Resin composition

The resin composition for FDM 3D printing, featuring a water-soluble polyester resin and a water-insoluble resin, addresses the challenge of hazardous support material removal in FDM by using neutral water, enhancing adhesion and toughness, and improving modeling accuracy and safety.

WO2024237059A1PCT designated stage expired Publication Date: 2024-11-21KAO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016365
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-04-26
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

FDM 3D printing methods require support materials that are difficult to remove without using hazardous strong alkaline solutions, posing safety and environmental risks, and existing solutions for support material removal in FDM methods are not versatile enough to handle various modeling materials effectively.

Method used

A resin composition comprising a water-soluble polyester resin with specific monomer units and a water-insoluble resin, allowing for support material removal with neutral water, enhancing adhesion to multiple modeling materials and providing flexibility and toughness.

Benefits of technology

Enables safe and efficient removal of support materials with neutral water, improving modeling accuracy and versatility across various modeling materials while reducing environmental and safety hazards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016365_21112024_PF_FP_ABST
    Figure JP2024016365_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention is a resin composition containing the following components A and B, wherein the content mass ratio of component B to component A is 0.32 or less. According to the present invention, it is possible to provide a resin composition that serves as a material for a soluble material for three-dimensional molding, the material being removable with neutral water while being highly adhesive to many types of molding materials and being flexible and hard to break. Component A: a water-soluble polyester resin α having aromatic dicarboxylic acid monomer units A that have a hydrophilic group, dicarboxylic acid monomer units B that do not have hydrophilic groups, and diol monomer units Component B: a non-water-soluble resin β having a SP value in the range of 15 (J / cm3)1 / 2 to 25 (J / cm3)1 / 2, and a glass transition temperature in the range of 80°C to 160°C
Need to check novelty before this filing date? Find Prior Art

Description

resin composition

[0001] The present invention relates to a resin composition.

[0002] A 3D printer is a type of rapid prototyping technology that creates three-dimensional objects based on 3D data such as 3D CAD and 3D CG. Known 3D printer methods include fused deposition modeling (hereinafter also referred to as FDM), inkjet ultraviolet curing, stereolithography, and laser sintering. Among these, FDM is a modeling method in which a modeling material is heated / melted and extruded to form a layered structure to create a three-dimensional object. Polymer filaments, toner powder materials, and the like are primarily used as modeling materials, but unlike other methods, FDM does not use chemical reactions in the modeling material. Therefore, FDM 3D printers, particularly those using polymer filaments as modeling materials, are compact and inexpensive, and have become increasingly popular in recent years as devices requiring minimal post-processing. In order to create three-dimensional objects with more complex shapes using the FDM method, the forming material that constitutes the three-dimensional object and the support material that supports the three-dimensional structure of the forming material are stacked to obtain a three-dimensional object precursor, and then the support material is removed from the three-dimensional object precursor to obtain the desired three-dimensional object.

[0003] One method for removing support material from a three-dimensional object precursor is to use a methacrylic acid copolymer as the support material and immerse the three-dimensional object precursor in a hot, strong alkaline aqueous solution to remove the support material (see, for example, JP-A 2012-509777). This method utilizes the fact that the carboxylic acid in the methacrylic acid copolymer is neutralized by the alkali and dissolves in the strong alkaline aqueous solution.

[0004] However, when the methacrylic acid copolymer disclosed in JP-A-2012-509777 is used as a support material, it is necessary to use a strong alkaline aqueous solution to remove the support material from the three-dimensional object precursor, and this strong alkaline aqueous solution is dangerous to people and places a heavy burden on the environment.

[0005] To address the above-mentioned issues, Japanese Patent Application Laid-Open No. 2017-030346 discloses a soluble material for three-dimensional modeling containing a specific water-soluble polyester resin. The soluble material for three-dimensional modeling disclosed in Japanese Patent Application Laid-Open No. 2017-030346 is suitable for manufacturing three-dimensional objects using the FDM method, and provides a support material that is resistant to moisture absorption and has a high dissolution rate in neutral water, allowing it to be rapidly removed from a three-dimensional object precursor without using a strong alkaline aqueous solution.

[0006] The present invention provides a resin composition containing the following components A and B, wherein the mass ratio of the component B to the component A is 0.32 or less. Component A: A water-soluble polyester resin α having an aromatic dicarboxylic acid monomer unit A having a hydrophilic group, a dicarboxylic acid monomer unit B not having a hydrophilic group, and a diol monomer unit. Component B: A water-soluble polyester resin α having a viscosity of 15 (J / cm 3 ) 1/2 More than 25 (J / cm 3 ) 1/2 A water-insoluble resin β having an SP value within the following range and a glass transition temperature within the range of 80°C or higher and 160°C or lower.

[0007] The present invention is a soluble material for three-dimensional modeling, which contains the resin composition.

[0008] The present invention is a method for manufacturing a three-dimensional object by a fused deposition modeling method, which includes a step of obtaining a three-dimensional object precursor containing a three-dimensional object and a support material, and a support material removal step of contacting the three-dimensional object precursor with neutral water to remove the support material, wherein the material of the support material is the soluble material for three-dimensional modeling.

[0009] Schematic diagram showing the shape of a three-dimensional object precursor produced in the examples. Detailed Description of the Invention

[0010] If the adhesion between the modeling material and the support material that make up the three-dimensional object is poor, the support material will be more likely to peel off from the modeling material during modeling of the three-dimensional object using the FDM method, which could result in a decrease in the modeling accuracy of the three-dimensional object. In order to improve adhesion to the modeling material, it is possible to develop a support material that is tailored to the specific modeling material, but since there are many types of modeling materials, there is a need for a support material that is highly adhesive to a wide variety of modeling materials and is highly versatile.

[0011] In the FDM method, which uses polymer filaments as the modeling material, a filament-shaped modeling material and a soluble material for 3D modeling, which serves as a support material, are supplied to a 3D printer and layered together to form a 3D object. However, if the supplied filament breaks during modeling, the supply of material stops, resulting in a decrease in productivity and modeling accuracy. Therefore, a flexible, break-resistant filament is required.

[0012] The present invention provides a resin composition that can be used as a soluble material for three-dimensional modeling, which can be removed with neutral water, has high adhesiveness to many types of modeling materials, and is flexible and unbreakable; a soluble material for three-dimensional modeling that contains the resin composition; and a method for manufacturing a three-dimensional object using the soluble material for three-dimensional modeling.

[0013] The present invention provides a resin composition containing the following components A and B, wherein the mass ratio of the component B to the component A is 0.32 or less. Component A: A water-soluble polyester resin α having an aromatic dicarboxylic acid monomer unit A having a hydrophilic group, a dicarboxylic acid monomer unit B not having a hydrophilic group, and a diol monomer unit. Component B: A water-soluble polyester resin α having a viscosity of 15 (J / cm 3 ) 1/2 More than 25 (J / cm 3 ) 1/2 A water-insoluble resin β having an SP value within the following range and a glass transition temperature within the range of 80°C or higher and 160°C or lower.

[0014] The present invention is a soluble material for three-dimensional modeling, which contains the resin composition.

[0015] The present invention is a method for manufacturing a three-dimensional object by a fused deposition modeling method, which includes a step of obtaining a three-dimensional object precursor containing a three-dimensional object and a support material, and a support material removal step of contacting the three-dimensional object precursor with neutral water to remove the support material, wherein the material of the support material is the soluble material for three-dimensional modeling.

[0016] According to the present invention, it is possible to provide a resin composition that can be used as a soluble material for three-dimensional modeling, which can be removed with neutral water, has high adhesiveness to many types of modeling materials, and is flexible and hard to break; a soluble material for three-dimensional modeling that includes the resin composition; and a method for manufacturing a three-dimensional object using the soluble material for three-dimensional modeling.

[0017] An embodiment of the present invention will be described below.

[0018] <Resin Composition> The resin composition of the present embodiment contains the following component A and component B, and the content mass ratio of component B to component A is 0.32 or less. Component A: Water-soluble polyester resin α having an aromatic dicarboxylic acid monomer unit A having a hydrophilic group, a dicarboxylic acid monomer unit B not having a hydrophilic group, and a diol monomer unit. Component B: 15 (J / cm 3 ) 1/2 More than 25 (J / cm 3 ) 1/2 A water-insoluble resin β having an SP value within the following range and a glass transition temperature within the range of 80°C or higher and 160°C or lower.

[0019] According to the resin composition of this embodiment, it is possible to provide a resin composition that can be used as a soluble material for three-dimensional modeling, which can be removed with neutral water, has high adhesion to many types of modeling materials, is flexible, and is not easily broken.

[0020] [Component A] Component A is a water-soluble polyester resin α having an aromatic dicarboxylic acid monomer unit A having a hydrophilic group (hereinafter also simply referred to as a hydrophilic group) other than the hydrophilic group constituting the polymerization for producing the water-soluble polyester resin α, a dicarboxylic acid monomer unit B having no hydrophilic group, and a diol monomer unit. In this specification, "water-soluble" means that 1 g of the component is dissolved in 100 g of neutral water and no precipitation occurs even when the water temperature is then maintained at 20°C. "Water-insoluble" means that the component does not dissolve when 1 g is added to 100 g of neutral water, or that even if it does dissolve, precipitation occurs when the temperature is returned to 20°C.

[0021] The neutral water may be water or an aqueous solution having a pH of 6 to 8. Specific examples of the neutral water include deionized water, pure water, tap water, and industrial water. Deionized water or tap water is preferred from the viewpoint of availability. The neutral water may also contain other components such as a water-soluble organic solvent and a surfactant. Examples of the water-soluble organic solvent include lower alcohols such as methanol, ethanol, and 2-propanol; glycol ethers such as propylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monotertiary butyl ether, and diethylene glycol monobutyl ether; and ketones such as acetone and methyl ethyl ketone. Examples of the surfactant include anionic surfactants such as alkyl sulfates, alkyl ether sulfates, olefin sulfonates, and alkyl ether carboxylates; cationic surfactants such as alkyl trimethylammonium salts; and nonionic surfactants such as polyoxyethylene alkyl ethers and alkyl glycosides.

[0022] [Aromatic dicarboxylic acid monomer unit A] From the viewpoint of imparting removability with neutral water, the hydrophilic group may be one or more selected from the group consisting of a primary amino group, a secondary amino group, a tertiary amino group, a quaternary ammonium base, an oxyalkylene group, a hydroxyl group, a carboxyl group, a carboxyl group, a phosphate group, a sulfonic acid group, and a sulfonate group. Among these, from the same viewpoint, one or more selected from the group consisting of a quaternary ammonium base, an oxyalkylene group, a carboxyl group, a phosphate group, and a sulfonate group are preferred, one or more selected from the group consisting of a quaternary ammonium base, an oxyalkylene group, and a sulfonate group are more preferred, and a sulfonate group is even more preferred.

[0023] The sulfonate group is —SO 3 M 3 (However, M 3 represents a counter ion of the sulfonic acid group constituting the sulfonate group, and from the viewpoint of imparting removability with neutral water, is preferably at least one or more selected from the group consisting of sodium ion, potassium ion, lithium ion, calcium ion, magnesium ion, ammonium ion, barium ion, and zinc ion, more preferably at least one or more selected from the group consisting of sodium ion, potassium ion, lithium ion, magnesium ion, and ammonium ion, even more preferably at least one or more selected from the group consisting of sodium ion and potassium ion, and even more preferably sodium ion.

[0024] The content of the hydrophilic group in the water-soluble polyester resin α is preferably 0.2 mmol / g or more, more preferably 0.5 mmol / g or more, and even more preferably 0.7 mmol / g or more from the viewpoint of imparting removability with neutral water, and is preferably 3.0 mmol / g or less, more preferably 2.0 mmol / g or less, and even more preferably 1.5 mmol / g or less from the viewpoint of moisture resistance required for modeling using a 3D printer. Note that the content of the hydrophilic group in this specification can be determined by the method described in the Examples.

[0025] The aromatic dicarboxylic acid for deriving the aromatic dicarboxylic acid monomer unit A is preferably one or more selected from the group consisting of sulfonate group-containing aromatic dicarboxylic acids and salts thereof, from the viewpoint of imparting removability with neutral water and the viewpoint of moisture resistance required for modeling using a 3D printer. Among these, from the same viewpoint, one or more selected from the group consisting of sulfophthalic acid, sulfonaphthalenedicarboxylic acid, and salts thereof are preferred, one or more selected from the group consisting of sulfophthalic acid and salts thereof are even more preferred, one or more selected from the group consisting of sulfoisophthalic acid, sulfoterephthalic acid, and salts thereof are even more preferred, and 5-sulfoisophthalic acid or a salt thereof is even more preferred.

[0026] The proportion of the amount of the aromatic dicarboxylic acid monomer unit A to the total amount of all monomer units in the water-soluble polyester resin α is preferably 1 mol% or more, more preferably 5 mol% or more, and even more preferably 10 mol% or more from the viewpoint of imparting removability with neutral water, and is preferably 35 mol% or less, more preferably 25 mol% or less, and even more preferably 15 mol% or less from the viewpoint of moisture resistance required for modeling using a 3D printer. In this specification, the proportion of each monomer unit in the resin is calculated by the method described in the Examples.

[0027] The proportion of the aromatic dicarboxylic acid monomer unit A to the total of all dicarboxylic acid monomer units in the water-soluble polyester resin α is preferably 2 mol% or more, more preferably 10 mol% or more, and even more preferably 20 mol% or more, from the viewpoint of imparting removability with neutral water, and is preferably 75 mol% or less, more preferably 50 mol% or less, and even more preferably 30 mol% or less, from the viewpoint of moisture resistance required for modeling using a 3D printer.

[0028] [Dicarboxylic Acid Monomer Unit B] From the viewpoint of moisture resistance required for modeling using a 3D printer, the dicarboxylic acid for deriving the dicarboxylic acid monomer unit B is preferably one or more selected from the group consisting of aromatic dicarboxylic acids having no hydrophilic groups and aliphatic dicarboxylic acids having no hydrophilic groups, and more preferably one or more selected from the group consisting of aromatic dicarboxylic acids having no hydrophilic groups.

[0029] Examples of the aromatic dicarboxylic acid having no hydrophilic group include one or more selected from the group consisting of benzenedicarboxylic acid, furandicarboxylic acid, and naphthalenedicarboxylic acid. Among these, from the viewpoint of moisture resistance required for modeling using a 3D printer, one or more selected from the group consisting of terephthalic acid, isophthalic acid, and 2,6-naphthalenedicarboxylic acid are preferred.

[0030] Examples of the aliphatic dicarboxylic acid having no hydrophilic group include one or more selected from the group consisting of malonic acid, succinic acid, glutaric acid, adipic acid, 1,4-cyclohexanedicarboxylic acid, and 1,3-adamantanedicarboxylic acid. Among these, adipic acid is preferred from the viewpoint of moisture resistance required for modeling using a 3D printer.

[0031] The ratio of the amount of substance of the dicarboxylic acid monomer unit B to the total amount of substance of all monomer units in the water-soluble polyester resin α is preferably 15 mol% or more, more preferably 25 mol% or more, and even more preferably 35 mol% or more, from the viewpoint of moisture resistance required for modeling using a 3D printer, and is preferably 49 mol% or less, more preferably 45 mol% or less, and even more preferably 40 mol% or less, from the viewpoint of imparting removability with neutral water.

[0032] The ratio of the amount of substance of the dicarboxylic acid monomer unit B to the total amount of all dicarboxylic acid monomer units in the water-soluble polyester resin α is preferably 30 mol% or more, more preferably 50 mol% or more, and even more preferably 70 mol% or more, from the viewpoint of moisture resistance required for modeling using a 3D printer, and is preferably 98 mol% or less, more preferably 90 mol% or less, and even more preferably 80 mol% or less, from the viewpoint of imparting removability with neutral water.

[0033] [Diol Monomer Unit] As the diol for deriving the diol monomer unit, an aliphatic diol, an aromatic diol, or the like can be used. From the viewpoint of easy availability of raw materials for the water-soluble polyester resin, an aliphatic diol is preferred.

[0034] The number of carbon atoms in the diol is preferably 2 or more from the viewpoint of imparting removability with neutral water, and is preferably 31 or less, more preferably 25 or less, even more preferably 20 or less, and still more preferably 15 or less from the viewpoint of moisture resistance required for modeling using a 3D printer.

[0035] The aliphatic diol may be one or more selected from the group consisting of chain diols and cyclic diols, with chain diols being preferred from the viewpoint of easy availability of raw materials.

[0036] From the viewpoint of imparting removability with neutral water and the viewpoint of moisture resistance required for modeling using a 3D printer, the chain diol is preferably one or more selected from the group consisting of ethylene glycol, propanediol, butanediol, neopentyl glycol, pentanediol, hexanediol, diethylene glycol, triethylene glycol, polyethylene glycol, dipropylene glycol, and polypropylene glycol, and more preferably one or more selected from the group consisting of ethylene glycol, 1,3-propanediol, and 1,6-hexanediol.

[0037] The water-soluble polyester resin α may contain a monomer unit other than the aromatic dicarboxylic acid monomer unit A, the dicarboxylic acid monomer unit B, and the diol monomer unit, as long as the effect of this embodiment is not impaired.

[0038] The method for producing the water-soluble polyester resin α is not particularly limited, and any conventionally known method for producing a polyester resin can be applied.

[0039] The weight average molecular weight of the water-soluble polyester resin α is preferably 1,000 or more, more preferably 3,000 or more, and even more preferably 4,000 or more from the viewpoint of moisture resistance required for modeling using a 3D printer, and is preferably 100,000 or less, more preferably 80,000 or less, and even more preferably 30,000 or less from the viewpoint of imparting removability with neutral water. In this specification, the weight average molecular weight is measured by the method described in the examples.

[0040] The glass transition temperature of the water-soluble polyester resin α is preferably 0° C. or higher, more preferably 5° C. or higher, and even more preferably 10° C. or higher from the viewpoint of moisture resistance required for modeling using a 3D printer, and is preferably 200° C. or lower, more preferably 160° C. or lower, and even more preferably 120° C. or lower from the viewpoint of imparting removability with neutral water. In this specification, the glass transition temperature is measured by the method described in the examples.

[0041] The content of the water-soluble polyester resin α in the resin composition is preferably 40% by mass or more, more preferably 50% by mass or more, and even more preferably 60% by mass or more, from the viewpoint of imparting removability with neutral water, and is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less, from the viewpoint of moisture resistance required for modeling using a 3D printer.

[0042] [Component B] The component B has a viscosity of 15 (J / cm 3 ) 1/2 More than 25 (J / cm 3 ) 1/2 The water-insoluble resin β has an SP value within the following range and a glass transition temperature within the range of 80°C or higher and 160°C or lower.

[0043] The SP value of the water-insoluble resin β is set to 15 (J / cm 3 ) 1/2 or more, and 17 (J / cm 3 ) 1/2 More than 18 (J / cm 3 ) 1/2 More preferably, 19 (J / cm 3 ) 1/2 More preferably, from the same viewpoint, 25 (J / cm 3 ) 1/2 or less, and 24 (J / cm 3 ) 1/2 Preferably, 23 (J / cm 3 ) 1/2 More preferably, 22.5 (J / cm 3 ) 1/2 The following is more preferable. In this specification, the SP value is the Hansen solubility parameter. The Hansen solubility parameter can be calculated based on the chemical structure by dividing the types of interaction energy acting between the molecules of a substance into three. Specifically, the following formula can be used. δ = (δ d 2 +δ p 2 +δ h 2 ) 1/2 where δd is the London dispersion force term, δ p is the molecular polarization term, δ h is called the hydrogen bond term. A more detailed definition and calculation of the Hansen solubility parameter is described in Charles M. Hansen, Hansen Solubility Parameters: A Users Handbook, 2nd Ed., C.M. Hansen, CRC Press, Boca Raton, FL, 2007. In addition, by using the computer software Hansen Solubility Parameters in Practice (HSPiP), the Hansen solubility parameter can be easily estimated from the chemical structure of a compound for which literature values ​​are unknown.

[0044] The glass transition temperature of the water-insoluble resin β is 80° C. or higher, preferably 85° C. or higher, and more preferably 90° C. or higher, from the viewpoint of heat resistance required for modeling using a 3D printer, and is 160° C. or lower, preferably 155° C. or lower, and more preferably 150° C. or lower, from the viewpoint of low melt viscosity required to facilitate ejection during modeling using a 3D printer. In this specification, the glass transition temperature is measured by the method described in the examples.

[0045] The water-insoluble resin β is 15 (J / cm 3 ) 1/2 25 or less (J / cm 3 ) 1/2Any water-insoluble resin having an SP value within the range of 0° C. to 160° C. and a glass transition temperature within the range of 80° C. to 160° C. can be used without particular limitation. Examples of the water-insoluble resin β include one or more selected from the group consisting of polyethylene resin, polybutylene resin, polystyrene resin, polycarbonate resin, ABS resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polyamide resin, and PPS resin. From the viewpoint of improving adhesion to the molding material, more specifically, it preferably contains one or more selected from the group consisting of acrylonitrile copolymer, styrene copolymer, polyolefin resin, polyester resin, polyacrylic resin, polyamide resin, polycarbonate resin, polyphenylsulfone resin, polyether ether ketone, polyetherimide, and copolymers thereof, more preferably contains one or more selected from the group consisting of polycarbonate resin, acrylonitrile copolymer, styrene copolymer, polyolefin resin, and copolymers thereof, and even more preferably contains one or more selected from the group consisting of polycarbonate resin and ABS resin.

[0046] The content of the water-insoluble resin β in the resin composition is preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, and even more preferably 3% by mass or less, from the viewpoint of not impairing removability with neutral water, and is preferably 0.5% by mass or more, more preferably 0.7% by mass or more, and even more preferably 1.0% by mass or more, from the viewpoint of improving toughness and improving adhesion to the molding material.

[0047] The mass ratio (content mass ratio) of the content of the water-insoluble resin β to the water-soluble polyester resin α in the resin composition is 0.32 or less, preferably 0.20 or less, and more preferably 0.15 or less, from the viewpoint of not impairing removability with neutral water, and is preferably 0.015 or more, more preferably 0.02 or more, and even more preferably 0.03 or more, from the viewpoint of improving toughness and improving adhesion to the molding material.

[0048] The resin composition may contain other components within a range that does not impair the effects of this embodiment. Examples of such other components include polymers other than the water-soluble polyester resin α and the water-insoluble resin β, plasticizers such as benzoic acid polyalkylene glycol diesters, fillers such as calcium carbonate, magnesium carbonate, glass spheres, graphite, carbon black, carbon fiber, glass fiber, talc, wollastonite, mica, alumina, silica, kaolin, whiskers, and silicon carbide, viscosity reducers, compatibilizers, and elastomers.

[0049] [Viscosity Reducer] The resin composition may contain a viscosity reducer from the viewpoint of controlling the molecular weight during the production of the water-soluble polyester resin α and from the viewpoint of improving removability with neutral water. Examples of the viscosity reducer include organic salt compounds represented by the following general formula (1): (R-SO 3- ) n X n+ (1) (In the general formula (1), R represents a hydrocarbon group having 1 to 30 carbon atoms which may have a substituent, n represents the number 1 or 2, and X n+ represents a cation, and when n is 1, X n+ represents a sodium ion, a potassium ion, a lithium ion, an ammonium ion, or a phosphonium ion; when n is 2, X n+ represents a magnesium ion, a calcium ion, a barium ion, or a zinc ion.)

[0050] In the general formula (1), R represents a hydrocarbon group having 1 to 30 carbon atoms, which may have a substituent, from the viewpoint of molecular weight control during the production of the water-soluble polyester resin α and improving removability with neutral water. The hydrocarbon group may be any of an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, and an aromatic hydrocarbon group. When the hydrocarbon group is an aliphatic hydrocarbon group, the number of carbon atoms of the hydrocarbon group is preferably 1 or more, more preferably 4 or more, and even more preferably 8 or more, from the viewpoint of molecular weight control during the production of the water-soluble polyester resin α, improving removability with neutral water, and imparting heat resistance and moisture resistance to the resin composition. The number of carbon atoms is preferably 30 or less, more preferably 25 or less, and even more preferably 20 or less. When the hydrocarbon group is an alicyclic hydrocarbon group, the number of carbon atoms in the hydrocarbon group is preferably 3 or more, more preferably 5 or more, even more preferably 6 or more, still more preferably 10 or more, and preferably 30 or less, more preferably 25 or less, and still more preferably 20 or less, from the viewpoints of molecular weight control during the production of the water-soluble polyester resin α, improving removability with neutral water, and imparting heat resistance and moisture resistance to the resin composition. When the hydrocarbon group is an aromatic hydrocarbon group, the number of carbon atoms in the hydrocarbon group is preferably 6 or more, more preferably 8 or more, even more preferably 10 or more, and preferably 30 or less, and more preferably 25 or less, from the viewpoints of molecular weight control during the production of the water-soluble polyester resin α, improving removability with neutral water, and imparting heat resistance and moisture resistance to the resin composition.

[0051] Furthermore, from the viewpoint of improving removability with neutral water and imparting heat resistance and moisture resistance to the resin composition, the substituent preferably contains one or more atoms selected from the group consisting of a hydrogen atom, a carbon atom, an oxygen atom, a nitrogen atom, a sulfur atom, a phosphorus atom, a silicon atom, and a halogen atom. Among these, a hydrocarbon group or a halogenated alkyl group having 1 to 22 carbon atoms is preferred, a hydrocarbon group or a halogenated alkyl group having 1 to 16 carbon atoms is more preferred, a hydrocarbon group or a halogenated alkyl group having 1 to 12 carbon atoms is even more preferred, and a hydrocarbon group having 1 to 12 carbon atoms is even more preferred.

[0052] In the general formula (1), X n+represents a sodium ion, potassium ion, lithium ion, ammonium ion, phosphonium ion, magnesium ion, calcium ion, barium ion, zinc ion, or phosphonium ion, from the viewpoint of molecular weight control during the production of the water-soluble polyester resin α, from the viewpoint of improving removability with neutral water, and from the viewpoint of imparting heat resistance and moisture resistance to the resin composition, and is preferably a sodium ion, potassium ion, lithium ion, magnesium ion, ammonium ion, or phosphonium ion, more preferably a sodium ion, lithium ion, ammonium ion, or phosphonium ion, even more preferably a lithium ion or phosphonium ion, and even more preferably a phosphonium ion. Among the phosphonium ions, from the viewpoint of ensuring the heat resistance required during the production of the water-soluble polyester resin α, a tetraalkylphosphonium ion is preferred, and a tetrabutylphosphonium ion is more preferred.

[0053] In the general formula (1), n ​​is preferably 1 from the viewpoint of molecular weight control during the production of the water-soluble polyester resin α, improving removability with neutral water, and imparting heat resistance and moisture resistance to the resin composition.

[0054] The content of the organic salt compound in the resin composition is preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 3% by mass or more, from the viewpoint of improving removability with neutral water, and is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less, from the viewpoint of imparting heat resistance and moisture resistance to the resin composition.

[0055] [Compatibilizer] The resin composition may contain a compatibilizer from the viewpoint of improving the compatibility between the water-soluble polyester resin α and the water-insoluble resin β. Examples of the compatibilizer include the LOTRYL (registered trademark) series (manufactured by SK Functional Polymers), which is a polymer obtained by copolymerizing ethylene with butyl acrylate or methyl acrylate; Bondfast (registered trademark) 7B, Bondfast 7M, and Bondfast CG-5001 (all manufactured by Sumitomo Chemical Co., Ltd.); Lotader (registered trademark) AX8840 (manufactured by Arkema), JONCRYL (registered trademark) ADR4370S, JONCRYL ADR4368CS, JONCRYL ADR4368F, JONCRYL ADR4300S, and JONCRYL ADR4468 (all manufactured by BASF), ARUFON (registered trademark) UG4035, ARUFON Examples of such a reactive compatibilizer include reactive compatibilizers having an epoxy group, such as UG4040 and ARUFON UG4070 (manufactured by Toagosei Co., Ltd.); reactive compatibilizers having an acid anhydride group, such as UMEX (registered trademark) 1010 (manufactured by Sanyo Chemical Co., Ltd.), ADMER (registered trademark) (manufactured by Mitsui Chemicals, Inc.), MODIPER (registered trademark) A8200 (manufactured by NOF Corporation), OREVAC (registered trademark) (manufactured by Arkema), FG1901 and FG1924 (manufactured by Kraton Polymers), TUFTEC (registered trademark) M1911, TUFTEC M1913 and TUFTEC M1943 (manufactured by Asahi Kasei Chemicals Corporation); and reactive compatibilizers having an isocyanate group, such as Carbodilite LA-1 (registered trademark) (manufactured by Nisshinbo).

[0056] From the viewpoint of imparting high toughness to the resin composition, the compatibilizer preferably has a glass transition temperature of 0°C or lower, more preferably a glass transition temperature of -10°C or lower, and even more preferably a glass transition temperature of -20°C or lower; from the viewpoint of maintaining the heat resistance of the resin composition, the compatibilizer preferably has a glass transition temperature of -80°C or higher, more preferably a glass transition temperature of -60°C or higher, and even more preferably a glass transition temperature of -40°C or higher.

[0057] The content of the compatibilizer in the resin composition is preferably 0.1 mass% or more, more preferably 0.4 mass% or more, even more preferably 0.5 mass% or more, even more preferably 0.9 mass% or more, and even more preferably 1.0 mass% or more, from the viewpoint of improving the compatibility between the water-soluble polyester resin α and the water-insoluble resin β, and is preferably 25 mass% or less, more preferably 20 mass% or less, even more preferably 18 mass% or less, and even more preferably 15 mass% or less, from the viewpoint of maintaining the heat resistance of the resin composition.

[0058] [Elastomer] The resin composition may contain an elastomer from the viewpoint of moldability when formed into a filament. From the viewpoint of moldability when formed into a filament, the elastomer is preferably at least one selected from the group consisting of acrylic elastomers, olefin elastomers, styrene elastomers, polyester elastomers, urethane elastomers, polyamide elastomers, and silicone elastomers, and more preferably an acrylic elastomer. Examples of the acrylic elastomer include Kuralyte (registered trademark) LA2250, Kuralyte LA2140, and Kuralyte LA4285 (all manufactured by Kuraray Co., Ltd.). Examples of the olefin elastomer include Kraton (registered trademark) ERS polymer (manufactured by Kraton Polymers). Examples of the styrene-based elastomer include Kraton A polymer, Kraton G polymer (both manufactured by Kraton Polymers), "Tuftec H" series, "Tuftec P" series (manufactured by Asahi Kasei Chemicals Corporation), Septon (registered trademark), and Hybler (registered trademark) (both manufactured by Kuraray Plastics Co., Ltd.).

[0059] From the viewpoint of imparting high toughness to the resin composition, the elastomer preferably has a glass transition temperature of 0°C or lower, more preferably -20°C or lower, and even more preferably -40°C or lower; from the viewpoint of maintaining the heat resistance of the resin composition, the elastomer preferably has a glass transition temperature of -80°C or higher, more preferably -70°C or higher, and even more preferably -60°C or higher.

[0060] The content of the elastomer in the resin composition is preferably 0.1% by mass or more, more preferably 0.4% by mass or more, even more preferably 0.5% by mass or more, still more preferably 0.9% by mass or more, and still more preferably 1.0% by mass or more, from the viewpoint of moldability when molding into filaments; and is preferably 20% by mass or less, more preferably 10% by mass or less, and still more preferably 5% by mass or less, from the viewpoint of maintaining the heat resistance of the resin composition.

[0061] The method for producing the resin composition is not particularly limited, and the resin composition can be produced by a known method. When producing a resin composition containing a water-soluble polyester resin α, a water-insoluble resin β, and the other components, the method for producing the resin composition may be a method for producing the resin composition by kneading the other components. The kneading can be performed using a kneader such as a batch kneader or a twin-screw extruder. The kneading is preferably melt kneading.

[0062] <Soluble Material for Three-Dimensional Modeling> The resin composition may be used as a soluble material for three-dimensional modeling that is used as a material for a support material that supports a three-dimensional object when manufacturing the three-dimensional object using an FDM 3D printer. That is, the soluble material for three-dimensional modeling of the present embodiment may be a soluble material for three-dimensional modeling that includes the resin composition.

[0063] The shape of the soluble material for three-dimensional modeling is not particularly limited, and examples thereof include pellets, powder, and filaments. From the viewpoint of modeling properties using a 3D printer, the filaments are preferred.

[0064] The diameter of the filament is preferably 0.5 mm or more, more preferably 1.0 mm or more, from the viewpoint of improving the formability by a 3D printer and the precision of three-dimensional objects, and from the same viewpoint, is preferably 3.0 mm or less.

[0065] When producing a filament, it is preferable to perform a drawing process from the viewpoint of improving toughness. The draw ratio in the drawing process is preferably 1.5 times or more, more preferably 2 times or more, even more preferably 3 times or more, and even more preferably 5 times or more, from the viewpoint of improving toughness and achieving both water solubility. From the same viewpoint, it is preferably 200 times or less, more preferably 150 times or less, even more preferably 100 times or less, and even more preferably 50 times or less. Furthermore, the drawing temperature in the drawing process is preferably within a range from a temperature 20°C lower than the glass transition temperature of the soluble material for three-dimensional modeling to a temperature 110°C higher than the glass transition temperature. From the viewpoint of improving toughness and thermal stability, the lower limit of the drawing temperature is more preferably 10°C lower than the glass transition temperature, and even more preferably the same temperature as the glass transition temperature. From the same viewpoint, the upper limit of the drawing temperature is more preferably 110°C higher than the glass transition temperature, more preferably 100°C higher than the glass transition temperature, and even more preferably 90°C higher than the glass transition temperature. The stretching may be performed while air-cooling the resin after it is discharged from the extruder, or by heating with hot air or a laser. The stretching may be performed in one step to a predetermined stretch ratio and filament diameter, or in multiple steps to a predetermined stretch ratio and filament diameter.

[0066] <Method for Manufacturing a Three-Dimensional Object> The method for manufacturing a three-dimensional object according to the present embodiment is a method for manufacturing a three-dimensional object using an FDM system, which includes a step of obtaining a three-dimensional object precursor including a three-dimensional object and a supporting material, and a step of contacting the three-dimensional object precursor with neutral water to remove the supporting material, wherein the supporting material is the soluble material for three-dimensional printing. This method for manufacturing a three-dimensional object enables the manufacturing of a three-dimensional object with high modeling accuracy.

[0067] [Step of obtaining a three-dimensional object precursor including a three-dimensional object and a supporting material] The step of obtaining a three-dimensional object precursor including a three-dimensional object and a supporting material can utilize the step of obtaining a three-dimensional object precursor including a three-dimensional object and a supporting material in a known method of manufacturing a three-dimensional object using an FDM-type 3D printer, except that the material of the supporting material is the soluble material for three-dimensional modeling.

[0068] The modeling material used to produce the three-dimensional object can be any resin that is used as a modeling material in conventional FDM-based three-dimensional object manufacturing methods. Examples of such modeling materials include thermoplastic resins such as ABS resin, polylactic acid resin, polycarbonate resin, 12-nylon, 6,6-nylon, 6-nylon, polyphenylsulfone resin, polyetheretherketone, and polyetherimide. Among these, polycarbonate resin, 12-nylon, 6,6-nylon, 6-nylon, polyphenylsulfone resin, polyetheretherketone, and polyetherimide are more preferred. Furthermore, the modeling material preferably contains the water-insoluble resin β.

[0069] [Support material removal process in which a three-dimensional object precursor is brought into contact with neutral water to remove the support material] In the support material removal process, the support material is removed by bringing the three-dimensional object precursor into contact with neutral water. From the viewpoints of cost and ease of operation, the method of bringing the three-dimensional object precursor into contact with neutral water is preferably a method of immersing the three-dimensional object precursor in neutral water. From the viewpoint of improving the removability of the support material, ultrasonic waves can be irradiated during immersion to promote dissolution of the support material.

[0070] The amount of neutral water used is preferably 10 times by mass or more, and more preferably 20 times by mass or more, relative to the support material from the viewpoint of solubility of the support material, and from the viewpoint of economy, is preferably 10,000 times by mass or less, more preferably 5,000 times by mass or less, even more preferably 1,000 times by mass or less, and even more preferably 100 times by mass or less, relative to the support material.

[0071] The time for which the soluble material for three-dimensional modeling is brought into contact with neutral water is preferably 5 minutes or more from the viewpoint of removability of the support material, and is preferably 180 minutes or less, more preferably 120 minutes or less, and even more preferably 90 minutes or less from the viewpoint of reducing damage to the three-dimensional object caused by prolonged contact with neutral water and from the viewpoint of economy. The washing temperature, although it depends on the type of model material, is preferably 15°C or more, more preferably 25°C or more, even more preferably 30°C or more, and even more preferably 40°C or more from the viewpoint of removability of the support material, reducing damage to the three-dimensional object, and from the viewpoint of economy, and is preferably 85°C or less, and more preferably 70°C or less from the same viewpoint.

[0072] [Other Uses] Because the resin composition has good adhesion to various resins, it can also be used as a base layer for a print-removing layer in printed matter, an intermediate layer in a laminate film, a coating agent, a water-soluble temporary fixing agent, etc. Because the water-soluble polyester resin α is water-soluble, a printed matter printed using the resin composition as a print-removing base layer or a laminate film using the resin composition as an intermediate layer can be easily peeled off by immersing it in warm water, thereby increasing the recycling rate and efficiency.

[0073] In relation to the above-described embodiments, the present invention further discloses the following compositions, etc.

[0074] <1> A resin composition containing the following components A and B, wherein the content mass ratio of component B to component A is 0.32 or less: Component A: a water-soluble polyester resin α having an aromatic dicarboxylic acid monomer unit A having a hydrophilic group, a dicarboxylic acid monomer unit B not having a hydrophilic group, and a diol monomer unit; Component B: 15 (J / cm 3 ) 1/2 More than 25 (J / cm 3 ) 1/2 <2> The SP value of the water-insoluble resin β is 15 (J / cm 3 ) 1/2 or more, and 17 (J / cm 3 ) 1/2More than 18 (J / cm 3 ) 1/2 More preferably, 19 (J / cm 3 ) 1/2 More preferably, 25 (J / cm 3 ) 1/2 or less than 24 (J / cm 3 ) 1/2 Preferably, 23 (J / cm 3 ) 1/2 More preferably, 22.5 (J / cm 3 ) 1/2The resin composition according to <1>, wherein the following is further preferred: <3> The resin composition according to <1> or <2>, wherein the water-insoluble resin β has a glass transition temperature of 80°C or higher, preferably 85°C or higher, more preferably 90°C or higher, and is 160°C or lower, preferably 155°C or lower, more preferably 150°C or lower. <4> The water-insoluble resin β is preferably one or more selected from the group consisting of polyethylene resin, polybutylene resin, polystyrene resin, polycarbonate resin, ABS resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polyamide resin, and PPS resin, and more preferably one or more selected from acrylonitrile copolymer, styrene copolymer, polyolefin resin, polyester resin, polyacrylic resin, polyamide resin, polycarbonate resin, polyphenylsulfone resin, polyether ether ketone, polyetherimide, and copolymers thereof, and more preferably one or more selected from the group consisting of polycarbonate resin, acrylonitrile copolymer, styrene copolymer, polyolefin resin, and copolymers thereof, and more preferably one or more selected from the group consisting of ABS resin, and polycarbonate resin, and more preferably one or more selected from the group consisting of <5> The resin composition according to any one of <1> to <4>, wherein the content of the water-insoluble resin β in the resin composition is preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, still more preferably 3% by mass or less, preferably 0.5% by mass or more, more preferably 0.7% by mass or more, and still more preferably 1.0% by mass or more. <6> The resin composition according to any one of <1> to <5>, wherein the content of the water-soluble polyester resin α in the resin composition is preferably 40% by mass or more, more preferably 50% by mass or more, still more preferably 60% by mass or more, and preferably 95% by mass or less, more preferably 90% by mass or less, and still more preferably 85% by mass or less.<7> The resin composition according to any one of <1> to <6>, wherein the mass ratio (content mass ratio) of the water-insoluble resin β to the water-soluble polyester resin α in the resin composition is 0.32 or less, preferably 0.20 or less, more preferably 0.15 or less, preferably 0.015 or more, more preferably 0.02 or more, and even more preferably 0.03 or more. <8> A soluble material for three-dimensional printing, comprising the resin composition according to any one of <1> to <7>. <9> The soluble material for three-dimensional printing according to <8>, which has a filamentous shape. <10> The soluble material for three-dimensional printing according to <9>, wherein the filament has a diameter of 0.5 to 3.0 mm. <11> A method for producing a three-dimensional object, comprising: a step of obtaining a three-dimensional object precursor containing a three-dimensional object and a supporting material; and a support material removal step of contacting the three-dimensional object precursor with neutral water to remove the supporting material, wherein the material of the supporting material is the soluble material for three-dimensional modeling according to any one of <8> to <10>. <12> The method for producing a three-dimensional object according to <11>, wherein the modeling material that is the material of the three-dimensional object contains the water-insoluble resin β. <13> The method for producing a three-dimensional object according to claim <12>, wherein the water-insoluble resin β preferably comprises one or more selected from the group consisting of polyethylene resin, polybutylene resin, polystyrene resin, polycarbonate resin, ABS resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polyamide resin, and PPS resin, more preferably comprises one or more selected from acrylonitrile copolymer, styrene copolymer, polyolefin resin, polyester resin, polyacrylic resin, polyamide resin, polycarbonate resin, polyphenylsulfone resin, polyether ether ketone, polyetherimide, and copolymers thereof, further preferably comprises one or more selected from the group consisting of polycarbonate resin, acrylonitrile copolymer, styrene copolymer, polyolefin resin, and copolymers thereof, and further preferably comprises one or more selected from the group consisting of ABS resin and polycarbonate resin.

[0075] <Method for preparing water-soluble polyester resin composition> A 2 L stainless steel separable flask (equipped with a K-shaped tube, a stirrer, and a nitrogen inlet tube) was charged with 97.7 g of dimethyl 2,6-naphthalenedicarboxylate (manufactured by Tokyo Chemical Industry Co., Ltd., first grade), 40.6 g of sodium dimethyl 5-sulfoisophthalate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 76.7 g of ethylene glycol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., special grade), 82 mg of titanium tetrabutoxide (manufactured by Tokyo Chemical Industry Co., Ltd., first grade), and 506 mg of sodium acetate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., special grade), and the mixture was heated with a mantle heater at normal pressure under a nitrogen atmosphere with stirring, raising the surface temperature of the heater from 140°C to 260°C over 1 hour, and then stirred at that temperature for 6 hours and 30 minutes to carry out a transesterification reaction. Next, 6.89 g of dodecylbenzenesulfonate tetrabutylphosphonium salt (Elecut S-418, manufactured by Takemoto Yushi Co., Ltd.) was added and stirred for 15 minutes. The surface temperature of the heater was then raised from 260 to 290°C over 30 minutes to allow the reaction to proceed. The reaction was then continued with stirring while gradually increasing the pressure to 100 Pa, yielding a water-soluble polyester resin composition containing water-soluble polyester resin α. It was assumed that excess ethylene glycol was distilled out of the reaction system, and that the diol unit and dicarboxylic acid unit reacted in equal amounts. The contents of water-soluble polyester resin α and dodecylbenzenesulfonate tetrabutylphosphonium salt contained in the water-soluble polyester resin composition, calculated from the amounts of raw materials added, are shown in Table 1. The ratios of aromatic dicarboxylic acid monomer unit A and dicarboxylic acid monomer unit B relative to the total of all dicarboxylic acid monomer units of water-soluble polyester resin α contained in the water-soluble polyester resin composition, as well as the weight-average molecular weight and hydrophilic group content, are shown in Table 2. The ratios of aromatic dicarboxylic acid monomer unit A and dicarboxylic acid monomer unit B were calculated from the amounts charged.

[0076]

[0077]

[0078] [Weight-average molecular weight (Mw)] A calibration curve was prepared from standard polystyrene using gel permeation chromatography (GPC) under the following conditions, and the weight-average molecular weight (Mw) was determined. Apparatus: HLC-8320 GPC (Tosoh Corporation, detector integrated type) Column: α-M × 2 (Tosoh Corporation, 7.8 mm I.D. × 30 cm) Eluent: 60 mmol / L phosphoric acid + 50 mmol / L lithium bromide dimethylformamide solution Flow rate: 1.0 mL / min Column temperature: 40°C Detector: RI detector Standard material: polystyrene

[0079] <Preparation of Resin Composition (Support Material)> Using a Labo Plastmill (Labo Plastmill 4C150 manufactured by Toyo Seiki Seisaku-sho, Ltd.), the raw materials were melt-kneaded under conditions of 230°C / 90 rpm / 10 min so as to obtain the compositions shown in Table 3, thereby obtaining Resin Compositions 1 to 5.

[0080] <Preparation of Filaments> Each of the resin compositions 1 to 5 was melted at a barrel temperature of 200°C using a Capillograph (Capillograph 1D manufactured by Toyo Seiki Seisaku-sho, Ltd.), extruded at an extrusion rate of 15 mm / min from a capillary having a diameter of 2.0 mm and a length of 10 mm, and wound up to a diameter of 1.7 mm to prepare a filament.

[0081] <Evaluation Method> [SP Value] The SP value was determined by the Hansen solubility parameter. The Hansen solubility parameter was calculated based on the chemical structure by dividing the types of interaction energy acting between the molecules of a substance into three. Specifically, the following formula was used: δ = (δ d 2 +δ p 2 +δ h 2 ) 1/2 where δ d is the London dispersion force term, δ p is the molecular polarization term, δ hmeans the hydrogen bond term, and the detailed definition and calculation of the Hansen solubility parameters were based on the description in Charles M. Hansen, Hansen Solubility Parameters: A Users Handbook, 2nd Ed., C.M. Hansen, CRC Press, Boca Raton, FL, 2007.

[0082] [Glass transition temperature] 25 to 10 mg of sample was precisely weighed and sealed in an aluminum pan. Using a DSC device (DSC7020 manufactured by Seiko Instruments Inc.), the sample was heated from 30°C to 230°C at a rate of 10°C / min, and then cooled to 30°C at a cooling rate of 150°C / min. The sample was again heated to 230°C at a rate of 10°C / min, and the glass transition temperature (°C) was determined from the resulting DSC curve. The results are shown in Table 3.

[0083] [Evaluation of Toughness] Measurement was carried out by a breaking elongation tensile test using a tension and compression tester (manufactured by Shimadzu Corporation, trade name "Autograph AGS-X"). A 10 cm filament was set with a support distance of 50 mm, and measurement was carried out at a crosshead speed of 10 mm / min to examine the breaking elongation (%). A high value of breaking elongation indicates high toughness. Five points were tested per sample, and the average value was taken as the measured value. The evaluation results are shown in Table 3.

[0084] [Adhesion to Modeling Material] Each filament of Resin Compositions 1 to 5 was supplied to an FDM 3D printer (FUNMAT PRO 410, manufactured by INTAMSYS) and extruded from a heat nozzle having a temperature of 250°C to form a three-dimensional object precursor 1 having the shape shown in Figure 1, containing the modeling material listed in Table 3. The three-dimensional object precursor 1 has a box-shaped three-dimensional object 11 with external dimensions of 24.0 mm in length, 25.0 mm in width, and 14.0 mm in height, and a rectangular parallelepiped support material 12 with external dimensions of 20 mm in length, 21 mm in width, and 10 mm in height. The three-dimensional object 11 is made of a modeling material, and the support material 12 is made of a resin composition. Three-dimensional object precursor 1 was modeled twice using each of the combinations of resin compositions 1 to 5 and the modeling materials listed in Table 3. The results were evaluated as follows: ○ (same as above) if the model was properly modeled both times; △ (same as above) if the model was properly modeled once and not properly modeled once due to insufficient adhesion; × (same as above) if the model was not properly modeled both times. The evaluation results are shown in Table 3.

[0085]

Claims

1. A resin composition comprising the following components A and B, in which the mass ratio of the component B to the component A is 0.32 or less. Component A: Water-soluble polyester resin α having an aromatic dicarboxylic acid monomer unit A having a hydrophilic group, a dicarboxylic acid monomer unit B not having a hydrophilic group, and a diol monomer unit. Component B: 15 (J / cm 3 ) 1/2 More than 25 (J / cm 3 ) 1/2 A water-insoluble resin β having an SP value within the following range and a glass transition temperature within the range of 80° C. or more and 160° C. or less.

2. The resin composition according to claim 1, wherein the water-insoluble resin β comprises at least one resin selected from the group consisting of ABS resin and polycarbonate resin.

3. A resin composition according to claim 1 or 2, wherein the content of the water-insoluble resin β is 20 mass% or less.

4. A soluble material for three-dimensional modeling, comprising the resin composition according to any one of claims 1 to 3.

5. The soluble material for three-dimensional fabrication according to claim 4, which is in the form of a filament.

6. The soluble material for three-dimensional fabrication according to claim 5, wherein the filament has a diameter of 0.5 to 3.0 mm.

7. A method for producing a three-dimensional object, comprising a step of obtaining a three-dimensional object precursor containing a three-dimensional object and a supporting material, and a supporting material removal step of contacting the three-dimensional object precursor with neutral water to remove the supporting material, wherein the material of the supporting material is a soluble material for three-dimensional modeling according to any one of claims 4 to 6.

8. The method for producing a three-dimensional object according to claim 7, wherein a modeling material which is a material for the three-dimensional object contains the water-insoluble resin β.

9. The method for producing a three-dimensional object according to claim 8, wherein the water-insoluble resin β includes at least one resin selected from the group consisting of ABS resin and polycarbonate resin.

Citation Information

Patent Citations

  • Use of polyvinyl alcohol and low polarity polymer blends as support structures in 3D printing

    JP2019531214A

  • Resin composition

    JP2020172639A

  • Antistatic heat-resistant polycarbonate resin composition

    JP5080017B2

  • Antistatic polycarbonate resin composition