Method for producing tetrafunctional thiol with episulfide resin as starting material

By converting episulfide resin into tetrafunctional thiol through a reaction with a polythiol compound and radical initiator, the method addresses the environmental concerns of lens manufacturing waste, enabling the reuse of episulfide resin and reducing waste disposal issues.

WO2024237221A1PCT designated stage expired Publication Date: 2024-11-21MITSUBISHI GAS CHEM CO INC
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017552
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-18
Filing Date
2024-05-13
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

The disposal of episulfide resin waste from the manufacturing of optical lenses poses environmental concerns and lacks effective reuse methods, with existing processes involving burning or burying, which is unsustainable.

Method used

A method involving heating episulfide resin with a polythiol compound in the presence of a radical initiator to produce tetrafunctional thiol, allowing for the reuse of episulfide resin as a starting material and reducing waste disposal.

Benefits of technology

This method effectively recycles episulfide resin, reducing environmental burden by converting it into a reusable tetrafunctional thiol that can be used in lens production or as a cleaning agent, thereby minimizing waste and promoting sustainable practices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017552_21112024_PF_FP_ABST
    Figure JP2024017552_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a method for producing a tetrafunctional thiol having a structure represented by formula (1), said method comprising a step for heating an episulfide resin and a polythiol compound in the presence of a radical initiator to produce a tetrafunctional thiol having a structure represented by formula (1). (In the formula, m represents an integer of 0-4, and n represents an integer of 0-2.)
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing tetrafunctional thiol using episulfide resin as starting material

[0001] The present invention relates to a method for producing a tetrafunctional thiol using an episulfide resin as a starting material.

[0002] Plastic lenses are lightweight, highly tough, and easily dyeable. The specific properties required of plastic lenses include low specific gravity, high transparency, and low yellowness, as well as optical properties such as a high refractive index, a high Abbe number, high heat resistance, and high strength. A high refractive index allows for thinner lenses, and a high Abbe number reduces chromatic aberration. In recent years, many organic compounds containing sulfur atoms have been reported with the aim of achieving a high refractive index and a high Abbe number. Among these, polyepisulfide compounds containing sulfur atoms are known to have a good balance between refractive index and Abbe number (Patent Document 1). Furthermore, because polyepisulfide compounds can react with various compounds, compositions containing various compounds have been proposed to improve their physical properties (Patent Documents 2 to 5).

[0003] Optical lenses containing episulfide resins are manufactured by cutting molded articles containing episulfide resins, and a large amount of cutting powder is generated as waste during this process. Furthermore, in the process of manufacturing molded articles containing episulfide resins, defective molded products or defective processed products may also be generated. Until now, such waste has simply been incinerated or buried as industrial waste, raising concerns about its impact on the environment. Furthermore, with the recent increase in environmental concern, there has been a demand for a technology that allows waste materials to be reused as starting materials, rather than simply being discarded.

[0004] Japanese Patent Laid-Open No. 09-110979 Japanese Patent Laid-Open No. 10-298287 Japanese Patent Laid-Open No. 2001-002783 Japanese Patent Laid-Open No. 2001-131257 Japanese Patent Laid-Open No. 2002-122701

[0005] An object of the present invention is to provide a technology for effectively utilizing and reusing episulfide resins, which have been treated as waste up until now.

[0006] In view of these circumstances, the present inventors have conducted extensive research and found that, according to the present invention described below, a tetrafunctional thiol can be produced using an episulfide resin as a starting material, and that episulfide resin that has previously been disposed of as waste can be reused. That is, the present invention is as follows: <1> A method for producing a tetrafunctional thiol having a structure represented by the following formula (1), comprising a step of heating an episulfide resin and a polythiol compound in the presence of a radical initiator to produce a tetrafunctional thiol having a structure represented by the following formula (1): (wherein m represents an integer of 0 to 4, and n represents an integer of 0 to 2.) <2> The method for producing a tetrafunctional thiol according to the above <1>, wherein the episulfide resin is obtained by polymerizing and curing a composition for optical materials containing an episulfide compound represented by the following formula (2): (wherein m represents an integer of 0 to 4, and n represents an integer of 0 to 2.) <3> The method for producing a tetrafunctional thiol according to the above <2>, wherein the content of the compound represented by formula (2) in the composition for optical materials is 40 to 99.999 mass%. <4> The method for producing a tetrafunctional thiol according to the above <2> or <3>, wherein the composition for optical materials further contains a polythiol compound. <5> The method for producing a tetrafunctional thiol according to any one of the above <2> to <4>, wherein the composition for optical materials further contains sulfur. <6> The method for producing a tetrafunctional thiol according to any one of the above <2> to <5>, wherein the composition for optical materials further contains a polyisocyanate compound. <7> The method for producing a tetrafunctional thiol according to any one of the above <1> to <6>, wherein the radical initiator is at least one selected from the group consisting of an azo compound, an organic peroxide, and a dihalogen. <8> The method for producing a tetrafunctional thiol according to any one of <1> to <7> above, wherein the polythiol compound is at least one selected from the group consisting of polythiol compounds having two or more functional thiol groups. <9> A composition for optical materials containing a tetrafunctional thiol obtained by the method for producing a tetrafunctional thiol according to any one of <1> to <8> above. <10> An optical material obtained by polymerizing and curing the composition for optical materials according to <9> above. <11> An optical lens comprising the optical material according to <10> above.

[0007] According to the present invention, a tetrafunctional thiol can be produced using an episulfide resin, which has previously been disposed of as waste, as a starting material. The tetrafunctional thiol produced by the present invention can be reused as a raw material for episulfide resin or as a cleaning agent for tanks during the production of eyeglass lenses.

[0008] [Method for producing tetrafunctional thiol using episulfide resin as a starting material] The method for producing a tetrafunctional thiol according to the present invention is a method for producing a tetrafunctional thiol having a structure represented by the following formula (1), and includes a step of heating an episulfide resin and a polythiol compound in the presence of a radical initiator to react the episulfide resin with the polythiol compound to produce the tetrafunctional thiol. In the formula, m represents an integer of 0 to 4, and preferably an integer of 0 to 1. In the formula, n represents an integer of 0 to 2, and preferably an integer of 0 to 1.

[0009] According to the production method of the present invention, a tetrafunctional thiol can be produced using an episulfide resin as a starting material. The reason why such an effect is achieved is presumed to be as follows. In the production method of the present invention, a polythiol compound reacts with a radical initiator, and the radical active species generated therein react with the episulfide resin, and this reaction chemically decomposes the episulfide resin, resulting in the production of a tetrafunctional thiol as a decomposition product of the episulfide resin.

[0010] The episulfide resin is preferably recovered at any stage from the manufacturing process of eyeglass lenses to the disposal process of eyeglasses. This makes it possible to reuse the episulfide resin, which is a material for eyeglass lenses. In the present invention, the episulfide resin produced in at least one of these processes is used as a starting material, and this episulfide resin and a polythiol compound are heated in the presence of a radical initiator to react with each other, thereby obtaining a tetrafunctional thiol, which is a decomposition product of the episulfide resin.

[0011] As described above, in the method for producing a tetrafunctional thiol of the present invention, an episulfide resin that would otherwise be discarded is used to produce the tetrafunctional thiol, thereby making it possible to reduce the amount of episulfide resin discarded by incineration, and as a result, it becomes possible to significantly reduce the burden on the environment.

[0012] (Episulfide Resin) The episulfide resin is a starting material in the production method according to the present invention. The episulfide resin is not particularly limited, and examples thereof include episulfide resins described in known documents such as JP-A-09-110979 and JP-A-10-298287.

[0013] The episulfide resin used in the present invention can preferably be one obtained by polymerizing and curing a composition for optical materials containing a compound represented by formula (2) as a polymerizable compound. Specific examples of the compound of formula (2) include episulfides such as bis(β-epithiopropyl)sulfide, bis(β-epithiopropyl)disulfide, bis(β-epithiopropylthio)methane, 1,2-bis(β-epithiopropylthio)ethane, 1,3-bis(β-epithiopropylthio)propane, and 1,4-bis(β-epithiopropylthio)butane. The compound of formula (2) may be used alone or in combination of two or more. Among these, preferred compounds are bis(β-epithiopropyl)sulfide (n=0 in formula (2)) and bis(β-epithiopropyl)disulfide (m=0, n=1 in formula (2)), and the most preferred compound is bis(β-epithiopropyl)sulfide (n=0 in formula (2)). The content of the compound represented by formula (2) in the composition for optical materials is preferably 40 to 99.999 mass%, more preferably 50 to 99.995 mass%, and particularly preferably 60 to 99.99 mass%.

[0014] The episulfide resin used in the present invention may contain a polythiol compound as a polymerizable compound in the composition for optical materials in order to improve the color tone of the resulting resin when heated. The content of the polythiol compound is typically 1 to 25% by mass, preferably 2 to 25% by mass, and particularly preferably 5 to 20% by mass, relative to 100% by mass of the total composition for optical materials. If the content of the polythiol compound is less than 1% by mass, yellowing may occur during lens molding, and if it exceeds 25% by mass, heat resistance may decrease. The polythiol compounds used in the present invention may be used alone or in combination of two or more types.

[0015] Specific examples thereof include methanedithiol, methanetrithiol, 1,2-dimercaptoethane, 1,2-dimercaptopropane, 1,3-dimercaptopropane, 2,2-dimercaptopropane, 1,4-dimercaptobutane, 1,6-dimercaptohexane, bis(2-mercaptoethyl)ether, bis(2-mercaptoethyl)sulfide, 1,2-bis(2-mercaptoethyloxy)ethane, 1,2-bis(2-mercaptoethylthio)ethane, 2,3-dimercapto-1-propanol, 1,3-dimercapto-2-propanol, 1,2 ,3-trimercaptopropane, 2-mercaptomethyl-1,3-dimercaptopropane, 2-mercaptomethyl-1,4-dimercaptobutane, 2-(2-mercaptoethylthio)-1,3-dimercaptopropane, 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 2,4-dimercaptomethyl-1,5-dimercapto-3-thiapentane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane , 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 1,1,1-tris(mercaptomethyl)propane, tetrakis(mercaptomethyl)methane, ethylene glycol bis(2-mercaptoacetate), ethylene glycol bis(3-mercaptopropionate), diethylene glycol bis(2-mercaptoacetate), diethylene glycol bis(3-mercaptopropionate), 1,4-butanediol bis(2-mercaptoacetate), 1,4-butanediol bis(3-mercaptopropionate) thioglycolate), trimethylolpropane tris-mercaptopropionate, trimethylolpropane tris-mercaptopropionate, pentaerythritol tetrakis-thioglycolate, pentaerythritol tetrakis-mercaptopropionate, 1,2-dimercaptocyclohexane, 1,3-dimercaptocyclohexane, 1,4-dimercaptocyclohexane, 1,3-bis(mercaptomethyl)cyclohexane, 1,4-bis(mercaptomethyl)cyclohexane, 2,5-dimercaptomethyl-1,4-dithiane, 2,5-dimercaptomethyl-1,4-dithiane, 2,5-bis(2-mercaptoethylthiomethyl)-1,4-dithiane, 2,5-dimercaptomethyl-1-thiane, 2,5-dimercaptoethyl-1-thiane, 2,5-dimercaptomethylthiophene, 1,2-dimercaptobenzene, 1,3-dimercaptobenzene, 1,4-dimercaptobenzene, 1,3-bis(mercaptomethyl)benzene, 1,4-bis(mercaptomethyl)benzene, 2,2'-dimercaptobiphenyl, 4,4'-dimercaptobiphenyl, bis(4-mercaptophenyl)methane, 2,2-bis(4-mercaptomethyl)methane Examples of suitable mercaptomethylphenyl compounds include 2,2-bis(4-mercaptophenyl)propane, bis(4-mercaptophenyl)ether, bis(4-mercaptophenyl)sulfide, bis(4-mercaptophenyl)sulfone, bis(4-mercaptomethylphenyl)methane, 2,2-bis(4-mercaptomethylphenyl)propane, bis(4-mercaptomethylphenyl)ether, bis(4-mercaptomethylphenyl)sulfide, 2,5-dimercapto-1,3,4-thiadiazole, 3,4-thiophenedithiol, and 1,1,3,3-tetrakis(mercaptomethylthio)propane. Among these, preferred specific examples include bis(2-mercaptoethyl) sulfide, 2,5-dimercaptomethyl-1,4-dithiane, 1,3-bis(mercaptomethyl)benzene, 1,4-bis(mercaptomethyl)benzene, 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and 5,7-dimercaptomethyl-1,11-dimercapto. 1,3,4-Trimethyl-1,4-dithiane, 4-mercaptomethyl-1,8-dimercapto-3,6,9-trithiaundecane, 1,1,3,3-tetrakis(mercaptomethylthio)propane, pentaerythritol tetrakis(mercaptopropionate), pentaerythritol tetrakis(thioglycolate), trimethylolpropane tris(thioglycolate), trimethylolpropane tris(mercaptopropionate), and more preferably bis(2-mercaptoethyl)sulfide, 2,5-bis(2-mercaptomethyl)-1,4-dithiane, 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 1,3-bis(mercaptomethyl)benzene, pentaerythritol tetrakismercaptopropionate, pentaerythritol tetrakisthioglycolate, and the most preferred compounds are bis(2-mercaptoethyl)sulfide, 2,5-dimercaptomethyl-1,4-dithiane, and 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane.

[0016] The episulfide resin used in the present invention may contain a polyisocyanate compound as a polymerizable compound in the composition for optical materials in order to improve the strength of the resulting resin. The content of the polyisocyanate compound is typically 1 to 25% by mass, preferably 2 to 25% by mass, and particularly preferably 5 to 20% by mass, relative to 100% by mass of the total composition for optical materials. If the content of the polyisocyanate compound is less than 1% by mass, the strength may decrease, and if it exceeds 25% by mass, the color tone may deteriorate. The polyisocyanate compound used in the present invention may be used alone or in combination of two or more types. Specific examples thereof include diethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, cyclohexane diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane, 1,4-bis(isocyanatemethyl)cyclohexane, isophorone diisocyanate, 2,6-bis(isocyanatemethyl)decahydronaphthalene, lysine triisocyanate, tolylene diisocyanate, o-tolidine diisocyanate, diphenylmethane diisocyanate, diphenyl ether diisocyanate, 3-(2'-isocyanatecyclohexyl)propyl isocyanate, isopropylidenebis(cyclohexyl isocyanate), 2,2'-bis(4-isocyanatephenyl)propane, triisocyanate, methyl ... Phenylmethane triisocyanate, bis(diisocyanatolyl)phenylmethane, 4,4',4''-triisocyanato-2,5-dimethoxyphenylamine, 3,3'-dimethoxybenzidine-4,4'-diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 4,4'-diisocyanatobiphenyl, 4,4'-diisocyanato-3,3'-dimethylbiphenyl, dicyclohexylmethane-4,4'-diisocyanate, 1,1'-methylenebis(4-isocyanatobenzene), 1,1'-methylenebis(3-methyl-4-isocyanatobenzene), m-xylylene diisocyanate, p-xylylene diisocyanate, m-tetramethylxylylene diisocyanate, p-tetramethylxylylene diisocyanate, 1,Examples of such isocyanate include 3-bis(2-isocyanate-2-propyl)benzene, 2,6-bis(isocyanatemethyl)naphthalene, 1,5-naphthalene diisocyanate, bis(isocyanatemethyl)tetrahydrodicyclopentadiene, bis(isocyanatemethyl)dicyclopentadiene, bis(isocyanatemethyl)tetrahydrothiophene, bis(isocyanatemethyl)norbornene, bis(isocyanatemethyl)adamantane, thiodiethyl diisocyanate, thiodipropyl diisocyanate, thiodihexyl diisocyanate, bis[(4-isocyanatemethyl)phenyl]sulfide, 2,5-diisocyanate-1,4-dithiane, 2,5-diisocyanatemethyl-1,4-dithiane, 2,5-diisocyanatemethylthiophene, dithiodiethyl diisocyanate, and dithiodipropyl diisocyanate.

[0017] However, the polyisocyanate compound used in the present invention is not limited to these, and these may be used alone or in combination of two or more. Preferred examples among these include isophorone diisocyanate, tolylene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, m-xylylene diisocyanate, p-xylylene diisocyanate, m-tetramethylxylylene diisocyanate, p-tetramethylxylylene diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, 1,4-bis(isocyanatomethyl)cyclohexane, bis(isocyanatomethyl)norbornene, and 2,5- At least one compound selected from diisocyanatemethyl-1,4-dithiane is used. Among these, preferred compounds are isophorone diisocyanate, tolylene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane, and m-xylylene diisocyanate, and most preferred compounds are isophorone diisocyanate, m-xylylene diisocyanate, and 1,3-bis(isocyanatemethyl)cyclohexane.

[0018] Furthermore, the ratio of SH groups in the polythiol compound to NCO groups in the polyisocyanate compound, i.e., [number of SH groups in the polythiol compound / number of NCO groups in the polyisocyanate compound] (SH groups / NCO groups), is preferably 1.0 to 2.5, more preferably 1.25 to 2.25, and even more preferably 1.5 to 2.0. If the ratio is below 1.0, the lens may turn yellow during molding, and if it exceeds 2.5, heat resistance may decrease.

[0019] The episulfide resin used in the present invention may contain sulfur as a polymerizable compound in the composition for optical materials in order to improve the refractive index of the resulting resin. The sulfur content is typically 0.1 to 15% by mass, preferably 0.2 to 10% by mass, and particularly preferably 0.3 to 5% by mass, based on 100% by mass of the total composition for optical materials. The sulfur used in the present invention may be in any form. Specifically, sulfur may be finely divided sulfur, colloidal sulfur, precipitated sulfur, crystalline sulfur, sublimated sulfur, or the like, with finely divided sulfur being preferred. The sulfur used in the present invention may be produced by any method. Examples of sulfur production methods include sublimation refining from natural sulfur ores, mining of sulfur buried underground by melting, and recovery methods using hydrogen sulfide obtained from the desulfurization process of petroleum or natural gas, among others. Any method is acceptable. The particle size of the sulfur used in the present invention is preferably smaller than 10 mesh, i.e., the sulfur is in the form of a fine powder smaller than 10 mesh. If the particle size of sulfur is larger than 10 mesh, it is difficult for the sulfur to completely dissolve. The particle size of sulfur is more preferably smaller than 30 mesh, and most preferably smaller than 60 mesh. The purity of sulfur used in the present invention is preferably 98% or more, more preferably 99.0% or more, even more preferably 99.5% or more, and most preferably 99.9% or more. When the purity of sulfur is 98% or more, the color tone of the obtained optical material is more improved compared to when it is less than 98%.

[0020] (Radical initiator) The radical initiator used in the present invention functions as a radical generator that induces a reaction between the episulfide resin and the polythiol compound. There are no particular limitations on the radical initiator used in the present invention, but it is preferably at least one selected from the group consisting of azo compounds, organic peroxides, and dihalogens, and more preferably an azo compound that is easy to handle. In the present invention, the amount of the radical initiator used is preferably 1 to 100 parts by mass, more preferably 5 to 50 parts by mass, and most preferably 8 to 25 parts by weight, based on 100 parts by mass of the episulfide resin used.

[0021] More preferred specific examples of the radical initiator include 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(imidazolin-2-yl)propane]disulfate dihydrate, 2,2'-azobis[2-(imidazolin-2-yl)propane], 2,2'-azobis Examples of suitable azo compounds include 2,2'-azobis(2-methylpropionamidine) dihydrochloride, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] n-hydrate, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2'-azobis[N-(2-propenyl)-2-methylpropionamide], 2,2'-azobis(N-butyl-2-methylpropionamide), 2,2'-azobis(isobutyrate) dimethyl, and 4,4'-azobis(4-cyanovaleric acid), as well as organic peroxides such as di-tert-butyl peroxide, dibenzoyl peroxide, and dicumyl peroxide. Among these, a more preferred example is 2,2'-azobis(isobutyronitrile) (AIBN).

[0022] (Polythiol Compound) The polythiol compound functions as a reactant with the episulfide resin. The polythiol compound used in the present invention may be used alone or in a mixture of two or more types. In the present invention, the amount of polythiol used is preferably 100 to 5,000 parts by mass, more preferably 200 to 2,000 parts by mass, and most preferably 500 to 1,500 parts by weight, based on 100 parts by mass of the episulfide resin used.

[0023] Specific examples of the polythiol compound used in the present invention include methanedithiol, methanetrithiol, 1,2-dimercaptoethane, 1,2-dimercaptopropane, 1,3-dimercaptopropane, 2,2-dimercaptopropane, 1,4-dimercaptobutane, 1,6-dimercaptohexane, bis(2-mercaptoethyl)ether, bis(2-mercaptoethyl)sulfide, 1,2-bis(2-mercaptoethyloxy)ethane, 1,2-bis(2-mercaptoethylthio)ethane, 2,3-dimercapto-1-propanol, 1 ...-1-propanol, 1,4-dimercapto-1-propanol, 1,4-dimercapto-1-propanol, 1,4-dimercapto-1-propanol, 1,4-dimercapto-1-propanol, 1,4-dimercapto-1- mercapto-2-propanol, 1,2,3-trimercaptopropane, 2-mercaptomethyl-1,3-dimercaptopropane, 2-mercaptomethyl-1,4-dimercaptobutane, 2-(2-mercaptoethylthio)-1,3-dimercaptopropane, 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 2,4-dimercaptomethyl-1,5-dimercapto-3-thiapentane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto -3,6,9-trithiaundecane, 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 1,1,1-tris(mercaptomethyl)propane, tetrakis(mercaptomethyl)methane, ethylene glycol bis(2-mercaptoacetate), ethylene glycol bis(3-mercaptopropionate), diethylene glycol bis(2-mercaptoacetate), diethylene glycol bis(3-mercaptopropionate), 1,4-butanediol bis(2-mercaptoacetate), 1,4-butanediol tetrakis(mercaptopropionate), trimethylolpropane tris(thioglycolate), trimethylolpropane tris(mercaptopropionate), pentaerythritol tetrakis(thioglycolate), pentaerythritol tetrakis(mercaptopropionate), 1,2-dimercaptocyclohexane, 1,3-dimercaptocyclohexane, 1,4-dimercaptocyclohexane, 1,3-bis(mercaptomethyl)cyclohexane, 1,4-bis(mercaptomethyl)cyclohexane, 2,5-dimercaptomethyl-1,4-dithiane, 2,5-dimercaptomethyl-1,4-dithiane, 2,5-bis(2-mercaptoethylthiomethyl)-1,4-dithiane, 2,5-dimercaptomethyl-1-thiane, 2,5-dimercaptoethyl-1-thiane, 2,5-dimercaptomethylthiophene, 1,2-dimercaptobenzene, 1,3-dimercaptobenzene, 1,4-dimercaptobenzene, 1,3-bis(mercaptomethyl)benzene, 1,4-bis(mercaptomethyl)benzene, 2,2'-dimercaptobiphenyl, 4,4'-dimercaptobiphenyl, bis(4-mercaptophenyl)methane, 2,2- Examples of such compounds include bis(4-mercaptophenyl)propane, bis(4-mercaptophenyl)ether, bis(4-mercaptophenyl)sulfide, bis(4-mercaptophenyl)sulfone, bis(4-mercaptomethylphenyl)methane, 2,2-bis(4-mercaptomethylphenyl)propane, bis(4-mercaptomethylphenyl)ether, bis(4-mercaptomethylphenyl)sulfide, 2,5-dimercapto-1,3,4-thiadiazole, 3,4-thiophenedithiol, and 1,1,3,3-tetrakis(mercaptomethylthio)propane. Among these, preferred specific examples include bis(2-mercaptoethyl)sulfide, 2,5-dimercaptomethyl-1,4-dithiane, 1,3-bis(mercaptomethyl)benzene, 1,4-bis(mercaptomethyl)benzene, 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 5,7-dimercaptomethyl-1,11- dimercapto-3,6,9-trithiaundecane, 1,1,3,3-tetrakis(mercaptomethylthio)propane, pentaerythritol tetrakismercaptopropionate, pentaerythritol tetrakisthioglycolate, trimethylolpropane tristhioglycolate), trimethylolpropane trismercaptopropionate, more preferably bis(2-mercaptoethyl)sulfide, 2,5-bis(2-mercaptomethyl)-1,4-dithiane, 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 1,3-bis(mercaptomethyl)benzene, pentaerythritol tetrakismercaptopropionate, pentaerythritol tetrakisthioglycolate, and the most preferred compounds are bis(2-mercaptoethyl)sulfide, 2,5-dimercaptomethyl-1,4-dithiane, and 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane.

[0024] The use of the tetrafunctional polythiol as the target product is not particularly limited. The tetrafunctional thiol as the target product can be used, for example, in the production of episulfide resin. Specific uses of the tetrafunctional thiol as the target product include tetrafunctional thiols for the production of optical materials (e.g., eyeglass lenses). It can also be used as a tank cleaner in eyeglass lens production.

[0025] (Method for Producing Tetrafunctional Thiol) The method for producing a tetrafunctional thiol of the present invention includes a step of heating an episulfide resin and a polythiol compound in the presence of a radical initiator. To cite one example of a production example, an episulfide resin and a polythiol compound are mixed, a radical initiator is added thereto, and the mixture is stirred at a temperature of preferably 80 to 120°C (more preferably 90 to 110°C) for preferably 2 to 10 hours (more preferably 4 to 8 hours). The resulting liquid is extracted with ethyl acetate and water, and the organic layer is concentrated. A column treatment of the resulting concentrated liquid can produce a tetrafunctional thiol having a structure represented by formula (1) above.

[0026] The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The episulfide resin used can be one recovered in at least one of the processes of manufacturing eyeglass lenses, manufacturing eyeglasses, and disposing of eyeglasses, but an episulfide resin prepared by oneself can also be used.

[0027] <Preparation of episulfide resin powder A> (1) Step: 68 parts by mass of bis(β-epithiopropyl)sulfide represented by the structural formula below, 25 parts by mass of sulfur, and 1.3 parts by mass of 2-(2-hydroxy-5-t-octylphenyl)-2H-benzotriazole as an ultraviolet absorber were added to a reactor and stirred at 60°C until dissolved. Subsequently, 0.5 parts by mass of 2-mercapto-1-methylimidazole was added as a pre-reaction catalyst to this mixed solution, and a pre-reaction was carried out at 60°C for 50 minutes, followed by cooling to 20°C. The reaction solution obtained here is referred to as pre-reaction solution A. Step (2): Separately from the step (1), 7 parts by mass of bis(2-mercaptoethyl) sulfide represented by the following structural formula, 0.2 parts by mass of dibutyltin dichloride as a reaction adjuster, and 0.03 parts by mass of triethylbenzylammonium chloride as a curing catalyst were mixed at 20°C to prepare a homogeneous solution A. Step (3): 7 parts by mass of the homogeneous solution A obtained in Step (2) was added to 100 parts by mass of the preliminary reaction solution A obtained in Step (1) above, mixed, and degassed for 80 minutes at 20°C under a reduced pressure of 20 Torr to obtain a composition A for optical materials. Step (4): The composition A for optical materials obtained in Step (3) above was filtered through a PTFE (polytetrafluoroethylene) filter with a pore size of 1 μm and poured into a lens mold consisting of two glass plates and tape, with a mold diameter of 75 mm and a center thickness of 5 mm. After pouring, the composition A for optical materials in the mold was gradually heated from 10°C to 60°C over 30 hours, held at 60°C for 7 hours, then heated to 100°C over 4 hours, and held at 100°C for 4 hours to polymerize and harden. After cooling, the mixture was released from the mold to obtain a cured optical material. The obtained optical material was ground with a cutting machine to obtain an episulfide resin powder A.

[0028] <Preparation of Episulfide Resin Powder B> Step (1): 79 parts by mass of bis(β-epithiopropyl)sulfide represented by the structural formula above, 14 parts by mass of sulfur, and 1.3 parts by mass of 2-(2-hydroxy-5-t-octylphenyl)-2H-benzotriazole as an ultraviolet absorber were added to a reactor and stirred at 60°C until dissolved. Subsequently, 0.5 parts by mass of 2-mercapto-1-methylimidazole was added as a pre-reaction catalyst to this mixture, and a pre-reaction was carried out at 60°C for 50 minutes, followed by cooling to 20°C. The reaction liquid obtained here is referred to as pre-reaction liquid B. Step (2): Separately from step (1), 7 parts by mass of bis(2-mercaptoethyl)sulfide represented by the structural formula above, 0.2 parts by mass of dibutyltin dichloride as a reaction adjuster, and 0.03 parts by mass of triethylbenzylammonium chloride as a curing catalyst were mixed at 20°C to obtain a homogeneous solution B. Step (3): 7 parts by mass of the homogeneous solution B obtained in Step (2) was added to 100 parts by mass of the preliminary reaction solution B obtained in Step (1) above, mixed, and degassed for 80 minutes at 20°C under a reduced pressure of 20 Torr to obtain a composition for optical materials B. Step (4): The composition for optical materials B obtained in Step (3) above was filtered through a PTFE (polytetrafluoroethylene) filter with a pore size of 1 μm and poured into a lens mold consisting of two glass plates and tape, with a mold diameter of 75 mm and a center thickness of 5 mm. After pouring, the composition for optical materials B in the mold was gradually heated from 10°C to 60°C over 30 hours, held at 60°C for 7 hours, then heated to 100°C over 4 hours, and held at 100°C for 4 hours to polymerize and harden. After cooling, the mixture was released from the mold to obtain a cured optical material. The obtained optical material was cut with a cutting machine to obtain an episulfide resin powder B.

[0029] Example 1 1 g of the episulfide resin powder A obtained above was mixed with 10 g of bis(2-mercaptoethyl) sulfide represented by the structural formula above, and 0.1 g of azodiisobutyronitrile AIBN was added as a radical initiator, followed by stirring at 100°C for 5 hours. The resulting transparent liquid was extracted with ethyl acetate and water, and the organic layer was concentrated. The resulting concentrated liquid was subjected to a column treatment to obtain 433 mg of bis(2,3-dimercaptopropyl) sulfide represented by the structural formula below. The NMR results of the obtained compound, measured using deuterated chloroform, are shown below. 1 H-NMR (500 MHz, CHLOROFORM-D) δ3.14-3.11 (2H), 2.97-2.87 (8H), 2.07-2.04 (2H), 1.66-1.625 (2H)

[0030] Example 2 1 g of the episulfide resin powder B obtained above was mixed with 10 g of bis(2-mercaptoethyl) sulfide represented by the structural formula above, and 0.1 g of azodiisobutyronitrile AIBN was added as a radical initiator, followed by stirring at 100°C for 5 hours. The resulting transparent liquid was extracted with ethyl acetate and water, and the organic layer was concentrated. The resulting concentrated liquid was subjected to a column treatment to obtain 433 mg of bis(2,3-dimercaptopropyl) sulfide represented by the structural formula above.

[0031] Comparative Example 1 1 g of the episulfide resin powder A obtained above was mixed in 10 g of ethylene glycol, and 0.1 g of azodiisobutyronitrile (AIBN) was added thereto as a radical initiator. The mixture was stirred at 100° C. for 5 hours, but the reaction did not proceed, and the episulfide resin powder was recovered as it was.

[0032]

[0033] As shown in Table 1, in Examples 1 and 2 in which the episulfide resin and the polythiol compound were heated in the presence of a radical initiator to cause the episulfide resin to react with the polythiol compound, bis(2,3-dimercaptopropyl) sulfide, a tetrafunctional thiol with excellent purity, was obtained. In contrast, in Comparative Example 1 in which the episulfide resin was reacted with ethylene glycol, the decomposition reaction did not proceed.

Claims

1. A method for producing a tetrafunctional thiol having a structure represented by the following formula (1), comprising the step of heating an episulfide resin and a polythiol compound in the presence of a radical initiator to produce a tetrafunctional thiol having a structure represented by the following formula (1): (In the formula, m represents an integer of 0 to 4, and n represents an integer of 0 to 2.) 2. The method for producing a tetrafunctional thiol according to claim 1, wherein the episulfide resin is obtained by polymerizing and curing a composition for optical materials containing an episulfide compound represented by the following formula (2): (In the formula, m represents an integer of 0 to 4, and n represents an integer of 0 to 2.) 3. The method for producing a tetrafunctional thiol according to claim 2, wherein the content of the compound represented by formula (2) in the composition for optical materials is 40 to 99.999 mass %.

4. The method for producing a tetrafunctional thiol according to claim 2 or 3, wherein the composition for optical materials further contains a polythiol compound.

5. The method for producing a tetrafunctional thiol according to any one of claims 2 to 4, wherein the composition for optical materials further contains sulfur.

6. The method for producing a tetrafunctional thiol according to any one of claims 2 to 5, wherein the composition for optical materials further contains a polyisocyanate compound.

7. A method for producing a tetrafunctional thiol described in any one of claims 1 to 6, wherein the radical initiator is at least one selected from the group consisting of an azo compound, an organic peroxide, and a dihalogen.

8. A method for producing a tetrafunctional thiol according to any one of claims 1 to 7, wherein the polythiol compound is at least one selected from the group of polythiol compounds having two or more functional thiol groups.

9. A composition for optical materials containing a tetrafunctional thiol obtained by the method for producing a tetrafunctional thiol according to any one of claims 1 to 8.

10. An optical material obtained by polymerizing and curing the composition for optical materials according to claim 9.

11. An optical lens comprising the optical material according to claim 10.

Citation Information

Patent Citations

  • Still picture recorder and image pickup optical system

    JP1990098287A

  • New linear alkyl sulfide type episulfide compound

    JP1997110979A

  • Novel resin for optical material

    JP1998298287A

  • Composition for optical material

    JP2001002783A

  • Composition for resin

    JP2001131257A