Process oil for rubbers

The use of a poly-internal olefin-based process oil with specific DBP and carbon number ranges addresses the insufficient processability of conventional paraffin oils, enhancing the compatibility and handling of rubber materials in tire applications.

WO2024237190A1PCT designated stage expired Publication Date: 2024-11-21KAO CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017379
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-05-10
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Conventional paraffin oils do not sufficiently improve the processability of rubber materials used in applications like automobile tires.

Method used

A process oil for rubber containing a poly-internal olefin, where the olefin has an average DBP value of 3.0 or more and 6.0 or less, and an average carbon number of 16 or more and 20 or less, is used to enhance processability.

Benefits of technology

The poly-internal olefin-based process oil significantly improves the processability of rubber materials, offering better compatibility, reduced torque during kneading, and improved handling characteristics compared to conventional paraffin oils.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

The present invention relates to a process oil for rubbers which includes a poly(internal olefin), wherein the poly(internal olefin) is a polymer of one or more olefins including an internal olefin. The olefins have an average DBP value of 3.0-6.0. The average number of carbon atoms of the olefins is 16-20. The present invention can provide a process oil for rubbers which is superior in processability improvement to conventional paraffin oils.
Need to check novelty before this filing date? Find Prior Art

Description

Rubber process oil

[0001] The present invention relates to a process oil for rubber.

[0002] Rubber materials used in automobile tires and the like are blended with extender oils, process oils, etc., for the purpose of improving processability, etc. It is known that paraffin oil is used as a process oil (for example, JP-A-10-25370).

[0003] The present invention relates to a process oil for rubber containing a polyinternal olefin, wherein the polyinternal olefin is an olefin polymer containing an internal olefin, the olefin having an average DBP value of 3 or more and 6 or less, and the olefin having an average carbon number of 16 or more and 20 or less. Detailed Description of the Invention

[0004] Conventional paraffin oils did not sufficiently improve processability, and there was room for improvement.

[0005] An object of the present invention is to provide a process oil for rubber which is superior in improving processability compared to conventional paraffin oils.

[0006] The present invention relates to a process oil for rubber containing a polyinternal olefin, wherein the polyinternal olefin is an olefin polymer containing an internal olefin, the olefin having an average DBP value of 3 or more and 6 or less, and the olefin having an average carbon number of 16 or more and 20 or less.

[0007] According to the present invention, it is possible to provide a process oil for rubber which is superior in improving processability compared to conventional paraffin oils.

[0008] An embodiment of the present invention will be described below.

[0009] <Rubber Process Oil> The rubber process oil of this embodiment is a rubber process oil containing a polyinternal olefin, wherein the polyinternal olefin is an olefin polymer containing an internal olefin, the olefin having an average DBP value of 3.0 or more and 6.0 or less, and the olefin having an average carbon number of 16 or more and 20 or less. The rubber process oil of this embodiment is superior to conventional paraffin oils in improving processability.

[0010] [Internal Polyolefin] The average DBP value (average value of double bond positions) in the olefin containing the internal olefin is 3.0 or more, preferably 3.2 or more, more preferably 3.4 or more, and even more preferably 3.8 or more, from the viewpoint of lowering the pour point, and is 6.0 or less, preferably 5.5 or less, more preferably 5.0 or less, and even more preferably 4.5 or less, from the viewpoint of reducing torque during kneading. In this specification, the average DBP value in the olefin is measured by the method described in the Examples.

[0011] The average carbon number of the olefin containing the internal olefin is 16 or more, preferably 17 or more, and more preferably 18 or more, from the viewpoint of compatibility with the rubber material, and from the same viewpoint, is 20 or less, and more preferably 18 or less.

[0012] From the viewpoint of safety in the working environment, the flash point of the polyinternal olefin is preferably 250° C. or higher, more preferably 260° C. or higher. The flash point of the polyinternal olefin is 300° C. or lower. In this specification, the flash point means a flash point measured in accordance with JIS K 2265.

[0013] The pour point of the polyinternal olefin is preferably −35° C. or higher, more preferably −30° C. or higher, and even more preferably −20° C. or higher, from the viewpoint of compatibility with rubber materials, and is preferably 0° C. or lower, more preferably −10° C. or lower, from the viewpoint of handling. In this specification, the pour point means the pour point measured in accordance with JIS K 2269.

[0014] The kinematic viscosity of the polyinternal olefin at 100°C is set to 40 mm from the viewpoint of compatibility with rubber materials. 2 / s or more is preferable, and 45 mm 2 / s or more is more preferable, and 50 mm 2 / s or more is more preferable, and from the viewpoint of handling, 75 mm 2 / s or less is preferable, and 70 mm 2 / s or less is more preferable, and 65 mm 2 In this specification, the kinematic viscosity refers to a kinematic viscosity measured in accordance with JIS K 2283.

[0015] The kinematic viscosity of the polyinternal olefin at 40°C is 7.0 mmHg from the viewpoint of compatibility with rubber materials. 2 / s or more is preferable, and 7.5 mm 2 / s or more is more preferable, and 8.2 mm 2 / s or more is more preferable, and from the viewpoint of handling, 14.0 mm 2 / s or less is preferable, and 12.0 mm 2 / s or less is more preferable, and 10.5 mm 2 / s or less is more preferable.

[0016] The density of the polyinternal olefin at 25°C is 0.7 g / cm3 from the viewpoint of compatibility with rubber materials. 3 More than 0.8 g / cm 3 More preferably, from the viewpoint of handling, 0.95 g / cm 3 Preferably, 0.90 g / cm or less 3 The following is more preferred: In this specification, the density at 25°C means the pour point measured in accordance with JIS K 2249-1.

[0017] The polyinternal olefin can be obtained by polymerizing an olefin containing the internal olefin by a known method. From the viewpoint of plasticization performance, the content of the internal olefin in the olefin containing the internal olefin is preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 100% by mass. The polyinternal olefin may be hydrogenated.

[0018] From the viewpoint of plasticizing performance, the content of the polyinternal olefin in the rubber process oil is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, still more preferably substantially 100% by mass, and even more preferably 100% by mass. In this specification, "substantially 100% by mass" refers to a state in which a trace amount of impurities and the like is inevitably contained.

[0019] The rubber composition of the present embodiment contains the above-described rubber process oil as a process oil. The rubber contained in the rubber composition preferably contains a conjugated diene rubber from the viewpoints of moldability, heat resistance, abrasion resistance, and mechanical strength of the rubber molded article.

[0020] Examples of the conjugated diene rubber include butadiene rubber (BR), styrene-butadiene rubber (SBR), natural rubber (NR), isoprene rubber (IR), acrylonitrile-butadiene rubber (NBR), styrene-butadiene-isoprene rubber (SBIR), styrene-isoprene rubber (SIR), styrene-isoprene-butadiene rubber (SIBR), hydrogenated butadiene rubber, and hydrogenated styrene-butadiene rubber. Of these, preferred is natural rubber and styrene-butadiene rubber. That is, the rubber process oil may be one or more conjugated diene rubber process oils selected from the group consisting of natural rubber and styrene-butadiene rubber.

[0021] The content of the polyinternal olefin in the rubber composition is preferably 0.2% by mass or more, more preferably 5% by mass or more, from the viewpoint of plasticization performance, and is preferably 40% by mass or less, more preferably 30% by mass or less, from the viewpoint of suppressing bleed-out.

[0022] The rubber composition may further contain various reinforcing agents, fillers, vulcanization accelerators, vulcanization aids, etc., which are used in the rubber industry.

[0023] The rubber composition can be produced by a known method for producing a rubber composition, except that the rubber process oil is used.

[0024] <Rubber Molded Article> The rubber molded article of the present embodiment is obtained by crosslinking the rubber composition. The rubber molded article can be produced by crosslinking the rubber composition by a known method.

[0025] The rubber molded article can be suitably used for various applications, for example, as a material for various tire parts such as a cap tread, a base tread, a carcass, a sidewall, and a bead portion, as well as a material for hoses, belts, mats, anti-vibration rubber, paints, and various other industrial products.

[0026] In relation to the above-described embodiment, the present invention further discloses the following compositions, etc.

[0027] <1> A rubber process oil containing a polyinternal olefin, wherein the polyinternal olefin is a polymer of an olefin containing an internal olefin, the olefin having an average DBP value of 3.0 or more and 6.0 or less, and the olefin having an average carbon number of 16 or more and 20 or less. <2> The rubber process oil according to <1>, wherein the olefin containing the internal olefin has an average DBP value (average value at double bond positions) of 3.0 or more, preferably 3.2 or more, more preferably 3.4 or more, even more preferably 3.8 or more, and 6.0 or less, preferably 5.5 or less, more preferably 5.0 or less, and even more preferably 4.5 or less. <3> The rubber process oil according to <1> or <2>, wherein the olefin containing the internal olefin has an average carbon number of 16 or more, preferably 17 or more, more preferably 18 or more, and 20 or less, more preferably 18 or less. <4> The rubber process oil according to any one of <1> to <3>, wherein the polyinternal olefin has a flash point of preferably 250° C. or higher, more preferably 260° C. or higher, and 300° C. or lower. <5> The rubber process oil according to any one of <1> to <4>, wherein the polyinternal olefin has a pour point of preferably −35° C. or higher, more preferably −30° C. or higher, even more preferably −20° C. or higher, and preferably 0° C. or lower, and more preferably −10° C. or lower. <6> The polyinternal olefin has a kinematic viscosity at 100° C. of 40 mm 2 / s or more is preferable, and 45 mm 2 / s or more is more preferable, and 50 mm 2 / s or more is more preferable, and 75 mm 2 / s or less is preferable, and 70 mm 2 / s or less is more preferable, and 65 mm 2<7> The process oil for rubber according to any one of <1> to <5>, wherein the kinematic viscosity at 40°C of the polyinternal olefin is 7.0 mm / s or less. 2 / s or more is preferable, and 7.5 mm 2 / s or more is more preferable, and 8.2 mm 2 / s or more is more preferable, and 14.0 mm 2 / s or less is preferable, and 12.0 mm 2 / s or less is more preferable, and 10.5 mm 2 <8> The process oil for rubber according to any one of <1> to <6>, wherein the density of the polyinternal olefin at 25°C is 0.7 g / cm or less. 3 More than 0.8 g / cm 3 More preferably, 0.95 g / cm 3 Preferably, 0.90 g / cm or less 3 The rubber process oil according to any one of <1> to <7>, wherein the following is more preferred: <9> The rubber process oil according to any one of <1> to <8>, wherein the content of the internal olefin in the olefin-containing internal olefin is preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 100% by mass. <10> The rubber process oil according to any one of <1> to <9>, wherein the content of the polyinternal olefin in the rubber process oil is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably substantially 100% by mass, and even more preferably 100% by mass. <11> The rubber process oil according to any one of <1> to <10>, wherein the rubber process oil is a process oil for one or more conjugated diene rubbers selected from the group consisting of natural rubber and styrene-butadiene rubber. <12> A rubber composition containing the rubber process oil according to any one of <1> to <11>. <13> The rubber composition according to <12>, wherein the content of the polyinternal olefin in the rubber composition is preferably 0.2% by mass or more, more preferably 5% by mass or more, and preferably 40% by mass or less, more preferably 30% by mass or less. <14> A rubber molded article obtained by crosslinking the rubber composition according to <12> or <13>.

[0028] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. Various measurement and evaluation methods are as follows.

[0029] <Measurement Method> [Method for Measuring Olefin Double Bond Distribution] The olefin double bond distribution was measured by gas chromatography (hereinafter abbreviated as GC). Specifically, olefins were reacted with dimethyl disulfide to form dithiolated derivatives, and then each component was separated by GC. The olefin double bond distribution was determined from each peak area. The equipment and analytical conditions used for the measurement are as follows. GC equipment: Product name HP6890 (manufactured by Hewlett-Packard) Column: Product name Ultra-Alloy-1HT capillary column 30 m x 250 μm x 0.15 μm (manufactured by Frontier Labs) Detector: Hydrogen flame ionization detector (FID) Injection temperature: 300°C Detector temperature: 350°C Oven: 60°C (0 min) → 2°C / min → 225°C → 20°C / min → 350°C → 350°C (5.2 min)

[0030] [Method of calculating average DBP value (average value of double bond positions)] For example, when the double bond distribution is a% by mass at C1, b% by mass at C2, c% by mass at C3, d% by mass at C4, e% by mass at C5, f% by mass at C6, g% by mass at C7, h% by mass at C8, and i% by mass at C9 (total 100% by mass), the average DBP value is calculated from (1×a+2×b+3×c+4×d+5×e+6×f+7×g+8×h+9×i) / 100. When multiple peaks overlap, the area is equally allocated to each peak to calculate the average DBP value.

[0031] [Method for measuring the content ratio of structural isomers] 0.05 g of alkyl glyceryl ether, 0.2 g of trifluoroacetic anhydride, and 1 g of deuterated chloroform were mixed, 1Measurement was carried out by H-NMR under the following measurement conditions: Nuclear magnetic resonance apparatus: Agilent 400-MR DD2, manufactured by Agilent Technologies, Inc. Observation range: 6410.3 Hz Data points: 65536 Measurement mode: Presat Pulse width: 45° Pulse delay time: 10 sec Number of accumulations: 128

[0032] [Various Physical Properties of Polyinternal Olefin] [Density at 25° C.] Measured in accordance with JIS K 2249-1.

[0033] [Kinematic Viscosity] The kinematic viscosity was evaluated using a Stabinger kinematic viscometer (SVM3000, manufactured by Anton Paar) that met the accuracy requirements of ASTM D7042, and was measured at 40°C and 100°C (mm 2 / s) was measured.

[0034] [Pour Point] Measured in accordance with JIS K 2269.

[0035] [Flash Point] The flash point was measured according to JIS K 2265 by the Cleveland open cup (COC) method.

[0036] <Production Example of Olefin Containing Internal Olefin> [Production Example of Olefin 1 Containing an Internal Olefin of 18 Carbons] 7,000 g (25.9 mol) of 1-octadecanol (Kalcol 8098, manufactured by Kao Corporation) as the raw material alcohol and 700 g (10% by mass based on the raw material alcohol) of γ-alumina (STREM Chemicals, Inc.) as the solid acid catalyst were charged into a flask equipped with a stirrer, and the reaction was carried out for 10 hours at 280°C while flowing nitrogen (7 L / min) through the system under stirring. After completion of the reaction, the alcohol conversion was 100%, and the C18 internal olefin purity was 98.2%. The obtained crude C18 internal olefin was transferred to a distillation flask and distilled at 148-158°C / 0.5 mmHg to obtain an olefin containing a C18 internal olefin (Olefin 1) with an olefin purity of 100%. The double bond distribution of the obtained olefin 1 was 0.8% by mass at C1, 31.3% by mass at C2, 22.9% by mass at C3, 15.5% by mass at C4, 10.8% by mass at C5, 7.2% by mass at C6, 5.3% by mass at C7, and 6.2% by mass in total at C8 and C9. The average DBP value was about 3.8.

[0037] [Production Example of Olefin 2 Containing a Carbon Number 16 Internal Olefin] 7,000 g (28.9 mol) of 1-hexadecanol (Kalcol 6098, manufactured by Kao Corporation) as the raw material alcohol and 700 g (10% by mass based on the raw material alcohol) of γ-alumina (STREM Chemicals, Inc.) as the solid acid catalyst were charged into a flask equipped with a stirrer, and the reaction was carried out for 5 hours at 280°C while flowing nitrogen (7 L / min) through the system under stirring. After completion of the reaction, the alcohol conversion rate was 100%, and the C16 internal olefin purity was 99.7%. The obtained crude C16 internal olefin was transferred to a distillation flask and distilled at 136-160°C / 4.0 mmHg to obtain an olefin containing a C16 internal olefin (Olefin 2) with an olefin purity of 100%. The double bond distribution of the obtained olefin 2 was 0.5% by mass at C1, 16.5% by mass at C2, 15.4% by mass at C3, 16.4% by mass at C4, 17.2% by mass at C5, 14.2% by mass at C6, and 19.8% by mass in total at C7 and C8. The average DBP value was about 4.7.

[0038] <Production Examples of Polyinternal Olefins> [Production Example of Polyinternal Olefin 1] A reactor equipped with a stirrer was charged with 2.21 mol of the olefin 1 and 0.11 mol of aluminum chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a catalyst, and the mixture was stirred at 120°C for 10 hours under a nitrogen atmosphere to carry out a reaction. Subsequently, 88 g of a 15% by mass aqueous solution of sodium hydroxide was added and stirred to deactivate the catalyst, followed by washing with water. Further, light components were removed at 180°C and 5 torr (gauge pressure), yielding polyinternal olefin 1.

[0039] [Production Example of Hydrogenated Polyinternal Olefin 1] 2207 g of the polyinternal olefin 1 and 225 g of a nickel catalyst (manufactured by Nikko Rica Corporation) were charged into a reactor equipped with a stirrer, and the mixture was reacted for 10 hours with stirring at a rotation speed of 600 rpm under a hydrogen flow rate of 5.0 L / min, a pressure of 2.0 MPa, and conditions of 200° C. Then, the catalyst was removed by filtration to obtain hydrogenated polyinternal olefin 1.

[0040] [Production Example of Polyinternal Olefin 2] Polyinternal olefin 2 was prepared in the same manner as in the production of polyinternal olefin 1, except that olefin 2 was used instead of olefin 1 as a raw material.

[0041] [Production Example of Hydrogenated Polyinternal Olefin 2] 2,448 g of polyinternal olefin 2 and 50 g of nickel catalyst (manufactured by Nikko Rica Corporation) were loaded into a reactor equipped with a stirrer, and the reaction was carried out for 18 hours with stirring at a rotation speed of 600 rpm, a hydrogen flow rate of 5.0 L / min, a pressure of 2.0 MPa, and 200°C. Thereafter, the catalyst was removed by filtration, and hydrogenated polyinternal olefin 2 was obtained.

[0042] Various physical properties of the polyinternal olefins and the like are shown in Table 1. In Table 1, Oil 1 and Oil 2 have the following meanings: Oil 1: naphthenic process oil, manufactured by Nippon Sun Oil Co., Ltd., trade name: SUNTHENE 410 Oil 2: paraffinic oil, manufactured by EXXONMOBIL, trade name: PAO8

[0043]

[0044] <Production Examples of Rubber Compositions and Rubber Molded Articles> Components other than zinc oxide, sulfur, and vulcanization accelerator shown in Table 2 were mixed in the formulation shown in Table 2 using a Banbury mixer (Toyo Seiki Co., Ltd., Labo Plastomill 10C100, capacity 600 cc) at a rotation speed of 70 rpm and a maximum temperature of 150°C for 4 minutes (Mixing 1), to obtain kneaded materials according to each Example and Comparative Example. Zinc oxide, sulfur, and vulcanization accelerator were added to each kneaded material, and the mixture was kneaded for 2 minutes at a maximum temperature of 100°C, to obtain unvulcanized rubber compositions according to each Example and Comparative Example. The obtained unvulcanized rubber compositions were heated at 145°C for 20 minutes to obtain sheet-shaped vulcanized rubber molded articles according to each Example and Comparative Example.

[0045] <Evaluation Method> [Evaluation of Processability] The torque at the end of kneading in Kneading 1 was measured, and the torque was expressed as a relative value, with the comparative example corresponding to each example being set at 100. Specifically, the values ​​of Examples 1 to 4 were expressed as relative values ​​to comparative example 1, and the values ​​of Examples 5, 6 and comparative example 3 were expressed as relative values ​​to comparative example 2. The smaller the value, the better the processability. The evaluation results are shown in Table 2.

[0046]

[0047] The symbols in Table 2 have the following meanings: SBR: emulsion-polymerized styrene-butadiene rubber, manufactured by Nippon Zeon Co., Ltd., trade name: NIPOL 1502, styrene content: 23.5% by mass Natural rubber: RSS #3 Oil 1: naphthenic process oil, manufactured by Nippon Sun Oil Co., Ltd., trade name: SUNTHENE 410 Oil 2: paraffinic oil, manufactured by EXXONMOBIL, trade name: PAO8 Silica: Tosoh Silica Corporation, trade name: Nipsil AQ, BET specific surface area: 205 m 2 / g Carbon black: HAF, manufactured by Tokai Carbon Co., Ltd., product name: Seast 3, DBP absorption capacity 101 cm 3 / 100g, N 2 AS: 79m 2 / g Silane coupling agent: bis(3-triethoxysilylpropyl)tetrasulfide, manufactured by Evonik, trade name: Si69 Antioxidant: N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., trade name: Nocrac 6C Stearic acid: manufactured by Kao Corporation, trade name: Lunac S-70V Zinc oxide: manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd., zinc oxide (primary grade) Sulfur: manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd., sulfur (powder, chemical grade) Vulcanization accelerator 1: sulfenamide-based vulcanization accelerator, N-cyclohexyl-2-benzothiazolyl sulfenamide, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., trade name: Noccela CZ-G Vulcanization accelerator 2: guanidine-based vulcanization accelerator, 1,3-diphenylguanidine, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., trade name: Noccela D

Claims

1. A rubber process oil containing a polyinternal olefin, wherein the polyinternal olefin is an olefin polymer containing an internal olefin, the olefin has an average DBP value of 3.0 or more and 6.0 or less, and the olefin has an average carbon number of 16 or more and 20 or less.

2. The rubber process oil according to claim 1, wherein the content of said polyinternal olefin in said rubber process oil is 70 mass% or more.

3. The rubber process oil according to claim 1 or 2, wherein the pour point of the polyinternal olefin is from -35°C to 0°C.

4. The rubber process oil according to any one of claims 1 to 3, wherein the rubber process oil is a process oil for one or more conjugated diene rubbers selected from the group consisting of natural rubber and styrene-butadiene rubber.

5. A rubber composition containing the rubber process oil according to any one of claims 1 to 4.

6. The rubber composition according to claim 5, wherein the content of the polyinternal olefin in the rubber composition is 0.2 mass % or more and 40 mass % or less.

7. A rubber molded article obtained by crosslinking the rubber composition according to claim 5 or 6.

Citation Information

Patent Citations

  • Lubricant base oil

    JP2023173003A

  • Synthetic lubricant basestocks and methods of preparation thereof

    US20140087984A1

  • Additive for rubber

    WO2020241765A1