol and stir for 4h to obtain a conductive slurry; use the conductive slurry to coat both sides of the pretreated aluminum foil current collector with a carbon coating thickness of 1μm, and bake at 90°C for 1min to obtain an aluminum foil carbon-coated current collector for lithium batteries.
[0085] experiment:
[0086] Performance tests were performed on Examples 1 to 6 and Comparative Examples 1 to 6, wherein:
[0087] Conductivity test: Use a probe tester to test the resistance of the carbon-coated aluminum foil current collector;
[0088] Adhesion test: LiFePO4 slurry was coated on carbon-coated aluminum foil current collector to make a surface density of 340g / m 2 , compacted density is 2.6g / cm 2 The electrode is used to test the bonding strength of the electrode;
[0089] The experimental results are shown in the following table:
[0090] in conclusion:
[0091] The data from Example 1 and Comparative Example 1 show that compared with conventional processes, the carbon-coated current collector prepared by this application has better conductivity and is not easy to fall off. The bonding force between the binder and the conductive powder is strong and is not easy to fall off. The data from Examples 2-3 and Comparative Examples 2-3 show that after pretreatment with the amino-terminated dendrimers and the thiol-modified carbon nanotube dispersion, the pole piece exhibits good conductivity and bonding strength. This is because, on the one hand, the amino-terminated dendrimers can self-assemble into a film loaded on the surface of the aluminum foil. On the other hand, after being treated with the etching solution, the sodium hydroxide in the etching solution reacts with the aluminum foil, making the aluminum foil surface rich in hydroxyl groups, which further form hydrogen bonds with the amino groups on the amino-terminated dendrimers. The film formed by the amino-terminated dendrimers can promote the curing of the epoxy resin, thereby improving the bonding strength. In addition, after the carbon nanotubes are thiol-modified, they can better coordinate with the metal aluminum foil and can be stably loaded on the aluminum foil surface, thereby ensuring that the amino-terminated dendrimer film does not affect the conductive properties of the current collector. The data from Examples 4-6 and Comparative Examples 4-6 show that citric acid is doped with polyaniline to obtain doped polyaniline. Citric acid carries multiple hydroxyl and carboxyl groups. Using 2-chloroethylamine hydrochloride to react with the hydroxyl groups can introduce amino groups, effectively improving the interaction between the polyaniline fragments and the epoxy resin binder. This improves the dispersion of the polyaniline in the epoxy resin and prevents it from falling off. Fluorinated polyaniline is obtained by reacting tridecafluorooctyltrimethoxysilane with carboxyl groups. The introduction of fluorine not only improves the adhesion to the epoxy resin but also improves heat resistance and mechanical strength. The data from Example 5 and Comparative Example 5 also show that the modification order of 2-chloroethylamine hydrochloride and tridecafluorooctyltrimethoxysilane cannot be adjusted because both hydroxyl and carboxyl groups in the doped polyaniline react with tridecafluorooctyltrimethoxysilane, while 2-chloroethylamine hydrochloride reacts only with hydroxyl groups. If tridecafluorooctyltrimethoxysilane is used first for modification, amino groups cannot be introduced. Simultaneous introduction of amino groups and fluorine on polyaniline is more effective than single modification.
[0092] Finally, it should be noted that the above description is merely a preferred embodiment of the present application and is not intended to limit the present application. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art may still modify the technical solutions described in the aforementioned embodiments or substitute equivalents for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included within the scope of protection of the present application.
Claims
1. A method for preparing a carbon-coated aluminum foil current collector for a lithium battery, comprising the following steps: Step 1: Degrease the surface of the aluminum foil and perform double-sided chemical etching using an etching solution; Washing with water and drying to obtain the etched aluminum foil current collector; Step 2: Mix the carbon nanotubes with sulfur powder, introduce nitrogen, and react at high temperature to obtain thiolated carbon nanotubes; disperse the amino-terminated dendrimers and thiolated carbon nanotubes in pure water to obtain a mixed dispersion, perform ultrasonic treatment, double-side coating on an aluminum foil current collector under vacuum conditions, and dry to obtain a pretreated aluminum foil current collector; Step 3: Aniline, ammonium persulfate and citric acid solution are mixed and stirred to obtain doped polyaniline; the doped polyaniline is crushed and dispersed in pure water, sodium hydroxide and 2-chloroethylamine hydrochloride are added, the temperature is increased to react, washed and dried to obtain modified polyaniline; the modified polyaniline is dispersed in anhydrous ethanol, tridecafluorooctyltrimethoxysilane is added, ultrasonicated, washed and dried to obtain fluorinated polyaniline; Step 4: Mix and stir conductive carbon black, fluorinated polyaniline, epoxy resin, nanosilver particles, polyvinyl pyrrolidone, water, and ethylene glycol to obtain a conductive slurry; apply the conductive slurry to both sides of the pretreated aluminum foil current collector, and dry to obtain an aluminum foil carbon-coated current collector for a lithium battery.
2. The method for preparing a carbon-coated aluminum foil current collector for lithium batteries according to claim 1, wherein: In step 1, the specific method for degreasing the surface of the aluminum foil is: electrolytic degreasing at a speed of 20 to 100 m / min and a corona power of 6 to 30 kW.
3. A method for preparing a carbon-coated aluminum foil current collector for lithium batteries according to claim 1 or 2, wherein: In step 1, the etching solution contains, by weight, 69-95% deionized water, 0.5-10% sodium hydroxide, 0.1-20% sodium borate, and 0.03-1% sodium gluconate.
4. A method for preparing a carbon-coated aluminum foil current collector for a lithium battery according to any one of claims 1 to 3, wherein: In step 2, the specific preparation method of the thiolated carbon nanotubes is: after mixing the carbon nanotubes and sulfur powder, nitrogen is introduced and reacted at 170-190° C. for 12-16 hours.
5. A method for preparing a carbon-coated aluminum foil current collector for lithium batteries according to any one of claims 1 to 4, wherein: In step 2, the contents of the components in the mixed dispersion are, by weight, 9 to 12 parts of amino-terminated dendrimers, 4 to 6 parts of thiol-modified carbon nanotubes, and 100 to 120 parts of pure water.
6. A method for preparing a carbon-coated aluminum foil current collector for a lithium battery according to any one of claims 1 to 5, wherein: In step 3, the specific preparation method of the doped polyaniline is: aniline, ammonium persulfate and citric acid solution are stirred and reacted for 20 to 24 hours.
7. A method for preparing a carbon-coated aluminum foil current collector for lithium batteries according to any one of claims 1 to 6, wherein: In step 3, the specific preparation method of the modified polyaniline is: crush the doped polyaniline and disperse it in pure water, add sodium hydroxide to adjust the pH value to 9-10, add 2-chloroethylamine hydrochloride, heat to 60-70° C. to react for 16-24 hours, wash and dry to obtain the modified polyaniline.
8. A method for preparing a carbon-coated aluminum foil current collector for lithium batteries according to any one of claims 1 to 7, wherein: In step 3, the specific preparation method of the fluorinated polyaniline is: taking the modified polyaniline and dispersing it in anhydrous ethanol, adding tridecafluorooctyltrimethoxysilane, ultrasonicating for 4 to 6 hours, washing, and drying.
9. A method for preparing a carbon-coated aluminum foil current collector for lithium batteries according to any one of claims 1 to 8, wherein: In step 4, the contents of the components in the conductive paste are, by weight, 15 to 20 parts of conductive carbon black, 8 to 10 parts of fluorinated polyaniline, 4 to 6 parts of epoxy resin, 2 to 3 parts of nanosilver particles, 6 to 8 parts of polyvinyl pyrrolidone, 30 to 38 parts of water, and 6 to 12 parts of ethylene glycol. 10 . An aluminum foil carbon-coated current collector prepared according to the method for preparing an aluminum foil carbon-coated current collector for a lithium battery according to any one of claims 1 to 9.
Citation Information
Patent Citations
Current collector carbon coated aluminum foil and its preparation method
CN102832392A
Carbon-coated aluminum foil for lithium ion batteries
CN109935837A
Carbon-coated aluminum foil for lithium battery and preparation method of carbon-coated aluminum foil
CN115050967A
Preparation method of carbon-coated aluminum foil current collector for lithium battery
CN116544421A
Nano-structure carbon layer foamed aluminium foil current collector with high electro-conductivity and fabrication method thereof
KR1020130120290A