Method for producing a web-shaped composite material having a structured surface, composite material of this kind, and use thereof

The method of applying a UV-curable lacquer layer with an adhesion promoter on a web-shaped composite material addresses the inefficiencies of existing decorative laminate production, achieving high mechanical and thermal resistance and improved adhesion for enhanced surface performance.

WO2024235897A1PCT designated stage expired Publication Date: 2024-11-21FRITZ EGGER GMBH & CO OG
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2024/063036
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2024-05-13
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing methods for producing decorative laminates with three-dimensional surface structures are costly and inefficient, with high energy consumption and adhesion issues between the substrate and radiation-curable coatings, leading to surface defects and wear resistance problems.

Method used

A method involving a web-shaped composite material with a UV-curable lacquer layer and an adhesion promoter layer, hardened by high-energy radiation, providing a structured surface with medium Martens hardness for improved mechanical and thermal resistance, and enhanced adhesion to the carrier material.

Benefits of technology

The method enables the production of a composite material with high mechanical and thermal resistance, excellent adhesion, and improved scratch resistance, suitable for texturing and coating surfaces, reducing production costs and surface defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2024063036_21112024_PF_FP_ABST
    Figure EP2024063036_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing a web-shaped composite material (30, 30') having a structured surface (13, 13'), comprising the steps: providing a web-shaped substrate (5) made of paper and / or plastic, applying a UV-curable coating layer (7) made of acrylated oligomer onto the substrate (5), forming a three-dimensional surface structure (13, 13ʹ) in the coating layer (7) which has been applied onto the substrate, and at least partially curing the coating layer by irradiation with high-energy radiation, preferably UV light. The aim of the invention is to be able to economically produce composite material of the aforementioned type using a method of this kind, which composite material is characterized by high mechanical strength and thermal resistance for use as a structuring means or as a coating material. This aim is achieved in that at least one adhesion promoter layer (8) containing acrylated oligomer, a reactive diluent and a photoinitiator which responds to high-energy radiation, preferably UV radiation, is applied onto the substrate (5) before the UV-curable coating layer (7) is applied, and in that the coating layer (7) comprising the three-dimensional surface structure (13, 13ʹ) is cured to such an extent that the composite material (30, 30ʹ), in the finished state, has an average Martens hardness according to DIN EN ISO 14577 in the range of 10-80 N / mm2, wherein the indenter used as a test element for measuring the Martens hardness is pressed into the structured surface of the coating layer (7). The invention also relates to a composite material (30, 30ʹ) of this kind and to the use thereof.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Method for producing a web-shaped composite material having a structured surface, such a composite material and its use

[0002] The invention relates to a method for producing a web-shaped composite material having a structured surface, comprising the steps of: providing a web-shaped carrier material made of paper and / or plastic, applying a UV-curable lacquer layer made of acrylated oligomer to the carrier material, producing a three-dimensional surface structure in the lacquer layer applied to the carrier material and at least partially curing the lacquer layer by irradiation with high-energy radiation, preferably UV light.

[0003] In the context of the present invention, irradiation with high-energy radiation is understood to mean, in particular, irradiation with UV rays (UV light) and also irradiation with electron beams.

[0004] In particular, the invention relates to a web-shaped composite material, preferably produced by a process of the type mentioned above, with a web-shaped carrier material made of paper and / or plastic and a lacquer layer made of acrylated oligomer applied to the carrier material, which has a three-dimensional surface structure.

[0005] Furthermore, the invention relates to a use of the composite material according to the invention as a structure-imparting agent for texturing an embossable material surface, in particular a resin-containing laminate surface, or as a coating material for workpiece surfaces.

[0006] Decorative laminates are known in the art and are used, for example, as floor coverings or as surface materials for walls, ceilings, or furniture such as cabinets, worktops, tabletops, or similar. Such laminates are typically composed of a substrate, e.g., an MDF or HDF board or resin-impregnated paper layers, a decorative layer, and a transparent protective layer applied thereon. The protective layer is intended to protect the decorative layer from wear, particularly abrasion. For example, traditional floor laminate panels have a melamine resin-impregnated, transparent-curing overlay paper as a protective layer. The material of the protective layer often contains particles that increase wear resistance, for example, quartz or corundum particles.

[0007] In order to faithfully imitate natural materials such as wooden floorboards or stone slabs with decorative laminates, both visually and haptically, such laminates are provided with a three-dimensional surface structure in the prior art, which preferably corresponds to the printed image of the decorative layer of the laminate. For example, to imitate wooden floorboards, depressions are pressed into the transparent protective layer during the pressing of a laminate structure comprising a wood decor paper. The depressions essentially overlap the wood pores depicted in the wood decor. Such depressions, which are designed to correspond to the depicted pores, are also referred to in specialist circles as synchronous pores.

[0008] Decorative laminates with fantasy or single-coloured decors (uni-coloured decors) are also known in the prior art, for example laminates for worktops or table tops whose transparent protective layer or top layer is provided with a three-dimensional surface structure.

[0009] To produce laminates with a three-dimensional surface structure, the state of the art uses, for example, press plates with a surface structure created by engraving. The laminate is produced using a so-called short-cycle press (KT press) under high pressure and high temperature, with the engraved press plate mounted on a press plate facing the transparent, curing protective layer. During the pressing of the laminate, temperatures of, for example, over 120°C and a pressure of over 50 bar prevail. The production of engraved press plates is costly. Furthermore, the press plates are subject to considerable wear due to the high compressive stress.

[0010] Furthermore, it is known in the prior art to texture resin-impregnated laminate surfaces by means of web-shaped structuring agents - also called embossing matrices - using pressure and temperature, i.e. to provide the laminate surface with a three-dimensional surface structure.

[0011] A method for producing such a web-shaped structuring agent is described, for example, in EP 2 146 805. The method involves applying a curable coating to a web-shaped plastic film and then bringing it into contact with a structuring roller. During contact with the structuring roller, the coating is cured using electron beam or UV radiation, so that the three-dimensional structure is permanently transferred into the coating of the plastic film. The cured coating is then removed from the structuring roller together with the plastic film. Before curing, the coating contains 20 to 50% of an acrylic oligomer, 15 to 35% of a monofunctional monomer, and 20 to 50% of a multifunctional monomer for crosslinking. Curing the coating using electron beam radiation is associated with high investment costs and high energy consumption.Furthermore, when reworking the method according to EP 2 146 805, it has been shown that the adhesion of various resins or radiation-curing lacquers to the web-shaped carrier material is often insufficient, so that part of the resin or lacquer is deposited in the structure of the textured roller and cures there. This results in a recurring surface defect in the cured coating on the web-shaped carrier material. Cleaning the textured roller so that resin or lacquer deposits are completely removed from its structure is very complex. EP 3 720 673 discloses a further method for transferring an embossed structure to at least part of a surface of a coating agent. The essential steps of the method are carried out using a composite consisting of a substrate and an embossed and at least partially cured coating, used as the embossing matrix of an embossing tool.The coating agent used to produce the composite coating is a radiation-curable coating agent of defined composition. EP 3 720 673 teaches that there should preferably be no additional layer between the substrate and the composite coating. However, internal tests have shown that the process according to EP 3 720 673 does not produce satisfactory adhesion between the substrate and a comparatively hard coating. Rather, when a corresponding composite is used as an embossing die under conventional pressing conditions with temperatures around 185°C and a pressure of over 50 bar, detachment (delamination) of the coating from the substrate occurs.

[0012] DE 10 2013 007 429 proposes the use of a polyethylene terephthalate (PET) film etched on at least one surface for producing a textured surface film or a textured embossing die. The etched PET film is said to exhibit excellent wetting and adhesion to the resins or lacquers used for coating, so that during the production process of the textured surface film or embossing die, no resin or lacquer deposits on a textured roller used for texturing occur. DE 10 2013 007 429 proposes the use of trichloroacetic acid in the presence of precipitated silica to etch the PET film. Although this treatment of PET films improves adhesion, it is questionable from an environmental perspective. Furthermore, such films are difficult to obtain on the market.EP 2 527 408 discloses a method for producing a web-shaped film, in particular a coating film for a carrier body, wherein the film has a matte surface. The method comprises the steps of: providing a substrate forming a plastic, metal, or paper film; coating the substrate with a solvent-free and water-free, electron-beam-curable lacquer comprising an acrylate and color pigments; irradiating the coated substrate in the uncrosslinked state of the lacquer from the coating side with monochromatic UV radiation, for example by means of an excimer UV lamp emitting UV radiation with a wavelength of 172 nm, to produce a matte surface of the lacquer without fully curing or crosslinking it; and subsequently irradiating the matte coating with electron beams to crosslink and fully cure the coating.An oligomer is added to the varnish to increase the scratch resistance of the cured coating; no photoinitiator effective in the range of monochromatic UV radiation is added to the varnish.

[0013] WO 2020 / 190751 discloses a textured pressboard for use in the production of decorative laminate. The textured pressboard is produced by a process comprising the following steps: applying a UV-curable acrylate mixture to a surface of a pressboard substrate, pre-curing using an excimer UV lamp to create microwrinkles, and irradiating the UV-curable acrylate mixture with electron beams to completely cure the UV-irradiated layer and form a structured coating layer. Based on this, the invention is based on the object of specifying a process of the type mentioned above with which a web-like composite material with a structured surface can be produced cost-effectively, which composite material is characterized by high mechanical and thermal resistance for use as a structuring agent or as a coating material.In particular, a corresponding composite material is to be provided which is suitable as a structure generator for texturing an embossable material surface or as a robust coating material for workpiece surfaces and can therefore be used advantageously.

[0014] This object is achieved by a method having the features specified in claim 1 or by a composite material having the features specified in claim 17. Advantageous embodiments of the invention are the subject of the claims dependent on claim 1. Inventive uses of the composite material are the subject of claims 18 and 19.

[0015] The method according to the invention is characterized in that, before applying the UV-curable lacquer layer, at least one adhesion promoter layer containing acrylated oligomer, a reactive diluent and a photoinitiator reacting to high-energy radiation, preferably UV radiation, is applied to the carrier material, and that the lacquer layer having the three-dimensional surface structure is cured to such an extent that the composite material in the finished state has an average Martens hardness according to DIN EN ISO 14577-1 (2003-05) in the range of 10 to 80 N / mm 2 , preferably in the range of 30 to 80 N / mm 2 wherein the indenter used as a test specimen for measuring the Martens hardness is pressed into the structured surface of the paint layer.

[0016] In the process according to the invention, the lacquer layer having the three-dimensional surface structure is preferably cured by irradiation with high-energy radiation, particularly preferably with UV light, to such an extent that the composite material in the finished state has an average Martens hardness according to DIN EN ISO 14577-1 (2003-05) in the above-mentioned range.

[0017] By means of the at least one adhesion promoter layer (primer layer) according to the invention, a web-like composite material with a structured surface, which is characterized by high mechanical and thermal resistance for use as a structuring agent or as a coating material, can be produced cost-effectively using a method of the type mentioned above. The composite material produced or designed according to the invention can advantageously be used as a structuring agent for texturing an embossable material surface and, alternatively, also as a coating material for workpiece surfaces.

[0018] The adhesion promoter layer according to the invention enables the lacquer layer, which can be cured by high-energy radiation, preferably UV light, to adhere very well to the carrier material after the production of a three-dimensional surface structure on the lacquer layer and a subsequent partial or complete curing of the lacquer layer by high-energy radiation, preferably UV irradiation, so that neither when removing the cured lacquer layer together with the carrier material from an embossing device used to produce or form the three-dimensional surface structure nor when removing a structure generator produced in this way from a material or laminate surface textured therewith, does an unacceptable delamination or detachment of the structured lacquer layer from the carrier material occur which is visible to the naked eye.

[0019] The adhesion promoter layer according to the invention is also advantageous with regard to the use of the web-like composite material with a structured surface as a coating material for workpiece surfaces. When the composite material according to the invention is used as a coating material for highly stressed surfaces, such as floor panel surfaces, the adhesion promoter layer significantly improves the abrasion and scratch resistance of the respective surface. The composite material according to the invention is characterized by very good abrasion and scratch resistance when used as a coating material for highly stressed surfaces, such as flooring.Furthermore, the adhesion promoter layer can prevent delamination or detachment of the structured lacquer layer from the carrier material at the cut edges or machined workpiece edges when workpieces coated with the composite material, for example, workpiece panels, are cut into smaller formats or when such workpieces are edge-machined. Furthermore, the adhesion promoter layer according to the invention can prevent delamination or detachment of the structured lacquer layer from the carrier material at the cut edges or machined workpiece edges when using the

[0020] Composite material as a coating material for workpiece surfaces that have a significantly curved surface area, for example a rounded panel edge, leads to a delamination or detachment of the structured lacquer layer from the carrier material at the curved surface area. The adhesion promoter layer according to the invention is particularly advantageous with regard to the use of the composite material as a coating material for the production of so-called high-pressure laminates (HPL) and laminates produced by continuous pressing (CPL), including in so-called postforming processes. The technical term postforming refers to the subsequent deformation (mold formation) of an already applied surface coating of material panels along an edge profile. The composite material according to the invention is used in such a case, ieWhen coating a material panel with a profiled edge, the excess composite material is left over the profiled edge. The excess composite material is then glued or bonded to the profiled edge in a subsequent process using a postforming machine. Components produced in this way are used where wood-based materials or other cellulose-based carrier substrates and their edges are exposed to particularly high levels of moisture, chemicals, and / or mechanical stress, for example, in bathroom and kitchen furniture, as well as reception and sales counters.

[0021] The cross-cut test according to DIN EN ISO 2409:2013 (June 2013) is commonly used to determine the adhesion of coatings. While the test results do not provide direct measured values, they can be assessed by comparing them with standard images showing various graded degrees of damage (characteristic values). The standard specifies cutting knives of a specific shape and size as the testing instrument. For the measurement with a multi-cutting device, a cut band consisting of several parallel notches is drawn into the coating to be assessed, extending all the way down to the substrate. Then, another cut band is scratched at a right angle to this. This creates a grid with numerous squares, the so-called grid cut. For evaluation, an adhesive tape with a defined adhesive force is pressed onto the cross-cut and then pulled away from the surface to remove any delaminated pieces.By comparison with the standard images, the characteristic values ​​Gt0 to Gt5 are assigned, where Gt0 corresponds to a low level of damage in which no part of the coating has flaked off, whereas Gt5 corresponds to a very high level of delamination or damage in which the flaked off area of ​​the coating is more than 65% of the parts.

[0022] Using the process according to the invention, composite materials for use as texturers for texturing embossable material surfaces and those for use as coating materials for workpiece surfaces could be produced with very good adhesion of the structured coating layer to the substrate. The cross-cut test according to DIN EN ISO 2409:2013 (June 2013) resulted in a cross-cut characteristic value of 0 to less than or equal to 0.5 for the composite materials produced according to the invention for use as texturers or for use as coating materials for workpiece surfaces.

[0023] The adhesion promoter layer enables a wide processing spectrum from elastic to hard for the lacquer, which is curable by high-energy radiation, preferably UV light. Furthermore, the lacquer made of acrylated oligomer, which is curable by high-energy radiation, preferably UV light, used in the process according to the invention, enables the establishment of a high hardness of the lacquer layer produced therefrom or of the three-dimensional surface structure produced therein. The web-shaped composite material, which has a structured surface and is particularly suitable as a structure-imparting agent for texturing an embossable material surface, has, according to the invention, a medium Martens hardness according to DIN EN ISO 14577-1 (2003-05) in the range of 10 to 80 N / mm 2 , preferably in the range of 30 to 80 N / mm 2This is beneficial for the composite material's high mechanical and thermal resistance when used in a heated press. The relatively hard, three-dimensional surface structure of the composite material enables a long service life, particularly as a texturer or as a coating material for heavily stressed workpiece surfaces. Furthermore, a high degree of hardness of the lacquer layer, including the three-dimensional surface structure, is advantageous for achieving high molding accuracy, particularly with regard to molding accuracy when pressing a negative structure into an embossable material surface or resin-containing laminate surface. This allows, for example, appropriately textured floor panels or laminate boards to be produced that exhibit a relatively high surface roughness or roughness depth Rz according to DIN EN ISO 4287 (2009-11).

[0024] When determining indentation or Martens hardness according to DIN EN ISO 14577-1 (2003-05), the test force F and the penetration depth h are measured continuously during the loading and unloading phases. Martens hardness (HM) is defined as the ratio of the maximum force F to the corresponding contact area of ​​the test specimen and is measured in N / mm 2 As a test specimen (indenter), either a pyramid or a spherical indenter is pressed slowly and at a constant speed into the surface to be tested. The conversion of the indentation depth to the contact surface must be determined for each indenter shape. The contact surface for the Vickers or Berkovich pyramid, which are commonly used as indenters, is calculated as the product of the square of the indentation depth h and the constant 26.43. The so-called Martens hardness (HM) is then calculated as follows: HM = F / (26.43 • h 2 ).

[0025] Martens hardness is measured, for example, using a FischerScope HM2000S measuring device from Helmut Fischer at a temperature of approximately 23°C and a relative humidity of approximately 50%. The measurement is performed with a test range of 300 mN / 20 s up to a maximum test force of 300 mN in accordance with DIN EN ISO 14577-1 (2003-05).

[0026] According to an advantageous embodiment of the method according to the invention, the at least one adhesion promoter layer is applied to the carrier material with a layer thickness in the range of 0.5 to 12 μm, preferably in the range of 1 to 10 μm, particularly preferably in the range of 2 to 5 μm, based on the dry state of the adhesion promoter layer. The layer thickness of the adhesion promoter layer is preferably applied or formed as thin as possible. The inventor has surprisingly found that this results in a particularly good bond between the lacquer layer and the carrier material. The inventor assumes that the adhesion promoter layer being formed as thin as possible improves or strengthens the bond between the lacquer layer and the carrier material in that the thin adhesion promoter layer simultaneously effects a chemical bond between the substrate surface of the carrier material and the binder of the lacquer layer.

[0027] Before applying the UV-curable lacquer layer, the adhesion promoter layer is preferably dried or cured to such an extent that it is at least contact dry.

[0028] The at least one adhesion promoter layer applied to the carrier material in the process according to the invention can, as stated above, be specified in more detail, particularly with regard to its layer thickness in the dry state. Alternatively or additionally, the at least one adhesion promoter layer can also be specified in more detail with regard to its basis weight (coating weight) in the dry state, which can be calculated from the layer thickness and the density of the adhesion promoter applied to the carrier material in the dry state. In the case of a carrier material made of film or whose surface provided with the adhesion promoter is defined by a film, the basis weight of the adhesion promoter in the dry state is, for example, in a range of approximately 0.3 to 15 g / m 2, preferably in a range of approximately 1 to 5 g / m 2 . In the case of a carrier material made of paper or whose surface is defined by the adhesion promoter, the basis weight of the adhesion promoter in the dry state is, for example, in a range of approximately 1 to 15 g / m 2 , preferably in a range of approximately 4 to 7 g / m 2. A further advantageous embodiment of the invention provides that an adhesion promoter is used for the adhesion promoter layer which contains 10 to 90 wt.%, preferably 40 to 70 wt.% acrylated oligomer, 5 to 30 wt.% reactive diluent, 0.5 to 10 wt.% UV-reactive photoinitiator and optionally 0.1 to 3 wt.% of one or more additives from a group comprising defoamers and substrate wetting agents, wherein the amounts of all constituents contained in the adhesion promoter add up to 100 wt.%. The acrylated oligomer is preferably at least di- or trifunctional, particularly preferably higher-functional. Polyurethane acrylate, for example, is used as the acrylated oligomer. The reactive diluent reduces the viscosity of the adhesion promoter.A low viscosity of the adhesion promoter promotes the formation of a thin, full-surface adhesion promoter layer on the substrate surface of the web-like carrier material when applied in small quantities. For this purpose, the viscosity of the adhesion promoter is preferably reduced to a minimum.

[0029] The defoamer optionally included in the adhesion promoter serves to combat (dissolve) air or gas inclusions that occur in the liquid adhesion promoter layer. Such inclusions, which appear in the form of foam bubbles, e.g., micro- and macrofoam bubbles, can cause pores and craters in the adhesion promoter layer, which prevent optimal adhesion between the substrate surface of the web-shaped carrier material and the binder of the subsequently applied UV-curable coating layer and / or reduce the surface quality of the texture enhancer.

[0030] The substrate wetting agent optionally included in the adhesion promoter serves to adjust the interfacial energy between the substrate surface of the web-like carrier material and the liquid adhesion promoter. For example, the substrate wetting agent reduces the interfacial energy or surface tension on the substrate. This optimizes the wetting of the substrate surface, resulting in uniform and good wetting of all areas of the substrate surface and thus a well-adhering, pore-free adhesion promoter layer.

[0031] UV-curable reactive diluents used in the adhesion promoter include, for example, 1,6-hexanediol diacrylate (HDDA), dipropylene glycol diacrylate (DPGDA), tripropylene glycol diacrylate (TPGDA), ethylene glycol dimethacrylate (EGDMA), triethylene glycol divinyl ether (DVE-3), or combinations / mixtures of these diluents. UV-sensitive photoinitiators used in the adhesion promoter layer include, for example, monoacylphosphine oxide (MAPO), bisacylphosphine oxide (BAPO), 2-hydroxy-2-methylphenylpropanone (HMPP), 1-hydroxycyclohexylphenyl ketone (CPK), and / or methylbenzoyl formate (MBF).

[0032] Optionally, the adhesion promoter layer may contain aminopropyltriethoxysilane (AMEO), for example in a proportion in the range of 3 to 8 wt.%.

[0033] Another or alternative embodiment of the invention provides that an adhesion promoter is used for the adhesion promoter layer which contains 10 to 90 wt.%, preferably 40 to 70 wt.% acrylated oligomer dispersion and / or acrylated oligomer emulsion, 5 to 30 wt.% reactive diluent, 0.5 to 10 wt.% UV-reactive photoinitiator and optionally 0.1 to 3 wt.% of one or more additives from a group comprising defoamers and substrate wetting agents, wherein the amounts of all constituents contained in the adhesion promoter add up to 100 wt.%. This embodiment is advantageous when the web-shaped carrier material to which the adhesion promoter layer and subsequently the UV-curable lacquer layer are applied consists of paper or is formed, among other things, from paper, wherein the adhesion promoter layer is applied to the paper.The bond between the adhesion promoter and the paper can be improved by adding a water content to the acrylated oligomer dispersion and / or acrylated oligomer emulsion. According to a further embodiment of the process according to the invention, the varnish used for the UV-curable varnish layer contains a water content of 100%.

[0034] 30 to 95 wt.% acrylated oligomer,

[0035] 10 to 70 wt.% mono- or multifunctional monomer,

[0036] 1 to 5 wt.% photoinitiator, and optionally

[0037] 1 to 6 wt.% of one or more additives from a group comprising defoamers, substrate wetting agents, release additives, waxes, and anti-settling agents, whereby the amounts of all components contained in the UV-curable coating add up to 100 wt.%. A UV-curable coating with a corresponding composition enables the creation of a high hardness of the resulting coating layer or the three-dimensional surface structure created thereon, for example, an embossed structure.

[0038] The inventor has surprisingly found that a composite material of the type mentioned at the outset can be produced cost-effectively using a UV-curable lacquer composed in this way, the three-dimensional surface structure or embossed structure produced on the lacquer layer having a high degree of hardness and molding accuracy, so that by means of the composite material according to the invention, when used as a structure generator, correspondingly large structure depths can be pressed into an embossable material surface, in particular a resin-containing laminate surface, without any noticeable or significant loss of depth.

[0039] According to a further embodiment, the lacquer used for the UV-curable lacquer layer contains 50 to 95 wt.% acrylated oligomer and / or

[0040] 10 to 40 wt.% mono- or multifunctional monomer and / or

[0041] 1 to 3 wt.% photoinitiator and / or 1 to 5 wt.% of one or more additives from a group comprising defoamers, substrate wetting agents, release additives, waxes, and anti-settling agents, wherein the amounts of all components contained in the UV-curable varnish add up to 100 wt.%. By using such a varnish, a composite material of the type mentioned above can be realized particularly advantageously. The relatively high proportion of acrylated oligomer, in combination with the mono- or multifunctional monomer, enables the high hardness of the three-dimensional surface structure formed from the varnish. By adding a release additive, a precise separation of the surface structure created in the varnish layer from an embossing tool, e.g., an embossing roller or embossing belt, as well as a precise separation of the composite material or structure-imparting agent from a material surface textured with it can be optimized.By adding wax as an additive, suboptimal curing on the surface of the paint layer, combined with permanent tackiness of the paint layer, can be prevented. Suboptimal curing and permanent tackiness can result from the interaction of atmospheric oxygen with the applied paint layer. By adding an anti-settling agent, settling of one or more specific components of the paint is prevented, so that the composition, in particular the hardness of the produced paint layer or three-dimensional surface structure, is essentially homogeneous across its layer thickness. With regard to the addition of a defoamer and / or substrate wetting agent to the paint composition and the resulting effects, reference is made to the above statements on corresponding additives of the adhesion promoter to avoid repetition.

[0042] The lacquer used for the UV-curable lacquer layer preferably contains no color pigment. The adhesion promoter used according to the invention also preferably contains no color pigment. This allows a high degree of transparency to be achieved in the composite material according to the invention, especially if its carrier material consists of or is formed from transparent paper or plastic.

[0043] A further embodiment of the invention provides that the photoinitiator of the UV-curable lacquer is selected such that this photoinitiator is suitable for absorbing light with a wavelength in the range of 360 to 420 nm, preferably in the range of 390 to 400 nm. This embodiment of the invention enables rapid and energy-efficient curing of the lacquer layer provided with the three-dimensional surface structure, so that the web-shaped composite material can be produced at a high production speed. The production or web speed of the composite material in the production process according to the invention can be, for example, in the range of 5 to 15 m / min.

[0044] According to a further embodiment of the process according to the invention, the adhesion promoter or the adhesion promoter layer and / or the lacquer used for the UV-curable lacquer layer contain urethane acrylate, polyester acrylate, epoxy acrylate or a mixture of two or three of these acrylates as an acrylated oligomer. These acrylates, in particular urethane acrylates, are characterized by high toughness, good adhesion, and high abrasion resistance. The composite material produced according to the invention thus acquires corresponding toughness and strength properties that lend it great robustness, particularly when the composite material is used as a coating material, but also for multiple uses as a texture imparter. Furthermore, when the composite material is used as a texture imparter, this embodiment contributes to high molding accuracy or embossing accuracy when texturing the relevant material surface, e.g., a laminate surface.

[0045] A further advantageous embodiment of the method according to the invention is characterized in that the UV-curable lacquer layer is applied by means of at least one UV light emitting LED emitter with a UV radiation output in the range of 8 to 16 W / cm 2 , preferably in the range of 10 to 14 W / cm 2 cured. This embodiment of the invention allows composite materials of the type mentioned here to be produced cost-effectively and in an energy-efficient manner with relatively low plant engineering expenditure.

[0046] The three-dimensional surface structure of the lacquer layer of the composite material according to the invention can be produced in various ways. An advantageous embodiment of the invention provides that the three-dimensional surface structure is produced by means of a mechanical embossing tool, preferably an embossing roller or a plate- or web-shaped structuring device. This embodiment makes it possible to produce a surface structure on the lacquer layer with depressions, wherein the depressions can, for example, have a depth greater than 100 μm, in particular greater than 200 μm, and occasionally even greater than 500 μm. The upper limit of the depth of the surface structure depends in particular on the layer thickness of the lacquer layer. The upper limit of the depth of the depressions can, for example, be in the range of approximately 1 to 2 mm.By means of such depressions in the surface structure of the composite material according to the invention, for example, wood pores can be reproduced in a deceptively similar manner to imitate natural wood or joints to imitate a plank or tiled floor.

[0047] If an embossing roller or the like is used in the method according to the invention to form the three-dimensional surface structure, the structure or composite formed from the web-shaped carrier material, the adhesion promoter layer and the lacquer layer is preferably guided around the embossing roller with a wrap angle in the range of approximately 60° to 200°, particularly preferably in the range of approximately 100° to 180°.

[0048] In an alternative or supplementary embodiment of the invention, it is provided that the three-dimensional surface structure is created by irradiation using a UV radiation source, wherein the UV radiation source emits UV light with a wavelength in the range of 100 to 230 nm, preferably in the range of 130 to 190 nm, particularly preferably in the range of 170 to 175 nm, especially preferably of approximately 172 nm. This irradiation gives the lacquer layer a very fine three-dimensional surface structure that conveys a matte optical impression. For this purpose, the lacquer layer is first irradiated with high-energy light, which preferably has a wavelength in the range of 170 to 175 nm, as a result of which a very thin surface layer of the lacquer is polymerized and thus hardened. During this irradiation, shrinkage occurs in an uppermost region of the lacquer layer, which causes what is known as microfolding.This creates a micro-fold on the surface of the lacquer layer. The UV radiation source used to create the micro-fold is, for example, a so-called excimer lamp, preferably an excimer laser. The height or depth of the three-dimensional surface structure created by the micro-fold is, for example, in a range of 50 to 300 nm, particularly in the range of 80 to 200 nm. The micro-fold results in the lacquer surface having a low gloss, i.e., a matte gloss.

[0049] A further advantageous embodiment of the method according to the invention is characterized in that the web-shaped carrier material used is a web-shaped carrier material made of paper and / or plastic that is at least partially permeable to high-energy radiation, in particular to UV light. This embodiment is advantageous from a manufacturing point of view. It enables the production of the composite material according to the invention in which the irradiation takes place at least partially from the side of the carrier material facing away from the structured surface.Accordingly, a further advantageous embodiment of the invention provides that a partial curing of the lacquer layer is carried out by irradiation with high-energy radiation, preferably UV light, during the production of the three-dimensional surface structure in such a way that the irradiation takes place at least partially from the side of the carrier material facing away from the structured surface.

[0050] The web-shaped carrier material can thus be moved at a relatively high conveying speed through a device for producing the three-dimensional surface structure, for example, a device equipped with an embossing roller. The initially flowable lacquer layer can be cured sufficiently quickly during the formation of the surface structure (embossed structure) by means of at least one emitter emitting high-energy radiation, preferably UV light, at a favorable position within the device, so that the carrier material, together with the lacquer layer having the surface structure, can then be pulled off or separated from the embossing roller or an embossing tool in a dimensionally stable manner. This embodiment of the invention is particularly advantageous from a manufacturing point of view.

[0051] The web-shaped carrier material used in the process according to the invention, which is at least partially permeable to high-energy radiation, in particular UV light, can also be referred to as a transparent web-shaped carrier material. A transparent carrier material is understood to be a light-permeable carrier material, which can be transparent or translucent.

[0052] Transparent materials allow the majority of light to pass through, although a small amount is usually absorbed and scattered. Examples of such transparent substrates are films made of polyethylene terephthalate (PET), polycarbonate (PC), or polymethyl methacrylate (PMMA). Translucent materials are characterized by the fact that, although light passes through them, the light is scattered within the material. Examples of translucent substrates are papers, particularly so-called parchment papers, which can be more or less translucent depending on the design. The basis weight of the transparent paper can, for example, be between 80 and 180 g / m². 2 be.

[0053] The web-shaped carrier material used according to the invention can, for example, have an emitted UV radiation dose in the range of 1,500 to 2,200 mJ / cm 2transmit 60 to 80% of the UV radiation. The measured transmitting UV radiation is then in the range of 900 to 1,760 mJ / cm 2 , especially in the range of 1,300 to 1,500 mJ / cm 2 .

[0054] An advantageous embodiment of the method according to the invention provides that the adhesion promoter layer applied to the web-shaped carrier material is pre-dried before applying the UV-curable lacquer layer. This can be done, for example, by irradiating the applied adhesion promoter layer with UV radiation and / or by thermal drying.A further advantageous embodiment of the method according to the invention is characterized in that a paper material web is used as the web-shaped carrier material, wherein an aqueous adhesion promoter is applied to the carrier material to produce the adhesion promoter layer, wherein the adhesion promoter layer is dried at least in the surface region before the UV-curable lacquer layer is applied thereto, and wherein the drying is carried out using UV radiation and temperatures in the range from 80° C to 160° C, preferably in the range from 90° C to 140° C, particularly preferably in the range from 100° C to 120° C.

[0055] The water content of the aqueous adhesion promoter improves the bond between the adhesion promoter and the fibers of the paper web. The water content is then removed or largely reduced by drying. This allows for a relatively thin adhesion promoter layer, which ensures a particularly good bond between the substrate surface of the web-like carrier material (paper) and the binder of the UV-curable coating layer.

[0056] An advantageous variant of the method according to the invention provides that a plastic film is used as the web-shaped carrier material, wherein the adhesion promoter layer is cured by means of high-energy radiation, preferably UV radiation, in particular UV-C radiation, before the UV-curable lacquer layer is applied to the adhesion promoter layer, at least to the extent that the adhesion promoter layer is solid and / or substantially non-adhesive on its surface, wherein the photoinitiator of the adhesion promoter layer is suitable for absorbing light with a wavelength in the range from 250 to 350 nm, preferably in the range from 270 to 330 nm, and wherein the adhesion promoter layer is cured with a UV radiation dose in the range from 60 to 200 mJ / cm 2 , preferably 100 to 160 mJ / cm 2is cured. The use of a plastic film as a web-shaped carrier material is advantageous in terms of material costs and the robustness of the carrier material and thus of the composite material, which is preferably used as a structuring or coating material. The pre-curing or curing of the adhesion promoter layer to the extent that its surface is solid and / or essentially non-adhesive before the UV-curable lacquer layer is applied to it improves the bond between the substrate surface of the carrier material (plastic film) and the binder of the UV-curable lacquer layer. This design has the particular advantage that the adhesion promoter unfolds its optimal effect directly at the interface and can therefore be applied in relatively small quantities to still achieve high or excellent adhesion values.The photoinitiator of the adhesion promoter layer used according to this embodiment enables rapid and energy-efficient curing or at least pre-curing of the adhesion promoter layer at the specified UV radiation dose, so that the composite material according to the invention can be produced at a high production speed.

[0057] A further advantageous embodiment of the method according to the invention is characterized in that the UV-curable lacquer layer is applied by means of at least one UV light emitting LED emitter with a UV radiation output in the range of 8 to 16 W / cm 2 , preferably in the range of 10 to 14 W / cm 2 is cured. This embodiment of the invention allows composite materials, in particular structural elements of the type mentioned here, to be produced cost-effectively and in an energy-efficient manner with relatively low plant engineering expenditure.

[0058] A further advantageous embodiment of the method according to the invention provides that the UV-curable lacquer layer is finally cured by means of at least one mercury vapor medium-pressure lamp or at least one UV-C lamp, wherein the final curing is preferably carried out using a UV radiation dose in the range of 500 to 3,000 mJ / cm 2is carried out. This embodiment of the invention enables composite materials, in particular structure-forming agents of the type mentioned here, to be manufactured at high production speeds. During the creation of the three-dimensional surface structure, the UV-curable lacquer layer applied to the adhesion promoter layer is partially cured (pre-cured). The lacquer layer is cured (partially cured) to such an extent that the composite comprising web-shaped carrier material, adhesion promoter, and lacquer layer can be peeled off an embossing tool, preferably an embossing roller, with high molding accuracy, so that a surface structure formed into the lacquer layer is removed from the embossing tool essentially without loss and with dimensionally stable properties. During this first curing step, for example, approximately 50 to 80% of the curing required for complete curing can take place.The final curing (post-curing) of the composite removed from the embossing tool then takes place by means of at least one medium-pressure mercury vapor lamp or at least one UV-C lamp using a UV radiation dose that is preferably in the range of 500 to 3,000 mJ / cm. 2 , for example in the range of 800 to 2,800 mJ / cm 2 , especially in the range of 1,000 to 2,500 mJ / cm 2 The curing (pre-curing) of the UV-curable lacquer layer applied to the adhesion promoter layer can thus, for example, take place while the lacquer layer is in contact with an embossing tool, whereas the final curing (post-curing) of the lacquer layer takes place when the lacquer layer is out of contact with the embossing tool.

[0059] It is also within the scope of the invention that the previously described final curing (post-curing) of the UV-curable lacquer layer is carried out by means of at least one medium-pressure mercury vapor lamp or at least one UV-C lamp after the three-dimensional surface structure of the lacquer layer has been produced in the form of a microfold by means of an excimer UV lamp.

[0060] A further advantageous embodiment of the method according to the invention is characterized in that the three-dimensional surface structure on the UV-curable lacquer layer is formed in such a way that, after the lacquer layer has hardened, it has an average roughness depth Rz according to DIN EN ISO 4287 (2009-11) in the range from 40 to 200 μm, preferably in the range from 100 to 200 μm. With an appropriately designed structure generator, three-dimensional surface structures can be created in embossable material surfaces, in particular resin-containing laminate surfaces, which give the surface in question the appearance of natural material, for example the appearance of a wood grain with pores.

[0061] The application quantity and thus the application weight of the UV-curable coating layer depends in particular on the required or to be achieved average roughness depth Rz of the cured coating layer. Furthermore, for economic reasons, it is expedient to limit the application quantity and thus the application weight of the UV-curable coating layer in order to avoid unnecessary material costs. In the process according to the invention, the application weight (application quantity) of the UV-curable coating layer is, for example, in a range of 10 to 250 g / m². 2 , preferably in a range of 25 to 200 g / m 2 , particularly preferably in a range of 30 to 100 g / m 2 .

[0062] The average roughness depth Rz is the arithmetic mean of individual roughness depths from five consecutive measurement sections in a roughness profile. The average roughness depth Rz is determined as follows: A defined measurement section on the surface of the workpiece in question or of the composite material according to the invention is divided into seven individual measurement sections, with the average measurement sections being of equal size. The roughness depth Rz is determined only over these five measurement sections, since the Gaussian filter to be used requires half a measurement section for pre- and post-run. For each of these individual measurement sections of the profile, the difference between the maximum and minimum values ​​is determined. The average value is calculated from the five individual roughness depths thus obtained.

[0063] The roughness depth Rz is measured according to DIN EN ISO 4287 (2009-11) and DIN EN ISO

[0064] 4288. The measuring instrument used to measure the roughness depth Rz must comply with DIN EN ISO 3274. The profile filter(s) used must comply with DIN EN ISO 11562.

[0065] Furthermore, the present invention relates to a web-shaped composite material, preferably produced by a process according to one of the above-mentioned embodiments, with a web-shaped carrier material made of paper and / or plastic and a lacquer layer made of acrylated oligomer, which is applied to the carrier material and has a three-dimensional surface structure, characterized in that the lacquer layer is connected to the carrier material via at least one adhesion promoter layer made of acrylated oligomer, a reactive diluent and a photoinitiator reacting to UV radiation, wherein the composite material in the finished state has an average Martens hardness according to DIN EN ISO 14577 -1 (2003-05) in the range from 10 to 80 N / mm 2, preferably in the range of 30 to 80 N / mm 2 wherein the indenter used as a test specimen to measure the Martens hardness was pressed into the structured surface of the paint layer.

[0066] The composite material according to the invention is characterized by the advantages described above with regard to the method according to the invention for producing the composite material.

[0067] An advantageous embodiment of the composite material according to the invention is characterized in that its adhesion promoter layer contains 10 to 90 wt. %, preferably 40 to 70 wt. % acrylated oligomer, 5 to 30 wt. % reactive diluent, 0.5 to 10 wt. % UV-reactive photoinitiator and optionally 0.1 to 3 wt. % of one or more additives from a group comprising defoamers and substrate wetting agents, wherein the amounts of all components contained in the adhesion promoter layer add up to 100 wt. %. The correspondingly formed composite material is characterized by high mechanical and thermal resistance for its use as a structuring agent or as a coating material. A further advantageous embodiment of the composite material according to the invention provides that an adhesion promoter is used for the adhesion promoter layer which contains 10 to 90 wt. %, preferably 40 to 70 wt.-% acrylated oligomer dispersion and / or acrylated oligomer emulsion, 5 to 30 wt.% reactive diluent, 0.5 to 10 wt.% UV-responsive photoinitiator, and optionally 0.1 to 3 wt.% of one or more additives from a group comprising defoamers and substrate wetting agents, wherein the amounts of all components contained in the adhesion promoter add up to 100 wt.%. The correspondingly formed composite material is also characterized by high mechanical and thermal resistance for its use as a structuring agent or as a coating material.

[0068] According to a further embodiment of the composite material according to the invention, this is characterized in that its lacquer layer having the surface structure has, after curing, an average roughness depth Rz according to DIN EN ISO 4287 (2009-11) in the range from 10 to 200 μm, preferably in the range from 40 to 200 μm, particularly preferably in the range from 100 to 200 μm.

[0069] The application weight of the UV-curable lacquer layer, for example, is in a range of 10 to 250 g / m 2 , preferably in a range of 25 to 200 g / m 2 , particularly preferably in a range of 30 to 100 g / m 2 .

[0070] The composite material according to the invention, if its web-shaped carrier material is a plastic film web that is at least partially permeable to high-energy radiation, in particular UV radiation, can also be advantageously used in the so-called CCl process for texturing embossed lacquer surfaces. CCI stands for Calender Coating Inert. Using the CCI process, paintable material panels, for example MDF, HDF, or plastic panels, can be provided with a high-gloss or matte lacquer surface. In this process, the material surface, preferably a wood-based material surface, is dried or cured using UV light through a transparent film in a calender after the application of UV lacquer. In the CCI process, the material surface is preferably first primed and then UV lacquer is applied as the final coat. The material panel coated with liquid UV lacquer is conveyed directly into the calender.There, the surface cures under inert conditions. In other words, an "encapsulated drying" of the coated material panel takes place under a film. The composite material according to the invention can advantageously be used as this film if its carrier material consists of or is formed from a plastic film web that is at least partially permeable to UV radiation. In this way, material panels with a textured coated surface can be produced that meet the highest quality requirements.

[0071] The invention thus particularly relates to the use of the composite material according to the invention as a structuring agent for texturing an embossable material surface, for example, in a press for producing decorative laminates under the influence of heat and pressure or in a coating process in which a surface of a sheet-like material, after application of UV varnish in a calender, is dried and / or cured by means of UV light through a transparent film in the form of the composite material. Likewise, the composite material according to the invention can be used to structure a material in a molten or plastically deformable state, for example, an edgeband.

[0072] A further advantageous use of the composite material according to the invention consists in its use as a coating material for workpiece surfaces, preferably for plate-shaped workpieces, in particular for surfaces of workpieces made of wood-based material, laminate, plastic and / or laminate or combinations of at least two such materials.

[0073] Compared to conventional laminates, which have a wear-resistant surface coating made of melamine-formaldehyde resin and are therefore often perceived as cool to the touch and cause audible impact noise when walked on, the composite material according to the invention, with its lacquered surface made of acrylated oligomer, is characterized by a significantly more pleasant feel and improved impact sound properties. Wood-based panels coated with the composite material according to the invention feel pleasantly "warm" to the touch.

[0074] The invention is explained in more detail below with reference to several exemplary embodiments. The drawings show schematically:

[0075] Fig. 1 shows a method and a device for producing a web-shaped composite material which can be used, for example, as a structure-forming agent for texturing an embossable material surface, in particular a resin-containing laminate surface, in a side view;

[0076] Fig. 2 shows a second embodiment of a method and a device for producing a web-shaped composite material which can be used, for example, as a structure generator for texturing an embossable material surface, in particular a resin-containing laminate surface, in a side view;

[0077] Fig. 3 shows a third embodiment of a method or a device (1') for producing a web-shaped composite material which can be used, for example, as a structure generator for texturing an embossable material surface, in particular a resin-containing laminate surface, in a side view;

[0078] Fig. 4 shows a use of the composite material according to the invention as a coating material for workpiece surfaces; Fig. 5 shows a further example of the use of the composite material according to the invention as a coating material for workpiece surfaces, and

[0079] Fig. 6 shows an example of the use of the composite material according to the invention as a structure generator.

[0080] Fig. 1 schematically shows a device 1 that can be used to carry out the method according to the invention and illustrates the method according to the invention by way of example. Using this device, three-dimensional structures 2, in particular replicas of wood grain, natural stone, mosaic, and / or tile pattern structures, can be transferred from a corresponding master structure, which is designed, for example, in the form of an embossing roller 3, to a carrier material 5 coated with UV-curable varnish 4.

[0081] The carrier material 5 is a web-shaped carrier material made of paper and / or plastic, which in the embodiment according to Fig. 1 is at least partially permeable to high-energy radiation, in particular to UV light. The carrier material 5 is provided as a roll 6 in wound form. For example, a film permeable to UV radiation is used as the carrier material 5, which is made of polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polycarbonate (PC), polymethyl methacrylate (PMMA), polyvinyl chloride (PVC) or another plastic permeable to UV radiation. The film can also be referred to as a transparent film. The thickness of the film is, for example, in the range of 50 to 200 μm, preferably in the range of 75 to 125 μm, particularly preferably in the range of 100 to 125 μm. Alternatively, transparent paper permeable to UV radiation is used as the web-shaped carrier material 5.The basis weight of the paper, for example, is in the range of 80 to 180 g / m. 2 , preferably in the range of 150 to 170 g / m 2 . A UV-curable lacquer layer 7 made of acrylate is applied to the carrier material 5.

[0082] Oligomer is applied, into which a three-dimensional surface structure is subsequently formed. The three-dimensional surface structure created in the lacquer layer 7 can also be referred to as a three-dimensional embossed structure.

[0083] According to the invention, at least one adhesion promoter layer 8 is applied to the carrier material 5 before the UV-curable lacquer layer 7 is applied, which layer contains acrylated oligomer, a reactive diluent and a photoinitiator reacting to UV radiation.

[0084] The adhesion promoter layer 8 contains, for example, 10 to 90% by weight, preferably 40 to 70% by weight of acrylated oligomer, at least 8% by weight, preferably at least 20% by weight of reactive diluent and 0.5 to 10% by weight, preferably 0.5 to 5% by weight of photoinitiator reacting with UV radiation.

[0085] The adhesion promoter used for the adhesion promoter layer 8 or the adhesion promoter layer formed therewith can, according to a preferred embodiment, have the following composition:

[0086] 60 to 90 wt.% Ebercryl 4265 from Allnex (as acrylated oligomer or comparable polyurethane acrylate),

[0087] 10 to 30 wt.% triethylene glycol divinyl ether (e.g. Ashland Rapidure DVE-3 or comparable monomer),

[0088] 5 to 10 wt.% methylbenzoylformate (MBF or comparable UV-responsive photoinitiator) and

[0089] 0.1 to 3 wt.% of one or more additives from a group comprising defoamers and substrate wetting agents, wherein the amounts of all components contained in the adhesion promoter layer add up to 100 wt.%.

[0090] The photoinitiator is suitable, for example, for absorbing light with a wavelength in the range of 250 to 350 nm, preferably in the range of 270 to 330 nm. The adhesion promoter is applied to the web-shaped carrier material 5, for example, by means of an engraved or rubberized application roller 9.

[0091] If transparent paper permeable to UV radiation is used as the carrier material 5, the adhesion promoter for forming the adhesion promoter layer 8 is preferably applied to the paper web in aqueous form, and the adhesion promoter layer 8 is thermally dried before applying the UV-curable lacquer layer 7. Drying can be carried out, for example, by means of a radiant heater device 10 facing the adhesion promoter layer 8. Alternatively or additionally, a thermal drying device, for example a radiant heater device (not shown), can also be arranged on the side 11 of the paper web 5 facing away from the adhesion promoter layer 8 (underside or back side).

[0092] The application quantity of the aqueous adhesion promoter is adjusted such that the adhesion promoter layer 8, in the dry state, has a layer thickness in the range of 0.5 to 12 μm, preferably in the range of 1 to 10 μm, particularly preferably in the range of 2 to 5 μm. In other words, the application quantity of the aqueous adhesion promoter on the paper web is adjusted, for example, such that the adhesion promoter layer 8, in the dry state, has a basis weight in the range of approximately 1 to 15 g / m 2 , preferably in the range of approx. 4 to 7 g / m 2 The drying of the adhesion promoter layer 8 takes place, for example, using temperatures in the range from 80°C to 160°C, preferably in the range from 90°C to 140°C, particularly preferably in the range from 100°C to 120°C.

[0093] If a plastic film web permeable to UV radiation is used instead of a paper web, the adhesion promoter for forming the adhesion promoter layer 8 is preferably applied in non-aqueous form to the plastic film web, and the adhesion promoter layer 8 is cured by UV radiation before the UV-curable lacquer layer 7 is applied, to such an extent that the adhesion promoter layer 8 is solid and / or essentially non-adhesive on its surface. This at least partial curing of the adhesion promoter layer 8 can be carried out, for example, by means of one or more UV lamps 12, preferably one or more UV-emitting LED lamps, which face the adhesion promoter layer and / or are arranged on the opposite side (underside or back) 11 of the web-shaped plastic film. The adhesion promoter layer 8 is cured, for example, with a UV radiation dose in the range of 60 to 200 mJ / cm 2 , preferably 100 to 160 mJ / cm2 hardened.

[0094] Furthermore, it is also within the scope of the invention to carry out the at least partial curing of the adhesion promoter layer 8 by combining thermal drying and radiation curing - as described above.

[0095] The application quantity of the non-aqueous adhesion promoter is adjusted such that the adhesion promoter layer 8 formed therefrom has a layer thickness in the dry state in the range of 0.5 to 12 μm, preferably in the range of 1 to 10 μm, particularly preferably in the range of 2 to 5 μm. In other words, the application quantity of the non-aqueous adhesion promoter on the plastic film web is adjusted, for example, such that the adhesion promoter layer 8 has a basis weight in the dry state in the range of approximately 0.3 to 15 g / m 2 , preferably in the range of approximately 1 to 5 g / m 2 has.

[0096] After the adhesion promoter layer 8 has been at least partially dried or at least partially cured, the UV-curable lacquer made of acrylated oligomer is applied thereto for the subsequent production or formation of a three-dimensional surface structure (embossed structure) 13.

[0097] For the UV-curable lacquer layer 7, a lacquer is preferably used as a structural lacquer which

[0098] 30 to 95 wt.% acrylated oligomer,

[0099] 10 to 70 wt.% mono- or multifunctional monomer, 1 to 5 wt.% photoinitiator, and optionally

[0100] 1 to 6 wt.% of one or more additives from a group comprising defoamers, substrate wetting agents, release additives, waxes, and anti-settling agents, wherein the amounts of all components contained in the UV-curable coating add up to 100 wt.%. The photoinitiator of the UV-curable coating is suitable for absorbing light with a wavelength in the range of 360 to 420 nm, preferably in the range of 390 to 400 nm.

[0101] The UV-curable coating can be applied using a roller or doctor blade application device, preferably a Commabar application device 14. The Commabar application device 14 has a special doctor blade formed from a roller into which a recess 14.1 of approximately 90° has been machined. This recess 14.1 makes the profiled rod-shaped blade appear like a comma in the side view (cross-sectional view). The adjustment of the Commabar or the outlet opening defined by the Commabar and the associated coating box can be achieved by changing its horizontal and vertical position as well as by changing the angle of rotation. Due to the rounded blade geometry, the shear forces acting on the UV-curable coating are lower than with conventional doctor blades. The Commabar system is advantageous when applying dilatant, viscoelastic UV coatings.The possible variation in application weight and viscosity is particularly large with the Commabar system.

[0102] The UV-curable lacquer layer is brought into contact with the embossing roller 3 or another master structure in a flowable state and therefore with relatively low pressure, so that the UV-curable lacquer enters the recesses of the outer surface of the embossing roller 3. The composite formed from the carrier material 5, the adhesion promoter layer 8, and the lacquer layer 7 is guided around the embossing roller (master structure) 3 with a clearly defined wrap angle (see Fig. 1). The wrap angle can, for example, be in the range of 60° to 200°, preferably in the range of 100° to 180°. The lacquer layer 7 is cured while it is in contact with the embossing roller (master structure) 3, ie during the formation of the surface structure 13, by irradiation with high-energy radiation, preferably UV light, wherein the irradiation preferably takes place from the side of the radiation-permeable, web-shaped carrier material 5 facing away from the surface structure 13.The irradiation device used for this purpose is designated 15 in Fig. 1. In addition to the irradiation in the area of ​​the embossing roller 3 from below, the irradiation of the lacquer layer in the area of ​​the embossing roller 3 can also be carried out from at least one of the sides of the embossing roller 3.

[0103] At least one UV-emitting LED lamp is preferably used as the irradiation device 15. The irradiation device 15 cures the lacquer layer 7 by emitting a UV radiation output in the range of 8 to 16 W / cm 2 , preferably in the range of 10 to 14 W / cm 2 , for example of about 12 W / cm 2 .

[0104] The lacquer layer 7 is cured (partially cured) in contact with the embossing roller (master structure) 3 to such an extent that the composite of web-shaped carrier material 5, adhesion promoter layer 8, and lacquer layer 7 can be removed from the embossing roller 3 with high molding accuracy. In particular, the surface structure 13 formed into the lacquer layer can be removed from the embossing roller 3 after this curing, essentially without loss of depth and with a stable shape. Subsequently, a post-curing (final curing) of the lacquer layer 7 and the underlying adhesion promoter layer 8 is carried out by means of at least one medium-pressure mercury vapor lamp 16 or at least one UV-C lamp, wherein this post-curing or final curing preferably takes place using a UV radiation dose in the range of 500 to 3,000 mJ / cm 2 The post-curing or final curing of the structure generator 17 is carried out, for example, with a surface-specific power of approximately 200 W / cm2 . The surface structure (embossed structure) 13 of the structure generator 17 produced in this way has, after this final post-curing (final curing), an average roughness depth Rz according to DIN EN ISO 4287 in the range from 10 to 200 μm, preferably in the range from 40 to 200 μm, particularly preferably in the range from 100 to 200 μm.

[0105] At the end of the device 1 for carrying out the manufacturing method according to the invention, the finished structure generator 17 is wound up.

[0106] The exemplary embodiment outlined in Fig. 2 differs from the example disclosed in Fig. 1 in that the embossing roller 3', as a hollow roller, has a radiation-permeable or transparent roller shell, wherein at least one irradiation device 15 is arranged within the embossing roller 3' and directed towards the contact area in which the UV-curable lacquer layer 7 contacts the embossing roller 3'. The web-shaped carrier material 5 can in turn be at least partially permeable to high-energy radiation, in particular to UV light. In the exemplary embodiment outlined in Fig. 2, however, it is also possible to use web-shaped carrier material 5 which is impermeable or substantially impermeable to UV light.

[0107] Below are further examples of compositions of the adhesion promoter used in the process according to the invention or corresponding tests, as well as the radiation-curable lacquer (top coat) for forming the surface structure (embossed structure) 13 of the structuring agent 17, and comparative examples. In particular, mean values ​​for the Martens hardness and measured values ​​for the roughness depth Rz for certain web-shaped carrier materials measured in laboratory tests are also given. Furthermore, measurement results of the cross-cut test are given. Adhesion promoters used in tests on the process according to the invention:

[0108] Internal designation Composition

[0109] Radiation-curable materials used in tests on the process according to the invention

[0110] Topcoats: Topcoat C 94 wt.% urethane acrylate, aliphatic, 5 to 6-functional,

[0111] 4 wt.% additives (defoamers, substrate wetting agents, release additive, wax, anti-settling agent),

[0112] 2% by weight photoinitiator (e.g. MAPO, BAPO, HMPP, CPK, MBF).

[0113] The Martens hardness was measured for the aforementioned Examples 1 to 10 using a FISCHERSCOPE HM2000S measuring device from Helmut Fischer in accordance with DIN EN ISO 14577-1 (2003-05), with the test range used being 300 mN / 20 s. To illustrate the influence of the carrier material 5 on the measured surface hardness of the texture generator 17, the Martens hardness of the carrier material (PET film Hostaphan® from Mitsubishi or paper) was also measured on its own, i.e., without adhesion promoter and without topcoat (cf. Examples 1 and 8). Furthermore, for comparison, the Martens hardness of a radiation-curable coating was measured on its own by peeling the coating (namely topcoat C) from a film to which the coating had previously been applied without primer (adhesion promoter) and then measuring it separately (cf. Example 10).

[0114] Cross-cut tests to determine the adhesion of the paint coating of the structure-forming element 17 according to the above-mentioned examples 2, 3, 4, and 6 each resulted in a Gt value of 0. This means that in these examples, no flaking and thus no significant damage (delamination) of the respective paint coating of the structure-forming element 17 could be detected. In examples 5 and 7, the cross-cut tests resulted in Gt values ​​of 2 and 1, respectively. However, these Gt values ​​are also good values, since an average Gt value of at least 3.5 is usually still considered a sufficient adhesion value.

[0115] Comparative tests in which the UV-curable lacquer layer made of the above-mentioned top coat A, B or C was applied directly to a plastic film (75 μm PET film Hostaphan® from Mitsubishi), ie without using one of the above-mentioned adhesion promoters VI, V2 or V2B, resulted in a very high delamination (Gt value 5) in the cross-cut test.

[0116] To assess the molding accuracy of the surface structure (embossed structure) 13 of the structure generator 17 produced according to the invention, its average roughness depth Rz was measured according to DIN EN ISO 4287 (2009-11) and compared with the average roughness depth Rz of the respective embossing roller 3 used. One of these embossing rollers has a simulated wood structure as the master structure, while another embossing roller has a plurality of negative pyramids as the master structure.

[0117]

[0118] Based on the above-mentioned measured values ​​of the average roughness depth Rz, it can be seen that the molding accuracy of the surface structure (embossed structure) in structuring agents produced according to the invention is excellent. Furthermore, it was determined by microscopic images that the inventive method produces a faithful molding of the master structure of the embossing roller 3 into the embossed structure 13 of the radiation-cured topcoat of the structuring agent 17.

[0119] The exemplary embodiment outlined in Fig. 3 differs from the examples disclosed in Figures 1 and 2 in that a mechanical embossing tool such as an embossing roller is not used to produce a three-dimensional surface structure 13' in the lacquer layer 7 applied to the web-shaped carrier material, but that in this exemplary embodiment a three-dimensional surface structure 13' is produced in the surface of the lacquer layer 7 by irradiation by means of a UV radiation source 20 which emits high-energy, very short-wave UV light with a wavelength in the range from 100 to 230 nm, preferably in the range from 130 to 190 nm, particularly preferably in the range from 170 to 175 nm, particularly preferably 172 nm. The UV radiation source 20 is, for example, an excimer laser device, preferably a xenon excimer laser device.

[0120] The excimer laser treatment causes a very thin surface layer of the lacquer to be at least partially polymerized and thus solidified or cured. The high-energy light emitted by the UV radiation source (excimer laser device) 20 penetrates the lacquer layer 7 only to a depth of approximately 50 to 300 nm, for example, approximately 120 nm, and triggers curing of the lacquer. This causes shrinkage of the very thin surface layer of the lacquer, leading to what is known as micro-wrinkles in the lacquer surface.

[0121] The excimer laser treatment is followed by post-curing (final curing) of the lacquer layer 7 and the underlying adhesion promoter layer 8 using at least one medium-pressure mercury vapor lamp 16 or at least one UV-C lamp. This post-curing or final curing corresponds to that described above with reference to the embodiment outlined in Fig. 1.

[0122] The sheet-like composite material produced according to the exemplary embodiment outlined in Fig. 3 has a matte surface due to the microfolding of the lacquer surface. The surface of the composite material treated in this way accordingly has a low degree of gloss. The microfolding of the lacquer surface ensures, in particular, that fingerprints resulting from manual contact with the cured lacquer layer 7 are barely visible on the lacquer surface of the composite material.

[0123] The advantageous properties of the composite material according to the invention are particularly evident when it is used as a structuring agent for texturing an embossable material surface. The composite material according to the invention or a corresponding structuring agent can be used, for example, in a press for producing decorative laminates under the influence of heat and pressure. Furthermore, the composite material according to the invention can be

[0124] The composite material can also be advantageously used in a coating process in which a surface of a sheet-like material, after application of UV varnish in a calender, is dried and / or cured by means of UV light through a transparent film in the form of the composite material according to the invention. Such a coating process can, in particular, be the aforementioned CCI process.

[0125] An alternative use in which the advantageous properties of the composite material according to the invention also come into play is its use as a coating material for workpiece surfaces, for example for plate-shaped workpieces, in particular for surfaces of workpieces made of wood material, laminate, plastic and / or laminate or of a combination of at least two such materials.

[0126] Fig. 4 outlines an exemplary embodiment of a use in which a web-shaped composite material 30, 30', produced, for example, according to a method as shown in one of Figures 1 to 3, is used as a coating material for a workpiece surface. The web-shaped composite material 30, 30' wound into a roll is unwound from the roll and fed together with a sheet- or sheet-shaped workpiece 40 to a continuously operating belt press 50, for example a double-belt press, for coating (laminating) the workpiece. Beforehand, a binding agent, e.g., adhesive or the like, is applied to the side of the composite material 30, 30' facing away from the three-dimensional surface structure 13, 13', e.g., the underside, and / or to the side of the sheet- or sheet-shaped workpiece 40 that is to be bonded to the composite material. This is done, for example, by means of an application roller system 60.In the belt press 50, the relevant surface of the workpiece 40 is coated with the composite material 30, 30' under the influence of pressure and, if necessary, heat. The three-dimensional surface structure 13, 13' of the composite material 30, 30' defines the visible surface of the finished coated workpiece 40. The continuously coated workpiece 40 is then cut to length using a cutting device 70. The resulting blanks 43 can be collected on an intermediate storage device 80.

[0127] Fig. 5 shows an exemplary embodiment of a use in which a composite material 30, 30' according to the invention, which has been produced, for example, according to a method as shown in one of Figures 1 to 3 and cut to a desired format, is used as a coating material for a plate-shaped workpiece (substrate) 40'. The workpiece 40' can be, for example, a wood-based panel or laminate panel. A resin-impregnated decorative paper 90 can be arranged between the workpiece 40' and the cut composite material 30, 30', which is preferably transparent in the finished state. The side of the plate-shaped workpiece 40' facing away from the composite material 30, 30' is preferably coated with a counter-tension material 95. The material stack thus formed is pressed into a press 50', e.g.a cycle press by the action of pressure and heat to form a laminate, for example a high-pressure laminate. The three-dimensional surface structure 13, 13' is located on the outer or upper side of the finished laminate.

[0128] Fig. 6 shows an embodiment of a device 100 for producing a structured surface of a plate-shaped material 40", which is designed, for example, as a wood-based panel and is fed from left to right in Fig. 6. The material 40" can have an elongated shape in order to be subsequently divided into smaller units. In addition, it is possible for the wood-based panel to already have its final shape and not be further divided after producing a structured surface on the panel.

[0129] A coating layer 7' is applied to the wood-based panel 40" by means of a coating device 140, which has a reservoir 400 for a coating 4 and a metering roller 9'. If necessary, one or more doctor devices for homogenizing the still liquid coating layer 7' or one or more other conventional devices can be provided.

[0130] A feed device 140 with a supply roll 160 is provided for feeding a web-shaped composite material 30, 30' according to the invention that is at least partially permeable to radiation (see Figures 1 to 3). In the region of a deflection roller 200, the web-shaped composite material 30, 30' is applied to the lacquer layer 7'.

[0131] A first curing step is performed using a first curing device 220, which is arranged above the web-shaped composite material 30, 30' in a region where the composite material 30, 30' is in contact with the lacquer layer 7'. For this purpose, radiation, for example UV radiation, is applied through the composite material 30, 30' onto the lacquer layer 7'. The structure of the composite material 30, 30' is thereby transferred to the surface of the lacquer layer 7'.

[0132] Further to the right in the transport direction in Fig. 6, after the first curing device 220, a lifting device 240 with a deflection roller 260 and a take-up roller 280 is provided, with which the web-shaped composite material 30, 30' is lifted from the lacquer layer 7'. Afterward, a surface structure corresponding to the structure of the absorber layer on the composite material is present on the only partially cured lacquer layer 7'.

[0133] Finally, a second curing device 300 is provided, which is designed to carry out a second curing step and emits radiation, in particular UV radiation.

[0134] For example, a UV lamp can be used for the first curing device 220 and the second curing device 300. The implementation of the invention is not limited to the exemplary embodiments illustrated in the schematic drawing. Rather, numerous variants are conceivable which make use of the invention disclosed in the claims even if the design deviates from the examples. For example, the thermal drying or curing of the adhesion promoter layer 8 before the application of the UV-curable lacquer layer 7 can be carried out from only one side, for example from the top side of the adhesion promoter layer 8. Furthermore, the embossing roller 3 can be assigned a plurality of irradiation devices, preferably UV-light-emitting LED radiators, which are arranged both outside and inside the embossing roller 3, which has a transparent roller shell, for curing the lacquer layer 7.

Claims

Patent claims 1. A method for producing a web-shaped composite material (30, 30') having a structured surface, comprising the steps: Providing a web-shaped carrier material (5) made of paper and / or plastic, Applying a UV-curable lacquer layer (7) made of acrylated oligomer to the carrier material (5), Creating a three-dimensional surface structure (13, 13') in the lacquer layer (7) applied to the carrier material (5) and at least partially curing the lacquer layer (7) by irradiation with high-energy radiation, preferably UV light, characterized in that before the application of the UV-curable lacquer layer (7), at least one adhesion promoter layer (8) containing acrylated oligomer, a reactive diluent and a photoinitiator reacting to high-energy radiation, preferably UV radiation, is applied to the carrier material (5), and that the lacquer layer (7) having the three-dimensional surface structure (13, 13') is cured to such an extent that the composite material (30, 30') in the finished state has an average Martens hardness according to DIN EN ISO 14577-1 (2003-5) in the range from 10 to 80 N / mm 2 , preferably in the range of 30 to 80 N / mm 2wherein the indenter used as a test body for measuring the Martens hardness is pressed into the structured surface of the lacquer layer (7).

2. Method according to claim 1, characterized in that the at least one adhesion promoter layer (8) has a layer thickness in the range of 0.5 to 12 μm, preferably in the range of 1 to 10 μm, particularly preferably in the range of 2 to 5 μm, based on the dry state of the adhesion promoter layer (8), is applied to the carrier material (5).

3. Method according to claim 1 or 2, characterized in that an adhesion promoter is used for the adhesion promoter layer (8) which 10 to 90 wt.%, preferably 40 to 70 wt.% acrylated oligomer, 5 to 30 wt.% reactive diluent, 0.5 to 10 wt.% UV-reactive photoinitiator and optionally 0.1 to 3 wt.% of one or more additives from a group comprising defoamers and substrate wetting agents, the amounts of all components contained in the adhesion promoter adding up to 100 wt.%.

4. The method according to claim 1 or 2, characterized in that for the adhesion promoter layer (8) an adhesion promoter is used which contains 10 to 90 wt.%, preferably 40 to 70 wt.% acrylated oligomer dispersion and / or acrylated oligomer emulsion, 5 to 30 wt.% reactive diluent, 0.5 to 10 wt.% photoinitiator reacting to UV radiation and optionally 0.1 to 3 wt.% of one or more additives from a group comprising defoamers and substrate wetting agents, the amounts of all components contained in the adhesion promoter adding up to 100 wt.%.

5. Method according to one of claims 1 to 4, characterized in that for the UV-curable lacquer layer (7) a lacquer is used which 30 to 95 wt.% acrylated oligomer, 10 to 70 wt.% mono- or multifunctional monomer, 1 to 5 wt.% photoinitiator, and optionally 1 to 6 wt.% of one or more additives from a group comprising defoamers, substrate wetting agents, release additives, waxes and anti-settling agents, wherein the amounts of all components contained in the UV-curable varnish add up to 100 wt.%.

6. Method according to one of claims 1 to 5, characterized in that the adhesion promoter and / or the lacquer used for the UV-curable lacquer layer (7) contains / contains urethane acrylate, polyester acrylate, epoxy acrylate or a mixture of two or three of these acrylates as acrylated oligomer.

7. Method according to one of claims 1 to 6, characterized in that the three-dimensional surface structure (13) is produced by means of a mechanical embossing tool, preferably an embossing roller (3, 3') or a plate- or web-shaped structure generator.

8. Method according to one of claims 1 to 6, characterized in that the three-dimensional surface structure (13') is produced by irradiation by means of a UV radiation source (20), wherein the UV radiation source emits UV light with a wavelength in the range from 100 to 230 nm, preferably in the range from 130 to 190 nm, particularly preferably in the range from 170 to 175 nm, particularly preferably 172 nm.

9. Method according to one of claims 1 to 8, characterized in that a web-shaped carrier material (5) made of paper and / or plastic which is at least partially permeable to high-energy radiation, in particular to UV light, is used as the web-shaped carrier material (5).

10. Method according to one of claims 1 to 7 or 9, characterized in that a partial curing of the lacquer layer (7) is carried out by irradiation with high-energy radiation, preferably UV light, during the production of the three-dimensional surface structure (13, 13') in such a way that the irradiation takes place at least partially from the side of the carrier material (5) facing away from the structured surface.

11. Method according to one of claims 1 to 10, characterized in that a material web made of paper is used as the web-shaped carrier material (5), wherein, to produce the adhesion promoter layer (8), an aqueous adhesion promoter is applied to the carrier material [5], wherein the adhesion promoter layer (8) is dried at least in the surface region before the UV-curable lacquer layer (7) is applied thereto, and wherein the drying is carried out using UV radiation and temperatures in the range from 80° C to 160° C, preferably in the range from 90° C to 140° C, particularly preferably in the range from 100° C to 120° C.

12. Method according to one of claims 1 to 10, characterized in that a plastic film or paper is used as the web-shaped carrier material (5), wherein the adhesion promoter layer (8) is cured by means of high-energy radiation, preferably UV radiation, before the UV-curable lacquer layer (7) is applied to the adhesion promoter layer (8) at least to such an extent that the adhesion promoter layer (8) is solid and / or substantially non-adhesive on its surface, wherein the photoinitiator of the adhesion promoter layer (8) is suitable for absorbing light with a wavelength in the range from 250 to 350 nm, preferably in the range from 270 to 330 nm, and wherein the adhesion promoter layer (8) is cured with a UV radiation dose in the range from 60 to 200 mJ / cm 2 , preferably 100 to 160 mJ / cm 2 is hardened.

13. Method according to one of claims 1 to 12, characterized in that the UV-curable lacquer layer is finally cured by means of at least one medium-pressure mercury vapor lamp (16) or at least one UV-C lamp, wherein the final curing is preferably carried out using a UV radiation dose in the range of 500 to 3,000 mJ / cm 2 is carried out.

14. The method according to any one of claims 1 to 13, characterized in that the photoinitiator of the UV-curable lacquer is suitable for absorbing light having a wavelength in the range from 360 to 420 nm, preferably in the range from 390 to 400 nm.

15. The method according to one of claims 1 to 14, characterized in that the three-dimensional surface structure (13) is formed in the UV-curable lacquer layer (7) in such a way that the three-dimensional surface structure (13) after curing of the lacquer layer (7) has an average roughness depth Rz according to DIN EN ISO 4287 (2009-11) in the range from 10 to 200 μm, preferably in the range from 40 to 200 μm, particularly preferably in the range from 100 to 200 μm.

16. Method according to one of claims 1 to 15, characterized in that an embossing roller (3, 3') is used to form the three-dimensional surface structure (13), wherein the composite formed from the web-shaped carrier material (5), the adhesion promoter layer (8) and the lacquer layer (7) is guided around the embossing roller (3, 3') with a wrap angle in the range of preferably 60° to 200°, particularly preferably in the range of 100° to 180°.

17. A web-shaped composite material (30, 30'), preferably produced by a process according to one of the preceding claims 1 to 16, comprising a web-shaped carrier material (5) made of paper and / or plastic and a lacquer layer (7) made of acrylated oligomer, which is applied to the carrier material (5) and has a three-dimensional surface structure (13, 13'), characterized in that the lacquer layer (7) is bonded to the carrier material (5) via at least one adhesion promoter layer (8) containing acrylated oligomer, a reactive diluent and a photoinitiator reacting to UV radiation, wherein the composite material (30, 30') in the finished state has an average Martens hardness according to DIN EN ISO 14577-1 (2003-05) in the range from 10 to 80 N / mm 2 , preferably in the range of 30 to 80 N / mm 2 wherein the indenter used as a test body for measuring the Martens hardness was pressed into the structured surface of the lacquer layer (7).

18. Use of the composite material (30, 30'] according to claim 17 as a structuring agent (17) for texturing an embossable material surface, preferably in a press for producing decorative laminate under the influence of heat and pressure or in a coating process in which a surface of a plate-shaped material is coated after application of UV varnish in Contact is brought with a transparent film in the form of the composite material (30, 30') and dried and / or cured through this by means of UV light.

19. Use of the composite material (30, 30') according to claim 17 as Coating material for workpiece surfaces, preferably for plate-shaped workpieces (40, 40'), in particular for surfaces of workpieces made of wood material, laminate, plastic and / or laminate or combinations of at least two such materials.

Citation Information

Patent Citations

  • Method for producing a textured surface film

    DE102013007429A1

  • Materials having a textured surface and methods for producing same

    EP2146805A2

  • Method for producing a film with a matt surface

    EP2527408A1

  • Method for transferring an embossed structure to the surface of a coating means and compound structure usable as an embossing die

    EP3720673A1

  • Surfacing materials and method of manufacture, including a textured press plate for use in the manufacture of decorative laminate