Chemical end-capped polypiperazine pyrophosphate-modified ammonium polyphosphate with high temperature resistance and bleed out resistance, preparation method therefor, and apparatus and application thereof
Modification of ammonium polyphosphate through chemically end-capped focused piperazine phosphate, the temperature and precipitation resistance of ammonium polyphosphate is improved, and its insufficient stability at high temperatures is solved, and the flame retardant performance and production continuity of composite materials are improved. .
Patent Information
- Application Number
- PCT/CN2024/105802
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-17
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-21
AI Technical Summary
The flame retardant effect, stability and other properties of existing ammonium polyphosphate are not ideal, especially in terms of high temperature and precipitation performance, which is difficult to meet the actual application needs.
Using chemically blocked focused piperazine phosphate modified ammonium polyphosphate, thermal polymerization and dehydration are dehydrated by thermal polymerization and ammonium polyphosphate, and thermally treated with the capping agent to form a chemically blocked with high temperature resistance and precipitation resistance. Focused piperazine phosphate modified ammonium polyphosphate, used for the preparation of flame retardant polypropylene.
It significantly improves the temperature and precipitation resistance of ammonium polyphosphate, improves the flame retardant performance of composite materials, ensures the whiteness and thermal stability of the product, and solves the problems of thermal decomposition temperature instability and continuous production of solid-phase synthesis products.
Smart Images

Figure CN2024105802_21112024_PF_FP_ABST
Abstract
Description
A chemically terminated focused piperazine phosphate modified ammonium polyphosphate with high temperature resistance and precipitation resistance, as well as its preparation method, device and application Technical Field
[0001] Technical Field
[0002] The present invention relates to the technical field of flame retardants, and in particular to a chemically terminated focused piperazine phosphate modified ammonium polyphosphate with high temperature resistance and precipitation resistance, as well as a preparation method, a device and an application thereof. Background Art
[0003] Ammonium polyphosphate (APP), also known as ammonium polyphosphate or condensed ammonium phosphate, is a long-chain inorganic polymer containing phosphorus and nitrogen. Its molecular formula is: (NH4) n+2 PnO 3n+1 Ammonium polyphosphate (APP) can be classified by its degree of polymerization into three types: oligomeric, mesomeric, and high-polymeric. The higher the degree of polymerization, the lower its water solubility, while a lower degree of polymerization increases its water solubility. Based on its structure, it can be divided into crystalline and amorphous forms. Crystalline ammonium polyphosphate is a long-chain, water-insoluble salt. Due to its advantages such as good chemical stability, low hygroscopicity, excellent dispersibility, low specific gravity, and low toxicity, it has been widely used in recent years as a flame retardant for plastics, rubber, and fibers. It can also be used to formulate intumescent fire-retardant coatings for fire protection on ships, trains, cables, and high-rise buildings. It is also used in the production of dry powder fire extinguishing agents for large-scale firefighting in coalfields, oil wells, and forests. The degree of polymerization of APP is crucial to its quality as a flame retardant. A higher degree of polymerization increases thermal stability and water resistance. APP serves as the acid and gas source for halogen-free intumescent flame retardant (IFR) systems. During combustion, APP forms an intumescent char layer in the condensed phase, isolating oxygen. It also generates ammonia, water vapor, and other gases in the gas phase to dilute the concentration of combustible gases, thereby slowing the combustion process. When ammonium polyphosphate is used as a flame retardant, it often needs to be combined with other substances that can provide carbon sources and gas sources to form an intumescent flame retardant in order to better exert the flame retardant effect.
[0004] Those skilled in the art have attempted to improve the performance of ammonium polyphosphate (AMP) through synthetic methods. Currently, the main raw materials for AMP production include phosphoric acid, phosphorus pentoxide, diammonium dihydrogen phosphate (MAP), diammonium hydrogen phosphate (DAP), urea phosphate, urea, melamine (MA), and dicyandiamide. Synthesis methods are under investigation both domestically and internationally, hoping to find a method for synthesizing AMP with a high degree of polymerization, low water solubility, and high temperature resistance. Current research results, both domestically and internationally, indicate that improved synthesis processes have yielded some improvements in AMP's degree of polymerization, water solubility, and thermal stability. However, due to structural limitations, these methods have not fundamentally resolved the challenges facing AMP, leading to the need to consider other methods for improving AMP.
[0005] Those skilled in the art have also tried to improve the performance of ammonium polyphosphate by compounding with other ingredients. For example, the prior art document "Zhang Yan, Research on the Flame Retardant Application of Piperazine Pyrophosphate / Ammonium Polyphosphate on Wollastonite Reinforced Polypropylene, Plastics Industry, May 2022" reported the research results of the combined use of ammonium polyphosphate (APP) and piperazine pyrophosphate (PAPP) to increase the flame retardant effect on wollastonite reinforced polypropylene. Piperazine pyrophosphate has good water resistance and charring properties, and contains acid source, carbon source and gas source. It can be used as a single-component IFR to play a flame retardant role in both the gas phase and the condensed phase. Although the use of piperazine pyrophosphate can overcome the shortcomings of ammonium polyphosphate, in the flame retardant system, piperazine pyrophosphate / ammonium polyphosphate needs to be added in a larger amount to play a role, and the addition of a large amount of flame retardant will have an adverse effect on the mechanical properties of the main material.
[0006] In addition to trying to compound ammonium polyphosphate with other flame retardants, researchers in this field have also tried to chemically modify ammonium polyphosphate. The widely used surface modification, surface activation treatment and microencapsulation coating are difficult to achieve ideal results due to the inherent physical and chemical properties of ammonium polyphosphate. The main reasons are as follows: (1) Defects in the molecular structure of ammonium polyphosphate itself. Regardless of the crystal form, the ammonium salt will begin to decompose at around 300°C, so its maximum decomposition temperature is unlikely to exceed 320°C; and the ammonium polyphosphate molecular chain is easily degraded and broken in acidic and alkaline solutions, so its modification can only be carried out in a relatively mild environment. (2) As a typical inorganic macromolecular polyphosphate, it has no active reactive groups, so it is difficult to chemically modify it structurally. After microencapsulation treatment, there is no chemical bond between the core material and the capsule wall material. It is just a simple physical coating. During the process of crushing and processing and blending, it is easily affected by external forces and shear forces, which damages the shell layer and reduces the effect of microencapsulation.
[0007] In summary, although ammonium polyphosphate has the advantages of low cost, environmental protection, and wide application, due to its own molecular structure defects and other reasons, the comprehensive performance of ammonium polyphosphate cannot meet the needs of practical applications. It is urgent to seek a new modification method of ammonium polyphosphate to comprehensively improve the performance of ammonium polyphosphate. Summary of the Invention
[0008] The present invention aims to provide a chemically terminated focused piperazine phosphate modified ammonium polyphosphate flame retardant with high temperature resistance and precipitation resistance, so as to solve the technical problems in the prior art of unsatisfactory flame retardant effect, stability and other properties of ammonium polyphosphate.
[0009] In order to achieve the above object, the present invention adopts the following technical solutions:
[0010] A chemically terminated piperazine phosphate-modified ammonium polyphosphate flame retardant with high heat resistance and precipitation resistance, wherein the structural formula of the piperazine phosphate-modified ammonium polyphosphate is shown in the following chemical formula, and the piperazine phosphate-modified ammonium polyphosphate is terminated by a capping agent;
[0011]
[0012] Wherein, n=300-1500, m=1000-2000; the end-capping agent is a nitrogen-containing compound having no hydroxyl group and an NH bond.
[0013] This solution also provides a method for preparing a chemically terminated focused piperazine phosphate modified ammonium polyphosphate flame retardant with high temperature resistance and precipitation resistance, comprising the following steps in sequence:
[0014] S1: Piperazine diphosphate is dehydrated by thermal polymerization to obtain focused piperazine phosphate;
[0015] S2: focusing piperazine phosphate and ammonium polyphosphate through thermal polymerization and dehydration to obtain focused piperazine phosphate modified ammonium polyphosphate;
[0016] S3: After the focused piperazine phosphate modified ammonium polyphosphate and the blocking agent are heat-treated, chemically blocked focused piperazine phosphate modified ammonium polyphosphate is obtained.
[0017] This solution also provides a highly heat-resistant and precipitation-resistant chemically terminated focused piperazine phosphate modified ammonium polyphosphate flame retardant for use in flame-retardant polypropylene.
[0018] Furthermore, the end-capping agent includes at least one of R-NH2, R=NH, melamine, urea, biguanidine and iminodiacetonitrile; and R is an alkyl group with 1 to 4 carbon atoms.
[0019] Furthermore, the molar ratio of the focused piperazine phosphate to the ammonium polyphosphate is 2.0-2.1:1; and the molar ratio of the capping agent to the focused piperazine phosphate modified ammonium polyphosphate is 2.0-2.2:1.
[0020] Furthermore, the reaction processes of S1-S3 are all carried out in an inert gas environment; the reaction temperature, pressure and time of S1 are 120-320°C, 0.05-0.3MPa, and 30-240min, respectively; the reaction temperature, pressure and time of S2 are 150-280°C, 0.05-0.3MPa, and 30-180min, respectively; the reaction temperature, pressure and time of S3 are 120-350°C, 0.1-1.5MPa, and 30-240min, respectively.
[0021] Furthermore, the reaction processes of S1-S3 are all carried out in a thermal polymerization reaction device; the polymerization reaction device includes a rotary furnace and a temperature control unit; a reaction chamber is provided in the rotary furnace, and a stirring screw is coaxially provided in the reaction chamber; the temperature control unit is used to control the temperature in the reaction chamber; during the reaction process, the stirring screw and the reaction chamber maintain different rotation directions.
[0022] Furthermore, the rotation speed of the stirring screw is 30-300 rpm, and the rotation speed of the reaction chamber is 3-120 rpm.
[0023] Furthermore, the flame retardant polypropylene comprises, by weight, 70-78 parts of polypropylene, 10-20 parts of chemically terminated focused piperazine phosphate modified ammonium polyphosphate, 5-15 parts of melamine polyphosphate, 0.5-6 parts of flame retardant synergist, 0.5-2 parts of coupling agent, 0.3-3 parts of lubricant, and 0.2-0.5 parts of antioxidant.
[0024] Furthermore, the melt index of polypropylene is 0-100 g / 10 min; the 1% thermal weight loss of melamine polyphosphate is ≥ 360°C; the flame retardant synergist includes at least one of anhydrous zinc borate, 3.5-hydrate zinc borate, zinc oxide, and zirconium phosphate; the coupling agent is a silane coupling agent, including at least one of aminosilane coupling agent KH-9120, isocyanate silane coupling agent KT-930, epoxy silane coupling agent KH-1006 and KH-9130; the lubricant includes at least one of ethylene bisstearamide, pentaerythritol stearate, silicone and amide wax; and the antioxidant includes at least one of antioxidant 168, antioxidant 1010 and antioxidant 1098.
[0025] Furthermore, flame-retardant polypropylene is prepared by the following method: chemically capped focused piperazine phosphate modified ammonium polyphosphate, melamine polyphosphate and a flame retardant synergist are added to a mixer and stirred at room temperature for 5-30 minutes; then the mixer temperature is increased to 80-160°C, a coupling agent is added and stirring is continued for 10-30 minutes; after cooling to room temperature, polypropylene, a lubricant and an antioxidant are added and stirred for 5-30 minutes; and flame-retardant polypropylene is obtained by extruding using a twin-screw extruder.
[0026] In summary, this technical solution improves the heat resistance and precipitation resistance of ammonium polyphosphate by means of specific chemical end-capping and chemical modification of ammonium polyphosphate and focused piperazine phosphate. The flame retardant is applied to the preparation process of composite materials to improve the overall flame retardant properties of the composite materials. In addition, the synthesis equipment of this solution can ensure uniform heating and complete polymerization during the synthesis process without sticking to the reactor, solving the problems of unstable thermal decomposition temperature and continuous production of solid-phase synthesis products. The flame retardant obtained by this process has the characteristics of excellent whiteness and thermal stability. The flame retardant of this solution is particularly suitable for use in the preparation of flame-retardant polypropylene, and comprehensively improves the various properties of flame-retardant polypropylene.
[0027] The beneficial effects of this technical solution are:
[0028] (1) The existing ammonium polyphosphate's heat resistance, especially its precipitation resistance, cannot meet the product requirements. This patent improves the heat resistance and precipitation resistance while improving the flame retardant effect.
[0029] (2) The synthesis equipment of this scheme can be used for continuous scale-up production. Under the use of appropriate process parameters, the product whiteness (whiteness greater than 95%) and thermal stability (1% thermogravimetric loss greater than 280°C) can be guaranteed. During the synthesis process, the materials are heated evenly, the polymerization is uniform and complete, and the reaction kettle is not contaminated. This solves the problem of unstable thermal decomposition temperature of solid-phase synthesis products and solves the problem of continuous production.
[0030] (3) The flame retardant polyolefin flame retardant formula has been updated and adjusted (to improve flame retardancy, heat resistance and precipitation resistance). By compounding the flame retardant formula and adding about 15%, the flame retardant effect reaches 1.6mmV-0, and the product has passed the UL 746C water immersion test and the GB / T 2423.50 "double 85" test for 1000h without precipitation. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] FIG1 is a front view of a polymerization reaction apparatus for continuous production according to Example 1.
[0032] FIG2 is a cross-sectional view taken along line AA of FIG1 .
[0033] FIG3 is a front view (cross-sectional view) of the stirring screw of Example 1. FIG.
[0034] FIG4 is a TG chart of commercially available ammonium polyphosphate of Experimental Example 1. DETAILED DESCRIPTION
[0035] The present invention will be further described in detail below with reference to the examples, but the embodiments of the present invention are not limited thereto. Unless otherwise specified, the technical means used in the following examples and experimental examples are conventional means well known to those skilled in the art, and the materials, reagents, etc. used are all commercially available.
[0036] The specific reference numerals are: cylinder 1, hot oil tank 2, cold oil tank 3, driven gear 4, drive gear 5, oil chamber 6, stirring screw 7, first motor 8, feed port 9, nitrogen outlet 10, discharge port 11, nitrogen inlet 12, load-bearing wheel 13, second motor 14, support column 15, first conduit 16, first oil pump 17, second conduit 18, second oil pump 19, first rotary joint 20, first rotating conduit 21, second rotary joint 22, second rotating conduit 23, third conduit 24, frame 25, insulation layer 26.
[0037] Example 1: Chemically terminated focused piperazine phosphate modified ammonium polyphosphate
[0038] (1) Synthesis process
[0039] The synthesis process of chemically terminated focused piperazine phosphate modified ammonium polyphosphate is roughly as follows:
[0040] Step 1: Piperazine diphosphate (Formula (4)) is heat-treated at 120-320°C for 30-240 minutes. In the polymerization equipment of this scheme, in an inert gas environment (e.g., nitrogen), under a pressure environment of 0.05-0.3 MPa, it is thermally polymerized and dehydrated to condense into a focused piperazine phosphate of a certain molecular weight (Formula (5)). The intermediate piperazine diphosphate can be synthesized using conventional methods in the prior art. For example, phosphoric acid (Formula (2)) and piperazine (Formula (3)) are used in a molar ratio of 2.0-2.2:1, and under conditions of 60-150°C and 0.1-1.0 MPa (using a conventional reactor in the prior art), in a reaction system with water or alcohol as a solvent, and the intermediate piperazine diphosphate is obtained by dehydration condensation for 30-300 minutes. The intermediate piperazine diphosphate used in this scheme is synthesized and purified using existing technologies, and the specific process of its synthesis and purification will not be repeated.
[0041] Step 2: Modify ammonium polyphosphate (Formula (1)) with focused piperazine phosphate, with the ratio of the two being 2.0-2.1:1 (molar ratio), and heat-treat at 150-280°C for 30-180min under an inert gas environment (e.g., nitrogen) and a pressure environment of 0.05-0.3MPa for thermal polymerization and dehydration to obtain focused piperazine phosphate modified ammonium polyphosphate (Formula (8)).
[0042] Step 3: Add a capping agent (the ratio of the capping agent to the focused piperazine phosphate modified ammonium polyphosphate is 2.0-2.2 parts: 1 part (molar ratio) and continue to heat treat in an inert gas environment (such as nitrogen) at a temperature of 120-350°C and a pressure of 0.1-1.5 MPa for 30-240 minutes. After cooling, grind the powder to obtain chemically capped focused piperazine phosphate modified ammonium polyphosphate (Formula (9), taking R-NH2 and R=NH as capping agents as an example).
[0043] The reaction equation for synthesizing the intermediate piperazine diphosphate in the prior art is shown in equation (10); the reaction equation for synthesizing focused piperazine phosphate is shown in equation (11) (first step); the reaction equation for modifying ammonium polyphosphate using focused piperazine phosphate is shown in equation (12) (second step); and the reaction equation for chemically end-capped focused piperazine phosphate modified ammonium polyphosphate is shown in equation (13) (using R-NH2 and R=NH as end-capping agents as an example) (third step). During the above three-step reaction process, the material stirring screw and the rotating furnace drum rotate in different directions. For example, the material stirring screw rotates counterclockwise at a speed of 30-300 rpm and the rotating furnace drum rotates clockwise at a speed of 3-120 rpm (preferably 3-60 rpm).
[0044] The end-capping agent is a nitrogen-containing compound without hydroxyl groups and having an NH bond, which may be: R-NH2 or R=NH, where R is an alkyl group with 1 to 4 carbon atoms; or melamine and its compounds without hydroxyl groups composed of R-NH2 and R=NH; or amino compounds without hydroxyl groups composed of R-NH2 and R=NH (for example, urea); or imino compounds without hydroxyl groups composed of R-NH2 and R=NH (for example, compounds containing guanidine groups (NH2)2-C=NH, biguanidine (1-(diaminomethylene)guanidine), and iminodiacetonitrile C4H5N3). In addition, in formulas (5), (8), (9), (11), and (12), n=300-1500. In formulas (1), (8), (9), (11), and (12), m=1000-2000. For ammonium polyphosphate (APP), a molecular weight range of more than 1000 is normally considered type II APP, which has a certain water resistance. If the molecular weight is too large, >2000, the molecular weight will be too large and not conducive to subsequent reactions. Therefore, m needs to be maintained at 1000-2000. In the subsequent examples and comparative examples, the ammonium polyphosphate used has an m value of 1000-1500.
[0045]
[0046] (2) Synthesis equipment
[0047] The dedicated equipment used in this technical solution is shown in Figure 1. The polymerization reaction equipment for continuous production includes a rotary furnace and a temperature control unit. The rotary furnace includes an inclined cylinder 1, and the temperature control unit includes a hot oil tank 2 and a cold oil tank 3.
[0048] Referring to Figures 1 and 2, a driven gear 4 is sleeved and fixed on the outside of the cylinder 1. The cylinder 1 and the driven gear 4 are concentrically arranged. There are two left and right drive gears 5 meshing with the driven gear 4, and the drive gear 5 drives the cylinder 1 to rotate. The cylinder 1 is a double-layer structure, including a coaxially arranged cylindrical inner wall and outer wall, an oil chamber 6 is formed between the inner wall and the outer wall, and the outer side of the outer wall is covered with an insulation layer 26. The cavity formed by the inner wall is a reaction chamber, and a stirring screw 7 is arranged in the reaction chamber. The upper and lower ends of the stirring screw 7 are rotatably connected to the top and bottom of the cylinder 1. The upper end of the stirring screw 7 is fixed to the output shaft of the first motor 8, and the first motor 8 is fixed on the frame 25. A feed port 9 and a nitrogen outlet 10 are provided at the top of the cylinder 1, and a discharge port 11 and a nitrogen inlet 12 are provided at the bottom of the cylinder 1. The outer wall of the cylinder 1 contacts two sets of upper and lower load-bearing wheels 13 (each set includes two load-bearing wheels 13). The load-bearing wheels 13 are fixed in position and rotatably connected to the frame 25, supporting the cylinder 1 and coordinating its rotation. The drive gear 5 is rotatably connected to the frame 25, and the second motor 14 is fixed to the frame 25. The drive gear 5 is driven by the second motor 14 through a conventional transmission structure in the prior art. The drive gear 5 drives the cylinder 1 to rotate via the driven gear 4. Several support columns 15 are provided in the oil chamber 6, parallel to the central axis of the cylinder 1. The upper and lower ends of the support columns 15 are fixed to the top and bottom of the cylinder 1.
[0049] The hot oil tank 2 is connected to a first conduit 16, which is equipped with a first oil pump 17. The cold oil tank 3 is connected to a second conduit 18, which is equipped with a second oil pump 19. The first conduit 16 is connected to a first rotating conduit 21 via a first rotary joint 20; the second conduit 18 is connected to a second rotating conduit 23 via a second rotary joint 22. One end of the first rotating conduit 21 is connected to the oil chamber 6 and is fixed to the bottom of the cylinder 1; one end of the second rotating conduit 23 is connected to the oil chamber 6 and is fixed to the top of the cylinder 1.
[0050] The temperature control unit also includes a third conduit 24. The lower end of the third conduit 24 is connected to two branches (branch A and branch B). Branch B connects to the first conduit 16, and branch A connects to the hot oil tank 2. Both branches A and B are equipped with corresponding control valves. The upper end of the third conduit 24 is connected to two branches (branch C and branch D). Branch D connects to the second conduit 18, and branch C connects to the cold oil tank 3. Both branches C and D are equipped with corresponding control valves. When the hot oil circulates, branch B and branch C are closed, the second oil pump 19 is turned off, the first oil pump 17 is turned on, and branch A and branch D are turned on. This creates a closed-loop circuit between the hot oil tank 2, the first conduit 16, the first rotating conduit 21, the oil chamber 6, the second rotating conduit 23, the second conduit 18, and the third conduit 24. Under the action of the first oil pump 17, the hot oil circulates throughout, maintaining the temperature within the reaction chamber. After the heating reaction is completed, the branch pipe A is closed, and the hot oil in the pipeline returns to the hot oil tank 2 under the action of the first oil pump 17 and the gravity of the hot oil. After the reaction is completed, the cold oil in the cold oil tank 3 is used to cool the reacted material.
[0051] When the cold oil is circulating, branch A and branch D are closed, the first oil pump 17 is turned off, branch B is turned on, branch C is turned on, and the second oil pump 19 is turned on. This forms a closed loop between the cold oil tank 3, the second conduit 18, the second rotating conduit 23, the oil chamber 6, the first rotating conduit 21, the first conduit 16, and the third conduit 24. Under the action of the second oil pump 18, the cold oil circulates through the reaction chamber, cooling it. After the cooling is complete, branch C is closed, and the cold oil in the pipeline is pumped back to the cold oil tank 3 under the action of the second oil pump 18. Following this process, hot oil circulation and cold oil circulation can be alternated according to actual needs, achieving continuous production.
[0052] The specific process of using the device is as follows:
[0053] A. At the beginning of the thermal polymerization reaction, the hot oil tank 2 begins operation, heating the oil to the processing temperature. Materials and inert protective gas are added to the reaction chamber, and the first oil pump 17 is started to press the hot oil in the hot oil tank 2 into the oil cavity 6 on the outer wall of the thermal polymerization rotary furnace barrel 1. The oil circulates between the hot oil tank 2 and the oil cavity 6 on the outer wall of the barrel 1, and the oil is quickly heated to the specified temperature and maintained at a constant temperature.
[0054] B. During the reaction, a circulation system is maintained between the hot oil tank 2 and the oil chamber 6 on the outer wall of the barrel 1 to maintain a constant temperature during the reaction time. The reaction pressure is adjusted by pumping or adding inert gas. Throughout the thermal polymerization process, the rotation direction of the stirring screw 7 remains opposite to that of the reaction chamber.
[0055] C. After the reaction is completed, the first oil pump 17 is started to pump the hot oil in the thermal polymerization reaction rotary furnace into the hot oil tank 2. Then, the second oil pump 19 is started to press the cold oil in the cold oil tank 3 into the oil cavity 6 on the outer wall of the thermal polymerization reaction cylinder 1. This allows the oil to circulate between the cold oil tank 3 and the oil cavity 6 on the outer wall of the rotary furnace, achieving rapid cooling.
[0056] D. After the temperature in the feed pipe drops to the specified temperature and the material is discharged, the second oil pump 19 is started to press the oil in the oil cavity 6 on the outer wall of the rotary furnace into the cold oil tank 3. The material and inert protective gas are then added. After the air in the feed pipe is exhausted, the hot oil in the hot oil tank 2 is pressed into the oil cavity 6 on the outer wall of the rotary furnace shell 1. Steps A to D are repeated to achieve continuous production.
[0057] In this synthesis process, the material (piperazine diphosphate) and an inert protective gas (nitrogen, 0.05-0.3 MPa) are added to a reaction chamber. Hot oil circulation raises the reaction chamber temperature to 120-320°C and maintains this constant temperature for 30-240 minutes, completing the first step. Nitrogen is then introduced to adjust the reaction pressure to 0.05-0.3 MPa, and the hot oil temperature is adjusted to 150-280°C. Ammonium polyphosphate (AMP) is then added to the reaction chamber, and thermal polymerization and dehydration proceed for 30-180 minutes to obtain the AMP modified with piperazine phosphate. Nitrogen is then introduced to adjust the reaction pressure to 0.1-1.5 MPa, and the hot oil temperature is adjusted to 120-350°C. A capping agent is then added to the reaction chamber, and the reaction is heat-treated for 30-240 minutes. After the reaction is complete, the material is discharged directly to a storage bin outside the system for cooling. This solution is mainly used to synthesize the target substance. It utilizes the functions of constant temperature heating and inert protective gas to maintain the reaction pressure of the above-mentioned equipment, as well as the function of the stirring screw 7 and the reaction chamber to maintain different rotation directions. It does not use cold oil cooling and continuous production functions. The use process is to add the material to the reaction chamber, fill the reaction chamber with nitrogen to adjust to the appropriate pressure, start the hot oil circulation to control the temperature of the reaction chamber, and keep the stirring screw 7 and the reaction chamber rotating in opposite directions during the reaction. The nitrogen pressure in the reaction chamber and the temperature of the hot oil tank 2 are adjusted according to the requirements of the different stages of the reaction. After the reaction is completed, no cold oil cooling is performed, and the material is directly taken out to the storage bin for cooling.
[0058] Example 2: Application of chemically terminated focused piperazine phosphate modified ammonium polyphosphate in flame retardant polypropylene
[0059] The raw materials for flame-retardant polypropylene include the following components, calculated by weight: 70-78 parts polypropylene, 10-20 parts chemically end-capped focused piperazine phosphate-modified ammonium polyphosphate, 5-15 parts melamine polyphosphate, 0.5-6 parts flame retardant synergist, 0.5-2 parts coupling agent, 0.3-3 parts lubricant, and 0.2-0.5 parts antioxidant. The flame-retardant polypropylene composition prepared using these raw materials not only exhibits good flame retardancy but also excellent precipitation resistance.
[0060] The melt index of polypropylene is 0-100 g / 10 min (temperature 230° C., load 2.16 kg); the 1% thermal weight loss of melamine polyphosphate (commercially available) is ≥ 360° C.; the flame retardant synergist includes at least one of anhydrous zinc borate, 3.5-hydrate zinc borate, zinc oxide, and zirconium phosphate; the coupling agent is a silane coupling agent, including at least one of aminosilane coupling agent KH-9120, isocyanate silane coupling agent KT-930, epoxy silane coupling agent KH-1006, and KH-9130; the lubricant includes at least one of ethylene bisstearamide, pentaerythritol stearate, silicone, and amide wax; and the antioxidant includes at least one of antioxidant 168, antioxidant 1010, and antioxidant 1098.
[0061] Flame retardant polypropylene is prepared by the following method:
[0062] Step 1: Add the chemically terminated focused piperazine phosphate modified ammonium polyphosphate, melamine polyphosphate and flame retardant synergist into a mixer and stir at room temperature for 5-30 minutes.
[0063] Step 2: In the mixture of step 1, increase the temperature of the mixer to 80-160°C, ensure that the temperature of the material in the mixer also reaches the set temperature, then add the coupling agent and continue stirring for 10-30 minutes.
[0064] Step 3: After cooling the mixture in step 2 to room temperature, add polypropylene, lubricant and antioxidant and stir for 5-30 minutes.
[0065] Step 4: The mixture of step 3 is extruded by a twin-screw extruder at a temperature of 180-260° C., and then subjected to a process of drawing and pelletizing, and then sieving and dehydrating to obtain flame-retardant polypropylene pellets.
[0066] Experimental Example 1: Synthesis and Performance Testing of Chemically End-Capped Piperazine Phosphate-Modified Ammonium Polyphosphate
[0067] This experimental example followed the synthetic route of Example 1 for the synthesis of specific materials. See Table 1 for raw materials and parameter selection. Furthermore, during the synthesis of focused piperazine phosphate, focused piperazine phosphate, and chemically terminated focused piperazine phosphate-modified ammonium polyphosphate (i.e., during steps 1-3), the dedicated equipment of this protocol was used. The material stirring screw was rotated counterclockwise at approximately 200 rpm, and the rotating furnace drum was rotated clockwise at approximately 50 rpm. The piperazine diphosphate used in Tests 1-4 was synthesized as follows: phosphoric acid and piperazine were mixed in a molar ratio of 2.05:1, reacted in an aqueous ethanol solution (50% ethanol by volume) at 80°C and 0.1 MPa for 210 minutes, and then purified and dried according to standard procedures. The resulting chemically terminated focused piperazine phosphate-modified ammonium polyphosphate was tested for performance, including the 1% thermogravimetric loss temperature and whiteness. The 1% thermogravimetric loss temperature was tested according to ASTM E2550-2007, and the whiteness was tested according to GB / T 5950. The test results are shown in Table 2. Domestic ammonium polyphosphate was purchased from the market, and its TG chart is shown in Figure 4.
[0068] [Corrected 30.07.2024 according to Rule 26] Table 1: Synthesis conditions of chemically terminated focused piperazine phosphate modified ammonium polyphosphate
[0069] [Corrected 30.07.2024 according to Rule 26] Table 2: Performance test results
[0070] [Corrected 30.07.2024 in accordance with Rule 26]
[0071] [Corrected 30.07.2024 in accordance with Rule 26]
[0072] From the above experimental results, it can be seen that the chemically terminated focused piperazine phosphate modified ammonium polyphosphate obtained by the synthesis method of this scheme has a more ideal whiteness (greater than 96%) and 1% thermal weight loss temperature (greater than 290°C) compared with the ordinary ammonium polyphosphate in the prior art.
[0073] Experimental Example 2: Specific synthesis and performance testing of flame retardant polypropylene
[0074] This experimental example carried out specific material synthesis according to the synthesis route of Example 2, and the raw materials and parameter selections are as follows:
[0075] Test 1: 76.5 parts of polypropylene, 15 parts of chemically terminated focused piperazine phosphate-modified ammonium polyphosphate (prepared in Test 1 of Experimental Example 1), 3 parts of melamine polyphosphate, 3 parts of flame retardant synergist, 0.5 parts of coupling agent, 0.5 parts of lubricant, and 0.5 parts of antioxidant.
[0076] Test 2: 76.5 parts of polypropylene, 15 parts of chemically terminated focused piperazine phosphate-modified ammonium polyphosphate (prepared in Test 2 of Experimental Example 1), 3 parts of melamine polyphosphate, 3 parts of flame retardant synergist, 0.5 parts of coupling agent, 0.5 parts of lubricant, and 0.5 parts of antioxidant.
[0077] Test 3: 76.5 parts of polypropylene, 15 parts of chemically terminated focused piperazine phosphate modified ammonium polyphosphate (prepared in Test 3 of Experimental Example 1), 3 parts of melamine polyphosphate, 3 parts of flame retardant synergist, 0.5 parts of coupling agent, 0.5 parts of lubricant, and 0.5 parts of antioxidant.
[0078] Test 4: 76.5 parts of polypropylene, 15 parts of chemically terminated focused piperazine phosphate modified ammonium polyphosphate (prepared in Test 4 of Experimental Example 1), 3 parts of melamine polyphosphate, 3 parts of flame retardant synergist, 0.5 parts of coupling agent, 0.5 parts of lubricant, and 0.5 parts of antioxidant.
[0079] Comparative test: 76.5 parts of polypropylene, 15 parts of ammonium polyphosphate (domestic), 3 parts of melamine polyphosphate, 3 parts of flame retardant synergist, 0.5 parts of coupling agent, 0.5 parts of lubricant, and 0.5 parts of antioxidant.
[0080] The melt index of polypropylene is specifically 20 g / 10 min; the flame retardant synergist is specifically zinc oxide; the coupling agent is specifically KH-9120; the lubricant is specifically ethylene bisstearamide; and the antioxidant is specifically antioxidant 168 and antioxidant 1010 mixed in a ratio of 1:1.
[0081] The composite material was prepared as follows:
[0082] Polypropylene, chemically terminated focused piperazine phosphate-modified ammonium polyphosphate (or domestically produced ammonium polyphosphate), melamine polyphosphate, and a flame retardant synergist are added to a mixer and stirred at room temperature for 15 minutes. The mixer temperature is then raised to 120°C. Once the material temperature reaches the set temperature, a coupling agent is added and stirring continues for 20 minutes. After cooling to room temperature, a lubricant and antioxidant are added and stirred for 10 minutes. The final mixture is extruded using a twin-screw extruder using conventional methods at a temperature of 160-220°C. The mixture is then subjected to stranding and pelletizing, followed by screening and dehydration to produce a flame-retardant polypropylene composite material.
[0083] The synthesized flame-retardant polypropylene composite was subjected to performance testing, including flame retardancy testing, the "double 85" test, and water immersion testing. The flame retardancy test was conducted according to the Test for Flammability of Plastic Materials for Parts in Devices and Appliances (UL 94); the 1000-hour "double 85" test was conducted according to GB / T 2423.50 Part 2, Test Cy: Steady-State Damp Heat, primarily for accelerated component testing; and the water immersion test was conducted according to Polymeric Materials - Use in Electrical Equipment Evaluations – UL 746C. The test results are detailed in Table 3.
[0084] [Corrected 30.07.2024 according to Regulation 26] Table 3: Flame retardant polypropylene performance test results
[0085] [Corrected 30.07.2024 in accordance with Rule 26]
[0086] Based on the above experimental data, the flame-retardant polypropylene produced by this solution exhibits superior flame retardancy, heat resistance, and precipitation resistance compared to domestically produced ammonium polyphosphate (AMP). Furthermore, the chemically terminated piperazine phosphate-modified AMP in this solution uses a relatively low dosage of approximately 15% to achieve a flame retardant rating of 1.6mm V-0. The product also passed the UL 746C water immersion test and the GB / T 2423.50 "Double 85" test for 1000 hours without precipitation.
[0087] Comparative Example 1
[0088] This comparative example is essentially the same as any of Tests 1-4 in Experimental Example 2, except that the chemically end-capped focused piperazine phosphate-modified ammonium polyphosphate is replaced with the product obtained by the first two steps of Experimental Example 1 (prepared with reference to Test 1 of Experimental Example 1), without chemical end-capping. Flame-retardant polypropylene was prepared using the resulting focused piperazine phosphate-modified ammonium polyphosphate, and performance testing (mechanical properties and flame retardancy) was then conducted. The experimental results are shown in Table 4 (where Tests 1-4 correspond to Tests 1-4 in Table 3, respectively). These experimental results demonstrate that end-capping with the hydroxyl-free, NH-bonded nitrogen-containing compound of this solution not only enhances the flame retardancy but also helps improve compatibility with the remaining polypropylene, resulting in enhanced mechanical properties.
[0089] Comparative Example 2
[0090] This comparative example is essentially the same as any of Tests 1-4 in Experimental Example 2, except that chemically capped focused piperazine phosphate modified ammonium polyphosphate is not used. Instead, a mixture of focused piperazine phosphate (prepared as described in Test 1 of Experimental Example 1) and ammonium polyphosphate is used, with a molar ratio of 2:1. The performance test results are shown in Table 4. Directly mixing focused piperazine phosphate and ammonium polyphosphate significantly reduces both flame retardancy and mechanical properties compared to the chemically modified samples in Tests 1-4.
[0091] Comparative Example 3
[0092] This comparative example is essentially the same as any of Tests 1-4 of Experimental Example 2, except that, instead of using chemically terminated focused piperazine phosphate to modify ammonium polyphosphate, a mixture of ammonium polyphosphate and chemically terminated focused piperazine phosphate is used, with a molar ratio of 1:2. The chemically terminated focused piperazine phosphate is prepared as follows: piperazine diphosphate is heat-treated at 260°C for 180 minutes, and then thermally polymerized and dehydrated to form focused piperazine phosphate in a nitrogen atmosphere at a pressure of 0.05 MPa. After the reaction is complete, a melamine capping agent is added (the mass ratio of capping agent to focused piperazine phosphate is 10:10,000). The mixture is then heat-treated in an inert gas atmosphere (e.g., nitrogen) at 280°C and a pressure of 0.2 MPa for 90 minutes. After cooling, the mixture is ground into powder to produce the chemically terminated focused piperazine phosphate.
[0093] The performance test results are shown in Table 4. Using a mixture of ammonium polyphosphate and chemically terminated piperazine phosphate as the additive, the precipitation resistance, flame retardancy, and mechanical properties of the chemically modified samples 1-4 were significantly reduced. This is because the end-capping of the nitrogen-containing compound with NH bonds and no hydroxyl groups not only improves the flame retardancy but also helps improve the compatibility with the rest of the polypropylene.
[0094] [Corrected 30.07.2024 according to Rule 26] Table 4: Comparative Performance Test Results 1-3 (N / A means the test was not performed)
[0095] [Corrected 30.07.2024 in accordance with Rule 26]
[0096] Based on the above experimental data, if the focused piperazine phosphate-modified ammonium polyphosphate is not chemically end-capped (Comparative Example 1), and the flame retardant is used in the production of flame-retardant polypropylene, the resulting polypropylene product exhibits reduced mechanical properties and flame retardant efficacy compared to the products of Tests 1-4, and also exhibits surface precipitation. If the focused piperazine phosphate and ammonium polyphosphate are directly mixed using conventional prior art methods (Comparative Example 2) without chemical reaction bonding, and the flame retardant is used in the production of flame-retardant polypropylene, the resulting polypropylene product exhibits reduced mechanical properties and flame retardant efficacy compared to the products of Tests 1-4 and Comparative Example 1, and exhibits surface precipitation. Simply mixing ammonium polyphosphate with chemically end-capped focused piperazine phosphate also results in undesirable phenomena such as reduced mechanical properties, surface precipitation, and reduced flame retardant efficacy.
[0097] Comparative Example 4
[0098] This comparative example was essentially the same as Test 1 of Experimental Example 1, except that during the three-step synthesis process, only the material stirring screw was kept rotating (consistent with Test 1 of Experimental Example 1), while the rotary furnace drum (reaction chamber) remained stationary. All other parameters remained unchanged. The resulting chemically terminated focused piperazine phosphate-modified ammonium polyphosphate was tested for whiteness and 1% thermogravimetric loss temperature. The experimental results are shown in Table 5 (Test 1 in Table 5 corresponds to Test 1 in Table 2).
[0099] Comparative Example 5
[0100] This comparative example was essentially the same as Test 1 of Experimental Example 1, except that during the three-step synthesis process, the rotational speed of the material stirring screw remained the same as in Test 1 of Experimental Example 1, but the rotational speed of the rotary furnace drum (reaction chamber) was set at 150 rpm (a relatively fast rotational speed). All other parameters remained unchanged. The resulting chemically terminated focused piperazine phosphate-modified ammonium polyphosphate was tested for whiteness and 1% thermogravimetric loss temperature. The experimental results are shown in Table 5.
[0101] Comparative Example 6
[0102] This comparative example was essentially the same as Test 1 of Experimental Example 1, except that during the three-step synthesis process, the material stirring screw was maintained at a relatively fast speed of 350 rpm. However, the rotational speed of the rotating furnace drum (reaction chamber) was maintained at the same speed as in Test 1 of Experimental Example 1, with all other parameters remaining unchanged. The obtained chemically terminated focused piperazine phosphate-modified ammonium polyphosphate was tested for whiteness and 1% thermogravimetric loss temperature. The experimental results are shown in Table 5.
[0103] [Corrected 30.07.2024 according to Rule 26] Table 5: Performance test results of chemically blocked focused piperazine phosphate modified ammonium polyphosphate of Comparative Examples 4-6
[0104] [Corrected 30.07.2024 in accordance with Rule 26]
[0105] During the preparation of chemically terminated focused piperazine phosphate, the material stirring screw and the rotating furnace drum (reaction chamber) rotate in opposite directions at a certain speed, which is crucial for improving the flame retardant's whiteness and reducing thermal weight loss. If only the material stirring screw rotates, even if its rotation speed is increased (Comparative Example 1 → Comparative Example 3), the resulting product's whiteness and 1% thermal weight loss temperature remain suboptimal. If the rotating furnace drum (reaction chamber) rotates too quickly (Comparative Example 2), this also affects improvements in whiteness and 1% thermal weight loss temperature.
[0106] Comparative Example 7
[0107] This comparative example is essentially the same as Test 1 of Experimental Example 2, except that, in preparing the chemically end-capped focused piperazine phosphate-modified ammonium polyphosphate, an equal amount of propanol was used as the end-capping agent, while all other conditions remained unchanged. The resulting flame-retardant polypropylene was subjected to performance testing: flame retardancy was V-0 according to UL 94 (3.2 mm), V-1 according to UL 94 (1.6 mm), precipitation was observed on the surface of the specimens after 1000 hours of the "Double 85" test, and precipitation was observed on the surface of the specimens according to the UL 746C water immersion test. The inventors previously tried alcohol, but none of the alcohols could achieve the desired results. Propanol is used here as an example for illustration.
[0108] Comparative Example 8
[0109] This comparative example is essentially the same as Test 1 of Experimental Example 2, except that, in the preparation of chemically end-capped focused piperazine phosphate-modified ammonium polyphosphate, an equal amount of phenol was used as the end-capping agent. All other conditions remained unchanged. The resulting flame-retardant polypropylene was subjected to performance testing: flame retardancy was UL 94 (3.2 mm) V-0, flame retardancy was UL 94 (1.6 mm) V-1, the "Double 85" test showed precipitation on the specimen surface after 1000 hours, and the UL 746C water immersion test showed precipitation on the specimen surface.
[0110] Comparative Examples 7 and 8 illustrate that the type of capping agent selected can also seriously affect the effect of the flame retardant. If a nitrogen-free but hydroxyl-containing capping agent (various alcohols, phenol, etc.) is used, the flame retardant properties of the composite material will be reduced and the problem of surface precipitation cannot be completely solved.
[0111] The above is only an embodiment of the present invention, and the common knowledge such as the specific technical solutions and / or characteristics in the solution are not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several variations and improvements can be made, which should also be regarded as the scope of protection of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the description can be used to interpret the content of the claims.
Claims
1. A highly heat-resistant and precipitation-resistant chemically terminated focused piperazine phosphate modified ammonium polyphosphate flame retardant, characterized in that: The structural formula of the focused piperazine phosphate modified ammonium polyphosphate is shown in the following chemical formula, and the focused piperazine phosphate modified ammonium polyphosphate is capped by a capping agent; Wherein, n=300-1500, m=1000-2000; the end-capping agent is a nitrogen-containing compound having no hydroxyl group and an NH bond.
2. The highly heat-resistant and precipitation-resistant chemically terminated focused piperazine phosphate modified ammonium polyphosphate flame retardant according to claim 1, characterized in that: The end-capping agent includes at least one of R-NH2, R=NH, melamine, urea, biguanide and iminodiacetonitrile; R is an alkyl group with 1 to 4 carbon atoms.
3. A highly heat-resistant and precipitation-resistant chemically terminated focused piperazine phosphate modified ammonium polyphosphate flame retardant according to claim 2, characterized in that: The molar ratio of the focused piperazine phosphate to the ammonium polyphosphate is 2.0-2.1:1; the molar ratio of the capping agent to the focused piperazine phosphate modified ammonium polyphosphate is 2.0-2.2:
1.
4. A method for preparing a highly heat-resistant and precipitation-resistant chemically terminated focused piperazine phosphate-modified ammonium polyphosphate flame retardant according to any one of claims 1 to 3, characterized in that: The method includes the following steps: S1: Piperazine diphosphate is dehydrated by thermal polymerization to obtain focused piperazine phosphate; S2: focusing piperazine phosphate and ammonium polyphosphate are subjected to thermal polymerization and dehydration to obtain focused piperazine phosphate modified ammonium polyphosphate; S3: After the focused piperazine phosphate modified ammonium polyphosphate and the capping agent are heat treated, chemically capped focused piperazine phosphate modified ammonium polyphosphate is obtained.
5. The method for preparing a highly heat-resistant and precipitation-resistant chemically terminated focused piperazine phosphate modified ammonium polyphosphate flame retardant according to claim 4, characterized in that: The reaction processes of S1-S3 are all carried out in an inert gas environment; the reaction temperature, pressure and time of S1 are 120-320°C, 0.05-0.3MPa, and 30-240min respectively; the reaction temperature, pressure and time of S2 are 150-280°C, 0.05-0.3MPa, and 30-180min respectively; the reaction temperature, pressure and time of S3 are 120-350°C, 0.1-1.5MPa, and 30-240min respectively.
6. The method for preparing a highly heat-resistant and precipitation-resistant chemically terminated focused piperazine phosphate modified ammonium polyphosphate flame retardant according to claim 5, characterized in that: The reaction processes of S1-S3 are all carried out in a thermal polymerization reaction device; the polymerization reaction device includes a rotary furnace and a temperature control unit; a reaction chamber is provided in the rotary furnace, and a stirring screw is coaxially provided in the reaction chamber; the temperature control unit is used to control the temperature in the reaction chamber; during the reaction process, the stirring screw and the reaction chamber maintain different rotation directions.
7. The method for preparing a highly heat-resistant and precipitation-resistant chemically terminated focused piperazine phosphate modified ammonium polyphosphate flame retardant according to claim 6, characterized in that: The rotation speed of the stirring screw is 30-300 rpm, and the rotation speed of the reaction chamber is 3-120 rpm.
8. Use of a highly heat-resistant and precipitation-resistant chemically terminated focused piperazine phosphate modified ammonium polyphosphate flame retardant according to any one of claims 1 to 3 in flame-retardant polypropylene.
9. The use of a highly heat-resistant and precipitation-resistant chemically terminated focused piperazine phosphate modified ammonium polyphosphate flame retardant according to claim 8 in flame-retardant polypropylene, characterized in that: The raw materials include, by weight: 70-78 parts of polypropylene, 10-20 parts of chemically terminated focused piperazine phosphate modified ammonium polyphosphate, 5-15 parts of melamine polyphosphate, 0.5-6 parts of flame retardant synergist, 0.5-2 parts of coupling agent, 0.3-3 parts of lubricant, and 0.2-0.5 parts of antioxidant; The melt index of polypropylene is 0-100g / 10min; the 1% thermal weight loss of melamine polyphosphate is ≥360°C; the flame retardant synergist includes at least one of anhydrous zinc borate, 3.5-water zinc borate, zinc oxide, and zirconium phosphate; the coupling agent is a silane coupling agent, including at least one of aminosilane coupling agent KH-9120, isocyanate silane coupling agent KT-930, epoxy silane coupling agent KH-1006 and KH-9130; the lubricant includes at least one of ethylene bis stearamide, pentaerythritol stearate, silicone and amide wax; the antioxidant includes at least one of antioxidant 168, antioxidant 1010 and antioxidant 1098.
10. The use of a highly heat-resistant and precipitation-resistant chemically terminated focused piperazine phosphate modified ammonium polyphosphate flame retardant according to claim 9 in flame-retardant polypropylene, characterized in that: The flame-retardant polypropylene is prepared by the following method: chemically terminated focused piperazine phosphate modified ammonium polyphosphate, melamine polyphosphate and a flame-retardant synergist are added into a mixer and stirred at room temperature for 5-30 minutes; then the temperature of the mixer is increased to 80-160°C, a coupling agent is added and the stirring is continued for 10-30 minutes; after cooling to room temperature, polypropylene, a lubricant and an antioxidant are added and stirred for 5-30 minutes; and the flame-retardant polypropylene is obtained by extruding with a twin-screw extruder.
Citation Information
Patent Citations
Multi-block or random copolymerized halogen-free flame-retardant macromolecule and flame-retardant polyolefin material thereof
CN114181397A
High-temperature-resistant and precipitation-resistant chemically-terminated focused piperazine phosphate modified ammonium polyphosphate as well as preparation method, device and application of high-temperature-resistant and precipitation-resistant chemically-terminated focused piperazine phosphate modified ammonium polyphosphate
CN116554482A
Method for preparing focused piperazine phosphate modified ammonium polyphosphate by using continuous production polymerization reaction equipment
CN118620216A
Cited By
Macromolecular phosphorus-nitrogen flame-retardant composite material as well as preparation method and application thereof
CN119912401A