Process for recycling silicon ingot cutting waste

The recycling process for diamond wire cutting waste from silicon ingots involves chemical treatment and granulation to form granules that can be safely reintroduced into a metallurgical silicon production furnace, addressing the challenges of handling fine powder and organic species, and enhancing recycling efficiency and safety.

WO2024235679A1PCT designated stage expired Publication Date: 2024-11-21ROSI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2024/062270
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-05-03
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

The recycling of waste from cutting silicon ingots using diamond wires poses challenges due to the fine powder nature of the waste, which is difficult to handle and poses explosiveness risks, and existing processes require extensive purification steps to remove abrasive particles and organic species.

Method used

A process involving the recovery of a sludge from diamond wire cutting waste, followed by chemical treatment with hydrogen peroxide to reduce organic species, drying and granulation under vacuum to form granules suitable for reintroduction into a metallurgical silicon production furnace, allowing for remelting and recycling without the need for abrasive particle removal.

Benefits of technology

The process effectively recycles silicon from diamond wire cutting waste by forming granules that can be safely introduced into a casting ladle, managing cooling sequences and reducing aluminum and calcium levels in liquid silicon, thus enhancing the recycling efficiency and safety without consuming additional raw materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

The invention relates to a method for recycling silicon ingot cutting waste comprising the following steps: a) recovering a first sludge, derived from said waste, formed by an aqueous mixture comprising silicon particles and organic species, but free of abrasive carbide-type particles; the first sludge having an initial weight percentage of organic species, b) chemically treating the first sludge so as to reduce the initial weight percentage of organic species and form a second sludge having a residual weight percentage of organic species of between 0.8% and 2%; c) drying and associated granulation of the second sludge, by heating under vacuum and stirring, to form granules including the silicon particles and the organic species, said granules having dimensions with an average value of greater than or equal to 150 µm and a moisture content of less than or equal to 2%; d) introducing the granules into a liquid silicon casting ladle, at the outlet of a silica reduction furnace, to help with the cooling of the liquid silicon to a refining temperature and / or to a casting temperature.
Need to check novelty before this filing date? Find Prior Art

Description

PROCESS FOR RECYCLING SILICON INGOT CUTTING WASTE FIELD OF THE INVENTION

[0001] The present invention relates to the silicon manufacturing chain. In particular, it relates to a process for recycling waste from the cutting of silicon ingots ("kerfs") by diamond wires, which provides for reintroducing the treated silicon into the metallurgical silicon manufacturing process by remelting. TECHNOLOGICAL BACKGROUND OF THE INVENTION

[0002] Silicon wafers, intended for the semiconductor or photovoltaic industry, are manufactured from silicon ingots, using metal wire cutting processes with the addition of carbide-type abrasives ("slurry sawing" in English terminology) or diamond wire cutting.

[0003] The width of the cutting wires is increasingly narrow, but remains proportional to the thickness of the cut wafers; these sawing processes therefore still generate a significant quantity of silicon waste: around 25 to 40% of the total mass of an ingot. Cutting is carried out under a continuous flow of cutting liquid to evacuate heat and chips. The liquid is made up of water and additives such as PEG (Polyethylene glycol), antifoam, surfactants. The cutting waste is found in the form of very fine powder (micro or nanoparticles of silicon with an oxidized surface), mixed with liquid additives, metallic contaminants, organic or inorganic species, and, in the case of cutting with abrasives, abrasive particles (for example SiC).

[0004] Document EP2712844A1 proposes a method for recycling silicon ingot cutting waste comprising SiC abrasive particles. This method comprises a step of purifying (using acidic or basic solutions) said waste, so as to obtain purified silicon particles and carbon-containing particles, the latter containing less than 0.25 ppm of boron and less than 0.5 ppm of phosphorus. The particles are then agglomerated in the form of pellets (preferably, having an average diameter greater than 2 - 5 mm), using a binder, for example a carbohydrate or a resin. The method then comprises a step of using said pellets as reactive materials in a reduction process (removal of oxygen) producing silicon.

[0005] Let us recall that a reduction process is usually carried out from quartz (SiO2) which reacts with silicon carbide or carbon, at temperatures around 2100°C, to give silicon.

[0006] According to EP2712844, SiO2, SiC or carbon can be added to the pellets to obtain appropriate proportions of initial reactive materials in the reduction furnace, at very high temperatures.

[0007] The liquid silicon, obtained at the outlet of the reduction furnace, is then collected in casting ladles and then cooled, to form blocks of metallurgical quality silicon. SUBJECT OF THE INVENTION

[0008] The present invention relates to a method for recycling silicon ingot cutting waste from diamond wire sawing, the waste therefore being free of abrasive particles, particularly carbide-type particles. The recycling method provides for treatment and shaping of said waste with a view to reintroducing it into the metallurgical silicon manufacturing process, by remelting in the casting ladle of a metallurgical silicon production furnace. BRIEF DESCRIPTION OF THE INVENTION

[0009] The present invention relates to a method for recycling silicon ingot cutting waste from diamond wire sawing comprising the following steps:

[0010] a) the recovery of a first sludge, from said waste, formed by an aqueous mixture comprising silicon particles and organic species, but devoid of abrasive particles of carbide type; the first sludge having an initial mass percentage of organic species defined in relation to the mass of solid matter contained in the first sludge,

[0011] b) chemical treatment of the first sludge so as to reduce the initial mass percentage of organic species and form a second sludge having a residual mass percentage of organic species of between 0.8% and 2% relative to the mass of solid matter contained in the second sludge;

[0012] c) drying and associated granulation of the second slurry, by heating under vacuum and stirring, to form granules including the silicon particles and the organic species, said granules having dimensions whose average value is greater than or equal to 150 μm and a humidity level less than or equal to 2%;

[0013] d) the introduction of the granules into a liquid silicon casting ladle, at the outlet of a silica reduction furnace, to participate in the cooling of the liquid silicon to a refining temperature and / or to a casting temperature.

[0014] According to advantageous characteristics of the invention, taken alone or in any feasible combination: the initial mass percentage of organic species is between 3% and 6%, typically of the order of 4%; the residual mass percentage of organic species is 1.3% + / - 0.2%; step c) is carried out at a temperature between 40°C and 100°C; the average size of the granules is approximately 0.8 mm; the moisture content of the granules is 1.5% + / - 0.2%; the mass proportion of the granules introduced into the casting ladle is between 1% and 5%; the chemical treatment of step b) is carried out with a dilute solution of hydrogen peroxide; the chemical treatment of step b) is carried out with a dilute solution of a mineral peroxide; step b) comprises at least one wash, two, or even three successive washes with pure water, after the treatment chemical, to obtain the second mud. DETAILED DESCRIPTION OF THE INVENTION

[0015] The invention relates to a method for recycling waste from the cutting of silicon ingots using diamond wires. The silicon contained in this waste is in the form of a very fine powder (silicon nanoparticles at least partially oxidized on the surface), mixed with liquid additives, metallic contaminants and organic or inorganic species. This waste mainly contains liquid matter, the mass percentage of silicon (which constitutes the majority of the solid matter) is between 2% and 10%.

[0016] The first step a) of the process consists of the recovery of a first sludge, from said waste, formed by an aqueous mixture comprising in particular silicon nanoparticles (also called silicon particles hereinafter) and organic species, and of course free of abrasive particles of the carbide type (in particular SiC).

[0017] The term "sludge" is used to describe a substance typically comprising more than 40% (mass percentage) of solid matter (consisting mainly of silicon nanoparticles), mixed in an aqueous solution. The first sludge may be obtained, from the cutting waste, by a known solid / liquid separation method chosen from filtration (for example vacuum filtration) or tangential filtration, sedimentation, centrifugation or cyclonic separation. Advantageously, in step a), the first sludge comprises approximately 50% solid matter and 50% liquid matter. The term "approximately" here means that the value of the mass percentage is + / -10% (absolute: that is to say that a mass percentage of approximately 50% may vary between 40% and 60%), or even + / - 5% (absolute).

[0018] Typically, the size distribution of silicon particles in the first slurry is between about 10nm and 5μm, typically centered at 0.6μm.

[0019] The first sludge has an initial percentage of organic species, typically between 3% and 6%, for example around 4%. Note that in the context of this description, we are talking about mass percentages of organic species, defined in relation to the mass of solid matter contained in the sludge.

[0020] These organic species come mainly from additives such as PEG (Polyethylene glycol), antifoam, surfactants, introduced into the cutting liquid and of which we know precisely the volume loaded with each cutting operation, and therefore in each volume of recovered waste.

[0021] The recycling process then comprises a step b) including a chemical treatment of the first sludge, which aims to reduce the initial mass percentage of organic species and to form a second sludge having a residual mass percentage of organic species of between 0.8% and 2%, this percentage being defined relative to the mass of solid matter contained in the second sludge. Preferably, the residual mass percentage of organic species is 1.3% + / - 0.2%.

[0022] Advantageously, the chemical treatment is carried out with a dilute solution of hydrogen peroxide (H2O2) or a mineral peroxide, for example based on potassium (K), sodium (Na), calcium (Ca), magnesium (Mg), etc. By dilute solution, we mean a solution consisting of peroxide and pure water (deionized water or ultra-pure water, having respectively a resistivity of a few hundred kohms.cm and a resistivity greater than 18.2 Mohms.cm).

[0023] The diluted solution may have a mass concentration of between 1% and 35% peroxide, with the remaining percentage being water.

[0024] The diluted solution is added to the first sludge, thus forming a first mixture. Note that no other acidic product is added to form the first mixture. The first mixture therefore consists of the first sludge, a peroxide (hydrogen or mineral), and water.

[0025] The respective proportions of dilute solution and first sludge in the first mixture will depend on the peroxide concentration and the type of peroxide. For example, for a hydrogen peroxide concentration of 35%, the first mixture preferably comprises one volume of dilute solution for one volume of first sludge; for a hydrogen peroxide concentration of 10%, the first mixture preferably comprises three volumes of dilute solution for one volume of first sludge. According to another example, for a potassium peroxide concentration of 6.7% K2S208 relative to the mass of solid matter in the first sludge, the first mixture preferably comprises one volume of dilute solution for one volume of first sludge.

[0026] The chemical treatment can be carried out by stirring the first mixture, so as to homogenize the distribution of the diluted solution among the silicon nanoparticles and other organic species or metallic contaminants of the first sludge.

[0027] The silicon particles in the first sludge mainly have a layer of silicon oxide on their surface; moreover, they are totally or partially "covered" by layers formed of long chains of organic species. The organic species are also mainly fixed to the surface of the nanoparticles in the first sludge. Hydrogen peroxide or other mineral peroxide, through an oxidation reaction of the organic species, will induce the segmentation of the long organic chains which promotes their detachment from the surface of the silicon particles.

[0028] Advantageously, the first mixture comprises approximately 5% to 10% solid matter and an additional percentage of liquid matter (in mass percentage): this liquid consistency promotes the suspension of silicon nanoparticles, organic species and metallic contaminants in the first mixture.

[0029] Stirring the first mixture then makes it possible to homogenize the distribution of silicon nanoparticles and other species suspended in the first mixture; stirring also makes it possible to increase the efficiency of the oxidation reaction segmenting the organic chains.

[0030] The chemical treatment can be carried out at a temperature between 20°C and 95°C, for a duration ranging from 10 min to 5 h.

[0031] After the chemical treatment, the first aqueous mixture comprises particles in homogeneous suspension, including silicon nanoparticles, organic species partially in the form of segmented chains (other organic species can still be attached to the surface of nanoparticles) and metallic contaminants.

[0032] A solid / liquid separation sequence of the first mixture is carried out to obtain on the one hand a second sludge and on the other hand a liquid loaded with organic species and metallic contaminants. The second sludge is composed of at least 40% solid matter. The liquid is discharged and treated as liquid effluent.

[0033] At this stage, an additional treatment with soda can optionally be carried out, to obtain a pH greater than or equal to ten, which makes it possible to eliminate most of the potential pollution by aluminum (often used to collect the cutting liquid).

[0034] Step b) may optionally comprise at least one wash, or even two or three successive washes with pure water, of the first sludge or of an intermediate sludge obtained before the final solid / liquid separation sequence resulting in the formation of the second sludge.

[0035] The residual quantity of organic species depends on the chemical treatment (dilution of the peroxide, time and other conditions of application of the treatment to the first sludge) and the water dilution rate of the successive washes. Indeed, these washes will be likely to result in a greater or lesser quantity of organic species, present in suspension in the liquid portion of the first mixture. The residual quantity of organic species can be evaluated and controlled by balances based on the measurement of total organic carbon (TOC) or on LECO type techniques by IGA ("Inductively gas analysis").

[0036] The washing(s) are followed by a solid / liquid separation to obtain a sludge comprising at least 40% solid matter.

[0037] The solid / liquid separation(s) of step b) can be carried out by known techniques such as sedimentation, centrifugation, cyclonic separation, filtration, or other.

[0038] Even if the elimination of a part of the organic species from the first sludge by the use of a dilute peroxide solution has been particularly described, this elimination can be carried out by other techniques known from the state of the art, such as extraction by a solvent, said solvent being able in particular to be chosen from toluene, dichloromethane, alcohol and acetone.

[0039] Note that the method according to the invention does not require that step b) includes a chemical treatment using an acid solution to purify the silicon particles from the first sludge. In the method according to the invention, it is not necessary for all the metal contaminants present in the first sludge to be specifically removed. Some of them are removed during step b), along with the excess portion of organic species, but it is acceptable for a residual portion of metal contaminants to remain in the second sludge.

[0040] The recycling process includes a subsequent step c), corresponding to the drying of the second sludge. The parameters of this drying combined with the presence of organic species (respecting the chosen residual mass percentage) in the second sludge induce granulation of the solid particles of said sludge. Drying / granulation is carried out by heating under vacuum and with stirring, to form granules including the silicon nanoparticles and the residual organic species. Carrying out this step under vacuum (of the order of 20 - 80 mbar) avoids the evaporation phenomenon which disperses the particles and discourages agglomeration. Heating is carried out in the temperature range 40°C - 100°C. Heating and stirring bring the silicon particles into contact with the organic species, the latter forming a binder and causing agglomeration of the particles in the form of granules.The drying / granulation step can be carried out in a vacuum dryer such as the Pan Dryer model offered by De Dietrich for other applications.

[0041] For example, the drying / granulation step can be carried out on Pan Dryer type equipment under the following conditions: Heating surface (bottom and walls of the equipment tank): approximately 1.25m 2 , of which heated bottom 0.17m²,After introducing the second sludge into the tank, pressure reduction (vacuum passage) to a pressure of 70mbar in the equipment,Heating the tank to 80°C,Initial temperature of the second sludge: approximately 48°C; initial humidity level of the second sludge: approximately 50%,Operation of the agitator and the lump breaker to obtain the desired granulometry of the granules;Final temperature of the granules: approximately 65°C; final humidity level of the granule powder: approximately 1.5%.

[0042] The adjustment of pressure, heating temperature, temperature rise, time, stirring parameters, combined with the residual content of organic species in the second sludge, allows the formation of granules having mainly dimensions greater than 70 μm and a humidity level less than or equal to 2%.

[0043] Advantageously, the moisture content of the granule powder is 1.5% + / - 0.2%. The moisture content can be measured on a sample taken from the granules, by differential weighing before and after heating with an infrared lamp.

[0044] The granules will generally have a polyhedral or spherical shape; the dimension or size of a granule can be defined as its "Sauter equivalent diameter". The "Sauter equivalent diameter" is the diameter of the sphere that would behave identically during a particle size measurement using a defined technique. An example of this is a Malvern-type laser diffraction measurement technique.

[0045] In the context of the present invention, it is desired to obtain a powder of granules whose size distribution is substantially in the form of a Gaussian; the maximum of the Gaussian is typically centered on an average dimension of the granules greater than or equal to 150 μm, ensuring an absence or a very low proportion of granules of size less than or equal to 70 μm. This requirement comes from the fact that the presence of granules of size less than 70 μm in a powder mainly composed of silicon brings a risk in terms of explosiveness of said powder. Advantageously, the maximum of the Gaussian distribution in size of the granules is centered on an average dimension of approximately 0.8 mm. In general, the average dimension of the granules (average of the dimensions of all the granules) is between 150 μm and 1 mm.

[0046] To maintain its moisture content less than or equal to 2%, the granule powder can be packaged and stored in an inert atmosphere, for example in a nitrogen or argon atmosphere, or in a vacuum, after step c).

[0047] The method then comprises a step d) corresponding to the introduction of the granules into a liquid silicon casting ladle, at the outlet of a silica reduction furnace, to participate in the cooling of the liquid silicon to a refining temperature (aimed at reducing the levels of aluminum and calcium contained in the raw liquid silicon) and / or to a casting temperature.

[0048] Liquid silicon, resulting from the silica reduction reaction, arrives in the casting ladle at a temperature of around 1700°C. It generally then passes through a refining temperature of around 1550°C, then a casting temperature of around 1480°C, before being cast into ingots.

[0049] The granule powder from step c), added to the casting ladle, allows the liquid silicon to be cooled to reach one and / or the other of these temperatures. The mass proportion of granules introduced into the casting ladle is preferably between 1% and 5%. By mass proportion, we mean the ratio between the mass of granules incorporated and the mass of liquid silicon in the casting ladle.

[0050] The moisture content of the granules targeted in step c) takes on its full importance here: in fact, the decomposition of water at the temperature of the liquid silicon in the casting ladle can lead to an explosion (hydrogen) if the quantity of water exceeds a few %.

[0051] As stated previously, it is not critical that a residual amount of metallic contaminants remain in the granules because diamond wire cutting waste contains metallic contaminant levels 10 times to 100 times lower than the levels in the ladle.

[0052] Furthermore, even if the silicon particles making up the granules contain silicon oxide (covering all or part of the surface of said particles), this oxide will be melted when the powder is introduced into the casting ladle, due to the high temperature (around 1700°C) and the presence of a SiO2 / Al2O3 / CaO slag.

[0053] The process according to the invention thus makes it possible to recycle the silicon contained in the waste resulting from the cutting of ingots using diamond wires, by implementing a reduced number of steps.

[0054] It should be remembered that with the reduction in the size of silicon particles in the “kerfs” (from micrometric to nanometric), linked to progress in cutting technologies (reduction in wire diameter), the recycling of these very fine particles can encounter several difficulties: the coating of silicon particles by organic species contained in the cutting liquid, which most of the state-of-the-art processes attempt to eliminate completely, the extreme fineness of the particles which leads to a high specific surface area of ​​the corresponding powder, which induces their explosiveness, the covering of the surface of the particles by a silicon oxide whose melting temperature is higher than the melting temperature of silicon itself (1420°C); the state-of-the-art processes therefore treat the particles with acid to remove this covering.

[0055] The method according to the invention takes advantage of the composition of the first slurry from diamond wire cutting waste and adjusts it so as to promote the shaping of granules, rich in silicon. It also defines characteristics of the granule powder particularly suited to remelting said powder in a liquid silicon casting ladle, at the outlet of a silica reduction furnace, making it possible, in addition to recycling the silicon, to manage the liquid silicon cooling sequences in a completely secure manner and without consuming extracted raw materials.

[0056] The invention is not limited to the embodiments and examples described and variant embodiments may be made without departing from the scope of the invention as defined by the claims.

Claims

A method for recycling silicon ingot cutting waste from diamond wire sawing, comprising the following steps: a) recovering a first sludge, from said waste, formed by an aqueous mixture comprising silicon particles and organic species, but devoid of abrasive carbide-type particles; the first sludge having an initial mass percentage of organic species defined relative to the mass of solid matter contained in the first sludge, b) chemically treating the first sludge so as to reduce the initial mass percentage of organic species and to form a second sludge having a residual mass percentage of organic species of between 0.8% and 2% relative to the mass of solid matter contained in the second sludge;c) drying and associated granulation of the second sludge, by heating under vacuum and stirring, to form granules including the silicon particles and the organic species, said granules having dimensions whose average value is greater than or equal to 150 μm and a humidity level less than or equal to 2%; d) introducing the granules into a liquid silicon casting ladle, at the outlet of a silica reduction furnace, to participate in the cooling of the liquid silicon to a refining temperature and / or to a casting temperature.; Recycling method according to the preceding claim, in which the initial mass percentage of organic species is between 3% and 6%, typically of the order of 4%. Recycling method according to one of the preceding claims, in which the residual mass percentage of organic species is 1.3% + / - 0.2%. Recycling method according to one of the preceding claims, in which step c) is carried out at a temperature between 40°C and 100°C. Recycling method according to one of the preceding claims, in which the average size of the granules is approximately 0.8 mm. Recycling method according to one of the preceding claims, in which the moisture content of the granules is 1.5% + / - 0.2%. Recycling method according to one of the preceding claims, in which the mass proportion of granules introduced into the casting ladle is between 1% and 5%. Recycling method according to one of the preceding claims, in which the chemical treatment of step b) is carried out with a dilute solution of hydrogen peroxide. Recycling method according to one of the preceding claims, in which the chemical treatment of step b) is carried out with a dilute solution of a mineral peroxide. Recycling method according to the preceding claim, in which step b) comprises at least one wash, two or even three successive washes with pure water, after the chemical treatment, to obtain the second sludge.

Citation Information

Patent Citations

  • Recycling of silicon kerfs from wafer sawing

    EP2712844A1

  • Method for improving yield of metal silicon prepared by smelting diamond wire cutting silicon sludge

    CN114772602A

  • Silicon recycling system and silicon recycling method

    JP2011121049A

  • Treatment process for recycling silicon ingot cutting waste

    US20210253435A1