Cu ALLOY POWDER FOR ADDITIVE MANUFACTURING USE, AND ADDITIVE-MANUFACTURED ARTICLE USING SAME

The Cu alloy powder with a controlled Ni/Si ratio and optional Ag additions addresses the challenges of achieving high relative density, formability, and conductivity in additive manufacturing, resulting in enhanced hardness and electrical conductivity in additively manufactured Cu alloy products.

WO2024236990A1PCT designated stage expired Publication Date: 2024-11-21SANYO SPECIAL STEEL CO LTD

Patent Information

Application Number
PCT/JP2024/015165
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-16
Filing Date
2024-04-16
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing Cu alloy powders for additive manufacturing face challenges in achieving high relative density, formability, hardness, and electrical conductivity due to the adverse effects of excessive Ni addition, which reduces conductivity and limits hardness enhancement through solid solution strengthening.

Method used

A Cu alloy powder composition with a specific range of Ni (1.20-7.30%) and Si (0.25-1.80%) mass ratio (3.00-6.00) is used, along with optional additions of Ag, to promote intermetallic compound precipitation, enhancing hardness and conductivity while maintaining formability, and employing a controlled Ni/Si ratio to balance properties.

Benefits of technology

The Cu alloy powder achieves high relative density, excellent formability, high hardness, and high electrical conductivity in additively manufactured objects, with the Ni/Si ratio and Ag additions optimizing the balance between hardness and conductivity, surpassing conventional Cu-Ni binary systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015165_21112024_PF_FP_ABST
    Figure JP2024015165_21112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are: a Cu alloy powder for additive manufacturing use, which can be shaped at a relatively high density and from which an additive-manufactured article having high hardness, a high electrical conductivity and a high thermal conductivity can be manufactured; and a shaped article using the Cu alloy powder for additive manufacturing use. The Cu alloy powder for additive manufacturing use contains, in % by mass, 1.20 to 7.30% of Ni, 0.25 to 1.80% of Si, 0.40% or less of Mg, one or more elements selected from Zr, Cr, Nb, Mn, Fe, Zn and Sn in a total amount of 0.00 to 2.00%, 0.000 to 0.020% of C, 0.000 to 0.020% of P, 0.000 to 0.020% of S, and a remainder comprising Cu and unavoidable impurities, wherein the ratio of the content of Ni to the content of Si, i.e., Ni / Si ratio, is 3.00 to 6.00, and the total content of Ni and Si is 1.50 to 9.00%.
Need to check novelty before this filing date? Find Prior Art

Description

Cu alloy powder for additive manufacturing and additive manufacturing body using the same

[0001] The present disclosure relates to a Cu alloy powder for additive manufacturing and an additive manufactured body using the same.

[0002] Due to their high electrical and thermal conductivity, Cu alloys are used in various coils, heat sinks, electrical contacts, molds, etc. Recently, in order to accommodate complex shapes, trials and investigations have been made into manufacturing using additive manufacturing (also known as 3D printers, three-dimensional modeling, additive manufacturing, etc.).

[0003] Generally, the Wiedemann-Franz law states that the ratio of a metal's thermal conductivity κ to its electrical conductivity δ is constant at a constant temperature T, regardless of the type of metal. Therefore, here, matters relating to both physical properties will be explained using only electrical conductivity.

[0004] However, when Cu powder is used for additive manufacturing, the Cu powder reflects the laser beam that is often used as a heat source in additive manufacturing. Therefore, even if Cu powder is used for additive manufacturing, it is difficult to sufficiently raise the temperature of the Cu powder to melt it and obtain a molded body with a high relative density and no residual pores.

[0005] Therefore, attempts have been made to obtain Cu alloy additive manufacturing bodies with high relative density by adding various additive elements, including Ni, to reduce the laser reflectivity of Cu alloy powder (or increase the laser absorption rate), making it easier to melt (see Patent Documents 1, 2, and 3).

[0006] However, the addition of excessive Ni reduces the electrical conductivity of the shaped body, thereby impairing the excellent physical properties that Cu originally possesses.

[0007] In addition, in recent years, the application of additive manufacturing methods to Cu alloy products used in environments where they are under stress or in contact with other components has begun to be considered. To withstand these usage environments, Cu alloy additive manufacturing products are also required to have high hardness. However, the effect of Ni on the required hardness of Cu alloy additive manufacturing products has not been studied in detail or given sufficient consideration.

[0008] JP 2021-17639 A JP 2022-188809 A International Publication No. 2018 / 199110

[0009] In the past, when using Cu alloy powder for additive manufacturing, it was difficult to find a Cu alloy shaped body that combines excellent formability (the ability to be shaped to a high relative density), high hardness, and high electrical conductivity, or a raw material powder that can achieve this. Therefore, an object of the present invention is to provide a Cu alloy powder for additive manufacturing that can achieve high levels of hardness, formability, relative density, and electrical conductivity, and a shaped body produced using the same.

[0010] However, if an attempt is made to increase the amount of Ni added to improve formability in response to laser reflection, the conductivity will be significantly reduced, making it difficult and not easy to achieve high levels of formability and conductivity.

[0011] Furthermore, in ingot materials, Ni is an element that easily dissolves in Cu. Therefore, even if we focus on solid solution strengthening as the main effect of Ni on hardness, it is unlikely that a significant increase in hardness can be expected due to solid solution strengthening, since there is no significant difference between the atomic radii of Cu and Ni. Therefore, it is difficult to derive a solution from the general idea of ​​solid solution strengthening.

[0012] Therefore, the problem that the present invention aims to solve is to provide a Cu alloy powder for additive manufacturing that has excellent moldability, allowing for the production of additive manufactured objects with high hardness, high electrical conductivity, and high thermal conductivity, and a manufactured object using the same.

[0013] As described above, simply focusing on Ni and increasing the amount of Ni results in a decrease in electrical conductivity, while solid solution strengthening is difficult to achieve an increase in hardness. Therefore, the present inventors conducted extensive research and found that, in a Ni-added Cu alloy, a composition that can achieve a good balance between the hardness, formability, and electrical conductivity of a shaped body can be achieved by adding a predetermined amount of Si as a third component in addition to Ni and specifying the Ni / Si mass ratio within a predetermined range, thereby achieving high hardness, excellent formability, and high electrical conductivity.

[0014] There are no literature documents that have examined in detail the effects of the simultaneous addition of Ni and Si to Cu on additive manufacturing and additive manufacturing bodies, and this is a new finding that has only been revealed through the present invention. In particular, additive manufacturing is a manufacturing method that involves rapid solidification, and factors that affect the conductivity and hardness of additive manufacturing bodies, such as the crystal grain size, constituent phases, and precipitate formation behavior, are thought to be significantly different from those of ingot manufacturing, and heat treatment behavior is also thought to be different. Furthermore, moldability is a requirement unique to additive manufacturing. A comprehensive study of these factors led to the present invention.

[0015] That is, the present disclosure provides the following aspects: [Aspect 1] A Cu alloy powder for additive manufacturing, comprising, by mass%, Ni: 1.20 to 7.30%, Si: 0.25 to 1.80%, Mg: 0.40% or less, a total of one or more of Zr, Cr, Nb, Mn, Fe, Zn, and Sn: 0.00 to 2.00%, C: 0.000 to 0.020%, P: 0.000 to 0.020%, and S: 0.000 to 0.020%, with the balance being Cu and unavoidable impurities, wherein the ratio of the Ni content to the Si content (Ni / Si) is 3.00 to 6.00, and the total content of Ni and Si is 1.50 to 9.00%. [Aspect 2] A Cu alloy powder for additive manufacturing, comprising, by mass%, Ni: 1.20 to 7.30%, Si: 0.25 to 1.80%, Mg: 0.40% or less, a total of one or more of Zr, Cr, Nb, Mn, Fe, Zn, and Sn: 0.00 to 2.00%, C: 0.000 to 0.020%, P: 0.000 to 0.020%, S: 0.000 to 0.020%, and Ag: more than 0% and 5.00% or less, with the balance being Cu and unavoidable impurities, wherein the ratio of Ni content to Si content Ni / Si is 3.00 to 6.00, and the total content of Ni and Si is 1.50 to 9.00%. [Aspect 3] A shaped body additively manufactured using the Cu alloy powder for additive manufacturing according to Aspect 1. [Embodiment 4] A shaped body produced by additive manufacturing using the Cu alloy powder for additive manufacturing according to embodiment 2.

[0016] When additive manufacturing is performed using the Cu alloy powder for additive manufacturing of the present invention, it is possible to obtain a molded body with a high relative density, high hardness, high electrical conductivity, and high thermal conductivity.

[0017] In the present invention, the Ni / Si mass ratio, which is the ratio of Ni content to Si content, is set to a predetermined range. By doing so, when the shaped body is aged, an intermetallic compound having a predetermined Ni to Si ratio is precipitated. This makes it possible to utilize precipitation strengthening, which is generally considered to have a stronger strengthening effect than solid solution strengthening. Furthermore, by promoting the precipitation of Ni, which is a readily soluble element, as an intermetallic compound (discharge from the Cu matrix), high electrical conductivity can also be obtained.

[0018] Furthermore, by setting the Ni / Si ratio within a predetermined range, it is possible to avoid excessive Ni-richness or Si-richness, and therefore, neither Ni nor Si remains in excessive concentrations in the Cu matrix after precipitation of the intermetallic compound, thereby obtaining high electrical conductivity.

[0019] Furthermore, high electrical conductivity can be obtained by keeping the total content of Mg, Zr, Cr, Nb, Mn, Fe, Zn, and Sn low and reducing the impurities of C, P, and S.

[0020] Furthermore, the addition of Ag as in embodiments 2 and 4 can further improve the balance between hardness and electrical conductivity while maintaining excellent formability. In the alloy of this embodiment, Ag is believed to provide the above benefits by further promoting the precipitation of the intermetallic compounds and the expulsion of elements such as Zr and Cr (if present) from the Cu matrix.

[0021] 1 is a graph showing the measurement results of the Examples and Comparative Examples, with the vertical axis representing electrical conductivity (% IACS) and the horizontal axis representing Vickers hardness (Hv). In this graph, the measurement results of Examples 1 to 29 are indicated by ○, and the measurement results of Comparative Examples 1 to 9 are indicated by ×.

[0022] Before describing the embodiments of the present invention, the reasons for specifying each component added to the Cu alloy powder of the present invention, and the reasons for specifying the Ni / Si ratio and Ni+Si will be explained. Note that % in the components refers to mass %. The remaining components consist of Cu and unavoidable impurities.

[0023] Ni: 1.20 to 7.30% Ni is an essential element for precipitating intermetallic compounds together with Si to increase hardness and also improve formability. However, excessive addition significantly reduces electrical conductivity. Addition of less than 1.20% is ineffective, while addition of more than 7.30% significantly reduces electrical conductivity. Therefore, the Ni content is set to 1.20 to 7.30%, preferably 2.25 to 6.00%, and more preferably 3.30 to 4.70%.

[0024] Si: 0.25 to 1.80% Si is an essential element for precipitating intermetallic compounds together with Ni to increase hardness and also improve formability. However, excessive addition significantly reduces electrical conductivity. Addition of less than 0.25% is ineffective, while addition of more than 1.80% significantly reduces electrical conductivity. Therefore, the Si content is set to 0.25 to 1.80%, preferably 0.55 to 1.45%, and more preferably 0.80 to 1.15%.

[0025] Mg: 0.40% or less Mg is an easily oxidizable element that reacts with oxygen to generate gas during molding, causing residual pores and reducing electrical conductivity. If the Mg content is 0.40% or less, the effect is minor. On the other hand, if the Mg content exceeds 0.40%, these adverse effects become significant. Therefore, the Mg content is set to 0-0.40%, preferably 0.10% or less, and more preferably 0.02% or less. Therefore, Mg is not an essential element, and therefore the Mg content can be 0%.

[0026] Sum of Zr, Cr, Nb, Mn, Fe, Zn, and Sn: 0.00 to 2.00%. When one or more of Zr, Cr, Nb, Mn, Fe, Zn, and Sn are contained, the total amount thereof is 2.00% or less by mass. These elements also have the effect of improving formability and hardness. However, compared to when the essential elements Ni and Si of the present invention are added in a predetermined ratio, the inclusion of Zr, Cr, Nb, Mn, Fe, Zn, and Sn reduces the balance between high hardness and high electrical conductivity. This is because all of these elements dissolve in the Cu matrix, thereby reducing the balance between high hardness and high electrical conductivity. From this perspective, when Zr, Cr, Nb, Mn, Fe, Zn, and Sn are contained, they can be treated as the total amount. However, when the total amount of these components exceeds 2.00%, the adverse effects become significant. On the other hand, if the total content of Zr, Cr, Nb, Mn, Fe, Zn, and Sn is 2.00% or less, the effect on the balance between high hardness and high electrical conductivity is slight. Therefore, the total content of Zr, Cr, Nb, Mn, Fe, Zn, and Sn is set to 0.00 to 2.00%, more preferably 0.90% or less, and even more preferably 0.05% or less.

[0027] C, P, and S: 0.000 to 0.020% each Since C, P, and S are all components that cause a decrease in electrical conductivity, it is desirable to strictly limit their upper limits. If each component is contained at 0.020% or less, the effect is slight, but if it exceeds 0.020%, the adverse effects become significant. Therefore, the contents of C, P, and S are all set to 0.000 to 0.020%, preferably 0.014% or less, and more preferably 0.009% or less.

[0028] Ni / Si: 3.00 to 6.00 The Ni / Si ratio is one of the most important indicators in the present invention. It is an indicator for achieving a balance between high hardness and high conductivity while maintaining high formability. When the Ni to Si mass ratio is less than 3.00 or more than 6.00, the balance between high hardness and high conductivity of the additively manufactured object is reduced. Therefore, the Ni / Si ratio is set to 3.00 to 6.00, preferably 3.55 to 4.95, and more preferably 3.85 to 4.30.

[0029] Ni + Si: 1.50 to 9.00% As described above, Ni and Si are important essential elements in the present invention, and if their total content is less than 1.50%, high hardness cannot be obtained, and if it exceeds 9.00%, electrical conductivity decreases. Therefore, the total content of Ni and Si (i.e., Ni + Si) is set to 1.50 to 9.00%, preferably 2.70 to 7.05%, and more preferably 3.90 to 5.10%.

[0030] Ag: 5.00% or less. When Ag is added when Ni and Si are contained within the above-mentioned ranges of Ni / Si ratio, Ni content, and Si content, the balance between high hardness and high electrical conductivity is further improved. Furthermore, the effect is even greater when one or more of Zr and Cr are contained. However, if added in excess, this effect is not observed. If added in excess of 5.00%, the effect of improving the balance between high hardness and high electrical conductivity is not observed, and the expensive Ag increases the material price. Therefore, when Ag is added as described in aspect 2, the Ag content is set to 5% or less, preferably 0.01 to 2.90%, and more preferably 0.03 to 0.90%.

[0031] [Regarding O and N] Because the powder in the present invention is an alloy, it inevitably contains the gas components oxygen and nitrogen. Generally, the content of these gas components differs between the surface and interior of the powder, and the content of the gas components per powder weight depends on the total surface area (i.e., particle size). Therefore, from the perspective of preventing residual pores and non-metallic inclusions due to oxygen and nitrogen in the layered manufactured product, the amount of oxygen (O content) contained in the powder is preferably 1000 ppm or less, more preferably 500 ppm or less. Furthermore, the amount of nitrogen (N content) is preferably 300 ppm or less, more preferably 150 ppm or less.

[0032] [Average particle size of powder] The powder of the present invention can be suitably used in additive manufacturing. There are various additive manufacturing methods, but when powder is used as a raw material, powder with an average particle size (volume average) of approximately 10 to 200 μm is used. The preferred average particle size is 15 to 40 μm for the laser powder bed method, 50 to 100 μm for the electron beam powder bed method, and 55 to 105 μm for the deposition method. The more preferred average particle size is 20 to 35 μm for the laser powder bed method, 65 to 85 μm for the electron beam powder bed method, and 70 to 90 μm for the deposition method.

[0033] [Powder fluidity, tap density, and average circularity] The powder of the present invention can be suitably used in additive manufacturing methods. From the viewpoint of the uniformity of the powder bed by the squeegee (a plate for spreading the powder at a constant thickness) in the powder bed method and the stability of powder supply through a feeder in the deposition method, the powder fluidity is preferably 30 s / 50 g, and more preferably 20 s / 50 g. From the same viewpoint, the tap density of the powder is preferably 50 to 80% of the true density, and more preferably 60 to 78%. From the same viewpoint, the average circularity of the powder is preferably 0.70 or more, and more preferably 0.75 or more.

[0034] Here, the flow rate can be measured by the Hall flow method or the like. The tap density can be measured by tapping the powder in a container and measuring the weight and volume. The true density can be measured by the gas displacement method or the like. The average circularity can be measured by a Morphologi 4 (manufactured by Malvern Instruments) or the like.

[0035] [Heat Treatment Temperature] In the layered product of the present invention, heat treatment precipitates intermetallic compounds, thereby increasing hardness and electrical conductivity. The lower limit of the heat treatment temperature can be 400°C, preferably 600°C, more preferably 650°C, and even more preferably 700°C. The upper limit of the heat treatment temperature is preferably 900°C, more preferably 850°C.

[0036] The present invention will be described in more detail with reference to the following examples. However, the present invention is not limited to the following examples. Cu alloy powders having the component compositions and Ni / Si ratios shown in Examples 1 to 29 and Comparative Examples 1 to 9 in Tables 1A and 1B were prepared, and shaped bodies were obtained by additive manufacturing using these Cu alloy powders. Note that the alloy compositions shown in Tables 1A and 1B are the component compositions of the Cu alloy powders, and the remainder of the alloy compositions shown in the tables is Cu and unavoidable impurities.

[0037] [Production of Raw Powder] Powders having the compositions shown in Tables 1A and 1B were produced by gas atomization using the following procedure. The raw powder materials were placed in an alumina crucible and melted by high-frequency heating in a vacuum or argon atmosphere. The resulting molten alloy was poured from a 5 mm diameter nozzle at the bottom of the crucible and immediately sprayed with high-pressure argon gas. This spraying broke the molten alloy into fine droplets, which cooled and solidified as they fell through the tower of the atomization device, becoming alloy powder. This alloy powder was sieved through a mesh with 63 μm openings, and the powder that passed through the mesh was used as the raw powder for the subsequent additive manufacturing process.

[0038] All powders had an oxygen content of 1000 ppm or less, a nitrogen content of 300 ppm or less, an average particle size (volume average) of 15 to 40 μm, a flowability of 30 s / 50 g or less, a ratio of tap density to true density of 50 to 80%, and an average circularity of 0.70 or more.

[0039]

[0040]

[0041] [Layered Manufacturing and Heat Treatment] Using these Cu alloy powders, a shaped body was produced by layered manufacturing. Specifically, layered manufacturing was carried out using a laser-heated powder bed type device (product name: EOS-M290) at an energy density of 200 J / mm 3 It was carried out at.

[0042] Using a pure Cu plate as the base material, we produced shaped bodies measuring 12 mm x 12 mm x 12 mm for measuring relative density and hardness, and shaped bodies measuring 10 mm x 10 mm x 70 mm for measuring electrical conductivity. These shaped bodies were separated from the plate by wire cutting and subjected to heat treatment at the temperatures and times shown in Table 2, and various evaluations of relative density, hardness, and electrical conductivity were performed. The results are shown in Table 2.

[0043] In the examples, the heat treatment was carried out in an Ar atmosphere, and the specimens were held at a predetermined temperature for a predetermined time, followed by furnace cooling. The heat treatment temperature was also varied for some specimens to evaluate the effect of the heat treatment conditions on the balance between hardness and electrical conductivity of the shaped body of this alloy.

[0044]

[0045] [Evaluation of the relative density of the molded body] The density of the molded body was measured by the Archimedes method. The Archimedes method involves measuring the weight of a test piece in air and in water, calculating the volume of the molded body from the difference between the weights, and dividing the volume by the air weight to calculate the density. The density of the raw material powder used was also measured by the gas displacement method. This method involves placing powder in a container with a specified volume, introducing a fixed amount of gas into it, calculating the volume of the powder from the gas pressure, and dividing the weight of the powder by the volume to calculate the density. The density of the powder was defined as the true density of the alloy, and the relative density of the molded body was evaluated as "density of the molded body / density of the powder × 100 (%)".

[0046] [Evaluation of Hardness of Shaped Object] The hardness of the shaped object was evaluated using a Vickers hardness tester. The test force was 2.94 N, and the average value of n=5 was evaluated.

[0047] [Evaluation of Electrical Conductivity of Shaped Object] To confirm the electrical conductivity of the shaped object, the specific resistance value was measured by the four-terminal method (JIS C 2525). The reciprocal of the specific resistance value was taken as the electrical conductivity, and the value of pure Cu (5.9 × 10 7 The electrical conductivity (% IACS) of each sample was evaluated, with the electrical conductivity (S / m) being 100% IACS. This measurement was performed using test pieces machined to dimensions of 3 mm x 2 mm x 60 mm at room temperature, with a current of 4 A and a voltage drop distance of 40 mm.

[0048] The results of Table 2 are shown in Figure 1, a graph with electrical conductivity (% IACS) on the vertical axis and Vickers hardness (Hv) on the horizontal axis. In the graph of Figure 1, Examples are plotted with a circle, while Comparative Examples are plotted with an x. Compared to the Comparative Examples, it can be seen that the Examples as a whole have a superior balance between hardness and electrical conductivity. Furthermore, Examples 21, 22, and 23, which contain Ag, are shifted to the upper right of Figure 1, demonstrating an even superior balance between hardness and electrical conductivity. Furthermore, Comparative Examples 7, 8, and 9, which are binary Cu-Ni alloys, have high electrical conductivity but extremely low hardness, and it can be seen from Figure 1 that the hardness and electrical conductivity are not compatible and are therefore unbalanced.

[0049] As described above, the powders of Examples 1 to 29 shown in Table 1A all satisfy the specified composition, Ni / Si ratio, and Ni+Si amount. The shaped bodies obtained by additive manufacturing using these powders using the powder bed method had a relative density of 99.0% or higher, as shown in Table 2, demonstrating excellent moldability. Furthermore, as shown in FIG. 1 , the shaped bodies using the powders of Examples 1 to 29 have a moderate balance of both hardness and conductivity compared to those manufactured by additive manufacturing using conventional powders. Compared to the plot positions of the comparative examples, the plot positions of the examples are shifted toward the upper right in FIG. 1 overall. In other words, the examples achieve both properties better than the comparative examples. In particular, Examples 21, 22, and 23, which contain Ag, are shifted further toward the upper right in FIG. 1 , confirming that they combine superior hardness and conductivity.

[0050] In Comparative Example 1, the Ni and Si contents were insufficient, and the Ni+Si content was also insufficient, resulting in poor relative density and poor moldability.In Comparative Example 2, the Ni and Si contents were excessive, and the Ni+Si content was also excessive, resulting in a significant decrease in conductivity.In Comparative Examples 3 and 6, the Ni / Si ratio was higher, and in Comparative Examples 4 and 5, the Ni / Si ratio was lower, resulting in a balance between hardness and conductivity that was inferior to that of the Examples.In Comparative Examples 7, 8, and 9, which are binary Cu-Ni systems and contain only trace amounts of Si as an impurity, the Ni / Si ratio was significantly off, resulting in extremely low hardness, and the balance between hardness and conductivity was poor and incompatible.

Claims

1. A Cu alloy powder for additive manufacturing, comprising, by mass, the following: Ni: 1.20-7.30%, Si: 0.25-1.80%, Mg: 0.40% or less, a total of one or more of Zr, Cr, Nb, Mn, Fe, Zn, Sn: 0.00-2.00%, C: 0.000-0.020%, P: 0.000-0.020%, and S: 0.000-0.020%, with the balance being Cu and unavoidable impurities, wherein the ratio of the Ni content to the Si content (Ni / Si) is 3.00-6.00, and the total content of Ni and Si is 1.50-9.00%.

2. A Cu alloy powder for additive manufacturing comprising, by mass, the following: Ni: 1.20-7.30%, Si: 0.25-1.80%, Mg: 0.40% or less, a total of one or more of Zr, Cr, Nb, Mn, Fe, Zn, Sn: 0.00-2.00%, C: 0.000-0.020%, P: 0.000-0.020%, S: 0.000-0.020%, and Ag: greater than 0% and 5.00% or less, with the balance being Cu and unavoidable impurities, wherein the ratio of the Ni content to the Si content Ni / Si is 3.00-6.00 and the total content of Ni and Si is 1.50-9.00%.

3. A molded body produced by additive manufacturing using the Cu alloy powder for additive manufacturing described in claim 1.

4. A molded body produced by additive manufacturing using the Cu alloy powder for additive manufacturing described in claim 2.

Citation Information

Patent Citations

  • Cu-BASED ALLOY POWDER

    JP2021017639A

  • Copper alloy powder, and additive-manufactured article

    JP2022188809A

  • Forming upper die processing technology

    CN114618988A

  • Copper alloy and application thereof

    CN115198140A

  • Copper alloy sheet material low in deflection coefficient and excellent in bendability

    JP2013040389A

Cited By

  • Additive manufacturing die steel and preparation method thereof

    CN121223108A

  • Additive manufacturing mold steel and method of making the same

    CN121223108B