Multilayer body capable of achieving high peel strength even with thin adhesive layer, method for producing same, and method for bonding base materials
By integrating adhesive compositions with varying stress levels in a laminate, high peel strength is achieved with a thin adhesive layer, addressing the challenge of compact structure design and storage while maintaining mechanical integrity under tensile stress.
Patent Information
- Application Number
- PCT/JP2024/015266
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2024-04-17
- Publication Date
- 2024-11-21
AI Technical Summary
Existing laminates face challenges in achieving high peel strength with thin adhesive layers, particularly when subjected to external forces, which hinders their ability to be compactly structured and stored while maintaining strength, as traditional methods like sewing and welding compromise strength, and adhesive thickness is often required for sufficient bonding.
The use of two or more types of curable adhesive compositions with different stress levels at 10 mm elongation, applied in parallel and integrated to form a thin adhesive layer, where one side with low stress and the other with high stress are strategically placed to enhance peel strength without increasing adhesive thickness.
This approach allows for high peel strength even with a thin adhesive layer, enabling the laminate to be designed for compact structures, miniaturization, folding, and storability, while maintaining mechanical integrity under tensile stress.
Smart Images

Figure JP2024015266_21112024_PF_FP_ABST
Abstract
Description
Laminate capable of achieving high peel strength even with a thin adhesive layer, its manufacturing method, and method for bonding between substrates
[0001] The present invention relates to a laminate that can achieve high peel strength even with a thin adhesive layer when an external force acts to move the bonded substrates apart, thereby enabling the design of a compact structure, a manufacturing method thereof, and a bonding method between substrates.
[0002] Flat cloth-like substrates, film-like substrates, and plate-like substrates can be bonded by at least partially stacking multiple substrates by sewing, fusing / welding, or gluing them together to ensure a large total area and three-dimensional formability as a whole laminate, and can be unfolded or expanded depending on the application. For this reason, the laminate is required to have sufficient bonding strength, particularly peel strength, against external forces that separate the constituent substrates (typically, peeling or pulling the substrates). On the other hand, in recent years, there has been an increasing demand for lighter weight and space-saving, and there is a demand for the laminate to be stored as a compact structure or folded for storage.
[0003] However, in sewing, in order to ensure bonding strength, it is necessary to ensure the thickness of the cloth-like or sheet-like substrate and the sewing area are wide, and the use of pinholes and sewing threads can reduce the bonding strength, making it particularly difficult to store the laminate as a compact structure while maintaining the strength of the substrate. Furthermore, when bonding sheet-like substrates such as cloth, fusion / welding of substrates does not ensure sufficient bonding strength, and when tensile or peeling stress is applied between the substrates, the laminate may easily separate.
[0004] In contrast, for example, as described in Patent Document 1, when substrates are joined together with an adhesive layer, structural integrity and weight reduction of the joint are possible without stitching, and there are advantages in that high peel strength can be ensured by ensuring sufficient adhesive strength between the substrates. However, in general, improving adhesive strength requires ensuring the thickness of the adhesive layer, and achieving high adhesive strength (particularly peel strength against tensile stress that tries to move the substrates away from each other) requires applying a relatively thick adhesive composition that forms the adhesive layer, which poses a trade-off problem in that the laminate cannot satisfy the required properties of a compact structure, such as miniaturization, thin layering, foldability, and storability.
[0005] On the other hand, Patent Document 2 proposes a flexible EL light-emitting device, which is a laminate characterized by being constructed by arranging a high-elasticity adhesive layer made of an elastic adhesive and a low-elasticity adhesive layer made of a low-elasticity adhesive side by side on a substrate. Specifically, when a flexible EL light-emitting device is fabricated on a flexible substrate, the high-elasticity adhesive has excellent conformability and low risk of breakage when the substrate is bent, but has poor moisture-blocking properties. In contrast, the low-elasticity adhesive has poor conformability and the risk of breakage when the substrate is bent, but has high moisture-blocking properties. Therefore, the laminate described in Patent Document 2 uses both adhesives in combination to ensure the flexibility of the substrate while preventing external moisture and oxygen from penetrating the flexible EL light-emitting device, which would otherwise reduce its light-emitting performance and light-emitting life. However, these two types of adhesive layers are arranged around the periphery of the laminate as independent and separate adhesive layers, and the two do not form an integrated adhesive layer. Furthermore, as mentioned above, the purpose of using adhesives with different elasticities in combination is to expect the two types of adhesive layers to perform different independent roles, and not to integrate the two to achieve high peel strength. In other words, the invention disclosed in Patent Document 2 has a different problem and effect from the present invention, and there is no description or suggestion of integrating different adhesive layers arranged in parallel to achieve high peel strength even with a thin adhesive layer against tensile stress that tries to move the substrate away.
[0006] JP 2011-152913 A JP 2011-204364 A
[0007] The object of the present invention is to provide a laminate that is highly industrially productive, can be produced at low cost, is applicable to laminates using not only fabric / film substrates but also various other substrates, and is capable of achieving high peel strength even with a thin adhesive layer when an external force acts to separate the bonded substrates, thereby enabling the design of a compact structure, a method for producing the same, and a method for bonding substrates together.
[0008] As a result of extensive investigation, the present inventors have found that the above-mentioned problems can be solved by a laminate having a structure in which (S1) a first cloth or sheet-like substrate and (S2) a second cloth or sheet-like substrate are bonded together by an adhesive layer formed by applying in parallel (A) two or more types of curable adhesive compositions, the stresses of which at 10 mm elongation in the stress-strain curve upon curing are in the range of 2 to 5 times that of each other, and integrating them, and have completed the present invention.
[0009] In particular, when two bonded substrates constituting a laminate are deformed so as to move away from each other, it is preferable that a curable adhesive composition that forms an adhesive layer with low stress when elongated by 10 mm is placed on the side that is subjected to deformation, and a curable adhesive composition that forms an adhesive layer with high stress when elongated by 10 mm is placed on the side that is not subjected to deformation, and that the adhesive layers that have different stresses when elongated by 10 mm are cured to become one.
[0010] Furthermore, it is preferable that the width of the entire integrated adhesive layer is in the range of 5 to 50 mm and that its thickness is 1 mm or less. The curable adhesive composition that forms the adhesive layer is not particularly limited, but is preferably at least one elastic adhesive composition selected from acrylic adhesives, urethane adhesives, epoxy adhesives, vinyl acetate adhesives, styrene-butadiene rubber adhesives, natural rubber adhesives, and silicone adhesives, and is particularly preferably a curable silicone rubber composition that cures by a hydrosilylation reaction.
[0011] Similarly, the above-mentioned problem can be solved by a method for producing a laminate, comprising the steps of: step (I): (S1) applying, onto a first fabric or sheet-like substrate, two or more types of curable adhesive compositions, the stresses at 10 mm elongation in a stress-strain curve when cured being in a range of 2 to 5 times that of each other, so as to be parallel to each other; step (II): (S2) laminating a second fabric or sheet-like substrate onto the curable adhesive compositions applied in step (I); step (III): before, after, or simultaneously with step (II), bringing the two or more types of curable adhesive compositions into contact or pressing them together to integrate them; and step (IV): curing the two or more types of integrated curable adhesive compositions by a curing reaction, thereby forming an adhesive layer between the (S1) first fabric or sheet-like substrate and the (S2) second fabric or sheet-like substrate.
[0012] In particular, when two bonded substrates constituting a laminate are deformed so as to move away from each other, it is preferred that the step (I) is a step of applying a curable adhesive composition that forms an adhesive layer with low stress when elongated by 10 mm on the side that is subjected to deformation, and a curable adhesive composition that forms an adhesive layer with high stress when elongated by 10 mm on the side that is not subjected to deformation, and that the step (III) is a step of pressing two or more types of curable adhesive compositions that have been applied in parallel between the bonded (S1) first cloth or sheet-like substrate and (S2) second cloth or sheet-like substrate after or simultaneously with step (II), thereby integrating them so that the thickness of the adhesive layer after curing is 1 mm or less.
[0013] The above-mentioned problems can also be solved by a method for bonding substrates, comprising: step (I'): applying two or more curable adhesive compositions, each of which has a stress at 10 mm elongation in the stress-strain curve after curing that is 2 to 5 times that of the other curable adhesive composition, to a first substrate in parallel with each other; step (II'): laminating a second substrate onto the curable adhesive composition applied in step (I'); step (III'): after step (II') or simultaneously with step (II'), bringing the two or more curable adhesive compositions into contact or pressure-bonding between the first substrate and the second substrate to integrate them; and step (IV'): curing the integrated two or more curable adhesive compositions by a curing reaction to form an adhesive layer between the first substrate and the second substrate. In this bonding method, the first substrate and the second substrate may each independently be a fabric or sheet-like substrate.
[0014] The laminate of the present invention can be achieved by arranging two or more adhesive layers with different moduli in parallel between substrates and using an integrated adhesive layer. This allows for superior industrial productivity and lower cost than sewing, and is versatile enough to be applied to laminates using a variety of substrates, not just fabric / film substrates. Furthermore, the laminate of the present invention can achieve high peel strength even with a thin adhesive layer when an external force acts to separate the bonded substrates. This allows for a thinner, more firmly bonded laminate with high peel strength, thereby providing a laminate that can be designed to meet the compactness requirements of miniaturization, thinning, foldability, and storage. The present invention also provides a method for producing the above laminate and a method for bonding substrates.
[0015] 1 is a cross-sectional view of a peel test piece according to one embodiment of the present invention; FIG. 2 is a top view of a peel test piece according to one embodiment of the present invention, in which adhesives A1 and B1 are arranged in parallel and integrally, as observed through the upper substrate 1; FIG. 3 is a perspective view of a peel test piece according to one embodiment of the present invention; FIG. 4 is a cross-sectional view of a peel test piece according to one embodiment of the present invention, during a peel test of a substrate; FIG. 5 is a stress-strain curve obtained when a peel test was conducted independently for adhesives A1 and B1 used in the present invention; FIG. 6 is a stress-strain curve obtained when a peel test was conducted independently for peel test pieces in which adhesives A1 and B1 are arranged in parallel and integrally, as an embodiment of the present invention; FIG. 7 is a stress-strain curve obtained when a peel test was conducted independently for adhesives A2 and B2 used in the present invention; FIG. 8 is a stress-strain curve obtained when a peel test was conducted on a peel test piece in which adhesives A2 and B2 are arranged in parallel and integrally, as an embodiment of the present invention; and FIG. 9 is a stress-strain curve obtained when a peel test was conducted on a peel test piece in which adhesives A1 and B1 were arranged in a dot pattern, as a comparative test. As a comparative test, a peel test was conducted on peel test pieces in which adhesive A1 and adhesive B1 were arranged in a mesh pattern, and the resulting stress-strain curves are shown.
[0016] [Laminate] The laminate according to the present invention is composed of (S1) a first fabric or sheet-like substrate, (S2) a second fabric or sheet-like substrate, and an adhesive layer (A) between these substrates. The substrates (S1) and (S2) are preferably at least partially bonded together by the adhesive layer, and the laminate is designed to undergo deformation so that the substrates move away from each other. Here, deformation refers to the action of an external force on the laminate that generates tensile stress that moves these substrates away from each other, and examples of deformation of the laminate include pulling, peeling, delamination, expansion, and unfolding between the substrates.
[0017] The type of laminate is not particularly limited, and laminates in which sheet (film) substrates are bonded to each other, a sheet (film) substrate and a base fabric, or base fabrics are bonded to each other are known as materials used in outdoor products, packaging materials, protective sheets, functional films, vehicle airbags, etc. Examples include laminated films, laminated plates, laminated fabrics, and laminated sheets. As long as the laminate has the structure of the present invention (particularly the structure of the adhesive layer), it may also be a multi-layer laminate in which two laminates are bonded together. For example, it may be a laminate in which an adhesive layer (A) is provided between two substrates (S1, S2) such as "S1 / A / S2 / A / S1" or "S1 / A / S2 / A / S1 / A / S2." Furthermore, a coating layer (e.g., a silicone rubber covering / coating layer for heat resistance reinforcement) may be provided on the inside or outside of the substrate constituting the laminate. As mentioned above, the substrates may be different or the same, and may be, for example, laminates in which thermoplastic resin film substrates, fabric substrates, or a thermoplastic resin film and fabric substrate are bonded together, which is preferable. The laminate may also be provided with a functional coating layer for the purpose of improving heat resistance, flame retardancy, or substrate strength. Additionally, if a specific portion of the laminate is subject to particularly strong heat or tensile stress, the laminate may further include a reinforcing substrate or heat-resistant substrate for the purpose of reinforcement, damage prevention, or improved heat resistance.
[0018] There are no particular limitations on (S1) the first fabric or sheet-like substrate and (S2) the second fabric or sheet-like substrate, and S1 and S2 may be the same or different.
[0019] The fabric substrate is a woven fabric or base fabric, preferably one containing fibers, and may be a woven, knitted, or nonwoven fabric, and may be sewn entirely or partially. Among these, woven fabrics are preferred due to their high mechanical strength, and a biaxial structure combining multiple warp threads and multiple weft threads is preferred. A triaxial structure combining multiple warp threads, multiple weft threads, and multiple diagonal threads is also possible. Of these, a biaxial structure base fabric is preferred, and a plain woven fabric is more preferred due to its strength and ease of manufacture. Plain woven fabrics are woven with warp and weft threads alternately crossing each other, resulting in more intersections between warp and weft threads than other weaves, such as twill and satin woven fabrics, and therefore have higher strengths such as tensile strength and tear strength. This makes the laminate of the present invention particularly useful when used in applications where strong tensile stress is applied instantaneously. The weave density is preferably at least 35 threads per inch for both the warp and weft threads. The total fineness of the yarn is not limited, but is preferably within the range of 100 to 2,000 dtex. The base fabric also includes OPW (One Piece Woven), which is not a flat base fabric but is woven seamlessly into a bag shape so that it can have a curved surface to match the shape of the desired product.
[0020] The fibers may be synthetic fibers, natural fibers, regenerated fibers, semi-synthetic fibers, inorganic fibers, or combinations thereof (including blends and woven fibers). Synthetic fibers, particularly polymer fibers, are preferred. Composite fibers, such as core-sheath fibers, side-by-side fibers, and splittable fibers, can also be used. For example, a base fabric or fabric made of a natural fiber selected from cotton, hemp, or flax; or a base fabric or fabric made of a synthetic fiber such as polyamide fiber or polyaramid fiber (e.g., nylon base fabric), polyimide fiber, or polyester fiber, may be used in the laminate of the present invention. The natural fibers selected from cotton, hemp, or flax have a high carbonization point of 500°C to 580°C, and therefore have excellent heat resistance. They have the practical advantage of being less susceptible to melting or damage due to heat, even at high temperatures, for example, when the laminate is deployed / deformed by inflation gas.
[0021] The sheet-like substrate is a flat substrate (excluding the above-mentioned cloth / base fabric), and includes substrates in the form of sheets, films, and plates. The type and material of the sheet-like substrate are not particularly limited, and may be paper, wood, metal, or synthetic resin, such as cardboard or paper; wood (plywood) sheet; metal sheet such as aluminum sheet; polyester sheet, polyamide sheet, polyimide sheet, polyaramid sheet, polyethylene sheet, polyvinyl chloride sheet, polyurethane sheet, polycarbonate sheet, or acrylic sheet. Furthermore, these sheet-like substrates may have a structure in which multiple sheets are stacked (for example, composite film, film-laminated paper, etc.).
[0022] The laminate of the present invention is characterized in that the substrate has a structure in which (A) two or more types of curable adhesive compositions, the stresses of which at 10 mm elongation in the stress-strain curve upon curing are in the range of 2 to 5 times that of each other, are applied in parallel to each other and bonded together with an integrated adhesive layer.
[0023] The curable adhesive composition used in the laminate of the present invention contains a combination of a composition with a high stress and a composition with a low stress at 10 mm elongation in the stress-strain curve of the adhesive layer obtained when each composition is cured alone (hereinafter, sometimes simply referred to as the "stress-strain curve"). The stress at 10 mm elongation in the stress-strain curve of the high-stress adhesive layer is 2 to 5 times, preferably 2 to 4 times, that of the low-stress adhesive layer. The stress-strain curve of the adhesive layer in the present invention was obtained using a tensile tester at a tension rate of 200 mm / min under conditions of 25°C and 50% RH (relative humidity) using a test piece having a 1 mm thick adhesive layer. If the stress of two or more adhesive layers is below the lower limit, the stress-strain curves of the two or more adhesive layers will not differ significantly, and the combined adhesive layer may not achieve high peel strength as a whole. Conversely, if the stress of two or more types of adhesive layers exceeds the upper limit, the difference in modulus between the two becomes too large, and even if the two are integrated, the adhesive layers tend to exhibit independent properties, so that it may not be possible to achieve high peel strength as a whole integrated adhesive layer.
[0024] The adhesive layer used in the laminate of the present invention is characterized in that it is an adhesive layer formed by applying two or more types of curable adhesive compositions, which have different stresses at 10 mm elongation in the stress-strain curve of the adhesive layer, in parallel to each other and integrating them. The curable adhesive compositions with different stresses may be two or three or more types, but from the standpoints of workability and technical effect, it is preferable to use two types of curable adhesive compositions.
[0025] Here, "applied parallel to each other" means that two or more types of curable adhesive compositions before curing are applied to a substrate without crossing each other. If the two are applied crossing each other in a mesh-like pattern or dispersed in a dot-like pattern, the technical effect of the present invention may not be achieved even if the adhesive layers are integrated.
[0026] Furthermore, the term "integrated adhesive layer" refers to two or more types of curable adhesive compositions that form an integrated adhesive layer without generating gaps between the adhesive layers before or during curing. For example, two or more types of curable adhesive compositions may be applied in parallel to a substrate without crossing each other, with substantially no gaps between them, forming an integrated adhesive layer without generating gaps between them upon curing. Alternatively, two or more types of curable adhesive compositions may be applied in parallel to a substrate without crossing each other, and before or during curing, the substrates may be stacked, and the two or more types of curable adhesive compositions may be brought into contact or pressed between the substrates by an external force, such as pressing the substrates, to form an integrated adhesive layer without generating gaps between them upon curing. Here, at the interface between the two or more types of curable adhesive compositions, the different compositions may be in contact or partially mixed with each other. It is particularly preferred that the two different compositions are cured in a partially mixed state at the contact surface, forming an integrated adhesive layer. However, as mentioned above, in order to achieve the technical effects of the present invention, the two or more types of curable adhesive compositions must be applied in parallel so that they do not intersect with each other; if the two compositions are completely mixed together, the technical effects may not be achieved.
[0027] The adhesive layer according to the present invention has a structure in which adhesive layers with different stresses are integrated by contact or mixing without forming gaps between them, and the adhesive layers with different stresses are arranged parallel to each other. Here, the adhesive layer on the higher stress side is a high-modulus adhesive layer that firmly bonds the substrates together and prevents their separation, but has poor deformability to external forces, particularly tensile forces acting in a direction that moves the substrates apart. On the other hand, the adhesive layer on the lower stress side is a low-modulus adhesive layer that, when used alone, has insufficient adhesive strength between the substrates but is flexible and has high deformability, particularly to tensile forces acting in a direction that moves the substrates apart. Therefore, by arranging these adhesive layers in parallel between the substrates and integrating them so that no gaps are formed between them, when the two substrates are deformed so as to move away from each other due to a tensile force (including, for example, an external force such as expansion, unfolding, or elongation between the substrates, and the action of inflation gas), the low-modulus adhesive layer on the side that is subjected to the deformation undergoes a large deformation to relieve the tensile force between the substrates, while the high-modulus adhesive layer on the side that is not subjected to the deformation can continue to firmly bond the substrates together, as shown in Figure 5. As a result, even when an external force acts to move the bonded substrates apart, even a thin adhesive layer of 1 mm or less can achieve high peel strength as a whole.
[0028] This change in adhesive behavior can be confirmed by the difference between the stress-strain curves of the adhesive layers obtained using each adhesive layer alone and the stress-strain curves of the adhesive layers when both are arranged in parallel and integrated (see, for example, the stress-strain curves shown in Figures 5 and 6, and Figures 7 and 8).
[0029] From the viewpoint of the technical effects of the present invention, when the two bonded substrates constituting the laminate are deformed so as to move away from each other, it is particularly preferable that a curable adhesive composition that forms an adhesive layer that has a low stress when elongated by 10 mm is placed on the side that is subjected to deformation, and a curable adhesive composition that forms an adhesive layer that has a high stress when elongated by 10 mm is placed on the side that is not subjected to deformation, and that the adhesive layers that have different stresses when elongated by 10 mm are cured so as to become one.
[0030] The adhesive strength of the two or more curable adhesive compositions constituting the adhesive layer can be appropriately designed depending on the type of laminate and the tensile stress and peel strength acting on the laminate. In particular, when the laminate is deployed by a strong expansion force such as an inflation gas, as in the case of a vehicle airbag, the stress F at 10 mm elongation of the adhesive layer obtained by curing the curable adhesive composition having the highest tensile stress (a1) among the two or more curable adhesive compositions constituting the adhesive layer can be determined based on the stress-strain curve of the adhesive layer measured by the above-mentioned method. a1 (a2) The stress F when elongated by 10 mm of the adhesive layer obtained by curing the curable adhesive composition having the lowest tensile stress is in the range of 40 to 240 (N / 50 mm), a2 is in the range of 20 to 60 (N / 50 mm), and a1 / F a2 ] is preferably in the range of 2.0 to 4.0. a1 may be in the range of 40 to 200, 50 to 180 (N / 50 mm), and the stress F a2 may be in the range of 20 to 55, or 25 to 50 (N / 50 mm). a1 / F a2 The value of ] may range from 2.5 to 3.5.
[0031] In the laminate according to the present invention, the integrated adhesive layer is preferably formed so as to bond two substrates together, and for example, in outdoor goods, packaging materials, protective sheets, functional films, vehicle airbags, etc., when two fabric or sheet-like substrates are bonded together to form an adhesive layer between the substrates as a substitute for sewing or for the purpose of ensuring the surface area of the entire laminate, the integrated adhesive layer according to the present invention is preferably formed so as to bond the ends of the substrates together. Furthermore, from the viewpoint of satisfying the required characteristics for compactness, such as miniaturization / thinning / foldability / storability, it is particularly preferable that the adhesive layer is designed to be thin overall.
[0032] Specifically, the width of the entire integrated adhesive layer is in the range of 5 to 50 mm, and in practice may be in the range of 10 to 45 mm.
[0033] The laminate of the present invention has the advantage that it can achieve high peel strength even when the overall thickness of the adhesive layer is designed to be thin in order to satisfy the required characteristics for compactness. The specific thickness of the adhesive layer can be designed appropriately depending on the intended use of the laminate and the type of substrate, but in uses such as outdoor goods, packaging materials, protective sheets, functional films, and vehicle airbags, the overall thickness (after curing) of the integrated adhesive layer can be designed to be 1 mm or less, and the thickness of the adhesive layer may be in the range of 0.01 to 1.00 mm, 0.05 to 1.00 mm, or 0.10 to 1.00 mm. The thickness of the adhesive layer can be designed to be thin by applying the curable adhesive composition before curing between the substrates, sandwiching a spacer or the like as necessary, and then pressing the adhesive layer from one of the substrates. Even with an adhesive layer of 0.9 mm or less, 0.8 mm or less, 0.7 mm or less, 0.6 mm or less, or 0.5 mm or less (for example, an adhesive layer thickness in the range of 0.05 to 0.50 mm, 0.10 to 0.50 mm), a practical peel strength can be achieved. This allows the thickness of the entire laminate to be designed to be thin compared to normal sewing or the use of adhesives, and has the advantage of being easily applicable to very compact structures such as folding structures.
[0034] The curable adhesive composition forming the adhesive layer is not particularly limited as long as it satisfies the condition of the stress at 10 mm elongation in the stress-strain curve upon curing described above, and two or more types of curable adhesive compositions with different adhesive layer stresses can be used without particular limitation, but from the standpoint of workability and technical effect, two types of curable adhesive compositions are preferred, and since the adhesive layer has a stress at 10 mm elongation, these are preferably elastic adhesive compositions. Furthermore, since the adhesive layer according to the present invention is arranged by applying them in parallel and must be integrated without any gaps, it is particularly preferable from a practical standpoint to select and use the same or similar curable adhesive compositions with different adhesive layer moduli upon curing (i.e., high modulus side / low modulus side).
[0035] Specifically, the curable adhesive composition forming the adhesive layer of the present invention is preferably at least one elastic adhesive composition independently selected from acrylic adhesives, urethane adhesives, epoxy adhesives, vinyl acetate adhesives, styrene-butadiene rubber adhesives, natural rubber adhesives, and silicone adhesives. Silicone adhesives are particularly preferred when heat resistance and flame retardancy are required for the laminate and its intended use. Seam sealants, which are adhesives used to seal seams, are particularly suitable for use in the present invention, particularly silicone seam sealants (commercially available from Dow Toray Industries, Inc., etc.).
[0036] The curing mechanism of the silicone adhesive usable in the present invention is not limited, and examples include addition reaction, condensation reaction, radical reaction by organic peroxide, radical reaction by UV irradiation, etc. In particular, the use of a curable silicone rubber composition that cures by an addition reaction is particularly preferred, as it cures quickly at relatively low temperatures.
[0037] One embodiment of the laminate according to the present invention uses an adhesive layer formed by applying two types of curable silicone rubber compositions, each of which has a stress at 10 mm elongation in the stress-strain curve upon curing within the above-mentioned range, in parallel to each other and integrating them into one layer. This curable silicone rubber composition contains (A) 100 parts by weight of a diorganopolysiloxane having at least two alkenyl groups per molecule, (B) 5 to 100 parts by weight of an organopolysiloxane resin and / or inorganic filler, (C) an organopolysiloxane having at least two silicon-bonded hydrogen atoms per molecule (an amount such that the silicon-bonded hydrogen atoms in this component are 0.6 to 20 moles per mole of alkenyl groups in components (A) and (B) combined), and (D) a catalytic amount of a hydrosilylation catalyst. The stress at 10 mm elongation in the stress-strain curve upon curing can be designed by the type and polymer length of component (A), the type and content of component (B), the type of component (C) (organopolysiloxane as a crosslinker or chain extender), and the crosslink density. Furthermore, this curable silicone rubber composition may optionally contain an adhesion promoter, a cure retarder, a colorant, etc.
[0038] Component (A) is a diorganopolysiloxane containing at least two alkenyl groups per molecule. Examples of alkenyl groups in component (A) include alkenyl groups having 2 to 12 carbon atoms, such as vinyl, allyl, butenyl, pentenyl, and hexenyl, with vinyl being preferred. Examples of silicon-bonded organic groups other than alkenyl groups in component (A) include alkyl groups having 1 to 12 carbon atoms, such as methyl, ethyl, and propyl; aryl groups having 6 to 12 carbon atoms, such as phenyl, tolyl, and xylyl; and halogenated alkyl groups having 1 to 12 carbon atoms, such as 3-chloropropyl and 3,3,3-trifluoropropyl, with methyl and phenyl being preferred.
[0039] Component (A) is a substantially linear organopolysiloxane, but may have a branch in part of the molecular chain. Furthermore, while there are no limitations on the viscosity of component (A), it is preferably within the range of 100 to 100,000 mPa·s, or 1,000 to 50,000 mPa·s, at 25°C. This is because, when the viscosity of component (A) is at or above the lower limit of this range, the mechanical strength of the resulting silicone rubber layer is improved, while, when the viscosity is at or below the upper limit of this range, the coatability of the resulting silicone rubber composition is improved. The viscosity of component (A) can be measured using a rotational viscometer in accordance with JIS K7117-1.
[0040] Examples of component (A) include dimethylpolysiloxanes terminally blocked with dimethylvinylsiloxy groups, dimethylsiloxane-methylvinylsiloxane copolymers terminally blocked with dimethylvinylsiloxy groups, dimethylsiloxane-methylphenylsiloxane copolymers terminally blocked with dimethylvinylsiloxy groups, and methyl(3,3,3-trifluoropropyl)siloxane-methylvinylsiloxane copolymers terminally blocked with dimethylvinylsiloxy groups.
[0041] Component (B) is an organopolysiloxane resin that improves the mechanical strength and adhesiveness of the silicone rubber layer, or an inorganic filler that is blended to adjust the viscosity of the composition or to improve the mechanical strength, heat resistance, or flame retardancy of the silicone rubber layer. The organopolysiloxane resin of component (B) has a resinous molecular structure, i.e., a structure represented by the formula: SiO 4 / 2 Siloxane having Q units represented by the formula: RSiO 3 / 2 The organopolysiloxane is mainly composed of siloxane units of the formula: R 2 SiO 2 / 2 siloxanes having D units represented by the formula: R 3 SiO 1 / 2 In the formula, R represents a monovalent hydrocarbon group having 1 to 12 carbon atoms. Specific examples include alkyl groups having 1 to 12 carbon atoms, such as methyl, ethyl, and propyl; alkenyl groups having 2 to 12 carbon atoms, such as vinyl, allyl, butenyl, pentenyl, and hexenyl; aryl groups having 6 to 12 carbon atoms, such as phenyl, tolyl, and xylyl; and halogenated alkyl groups having 1 to 12 carbon atoms, such as 3-chloropropyl and 3,3,3-trifluoropropyl. Of these, methyl, vinyl, and phenyl groups are preferred. In particular, the organopolysiloxane resin of component (B) preferably contains alkenyl groups in its molecule, as this further improves the mechanical strength of the silicone rubber layer.
[0042] Examples of the organopolysiloxane resin of component (B) include (CH 3 ) 3 SiO 1 / 2 Units and SiO 4 / 2 Resin consisting of units, (CH 3 ) 3 SiO 1 / 2 Units and (CH 2 =CH)SiO 3 / 2 Units and SiO 4 / 2 Resin consisting of units, (CH 2 =CH)(CH 3 ) 2 SiO 1 / 2 Units and SiO 4 / 2 Resin consisting of units, (CH2 =CH)(CH 3 ) 2 SiO 1 / 2 Units and (CH 2 =CH)SiO 3 / 2 Units and SiO 4 / 2 Resins that are liquid at room temperature, or even solid resins that are compatible with component (A), are preferred.
[0043] On the other hand, known inorganic fillers can be used as the component (B), and specific examples include fine powder silica fillers such as fumed silica, precipitated silica, and calcined silica; reinforcing fillers such as fumed titanium oxide; non-reinforcing fillers such as crushed quartz, diatomaceous earth, iron oxide, titanium oxide, aluminum oxide, aluminum hydroxide, calcium carbonate, magnesium carbonate, and magnesium hydroxide; and fillers obtained by treating these fillers with organosilicon compounds such as organosilanes and organopolysiloxanes. 2 Ultrafine powder silica having a surface-treatment coefficient of 1 / g or more is preferred. Among these, surface-treated ultrafine powder silica, for example, silica previously surface-treated with organosilane, organosilazane, diorganocyclopolysiloxane, etc., is more preferred.
[0044] The content of component (B) is in the range of 5 to 100 parts by mass, preferably 10 to 80 parts by mass, per 100 parts by mass of component (A), in order to improve the adhesive strength of the resulting adhesive layer and its permeability into the base fabric, while also improving thin-layer application properties and achieving the thin adhesive layer required in the present invention. Furthermore, when ultrafine powdered silica is used as component (B), the content is preferably in the range of 5 to 15 parts by mass per 100 parts by mass of component (A). This is because if the content of fine powdered silica exceeds 15 parts by mass, the viscosity of the composition becomes too high, making it difficult to coat the base fabric without a solvent, and if it is less than 5 parts by mass, the mechanical strength of the silicone rubber layer decreases.
[0045] Component (C) is a crosslinking agent for the composition, and is an organopolysiloxane containing at least two silicon-bonded hydrogen atoms per molecule. Examples of silicon-bonded organic groups other than hydrogen atoms in component (C) include alkyl groups having 1 to 12 carbon atoms, such as methyl, ethyl, and propyl; aryl groups having 6 to 12 carbon atoms, such as phenyl, tolyl, and xylyl; and halogenated alkyl groups having 1 to 12 carbon atoms, such as 3-chloropropyl and 3,3,3-trifluoropropyl, with methyl and phenyl being preferred.
[0046] The molecular structure of component (C) is not limited, and examples thereof include linear, branched, partially branched linear, cyclic, and resinous. The viscosity of component (C) is not limited, but preferably has a kinematic viscosity of 1 to 1,000 mm at 25°C. 2 / s. This is because, when the viscosity of component (C) is at or above the lower limit of the above range, the mechanical strength of the resulting silicone rubber layer is improved, while, when it is at or below the upper limit of the above range, the coatability of the resulting silicone rubber composition is improved. The viscosity of component (C) can be measured using an Ubbelohde viscometer in accordance with JIS Z8803.
[0047] Examples of component (C) include methylhydrogenpolysiloxanes blocked at both ends with trimethylsiloxy groups, dimethylsiloxane-methylhydrogensiloxane copolymers blocked at both ends with trimethylsiloxy groups, methylphenylsiloxane-methylhydrogensiloxane copolymers blocked at both ends with dimethylphenylsiloxy groups, cyclic methylhydrogenpolysiloxanes, copolymers of dimethylhydrogensiloxy units and SiO 4 / 2 Furthermore, a diorganopolysiloxane capped at both ends with diorganohydrogensiloxy groups (e.g., a dimethylpolysiloxane capped at both ends with dimethylhydrogensiloxy groups) which serves as a so-called chain extender may be used in combination as part or all of component (C), and can be used to adjust the mechanical strength, elongation, and flexibility of the adhesive layer obtained by curing the composition.
[0048] The amount of component (C) is such that the number of silicon-bonded hydrogen atoms in the organopolysiloxane is 0.6 to 20 moles, and preferably 0.6 to 15 moles, or 0.8 to 10 moles, or 0.8 to 5.0 moles per mole of alkenyl groups in components (A) and (B) combined.
[0049] Component (D) is a hydrosilylation catalyst for curing the composition. Examples of component (D) include platinum-based catalysts, rhodium-based catalysts, and palladium-based catalysts, with platinum-based catalysts being preferred due to their ability to significantly accelerate curing. Examples of platinum-based catalysts include platinum fine powder, chloroplatinic acid, an alcohol solution of chloroplatinic acid, platinum-alkenylsiloxane complexes, platinum-olefin complexes, platinum-carbonyl complexes, and catalysts in which these platinum-based catalysts are dispersed or encapsulated in a thermoplastic resin such as a silicone resin, a polycarbonate resin, or an acrylic resin. Among these, platinum-alkenylsiloxane complexes are preferred. Other catalysts that promote hydrosilylation reactions include non-platinum metal catalysts such as iron, ruthenium, and iron / cobalt. In addition to heat, hydrosilylation reaction catalysts such as photoactivatable platinum complex curing catalysts that promote hydrosilylation reactions upon exposure to high-energy rays such as ultraviolet light may also be used. The photoactivatable hydrosilylation catalyst may be a β-diketone platinum complex or a platinum complex having a cyclic diene compound as a ligand.
[0050] The content of component (D) is a catalytic amount, and is preferably an amount such that, when the entire curable silicone rubber composition is taken as 100 parts by mass, the metal atoms are in the range of 0.01 to 500 ppm, 0.01 to 100 ppm, 0.01 to 80 ppm, or 0.10 to 80 ppm by mass. If the amount is less than the lower limit, the curing reaction may not proceed sufficiently, and if the amount is more than the upper limit, it may be uneconomical.
[0051] The curable silicone rubber composition may contain other optional components as long as they do not impair the technical effects of the present invention. Specific examples of such optional components include a cure retarder, an adhesion promoter, a non-reactive organopolysiloxane such as polydimethylsiloxane or polydimethyldiphenylsiloxane, an antioxidant such as a phenol, quinone, amine, phosphorus, phosphite, sulfur, or thioether, a light stabilizer such as a triazole or benzophenone, a flame retardant such as a phosphate ester, halogen, phosphorus, or antimony, one or more antistatic agents such as a cationic surfactant, anionic surfactant, or nonionic surfactant, a dye, or a pigment.
[0052] The composition may contain an adhesion promoter as another optional component, such as (E) an epoxy group-containing organosilicon compound. Examples of such component (E) include epoxy group-containing organoalkoxysilanes such as γ-glycidoxypropyltrimethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; and epoxy group-containing organopolysiloxanes such as epoxy group-containing organopolysiloxanes having silicon-bonded vinyl groups and alkoxy groups, epoxy group-containing organopolysiloxanes having silicon-bonded hydrogen atoms, and epoxy group-containing organopolysiloxanes having silicon-bonded hydrogen atoms and alkoxy groups.
[0053] The composition may also contain an optional component (F), an organic titanium compound. Examples of component (F) include organic titanate esters such as tetraisopropyl titanate, tetrabutyl titanate, and tetraoctyl titanate; and titanium chelate compounds such as diisopropoxybis(acetylacetonate)titanium and diisopropoxybis(ethyl acetoacetate)titanium. The content of component (F) is within the range of 0.1 to 5 parts by mass per 100 parts by mass of component (A).
[0054] The composition may also contain a cure retarder (G) as an optional component. Examples of such component (G) include alkyne alcohols such as 3-methyl-1-butyn-3-ol, 3,5-dimethyl-1-hexyn-3-ol, and phenylbutynol; eneyne compounds such as 3-methyl-3-penten-1-yne and 3,5-dimethyl-3-hexen-1-yne; tetramethyltetrahexenylcyclotetrasiloxane, and benzotriazole. The content of component (G) is typically within the range of 0.01 to 10 parts by mass per 100 parts by mass of component (A).
[0055] There are no particular restrictions on the method for preparing such a curable silicone rubber composition, and it can be easily produced by uniformly kneading the components in a mixer such as a kneader mixer, pressure kneader mixer, or Ross mixer.
[0056] Such a curable silicone rubber composition may be a one-component package, or may be a multi-component (multi-component) curable silicone rubber composition in which the main component and crosslinking agent / curing agent components are separated into two or more packages.
[0057] [Method for Producing Laminate] The laminate of the present invention can be obtained by a production method including the following steps: Step (I): (S1) applying two or more types of curable adhesive compositions, the stresses of which, when cured, at 10 mm elongation in the stress-strain curve are in the range of 2 to 5 times each other, onto a first fabric or sheet-like substrate so that they are parallel to each other; Step (II): (S2) laminating a second fabric or sheet-like substrate onto the curable adhesive compositions applied in step (I); Step (III): before, after, or simultaneously with step (II), the two or more types of curable adhesive compositions are brought into contact or pressed together to integrate them; and Step (IV): curing the two or more types of integrated curable adhesive compositions by a curing reaction to form an adhesive layer between (S1) the first fabric or sheet-like substrate and (S2) the second fabric or sheet-like substrate.
[0058] Step (I) is (S1) a step of applying two or more types of curable adhesive compositions, each having a stress at 10 mm extension in the range of 2 to 5 times that of the other, parallel to each other onto a first backing fabric or sheet-like substrate. The application method is not particularly limited, but can be carried out using a device such as a dispenser. The dispenser that can be used may be capable of mixing multiple components (multiple liquids), and since the compositions are applied in parallel, an application device in which multiple dispensers are arranged in parallel, such as a dual dispenser, may be used. The type of substrate and the curable adhesive composition are as described above.
[0059] In step (I), two or more types of curable adhesive compositions must be applied parallel to each other, and it is preferable to apply the uncured curable adhesive compositions linearly and parallel. The different uncured curable adhesive compositions applied linearly may be in contact with each other at the time of application so that they are ultimately integrated, or may be applied with a distance between them that allows them to come into contact or be pressed together in the subsequent step (III). Furthermore, depending on the application of the final laminate, it is preferable that the uncured curable adhesive composition applied linearly be applied continuously and parallel to the entire periphery of the substrate or to the lamination site so as not to create gaps between the substrates. On the other hand, if different uncured curable adhesive compositions are applied in a completely intersecting mesh pattern, or if they are overcoated or applied in a dispersed dot pattern, the technical effect of achieving high peel strength as an adhesive layer as a whole by using two or more adhesive layers with different moduli in combination may not be achieved.
[0060] In the above-mentioned step (I), when the two bonded substrates constituting the laminate deform so that they move away from each other, it is preferable to apply a curable adhesive composition that forms an adhesive layer with low stress when elongated by 10 mm on the side that is subjected to deformation, and a curable adhesive composition that forms an adhesive layer with high stress when elongated by 10 mm on the side that is not subjected to deformation. As already explained, by arranging adhesive layers with different moduli in parallel between the substrates and integrating them so that no gaps are formed between the adhesive layers, when the two substrates deform so that they move away from each other due to tensile forces (including, for example, external forces such as expansion, unfolding, and elongation between the substrates and the action of inflation gas), as shown in Figure 5, for example, the low-modulus adhesive layer on the deformed side deforms significantly to relieve the tensile force between the substrates, while the high-modulus adhesive layer on the non-deformed side can continue to firmly bond the substrates. This is because, even if the adhesive layer is thin, less than 1 mm, when an external force acts to move the bonded substrates away from each other, the adhesive layer as a whole can achieve high peel strength.
[0061] The amount of the curable adhesive composition applied in step (I) is preferably such that the width of the entire adhesive layer obtained by integration after step (III) is in the range of 5 to 50 mm, and in practical terms, is preferably in the range of 10 to 45 mm.
[0062] Similarly, since the laminate according to the present invention satisfies the required characteristics for compactness, it has the advantage of being able to achieve high peel strength even when the overall thickness of the adhesive layer is designed to be thin, so the amount of curable adhesive composition applied in step (I) is preferably such that the overall thickness (after curing) of the integrated adhesive layer after step (III) is 1 mm or less, and it is particularly preferable to apply an amount such that the thickness of the adhesive layer is in the range of 0.01 to 1.00 mm. Note that the thickness of the adhesive layer after curing can also be adjusted by pressing the curable adhesive compositions applied in parallel to each other to a constant thickness in step (III) described below.
[0063] Step (II) is a step of laminating a second cloth or sheet-like substrate (S2) onto the curable adhesive composition applied in step (I). On the other hand, step (III) is a step of integrating two or more types of curable adhesive compositions by contacting or pressing them together. Step (III) may be performed simultaneously with, before, after, or at any timing with step (II), as long as it is performed after step (I). Conveniently, step (III) is performed after step (II) or simultaneously with step (II), by pressing two or more types of curable adhesive compositions applied in parallel between the laminated first cloth or sheet-like substrate (S1) and second cloth or sheet-like substrate (S2), thereby integrating them so that the thickness of the adhesive layer after curing is 1 mm or less. For example, by laminating (S2) a second backing fabric or sheet-like substrate onto the curable adhesive composition applied in parallel in step (I), and then simultaneously with or after the lamination, applying pressure (for example, by crushing by hand or with a press) to the curable adhesive composition applied in parallel from one or both sides of the substrate, the curable adhesive compositions applied in parallel can be integrated without gaps, and the thickness of the adhesive layer after curing can be adjusted to the desired thinness (preferably 1 mm or less).
[0064] Step (IV) is a step of curing the integrated two or more curable adhesive compositions by a curing reaction to form an adhesive layer between (S1) the first fabric or sheet-like substrate and (S2) the second fabric or sheet-like substrate, and can be selected depending on the type of curable adhesive composition. For example, when the curable adhesive composition of the present invention is a curable silicone rubber composition that cures by a hydrosilylation reaction, the entire laminate is placed in a hot air drying oven or the like to be heat-cured, typically at a curing temperature in the range of 20°C to 200°C, preferably 90°C to 150°C, for a period of several seconds to several hours depending on the thickness of the adhesive layer and the application shape.
[0065] The laminate of the present invention may further include a functional coating layer on the surface or inner surface of the substrate constituting the laminate, preferably on both surfaces, at any time (e.g., before or after step (IV) or at the substrate stage before lamination). For example, a curable resin coating layer may be provided for the purpose of improving heat resistance, flame retardancy, and mechanical strength (e.g., tear strength), or a curable silicone rubber layer may be provided. For example, a laminate having a silicone rubber layer on the substrate surface may be formed by applying a curable silicone rubber layer to both surfaces of the laminate or substrate (e.g., a base fabric) before or after step (IV) and then placing the entire laminate in a hot air drying oven or the like to heat and cure it. The step of forming a functional coating layer on the substrate or laminate surface may be performed simultaneously with the above steps (I) to (IV). For example, the formation of the adhesive layer in step (IV) and the formation of the functional coating layer on the substrate or laminate surface may be performed simultaneously by placing the laminate in a hot air drying oven or the like. The method for forming the coating layer is not particularly limited, and any known coating method may be used, such as coating the substrate or laminate surface with a curable resin coating agent evenly and uniformly using a knife coater.
[0066] The amount of coating of the functional coating layer can be selected arbitrarily depending on the function and purpose of the coating layer. When the laminate is an airbag for a vehicle, the coating agent is applied in an amount of 35 g / m 2 With the following application amount, it is preferable that the burning rate in the combustion test FMVSS No. 302 for automobile interior materials is 80 mm / min or less.
[0067] When the laminate according to the present invention has a specific portion that is particularly subject to strong heat or tensile stress, the laminate may further include a step of attaching, at any time, a reinforcing substrate or a heat-resistant substrate for the purpose of reinforcement, damage prevention, or improving heat resistance, etc. For example, when the laminate according to the present invention is an airbag that deploys and inflates by inflation gas ejected from an inflator, the laminate may include a step of arranging a heat-resistant reinforcing fabric having a thickness of about 5 to 50 μm as a reinforcing substrate or a heat-resistant substrate in the portion of the airbag that comes into contact with the inflation gas.
[0068] Furthermore, in order to satisfy the required characteristics for compactness, the laminate of the present invention may further include a step of transforming the obtained laminate into a structure suitable for sewing, folding, storage, etc.
[0069] [Method for bonding substrates] The present invention can be widely used as a method for bonding substrates, and even if the adhesive layer is thin, when an external force acts to move the bonded substrates apart, the adhesive layer as a whole can achieve high peel strength. When used as a method for bonding substrates, the shape and thickness of the substrates are arbitrary, and the method can be used to bond any substrate, not just cloth-like or sheet-like.
[0070] Specifically, the bonding method according to the present invention comprises the following steps: Step (I'): applying two or more types of curable adhesive compositions, the stresses of which at 10 mm elongation in the stress-strain curve when cured are in the range of 2 to 5 times that of each other, onto a first substrate so that the curable adhesive compositions are parallel to each other; Step (II'): laminating a second substrate onto the curable adhesive composition applied in Step (I'); Step (III'): after Step (II') or simultaneously with Step (II'), bringing the two or more types of curable adhesive compositions into contact or pressure-bonding between the first substrate and the second substrate to integrate them; and Step (IV'): curing the two or more types of integrated curable adhesive compositions by a curing reaction to form an adhesive layer between the first substrate and the second substrate.
[0071] The above steps (I') to (IV') are steps similar to steps (I) to (IV) in the method for producing a laminate, and can be carried out in the same manner as steps (I) to (IV), except that the shapes of the first substrate and the second substrate are not limited to cloth or sheet-like substrates. In particular, when the two substrates are deformed so as to move away from each other, the above step (I') may be a coating step in which a curable adhesive composition that forms an adhesive layer with low stress when elongated by 10 mm is placed on the side that is subjected to deformation, and a curable adhesive composition that forms an adhesive layer with high stress when elongated by 10 mm is placed on the side that is not subjected to deformation, for the same reasons as explained in step (I). The curable adhesive composition that can be used in the bonding method of the present invention is also the same as above, and a curable silicone rubber composition can be preferably used.
[0072] The laminate of the present invention, its manufacturing method, and the method for bonding substrates will be described below with reference to examples. However, it goes without saying that the laminate of the present invention is not limited to the following examples, and that it is also possible to use a curable adhesive composition other than a silicone-based one.
[0073] [Measurement of stress-strain curve] A test piece having a 1 mm adhesive layer was pulled at both ends of the substrate at a tension speed of 200 mm / min using a tensile tester at 25°C and 50% RH (relative humidity) to measure its stress-strain curve, as shown in Figure 4. The measured stress (N / 50 mm) at 10 mm elongation for curable silicone rubber compositions A1, B1, A2, and B2, which show the stress-strain curves shown in Figures 5 and 7, are shown in Table 1 below. The figure numbers for the combined stress-strain curves of both compositions are also shown in the table.
[0074] Example 1 Curable silicone rubber compositions A1 and B1, each of which independently exhibits the stress-strain curve shown in Figure 5, were applied in parallel to a first backing fabric at a centerline spacing of 10 mm from a 6 mm diameter nozzle, as shown in Figure 2. A second backing fabric was then placed on top of the fabric via a 1 mm thick spacer, and compressed onto the backing fabric to integrate the applied curable silicone rubber compositions A1 / B1. This was then cured for 24 hours at 25°C and 50% RH to obtain a test piece (laminate) with an integrated adhesive layer consisting of 1 mm-thick parallel adhesive layers made of curable silicone rubber compositions A1 / B1. Note that, in applying the curable silicone rubber compositions A1 and B1, for measuring the stress-strain curve of the test piece, the curable silicone rubber composition A1, which forms a low-modulus adhesive layer, was applied to the side where a force that pushes the substrate away from the other side due to tensile stress acts, and the curable silicone rubber composition B1, which forms a high-modulus adhesive layer, was applied to the opposite side, and these adhesive layers were integrated.
[0075] As shown in Figure 6, the stress-strain curve of the adhesive layer formed by curing the curable silicone rubber compositions A1 and B1 that were applied in parallel and then integrated together had a much higher tensile stress peak value than the stress-strain curves when either adhesive layer was used alone, and the elongation (mm) giving the peak value was much longer than the yield point when either was used alone, thereby achieving high peel strength.
[0076] Example 2 A test piece (laminate) having an adhesive layer in which parallel adhesive layers each having a thickness of 1 mm and made of curable silicone rubber compositions A2 / B2 were integrated was obtained in the same manner as in Example 1, except that curable silicone rubber compositions A2 and B2, which exhibit the stress-strain curve shown in FIG. 7, were used instead of curable silicone rubber compositions A1 and B1.
[0077] As shown in Figure 8, the stress-strain curve of the adhesive layer formed by curing the curable silicone rubber compositions A2 and B2 that were applied in parallel and then integrated together had a much higher peak value of tensile stress than the stress-strain curves when either adhesive layer was used alone, and the elongation (mm) giving the peak value was much longer than the yield point when either was used alone, thereby achieving high peel strength.
[0078] Comparative Example 1 (Dot-like Application) The curable silicone rubber compositions A2 and B2, which exhibit the stress-strain curves shown in FIG. 7, were applied in dot form from a nozzle with a diameter of 2 mm over the same application area as in Example 2, instead of being applied in parallel. The same procedure was followed as in Example 2, except that a test piece (laminate) was obtained comprising an adhesive layer in which dot-like adhesive layers each 1 mm thick made of curable silicone rubber compositions A2 / B2 were applied together and integrated.
[0079] As shown in Figure 9, the stress-strain curve of the adhesive layer formed by curing the curable silicone rubber compositions A2 and B2 applied in dots and integrating the two differs from the stress-strain curve of the adhesive layer according to Example 2 shown in Figure 8 in that the elongation (mm) giving the peak value of tensile stress was smaller than that of adhesive layer B1 (alone), and the peak value of tensile stress was also lower. Therefore, it was found that even if two or more types of curable adhesive compositions whose stresses at 10 mm elongation on the stress-strain curve after curing are in the range of 2 to 5 times each other are used, when both are applied in dots, high peel strength cannot be achieved.
[0080] Comparative Example 2 (Mesh Coating) The curable silicone rubber compositions A2 and B2, which exhibit the stress-strain curves shown in FIG. 7, were coated in the same manner as in Example 2, except that instead of being coated in parallel, both compositions were coated from a nozzle with a diameter of 2 mm onto the same coating area as in Example 2 so that the two compositions intersected and formed a mesh-like pattern. A test piece (laminate) was obtained in which 1 mm-thick mesh-like adhesive layers made of curable silicone rubber compositions A2 / B2 were coated one on top of the other to form an integrated adhesive layer.
[0081] As shown in Figure 10, the stress-strain curve of the adhesive layer formed by curing the curable silicone rubber compositions A2 and B2 applied in a network pattern and integrating the two differs from the stress-strain curve of the adhesive layer according to Example 2 shown in Figure 8 in that the elongation (mm) giving the peak value of tensile stress is greater than that of adhesive layer B2 (alone), but the peak value of tensile stress is lower than not only adhesive layer B2 (alone) but also adhesive layer A2 (alone). Therefore, even if two or more types of curable adhesive compositions whose stresses at 10 mm elongation in the stress-strain curve upon curing are in the range of 2 to 5 times each other are used, it was found that high peel strength cannot be achieved when the two are applied in a network pattern in a cross-like manner rather than parallel to each other.
[0082] [Summary] As shown in Figures 6 and 8, the laminate of the present invention is formed by curing two types of curable silicone rubber compositions (A, B) that are applied in parallel and have stresses at 10 mm elongation in the stress-strain curve after curing that are in the range of 2 to 5 times that of each other, and has an adhesive layer in which the two compositions are integrated, so it was found that high peel strength can be achieved between the base fabrics even with a thin adhesive layer. On the other hand, as shown in Figure 9 (dot-like application) and Figure 10 (net-like application), if the two types of curable silicone rubber compositions (A, B) are not applied in parallel, high peel strength cannot be achieved between the base fabrics even with an adhesive layer in which the two compositions are integrated, and the technical effect of the present invention cannot be achieved.
[0083] The laminate of the present invention can achieve high peel strength even with a thin adhesive layer when an external force is applied to move the bonded substrates apart, making it possible to design compact structures and has the advantage of being able to provide laminate materials and structures that are thin and have excellent peel strength, meeting requirements for thin layering, foldability, storability, and light weight, for outdoor goods, packaging materials, protective sheets, functional films, vehicle airbags, etc. Furthermore, because the laminate does not require sewing or the provision of a thick adhesive layer, it has the advantages of being excellent in appearance and space-saving, and can be stored or stowed compactly and lightly even in a small space and used.
[0084] 1 Cloth-like base material 1 2 Cloth-like base material 2 A1 Adhesive layer A1 A2 Adhesive layer A2
Claims
1. A laminate comprising: (S1) a first cloth or sheet-like substrate; and (S2) a second cloth or sheet-like substrate, (A) formed by applying in parallel two or more types of curable adhesive compositions, the stresses of which at 10 mm elongation in the stress-strain curve when cured are in the range of 2 to 5 times that of the other composition, and bonding the two together with an integrated adhesive layer.
2. The stress F of the adhesive layer obtained by curing the curable adhesive composition having the highest tensile stress (a1) among two or more types of curable adhesive compositions constituting the adhesive layer, when elongated by 10 mm a1 (a2) the stress F when elongated by 10 mm of the adhesive layer obtained by curing the curable adhesive composition having the lowest tensile stress is in the range of 40 to 240 (N / 50 mm); a2 is in the range of 20 to 60 (N / 50 mm), and a1 / F a2 2. The laminate according to claim 1, wherein the value of [Ratio of Molecular Weight of Layer] is in the range of 2.0 to 4.
0.
3. A laminate according to claim 1 or 2, wherein when two bonded substrates constituting the laminate are deformed so as to move away from each other, a curable adhesive composition that forms an adhesive layer with low stress when elongated by 10 mm is arranged on the side that is subjected to deformation, and a curable adhesive composition that forms an adhesive layer with high stress when elongated by 10 mm is arranged on the side that is not subjected to deformation, and the adhesive layers having different stresses when elongated by 10 mm are cured to become one.
4. The laminate according to any one of claims 1 to 3, wherein the adhesive layer is an adhesive layer formed by curing two types of curable adhesive compositions, the two types of curable adhesive compositions being applied in parallel to each other and cured so as to become one body.
5. The laminate according to any one of claims 1 to 3, wherein the width of the entire integrated adhesive layer is in the range of 5 to 50 mm, and the thickness is 1 mm or less.
6. The laminate according to any one of claims 1 to 3, wherein the curable adhesive composition forming the adhesive layer is at least one elastic adhesive composition independently selected from an acrylic adhesive, a urethane adhesive, an epoxy adhesive, a vinyl acetate adhesive, a styrene-butadiene rubber adhesive, a natural rubber adhesive, and a silicone adhesive.
7. The laminate according to any one of claims 1 to 3, wherein the curable adhesive composition forming the adhesive layer is a curable silicone rubber composition containing: (A) 100 parts by mass of a diorganopolysiloxane having at least two alkenyl groups per molecule; (B) 5 to 100 parts by mass of an organopolysiloxane resin and / or inorganic filler; (C) an organopolysiloxane having at least two silicon-bonded hydrogen atoms per molecule (an amount such that the number of silicon-bonded hydrogen atoms in this component is 0.6 to 20 moles per mole of alkenyl groups in components (A) and (B) combined); and (D) a catalytic amount of a hydrosilylation catalyst.
8. A method for producing a laminate according to any one of claims 1 to 6, comprising the steps of: step (I): (S1) applying onto a first cloth or sheet-like substrate two or more types of curable adhesive compositions, the stresses of which at 10 mm elongation in a stress-strain curve when cured are within a range of 2 to 5 times that of each other, so as to be parallel to each other; step (II): laminating a second cloth or sheet-like substrate (S2) onto the curable adhesive composition applied in step (I); step (III): before step (II), after step (II), or simultaneously with step (II), bringing the two or more types of curable adhesive compositions into contact or pressing them together to integrate them; and step (IV): curing the two or more types of curable adhesive compositions that have been integrated by a curing reaction to form an adhesive layer between the first cloth or sheet-like substrate (S1) and the second cloth or sheet-like substrate (S2).
9. A method for producing a laminate according to claim 8, wherein the step (III) is a step of contacting or pressing two or more types of curable adhesive compositions applied in parallel between (S1) a first cloth or sheet-like substrate and (S2) a second cloth or sheet-like substrate, thereby integrating the two types of curable adhesive compositions so that the thickness of the adhesive layer after curing is 1 mm or less.
10. A method for producing a laminate as claimed in claim 8, wherein two bonded substrates constituting the laminate are deformed so as to move away from each other, and wherein the step (I) is a step of applying a curable adhesive composition that forms an adhesive layer with low stress when elongated by 10 mm is placed on the side that is subjected to deformation, and a curable adhesive composition that forms an adhesive layer with high stress when elongated by 10 mm is placed on the side that is not subjected to deformation, and the step (III) is a step of pressing two or more types of curable adhesive compositions applied in parallel between the bonded (S1) first cloth or sheet-like substrate and (S2) second cloth or sheet-like substrate after or simultaneously with step (II), thereby integrating them so that the thickness of the adhesive layer after curing is 1 mm or less.
11. A method for bonding substrates comprising the steps of: step (I'): applying two or more types of curable adhesive compositions onto a first substrate, the two or more types of curable adhesive compositions each having a stress at 10 mm elongation in a range of 2 to 5 times that of the other type when cured in a stress-strain curve, so that the two or more types are parallel to each other; step (II'): laminating a second substrate onto the curable adhesive composition applied in step (I'); step (III'): after step (II') or simultaneously with step (II'), bringing the two or more types of curable adhesive compositions into contact or pressure-bond between the first substrate and the second substrate to integrate them; and step (IV'): curing the two or more types of curable adhesive compositions that have been integrated by a curing reaction to form an adhesive layer between the first substrate and the second substrate.
12. A method for bonding substrates according to claim 11, wherein the two substrates are deformed so as to move away from each other, and step (I') is a step of applying a curable adhesive composition that forms an adhesive layer with low stress when elongated by 10 mm on the side that is subjected to deformation, and a curable adhesive composition that forms an adhesive layer with high stress when elongated by 10 mm on the side that is not subjected to deformation.
13. The method for producing a laminate according to claim 8 or the method for bonding substrates according to claim 11, wherein the curable adhesive composition forming the adhesive layer is a curable silicone rubber composition containing: (A) 100 parts by mass of a diorganopolysiloxane having at least two alkenyl groups per molecule; (B) 5 to 100 parts by mass of an organopolysiloxane resin and / or inorganic filler; (C) an organopolysiloxane having at least two silicon-bonded hydrogen atoms per molecule (an amount such that the number of silicon-bonded hydrogen atoms in this component is 0.6 to 20 moles per mole of alkenyl groups in components (A) and (B) combined); and (D) a catalytic amount of a hydrosilylation catalyst.
Citation Information
Patent Citations
Airbag
JP2011152913A
El light emitting element
JP2011204364A
Panel joint body
JP2015105059A
Article with stripes of pressure sensitive adhesive
JP2016526587A
Metal resin joint method
JP2019069534A