Electronic component and film forming method
The alumina film with a film-like and particle layer configuration and controlled film forming method addresses the trade-off between barrier properties and stress in electronic component protective films, enhancing thickness and reducing cracking risks through stress distribution and uniform particle placement.
Patent Information
- Application Number
- PCT/JP2023/044675
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-17
- Filing Date
- 2023-12-13
- Publication Date
- 2024-11-21
AI Technical Summary
The existing protective films for electronic components face a trade-off between barrier properties and stress levels, where thinner films offer lower barrier properties but higher stress, leading to potential cracking under external forces, while thicker films increase stress and crack risk.
An alumina film with a film-like portion and a particle layer on its surface, where the film-like portion and particle layer are bonded to the element body, and the average thickness is maintained between 0.05 μm and 2.0 μm, with particles spaced 1.3 μm or less, and a film forming method involving ultrasonic misting and controlled heating to enhance thickness and reduce stress.
The solution effectively increases the alumina film's thickness for improved barrier properties while minimizing stress and cracking risks, ensuring the film's integrity under external forces by distributing stress through the particle layer and maintaining uniform particle distribution.
Smart Images

Figure JP2023044675_21112024_PF_FP_ABST
Abstract
Description
Electronic component and film formation method
[0001] The present disclosure relates to an electronic component and a film forming method.
[0002] The invention described in Patent Document 1 comprises an element body, internal electrodes, external electrodes, and a protective film. The internal electrodes are located inside the element body. The protective film covers the outer surface of the element body. The protective film is an alumina film. The thickness of the protective film is 0.05 μm to 2 μm. The external electrodes are laminated on the outer surface of the protective film. The external electrodes are electrically connected to the internal electrodes.
[0003] Patent No. 4637440
[0004] In a protective film such as that described in Patent Document 1, the thinner the film, the lower the barrier properties of the protective film. On the other hand, increasing the film thickness to ensure the barrier properties increases the stress of the protective film. Furthermore, if the stress of the protective film is high, when an external force is applied to the protective film, the external force may trigger cracks in the protective film. Therefore, a technology is desired that can increase the thickness of the protective film while suppressing the occurrence of cracks in the protective film.
[0005] In order to solve the above-described problems, one aspect of the present disclosure is an electronic component comprising an element body and an alumina film covering an outer surface of the element body, wherein the alumina film has an alumina film portion in contact with the outer surface of the element body and a particle layer located on the outer surface side of the film portion, the particle layer including a plurality of alumina particles bonded to the outer surface of the film portion, the average thickness of the alumina film including the film portion and the particle layer is 0.05 μm or more and 2.0 μm or less, and the spacing between the particles is 1.3 μm or less.
[0006] In addition, in order to solve the above-mentioned problems, one aspect of the present disclosure is a film formation method for forming an alumina film on an outer surface of an element body, the film formation method comprising: a loading step of loading the element body into a first chamber capable of heating an internal atmosphere; a mist-forming step of using ultrasonic waves to turn a liquid raw material containing aluminum atoms and oxygen atoms into a mist in a second chamber; a supply step of supplying the mist-formed raw material together with a carrier gas from the second chamber into the first chamber; and a first heating step of heating the inside of the first chamber to a first temperature while performing the supply step, and further comprising: a second heating step of heating the inside of the first chamber to a second temperature defined as a temperature lower than the first temperature after the first heating step while performing the supply step.
[0007] According to the above configuration, the thickness of the alumina film can be increased while suppressing the occurrence of cracks in the alumina film.
[0008] FIG. 1 is a perspective view of an electronic component. FIG. 2 is a side view of the electronic component. FIG. 3 is a cross-sectional view taken along line 3-3 in FIG. 2. FIG. 4 is an end view of the vicinity of the alumina film taken along line 4-4 in FIG. 2. FIG. 5 shows the measurement results of a scratch strength test. FIG. 6 is an explanatory diagram illustrating a method for manufacturing an electronic component. FIG. 7 is an explanatory diagram illustrating a method for manufacturing an electronic component. FIG. 8 is an explanatory diagram illustrating a method for manufacturing an electronic component. FIG. 9 is an explanatory diagram illustrating a method for manufacturing an electronic component.
[0009] An embodiment of an electronic component will now be described with reference to the drawings. The drawings may show components enlarged for ease of understanding. The dimensional proportions of the components may differ from those in the actual components or from those in other drawings.
[0010] <Regarding the Electronic Component> As shown in FIG. 1 , the electronic component 10 is, for example, a surface-mount type negative temperature coefficient thermistor component mounted on a circuit board or the like. Note that a negative temperature coefficient thermistor component has the characteristic that its resistance value decreases as the temperature increases. The electronic component 10 includes an element body 20. The element body 20 is generally rectangular prism-shaped and has a central axis CA. Note that, hereinafter, an axis extending along the central axis CA is referred to as a first axis X. Furthermore, one of the axes perpendicular to the first axis X is referred to as a second axis Y. Furthermore, an axis perpendicular to the first axis X and the second axis Y is referred to as a third axis Z. Additionally, one of the directions along the first axis X is referred to as a first positive direction X1, and the direction along the first axis X opposite to the first positive direction X1 is referred to as a first negative direction X2. One of the directions along the second axis Y is defined as a second positive direction Y1, and the direction along the second axis Y opposite to the second positive direction Y1 is defined as a second negative direction Y2. Furthermore, one of the directions along the third axis Z is defined as a third positive direction Z1, and the direction along the third axis Z opposite to the third positive direction Z1 is defined as a third negative direction Z2.
[0011] The outer surface 21 of the element body 20 has six flat surfaces 22. The term "surface" of the element body 20 as used herein refers to a surface that can be observed when the entire element body 20 is observed. In other words, even if there are minute irregularities or steps that are not visible unless a portion of the element body 20 is magnified and observed using a microscope or the like, the surface is still referred to as a flat or curved surface. The six flat surfaces 22 face in different directions. The six flat surfaces 22 are broadly divided into a first end surface 22A facing the first positive direction X1, a second end surface 22B facing the first negative direction X2, and four side surfaces 22C. The four side surfaces 22C are, respectively, a surface facing the third positive direction Z1, a surface facing the third negative direction Z2, a surface facing the second positive direction Y1, and a surface facing the second negative direction Y2.
[0012] The arithmetic mean roughness (Ra) of the outer surface 21 of the element body 20 is 0.5 μm or less. The arithmetic mean roughness of the outer surface 21 of the element body 20 is measured using a laser microscope. For example, during the manufacturing process of the electronic component 10, when the outer surface 21 is exposed, the measurement is performed by linearly scanning an arbitrary location on the outer surface 21 over a length of 300 μm or more.
[0013] Furthermore, on the outer surface 21 of the element body 20, the boundary portions between two adjacent flat surfaces 22 and the boundary portions between three adjacent flat surfaces 22 are curved. In other words, the corners of the element body 20 are so-called R-chamfered.
[0014] As shown in Fig. 2, the element body 20 has a larger dimension along the first axis X than along the third axis Z. Also, as shown in Fig. 1, the element body 20 has a larger dimension along the first axis X than along the second axis Y. The material of the element body 20 is a semiconductor. Specifically, the material of the element body 20 is a ceramic obtained by firing a metal oxide containing at least one of Mn, Fe, Ni, Co, Ti, Ba, Al, and Zn.
[0015] 3 , the electronic component 10 includes two first internal electrodes 41 and two second internal electrodes 42. The first internal electrodes 41 and the second internal electrodes 42 are located inside the element body 20.
[0016] The first internal electrode 41 is made of a conductive material. For example, the first internal electrode 41 is made of palladium. The second internal electrode 42 is made of the same material as the first internal electrode 41.
[0017] The first internal electrode 41 has a rectangular plate shape. The main surface of the first internal electrode 41 is perpendicular to the second axis Y. The second internal electrode 42 has the same rectangular plate shape as the first internal electrode 41. The main surface of the second internal electrode 42 is perpendicular to the second axis Y, similar to the first internal electrode 41.
[0018] The dimension of the first internal electrode 41 in the direction along the first axis X is smaller than the dimension of the element body 20 in the direction along the first axis X. Also, as shown in Fig. 1 , the dimension of the first internal electrode 41 in the direction along the third axis Z is approximately two-thirds of the dimension of the element body 20 in the direction along the third axis Z. The dimensions of the second internal electrode 42 in each direction are the same as those of the first internal electrode 41.
[0019] 3, the first internal electrodes 41 and the second internal electrodes 42 are positioned alternately in the direction along the second axis Y. That is, a total of four internal electrodes are arranged alternately in the order of the first internal electrode 41, the second internal electrode 42, the first internal electrode 41, and the second internal electrode 42 from the side surface 22C facing the second positive direction Y1 toward the second negative direction Y2. In this embodiment, the distances between the internal electrodes in the direction along the second axis Y are equal.
[0020] 1, the two first internal electrodes 41 and the two second internal electrodes 42 are both located at the center of the element body 20 in the direction along the third axis Z. On the other hand, as shown in Fig. 3, the first internal electrodes 41 are located closer to the first positive direction X1, and the second internal electrodes 42 are located closer to the first negative direction X2.
[0021] Specifically, the end of the first internal electrode 41 on the first positive direction X1 side coincides with the end of the element body 20 on the first positive direction X1 side. The end of the first internal electrode 41 on the first negative direction X2 side is located inside the element body 20 and does not reach the end of the element body 20 on the first negative direction X2 side. On the other hand, the end of the second internal electrode 42 on the first negative direction X2 side coincides with the end of the element body 20 on the first negative direction X2 side. The end of the second internal electrode 42 on the first positive direction X1 side is located inside the element body 20 and does not reach the end of the element body 20 on the first positive direction X1 side.
[0022] As shown in FIG. 3 , the electronic component 10 includes an alumina film 50. The alumina film 50 covers the outer surface 21 of the element body 20. In this embodiment, the alumina film 50 covers the entire area of the outer surface 21 of the element body 20. In this embodiment, the alumina film 50 indicates that the main component of the film is alumina. Specifically, the alumina film 50 is a film in which the total atomic percentage of aluminum atoms and oxygen atoms contained in the film is 80% or more. In this embodiment, the alumina film 50 also contains hydrogen atoms and carbon atoms.
[0023] The electronic component 10 includes a first external electrode 61 and a second external electrode 62. The first external electrode 61 is located on the outer surface of the alumina film 50. The first external electrode 61 includes a first base electrode 61A and a first metal layer 61B. The first base electrode 61A is laminated on the alumina film 50 over a portion of the outer surface 21 of the element body 20, including the first end face 22A. The first base electrode 61A is a five-sided electrode that covers the first end face 22A of the element body 20 and portions of the four side faces 22C facing the first positive direction X1. In this embodiment, the first base electrode 61A is made of copper and glass. The first base electrode 61A is a sintered body.
[0024] 3, the first metal layer 61B covers the first base electrode 61A from the outside. Therefore, the first metal layer 61B is laminated on the first base electrode 61A. Furthermore, a portion of the first metal layer 61B protrudes from the first base electrode 61A. In other words, a portion of the outer edge of the first metal layer 61B directly covers the alumina film 50 without the first base electrode 61A in between. Although not shown in the figure, the first metal layer 61B has a two-layer structure consisting of a nickel layer and a tin layer, in this order from the first base electrode 61A side.
[0025] The second external electrode 62 includes a second base electrode 62A and a second metal layer 62B. The second base electrode 62A is laminated on the alumina film 50 over a portion of the outer surface 21 of the element body 20, including the second end face 22B. The second base electrode 62A is a five-sided electrode that covers the second end face 22B of the element body 20 and portions of the four side faces 22C facing the first negative direction X2. In this embodiment, the second base electrode 62A is made of the same material as the first external electrode 61, that is, copper and glass. Like the first base electrode 61A, the second base electrode 62A is a sintered body.
[0026] The second metal layer 62B covers the second base electrode 62A from the outside. Therefore, the second metal layer 62B is stacked on the second base electrode 62A. Furthermore, a portion of the second metal layer 62B protrudes from the second base electrode 62A. In other words, a portion of the outer edge of the second metal layer 62B directly covers the alumina film 50 without the second base electrode 62A in between. Although not shown, the second metal layer 62B, like the first metal layer 61B, has a two-layer structure consisting of a nickel layer and a tin layer, in this order from the second base electrode 62A side.
[0027] The second external electrode 62 does not reach the first external electrode 61 on the side surface 22C, and is spaced apart from the first external electrode 61 in the direction along the first axis X. In addition, the first external electrode 61 and the second external electrode 62 are not stacked in the central portion of the side surface 22C of the element body 20 in the direction along the first axis X, and the alumina film 50 is exposed. Note that in Figures 1 to 3, the first external electrode 61 and the second external electrode 62 are shown by two-dot chain lines.
[0028] The first external electrode 61 and the end of the first internal electrode 41 on the first positive direction X1 side are connected via a first through portion 71 that penetrates the alumina film 50. Therefore, the first external electrode 61 is electrically connected to the first internal electrode 41. Note that, as will be described in detail later, the first through portion 71 is formed during the manufacturing process of the electronic component 10 when palladium that constitutes the first internal electrode 41 extends toward the first external electrode 61 side.
[0029] The second external electrode 62 and the end of the second internal electrode 42 on the first negative direction X2 side are connected via a second through portion 72 that penetrates the alumina film 50. Therefore, the second external electrode 62 is electrically connected to the second internal electrode 42. Like the first through portion 71, the second through portion 72 is formed by the palladium constituting the second internal electrode 42 extending toward the second external electrode 62 during the manufacturing process of the electronic component 10. Note that while FIG. 3 illustrates the first internal electrode 41 and the first through portion 71 as separate components with a boundary, in reality, there is no clear boundary between them. The same applies to the second through portion 72. The first through portion 71 is not shown in FIG. 1.
[0030] <Regarding the Alumina Film> As shown in Fig. 4, the alumina film 50 has a film portion 51 and a particle layer 52. The film portion 51 is made of alumina. The film portion 51 is a portion where alumina exists without interruption when tracing the outer surface 21 of the element body 20 along the shape of the outer surface 21. The film portion 51 is in contact with the outer surface 21 of the element body 20. More specifically, the film portion 51 covers the entire outer surface 21 of the element body 20.
[0031] The particle layer 52 is located on the outer surface side of the film-like portion 51. The particle layer 52 contains a plurality of particles 53 made of alumina. The plurality of particles 53 are bonded to the outer surface of the film-like portion 51. Note that in FIG. 4, only some of the particles 53 are labeled with reference numerals. Also, in FIG. 4, some of the particles 53 appear to be separated from the film-like portion 51, but when viewed from the end by shifting the particle layer 52 in the depth direction of the paper in FIG. 4, the particles 53 are bonded to the outer surface of the film-like portion 51.
[0032] Each particle 53 has a variety of shapes. For example, when the alumina film 50 is viewed from an end face in a cross section perpendicular to one of the flat surfaces 22 of the element body 20, the particle 53 may be elliptical or may have a distorted shape due to bonding of multiple particles 53.
[0033] The spacing P between the particles 53 is 1.3 μm or less. In this embodiment, the maximum length of the spacing P between the particles 53 is 0.51 μm. The spacing P between the particles 53 is measured as follows. First, a cross section perpendicular to one of the planes 22 of the element body 20 and including the alumina film 50 is photographed using an electron microscope. Next, an approximate straight line L1 is drawn with respect to the outer surface 21 for the photographed image. The approximate straight line L1 can be determined, for example, by the least squares method. Then, the shortest distance between the particles 53 in a direction parallel to this approximate straight line L1 is defined as the spacing P between the particles 53. Note that FIG. 4 shows only the maximum spacing P as a representative example.
[0034] The average thickness of the alumina film 50 including the film portion 51 and the particulate layer 52 is 0.05 μm or more and 2.0 μm or less. The average thickness of the alumina film 50 is the sum of the average thickness of the film portion 51 and the average thickness of the particulate layer 52. In this embodiment, the average thickness of the alumina film 50 is 0.57 nm.
[0035] The average thickness of the membrane portion 51 is 0.3 μm. The thickness of the membrane portion 51 is the shortest distance from a position on the membrane portion 51 on the outer surface 21 side of the element body 20 to the outer surface of the membrane portion 51. The average thickness of the membrane portion 51 is measured as follows.
[0036] First, a cross section perpendicular to one of the planes 22 of the element body 20 and including the alumina film 50 is photographed using an electron microscope. Next, a range in the photographed image is identified in the direction along the outer surface of the film portion 51. Within this range, the cross-sectional area of the film portion 51 is calculated by image processing for a measurement range of at least 5 μm or more. Then, the cross-sectional area of the film portion 51 in the calculated measurement range is divided by the length of the measurement range to calculate the thickness of the film portion 51 in that cross section. This is the average thickness of the film portion 51.
[0037] The average thickness of the particle layer 52 is 0.27 μm. The average thickness of the particle layer 52 is calculated as follows: A cross section perpendicular to one of the planes 22 of the element body 20 and including the alumina film 50 is photographed using an electron microscope. Next, a range in the photographed image is identified in a direction along the outer surface of the film portion 51. Within this range, the sum of the cross-sectional areas of the particles 53 is calculated by image processing for a measurement range of at least 5 μm. The thickness of the particle layer 52 in the cross section is calculated by dividing the calculated sum of the cross-sectional areas of the particles 53 in the measurement range by the length of the measurement range. This is the average thickness of the particle layer 52. Note that within the measurement range of the particle layer 52, there are areas where particles 53 are present and areas where particles 53 are not present. In areas where particles 53 are not present, the thickness of the particle layer 52 is locally zero. Therefore, the average thickness of the particle layer 52 calculated using the above method is a value small relative to the particle diameter of each particle 53.
[0038] The ratio of the average thickness of the particle layer 52 to the average thickness of the alumina film 50 is 20% or more and 70% or less. Specifically, in this embodiment, the ratio of the average thickness of the particle layer 52 to the average thickness of the alumina film 50 is approximately 47.4%.
[0039] <Scratch Strength Test of Alumina Film> Here, a test was conducted to measure the scratch strength of the alumina film 50. In this test, the external force required to scratch the outer surface of the alumina film 50 and cause damage to the interior of the alumina film 50 was defined as the "scratch strength."
[0040] First, a plurality of samples were prepared, each of which had an alumina film 50 including a film portion 51 and a particle layer 52 formed on a silicon substrate. The thickness of the alumina film 50 was varied within a range of 0.05 μm to 0.95 μm for each sample.
[0041] In this scratch strength test, a sample was fixed on a table, and a probe was brought into close contact with the outer surface of the alumina film 50 of the sample. Then, the table on which the sample was fixed was moved at a constant speed while increasing the pressure of the probe against the alumina film 50. At this time, the pressure force at which a scratch was generated inside the alumina film 50, specifically, exposing the silicon substrate, was measured as the scratch strength.
[0042] As shown in Figure 5, there was a tendency for the scratch strength to increase as the thickness of the alumina film 50 decreased. In particular, when the thickness of the alumina film 50 exceeded approximately 0.2 µm, the scratch strength remained at a low level of generally less than 20 mN. On the other hand, when the thickness of the alumina film 50 was approximately 0.2 µm or less, the scratch strength increased sharply as the thickness decreased. Therefore, from the viewpoint of preventing the occurrence of cracks, it was found that a thickness of 0.2 µm or less is preferable for the alumina film 50.
[0043] <Method for Manufacturing Electronic Component> Next, a method for manufacturing electronic component 10 will be described. As shown in Fig. 6, the method for manufacturing electronic component 10 includes a laminate preparation step S11, a rounded chamfering step S12, a loading step S13, a mist-forming step S14, a supply step S15, a first heating step S16, and a second heating step S17. The method for manufacturing electronic component 10 also includes a conductor application step S18, a curing step S19, and a plating step S20.
[0044] First, in forming the element body 20, a laminate is prepared in the laminate preparation step S11. The laminate at this stage is in a state before R-chamfering and has a rectangular parallelepiped shape with six flat surfaces 22. For example, first, a plurality of ceramic sheets that will become the element body 20 are prepared. The sheets are thin plates. A conductive paste that will become the first internal electrode 41 is laminated on the sheets. A ceramic sheet that will become the element body 20 is laminated on the laminating paste. A conductive paste that will become the second internal electrode 42 is laminated on the sheets. In this manner, the ceramic sheets and the conductive paste are laminated. The laminated sheets are then pressed in the stacking direction using a mold press or other means. The pressed sheet is then cut to a predetermined size to form an unfired laminate. The unfired laminate is then fired at a high temperature to prepare the laminate.
[0045] Next, an R-chamfering process step S12 is performed. In the R-chamfering process step S12, the laminate prepared in the laminate preparation process S11 is R-chamfered. This process provides an element body 20 with R-chamfered corners.
[0046] Next, the introduction step S13 to the second heating step S17 are performed sequentially. The introduction step S13 to the second heating step S17 are performed using a film formation apparatus 100. As shown in FIG. 7 , the film formation apparatus 100 includes a first chamber 91. The first chamber 91 is capable of heating the atmosphere therein. Specifically, the first chamber 91 includes a heater 91A, a container body 91B, and an exhaust passage 91C. The heater 91A is located at the bottom of the container body 91B. By driving the heater 91A, the atmosphere within the container body 91B is heated. The exhaust passage 91C is connected to the container body 91B. The interior of the container body 91B is connected to the outside via the exhaust passage 91C.
[0047] The film forming apparatus 100 includes a second chamber 92, a liquid supply nozzle 93, and a gas supply nozzle 94. The second chamber 92 includes an ultrasonic generator 92A, a container body 92B, and a communication passage 92C. The ultrasonic generator 92A is located at the bottom of the container body 92B. By driving the ultrasonic generator 92A, the liquid supplied to the container body 92B can be converted into a mist. The communication passage 92C connects the container body 91B of the first chamber 91 to the container body 92B of the second chamber 92. In other words, the inside of the container body 92B of the second chamber 92 is connected to the inside of the container body 91B of the first chamber 91 via the communication passage 92C. The liquid supply nozzle 93 can supply liquid precursor material into the container body 92B. The gas supply nozzle 94 can supply carrier gas into the container body 92B.
[0048] 6, a loading step S13 is performed. As shown in Fig. 7, in the loading step S13, the element body 20 is loaded into the first chamber 91 of the film forming apparatus 100. Then, the heater 91A of the first chamber 91 is driven to heat the atmosphere in the first chamber 91.
[0049] Next, as shown in FIG. 6, a mist-forming step S14 is performed. As shown in FIG. 8, in the mist-forming step S14, the liquid raw material is introduced into the second chamber 92 via the liquid supply nozzle 93. The ultrasonic generator 92A is then driven to turn the raw material into a mist using ultrasonic waves. Note that the mist-like state refers to a state in which the raw material is in the form of droplets with a particle size of 10 μm or less. The raw material contains aluminum acetylacetonate, methanol, and water. That is, the raw material contains aluminum atoms and oxygen atoms. Furthermore, the raw material contains carbon atoms and hydrogen atoms.
[0050] Next, as shown in FIG. 6 , a supply step S15 is performed. As shown in FIG. 9 , in the supply step S15, a carrier gas is supplied into the second chamber 92 via the gas supply nozzle 94. As a result, the mist-like raw material is supplied from the second chamber 92 to the first chamber 91 together with the carrier gas. The carrier gas is, for example, an inert gas such as oxygen, ozone, nitrogen, or argon. The carrier gas may also be a reducing gas such as hydrogen gas or forming gas. Note that excess carrier gas and excess raw material supplied into the first chamber 91 are exhausted to the outside of the film forming apparatus 100 via an exhaust passage 91C.
[0051] Next, as shown in FIG. 6 , a first heating step S16 is performed. In the first heating step S16, the atmosphere in the first chamber 91 is heated while the supplying step S15 is being performed. Specifically, in the first heating step S16, the heater 91A is driven to heat the inside of the first chamber 91 to a first temperature. By heating, the particle size of the mist that flows into the first chamber 91 from the second chamber 92 is reduced. The temperature inside the first chamber 91 at this time is, for example, several hundred degrees. In the first heating step S16, the mist-like raw material is supplied to the element body 20 while vaporizing. As a result, a dense film portion 51 is formed on the outer surface 21 of the element body 20.
[0052] Next, the second heating step S17 is performed. In the second heating step S17, after the first heating step S16, the first chamber 91 is heated to a second temperature defined as a temperature lower than the first temperature while the supplying step S15 is being performed. The second temperature is, for example, a temperature approximately 100 degrees lower than the first temperature. In this way, when the first chamber 91 is heated to the second temperature in the second heating step S17, the particle size of the mist-like raw material becomes larger than that in the first heating step S16. That is, in the second heating step S17, the particle size of the mist in the first chamber 91 becomes larger than that in the first heating step S16. Such mist with large particle size adheres to the film portion 51 to form particles 53. In this step, a plurality of particles 53 are formed in the film portion 51, and a particle layer 52, which is part of the alumina film 50, is formed.
[0053] Furthermore, the atomic composition ratio of the raw materials is kept constant during the above-described mist-forming step S14, supply step S15, first heating step S16, and second heating step S17. That is, the composition ratio of the mist formed from the raw materials is approximately the same at any time during the above steps. These steps from the introduction step S13 to the second heating step S17 constitute a film formation method for forming an alumina film 50 on the outer surface 21 of the element body 20.
[0054] Next, a conductor application step S18 is performed. In the conductor application step S18, a conductor paste is applied to two locations on the surface of the alumina film 50: a portion including a portion covering the first end face 22A of the element body 20, and a portion including a portion covering the second end face 22B of the element body 20. Specifically, the conductor paste is applied to cover the alumina film 50 over the entire first end face 22A and portions of the four side faces 22C. The conductor paste is also applied to cover the alumina film 50 over the entire second end face 22B and portions of the four side faces 22C.
[0055] Next, a curing step S19 is performed. Specifically, the curing step S19 involves heating the element body 20. In the curing step S19, the conductive paste applied in the conductive material application step S18 is fired to form the first base electrode 61A and the second base electrode 62A.
[0056] In this embodiment, during heating in the curing step S19, the Kirkendall effect, which arises from the difference in diffusion rate between the first internal electrode 41 and the first base electrode 61A, attracts palladium contained in the first internal electrode 41 toward the first base electrode 61A containing copper. As a result, the first through portion 71 extends from the first internal electrode 41 toward the first base electrode 61A, penetrating the alumina film 50. This connects the first internal electrode 41 and the first base electrode 61A. The same applies to the second through portion 72 connecting the second internal electrode 42 and the second base electrode 62A.
[0057] Next, a plating step S20 is performed. Electroplating is performed on the first base electrode 61A and the second base electrode 62A. As a result, a first metal layer 61B is formed on the surface of the first base electrode 61A. Furthermore, a second metal layer 62B is formed on the surface of the second base electrode 62A. Although not shown, the first metal layer 61B and the second metal layer 62B are electroplated with two types of metal, nickel and tin, to form a two-layer structure. In this manner, the electronic component 10 is formed.
[0058] <Effects of this Embodiment> (1) According to the above embodiment, the thickness of the alumina film 50 as a whole is sufficient to ensure barrier properties. Furthermore, the alumina film 50 includes a film portion 51 and particles 53. This configuration allows stress in the alumina film 50 to be released between the particles 53, compared to when the entire alumina film 50 is composed of the film portion 51. This prevents localized stress buildup in the alumina film 50, thereby suppressing cracking even when an external force is applied. Furthermore, the spacing P between the particles 53 is 1.3 μm or less, preventing impact concentration on a single particle 53 when an impact or the like is applied from outside the particle 53 layer. In other words, the spacing P between the particles 53 can protect the element body 20.
[0059] (2) In the above embodiment, the ratio of the average thickness of the particle layer 52 to the average thickness of the alumina film 50 is 20% or more. This configuration allows the particle layer 52 to sufficiently mitigate the stress on the alumina film 50. Furthermore, in the above embodiment, the ratio of the average thickness of the particle layer 52 to the average thickness of the alumina film 50 is 70% or less. This configuration allows the film portion 51 to sufficiently provide barrier properties.
[0060] (3) In the above embodiment, the arithmetic mean roughness of the outer surface 21 of the element body 20 is 0.5 μm or less. If the arithmetic mean roughness of the outer surface 21 of the element body 20 is appropriately large, there is a risk that the unevenness of the outer surface 21 of the element body 20 will also be reflected in the outer surface of the membrane portion 51. If the outer surface of the membrane portion 51 is uneven in this way, the particles 53 will accumulate in depressions in the membrane portion 51 during manufacturing, making it difficult for the particles 53 to be positioned uniformly on the outer surface of the membrane portion 51. With the above configuration, the arithmetic mean roughness of the outer surface 21 of the element body 20 is appropriately small, thereby preventing the particles 53 from being positioned unevenly on the outer surface of the membrane portion 51, as described above.
[0061] (4) According to the above embodiment, the atomic composition ratio of the raw material is constant in the mist-forming step S14, the supplying step S15, the first heating step S16, and the second heating step S17. With this configuration, the composition ratio does not change in the step of forming the film portion 51 or the step of forming the particles 53. Since the composition ratio of the film portion 51 and the particles 53 is approximately the same, a boundary is unlikely to occur between these components, and the particles 53 are unlikely to fall off from the film portion 51.
[0062] <Modifications> The above embodiment and the following modifications can be implemented in combination with each other within the scope of technical compatibility.
[0063] In the above embodiment, the electronic component 10 is not limited to a negative temperature coefficient thermistor component. For example, the electronic component 10 may be a piezoelectric component, a multilayer ceramic capacitor, an inductor, or the like.
[0064] In the above embodiment, the number of first internal electrodes 41 and second internal electrodes 42 is not limited to the example in the above embodiment. The number of first internal electrodes 41 may be less than two or more than two. The same applies to the second internal electrodes 42.
[0065] In the above embodiment, the materials of the first base electrode 61A and the second base electrode 62A are not limited to those in the above embodiment. For example, the materials of the first base electrode 61A and the second base electrode 62A may be a mixture of silver and glass.
[0066] In the above embodiment, the alumina film 50 does not have to cover the entire element body 20. It is sufficient that the alumina film 50 covers at least a portion of the outer surface 21 of the element body 20.
[0067] In the above embodiment, the spacing P between the particles 53 in the alumina film 50 is not limited to the example of the above embodiment as long as it is 1.3 μm or less. In the above embodiment, the average thickness of the alumina film 50 is not limited to the example of the above embodiment as long as it is 0.05 μm or more and 2.0 μm or less.
[0068] In the above embodiment, the ratio of the average thickness of the particle layer 52 to the average thickness of the alumina film 50 may be less than 20% or more than 70%. The greater the ratio of the particle layer 52 in the alumina film 50, the more suppression of stress in the alumina film 50 can be expected. Furthermore, the greater the ratio of the membrane portion 51 in the alumina film 50, the more improvement in the barrier properties of the alumina film 50 can be expected.
[0069] In the above embodiment, the alumina film 50 may contain other atoms in addition to oxygen atoms and aluminum atoms. For example, the alumina film 50 may contain atoms other than carbon atoms and hydrogen atoms. Furthermore, the alumina film 50 may not contain carbon atoms and hydrogen atoms.
[0070] In the above embodiment, the chemical raw materials used in the mist-forming step S14, the supplying step S15, the first heating step S16, and the second heating step S17 are not limited to those described in the above embodiment. For example, the raw materials may be organic salts containing aluminum, organic solvents, etc. Furthermore, the raw materials may or may not contain water.
[0071] In the above embodiment, the atomic composition ratio of the raw materials may be changed during the execution of the mist-forming step S14, the supplying step S15, the first heating step S16, and the second heating step S17. Even when the raw material composition ratio is changed, the alumina film 50 only needs to have a total atomic percentage of aluminum atoms and oxygen atoms of 80% or more and be mainly composed of alumina.
[0072] In the above embodiment, the arithmetic mean roughness of the outer surface 21 of the element body 20 is not limited to the example in the above embodiment. For example, the arithmetic mean roughness of the outer surface 21 of the element body 20 may be greater than 0.5 μm.
[0073] In the above embodiment, the film portion 51 and the particle layer 52 are formed by different heating temperatures in the first heating step S16 and the second heating step S17, but the film portion 51 and the particle layer 52 may be formed by other methods. For example, the film portion 51 and the particle layer 52 may be formed by differentiating the frequency of the ultrasonic waves in the ultrasonic generator 92A. Note that in the above embodiment, the method for forming the alumina film 50 is not limited to the method of adhering a mist of raw material to the element body 20.
[0074] <Supplementary Notes> The technical concepts that can be derived from the above embodiments and modifications are described below. [1] An electronic component comprising an element body and an alumina film covering an outer surface of the element body, the alumina film having an alumina film portion in contact with the outer surface of the element body and a particle layer located on the outer surface side of the film portion, the particle layer including a plurality of alumina particles bonded to the outer surface of the film portion, the average thickness of the alumina film including the film portion and the particle layer is 0.05 μm or more and 2.0 μm or less, and the spacing between the particles is 1.3 μm or less.
[0075] [2] The electronic component according to [1], wherein the ratio of the average thickness of the particle layer to the average thickness of the alumina film is 20% or more and 70% or less. [3] The electronic component according to [1] or [2], wherein the arithmetic mean roughness of the outer surface of the element body is 0.5 μm or less.
[0076] [4] A method for forming an alumina film on the outer surface of an element body, comprising: a loading step of loading the element body into a first chamber capable of heating the internal atmosphere; a mist-forming step of using ultrasonic waves to turn a liquid raw material containing aluminum atoms and oxygen atoms into a mist in a second chamber; a supply step of supplying the mist-formed raw material together with a carrier gas from the second chamber into the first chamber; and a first heating step of heating the inside of the first chamber to a first temperature while performing the supply step; and further comprising, after the first heating step, a second heating step of heating the inside of the first chamber to a second temperature defined as a temperature lower than the first temperature while performing the supply step.
[0077] [5] The film forming method according to [4], wherein the atomic composition ratio of the raw material is kept constant during the mist-forming step, the supplying step, the first heating step, and the second heating step.
[0078] REFERENCE SIGNS LIST 10... Electronic component 20... Element body 21... Outer surface 41... First internal electrode 42... Second internal electrode 50... Alumina film 51... Film portion 52... Particle layer 53... Particles 61... First external electrode 62... Second external electrode
Claims
1. An electronic component comprising: an element body; and an alumina film covering the outer surface of the element body, wherein the alumina film has an alumina film portion in contact with the outer surface of the element body, and a particle layer located on the outer surface side of the film portion, wherein the particle layer includes a plurality of alumina particles bonded to the outer surface of the film portion, the average thickness of the alumina film including the film portion and the particle layer is 0.05 μm or more and 2.0 μm or less, and the spacing between the particles is 1.3 μm or less.
2. The electronic component according to claim 1, wherein the ratio of the average thickness of said particle layer to the average thickness of said alumina film is 20% or more and 70% or less.
3. The electronic component according to claim 1 or 2, wherein the arithmetic mean roughness of the outer surface of the element body is 0.5 μm or less.
4. A method for forming an alumina film on the outer surface of an element body, comprising: a loading step of loading the element body into a first chamber capable of heating an internal atmosphere; a mist-forming step of using ultrasonic waves to turn a liquid raw material containing aluminum atoms and oxygen atoms into a mist in a second chamber; a supply step of supplying the mist of the raw material together with a carrier gas from the second chamber into the first chamber; a first heating step of heating the inside of the first chamber to a first temperature while performing the supply step; and further comprising, after the first heating step, a second heating step of heating the inside of the first chamber to a second temperature defined as a temperature lower than the first temperature while performing the supply step.
5. The film forming method according to claim 4, wherein a composition ratio of atoms contained in the raw material is kept constant during the mist-forming step, the supplying step, the first heating step, and the second heating step.
Citation Information
Patent Citations
Electronic component and its manufacture
JP1996330106A
Metallic oxide film resistor and its manufacture
JP1997289101A
Ceramic element and manufacturing method of the same
JP2003272906A
Electronic chip component and its manufacturing method