Methane adsorbing material and methane adsorbing device

A methane adsorbent and adsorption device utilizing materials with a specific formula and structure effectively address the need for efficient methane adsorption, surpassing existing technologies in capacity and application.

WO2024237307A1PCT designated stage expired Publication Date: 2024-11-21MURATA MFG CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018123
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-18
Filing Date
2024-05-16
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Current technologies lack an effective methane adsorbent and methane adsorption device capable of efficiently adsorbing methane, with conventional TiO2 being used primarily as a catalyst and not utilized alone as an adsorbent, and there is a need for innovative applications of two-dimensional materials like MXene.

Method used

Development of a methane adsorbent and methane adsorption device using materials represented by the formula MQaOb, where M is an early transition metal and Q is from Groups 12, 13, 14, 15, 16, excluding oxygen, forming nanofibers and two-dimensional substances with a specific crystal structure, manufactured through a protic solvent reaction, resulting in high methane adsorption capacity.

Benefits of technology

The novel methane adsorbent demonstrates a significant ability to adsorb methane, with a large specific surface area and suitable crystal structure, outperforming comparative examples in methane adsorption efficiency, and can be used in devices for storage and transport.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018123_21112024_PF_FP_ABST
    Figure JP2024018123_21112024_PF_FP_ABST
Patent Text Reader

Abstract

A methane adsorbing material composed of a material containing a two-dimensional substance and / or nanofibers represented by the formula MQaOb (in the formula, M is at least one element selected from the group consisting of elements in groups 3, 4, 5, 6, and 7, Q is at least one element (excluding O) selected from the group consisting of elements in groups 12, 13, 14, 15, and 16, a is greater than or equal to 0 and less than or equal to 2, and b is greater than 0 and less than or equal to 2).
Need to check novelty before this filing date? Find Prior Art

Description

Methane adsorbent and methane adsorption device

[0001] The present disclosure relates to a methane adsorbent and a methane adsorption device.

[0002] Conventionally, as an oxide containing a metal, for example, TiO 2 In Non-Patent Document 1, reduced TiO 2 Several types of gold nanoparticles with different shapes supported on the surface, H 2 Catalytic activity for dissociation has been reported.

[0003] Recently, layered materials having one or more layers, so-called two-dimensional materials, have been attracting attention. MXene is known as one of the two-dimensional materials. MXene is a material that can be formed by a specific layered material (typically Ti 3 C 2 The main body of the layer has a surface modification / termination T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an oxygen atom, and a hydrogen atom), and Ti 3 C 2 T x or Ti 3 C 2 T s and may have the form of nanoflakes (or nanosheets) (see Non-Patent Documents 2 and 3).

[0004] Boronat, Merce et al. JPCA (2009), 113, 16, 3750-3757Mikhail Shekhirev, et al., "Characterization of MXenes at every step, from their precursors to single flakes and assembled films", Progress in Materials Science, Volume 120 (2021) 100757Asia Sarycheva, et al., "Raman Spectroscopy Analysis of the Structure and Surface Chemistry of Ti3C2Tx MXene", Chemistry of Materials, 2020, Volume 32, Issue 8, pp. 3480-3488Hussein O. Badr, et al., "Bottom-up, scalable synthesis of anatase nanofilament-based two-dimensional titanium carbo-oxide flakes", Materials Today (2021) https: / / doi.org / 10.1016 / j.mattod.2021.10.033

[0005] Conventionally known TiO 2 As shown in the above-mentioned Non-Patent Document 1, TiO is generally used in combination with a metal (e.g., Au) as a hydrogen activation catalyst. 2 is not used as an adsorbent by itself, and its adsorption of methane has not been investigated.

[0006] Research and development into MXene is currently underway, and there is a possibility that applications may be expanded further for two-dimensional materials different from MXene.

[0007] It is an object of the present disclosure to provide a novel methane adsorbent and a methane adsorption device including such a methane adsorbent.

[0008] According to one aspect of the present disclosure, a compound of the formula: a O b (wherein M is at least one element selected from the group consisting of Groups 3, 4, 5, 6, and 7; Q is at least one element selected from the group consisting of Groups 12, 13, 14, 15, and 16 (excluding O); a is 0 or more and 2 or less; and b is 0 or more and 2 or less.)

[0009] According to another aspect of the present disclosure, there is provided a methane adsorption device including the above-described methane adsorbent.

[0010] In accordance with the present disclosure, novel methane adsorbents and methane adsorption devices including such methane adsorbents are provided.

[0011] 1 shows a schematic cross-sectional view of a methane adsorption device according to one embodiment of the present disclosure; 2 shows an XRD pattern of the material (TiCO) produced in Example 1; 3 shows a graph of methane gas adsorption at room temperature for the dried powder of Example 1 and the dried powder of Comparative Example 1; 4 shows an SEM image of the material (TiCO) produced in Example 1; and 5 shows another SEM image of the material (TiCO) produced in Example 1.

[0012] (Embodiment 1: Methane Adsorbent) This embodiment relates to a methane adsorbent made of a material containing a predetermined nanofiber and / or a predetermined two-dimensional material. In this disclosure, the simple term "material" refers to a "material containing a predetermined nanofiber and / or a predetermined two-dimensional material" (in other words, a material containing at least one of a predetermined nanofiber and a predetermined two-dimensional material). In this embodiment, the material containing the nanofiber and / or a two-dimensional material typically refers to a material that is solid and does not contain a binder or the like (e.g., a polymer). In a narrow sense, the material containing the nanofiber and / or a two-dimensional material can refer to a material that is substantially composed of at least one of a nanofiber and a two-dimensional material (which may include other objects, impurities, etc. that may inevitably be mixed in). However, the material containing the nanofiber and / or a two-dimensional material is not limited to these.

[0013] The methane adsorbent is composed of a material containing nanofibers and / or two-dimensional materials. In this specification, the term "composed of" means that this embodiment includes aspects in which, in addition to the material containing nanofibers and / or two-dimensional materials, other materials such as additives suitable for the adsorbent are included, aspects essentially consisting of materials containing nanofibers and / or two-dimensional materials (which may contain other objects or impurities that may inevitably be mixed in), and aspects consisting only of materials containing nanofibers and / or two-dimensional materials. The material contained in the methane adsorbent of this embodiment is nanofibers and / or two-dimensional materials of a predetermined material (substance). The predetermined material that can be used in this embodiment is represented by the following formula (1): MQ a O b... (1) (In the formula, M is at least one element selected from the group consisting of Groups 3, 4, 5, 6 and 7, and may include at least one element selected from the group consisting of so-called early transition metals, for example, Sc, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo and Mn, and preferably at least one element selected from the group consisting of Ti, V, Cr, Mo and Mn; Q is at least one element selected from the group consisting of Groups 12, 13, 14, 15 and 16 (excluding O), and may include at least one element selected from the group consisting of B, C, N, Si, P and S; a is 0 or more and 2 or less; and b is 0 or more and 2 or less.)

[0014] The above-mentioned predetermined material will be hereinafter also referred to simply as "MQO." Examples of MQO include TiO 2 , TiCO, TiCON, VO 2 , VCO, VCON, CrO 2 , CrCO, CrCON, MoO 2 , MoCO, MoCON, MnO 2 , MnCO, MnCON, etc. For example, in formula (1), M may be Ti and Q may be C. Also, for example, in formula (1), a may not be 0.

[0015] MQO has a crystal structure different from the hexagonal system. Although the present embodiment is not bound by any theory, the crystal structure of MQO is currently considered to be anatase type, lepidocrocite type, or a mixture of these. For example, the crystal structure of MQO may be lepidocrocite type.

[0016] MQO can be produced, for example, using a first raw material and a second raw material as follows: The first raw material contains at least M, and the second raw material contains at least Q, and the first raw material and the second raw material are capable of reacting in a protic solvent to produce MQO.

[0017] As the first raw material, a material represented by the following formula (2) can be used: M c A 1d ... (2) (wherein M is as defined above, A 1 is at least one element selected from the group consisting of Groups 12, 13, 14, 15, and 16, and may include, for example, at least one element selected from the group consisting of B, C, N, O, Si, P, and S; and c and d are each independently 1 to 5. However, the material represented by formula (2) must be different from the product MQO. The material represented by formula (2) may typically have no peak in its X-ray diffraction (XRD) pattern in a diffraction angle 2θ range of 2° to 12°.

[0018] Examples of the first raw material represented by formula (2) include TiB 2 , TiB, TiC, TiN, TiO 2 , Ti 5 Si 3 , Ti 2 SbP, VO 2 , V 2 O 4 , NbC, Nb 2 O 5 , MoO 2 , MoO 3 , MoS 2 , MnO 2 , Mn 3 O 4 , MnCO 3 MnO that can be used as the first raw material 2 In the XRD pattern, the material has a peak near 2θ=13° and no peak in the 2θ range of 2° or more and 12° or less.

[0019] Alternatively, or in addition to the above, a material represented by the following formula (3) (hereinafter also simply referred to as a "MAX phase" or "MAX raw material") may be used as the first raw material. m A 2 X n ...(3) (wherein M is as defined above, X is at least one element selected from the group consisting of C and N, n is 1 or more and 4 or less, m is greater than n and 5 or less, A 2is at least one element selected from the group consisting of Groups 12, 13, 14, 15 and 16, and is usually a Group A element, typically Group IIIA and Group IVA, and more particularly may include at least one element selected from the group consisting of Al, Ga, In, Tl, Si, Ge, Sn, Pb, P, As, S and Cd, preferably Al). The MAX phase is m X n (which may have a crystal lattice where each X is located in an octahedral array of M), 2 The MAX phase has a crystal structure in which layers composed of atoms are located. When m=n+1, typically, one layer of X atoms is located between each of n+1 layers of M atoms (collectively referred to as "M m X n layer), and the layer next to the n+1-th layer of M atoms is A 2 Atomic layer ("A 2 The MAX phase has repeating units arranged in "atomic layers." However, the MAX phase is not limited to this.

[0020] Examples of the first raw material represented by formula (3) include Ti 3 AlC 2 , Ti 3 GaC 2 , Ti 3 SiC 2 These include:

[0021] As the first raw material, the material represented by formula (2) and the material represented by formula (3) may be used together (for example, as a mixture).

[0022] As the second raw material, an ionically bondable substance having a carbon-containing group can be used. The ionically bondable substance having a carbon-containing group contains C. Examples of the ionically bondable substance include ammonium salts, phosphates, sulfates, etc.

[0023] More specifically, a quaternary ammonium salt may be used as the second raw material. Examples of quaternary ammonium salts include tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide (TEAH), tetrapropylammonium hydroxide (TPAH), tetrabutylammonium hydroxide (TBAH or TBAOH), benzyltrimethylammonium hydroxide, tetrabutylammonium fluoride (TBAF), tetrabutylammonium chloride (TBACl), tetrabutylammonium bromide (TBAB), tetrabutylammonium iodide (TBAI), benzyltriethylammonium chloride (BTEAC), hexadecyltrimethylammonium bromide, cetyltrimethylammonium bromide (CTAB), benzethonium chloride, benzalkonium chloride, and cetylpyridinium chloride (CPC). Among these, TMAH and TBAOH are preferred.

[0024] Alternatively, or in addition to the above, other ion-binding substances containing P and / or S, etc. may be used as the second raw material.

[0025] The protic solvent may be any solvent capable of at least partially dissolving the first and second raw materials, and may be, in particular, an aqueous solvent. Examples of the protic solvent include water, alcohol (e.g., ethanol, 1-propanol, isopropanol), and carboxylic acids (e.g., acetic acid and formic acid). The aqueous solvent may be composed of water and, optionally, a liquid substance compatible with water (e.g., a protic solvent other than water), and is preferably water.

[0026] The first and second raw materials are reacted in a protic solvent. The second raw material can be added to the protic solvent in advance. The ratio of the second raw material to the total of the protic solvent and the second raw material can be, for example, 5% by mass or more, particularly 20% by mass or more, and / or, for example, 80% by mass or less, particularly 50% by mass or less. The first raw material can be further added to the protic solvent to which the second raw material has been added, and mixed. In this mixture, a reaction to produce MQO proceeds. The temperature (reaction temperature) of the mixture (which may contain the reaction product) can be, for example, 15°C or more, particularly 40°C or more, and / or, for example, 100°C or less, particularly 80°C or less. The mixing time (reaction time) can be, for example, one day or more, particularly two days or more, and / or, for example, 10 days or less, particularly 7 days or less. Mixing can be performed, for example, by rotating a magnetic stirrer placed in a container while maintaining the reaction temperature using a hot plate stirrer and a warm water bath. However, the treatment operations and conditions (temperature, time, etc.) that can cause the reaction to proceed are not limited to those described above, and may be selected appropriately depending on the first raw material, second raw material, protic solvent, etc. that are used.

[0027] The above reaction produces MQO, which may eventually grow into MQO nanofibers and then MQO nanoflakes. While not limiting the present disclosure, the resulting MQO nanofibers may be in the form of nanoribbons extending in nanoscale widths. Alternatively, multiple MQO nanofibers (e.g., nanoribbons) may bond and / or integrate with each other to grow into two-dimensionally extending nanoflakes. Alternatively, multiple MQO nanoflakes may overlap each other (e.g., by van der Waals forces) to form stacks. While the present disclosure is not bound by any theory, the production and growth of MQO may be thought of as a bottom-up synthesis reaction (see, for example, Non-Patent Document 4).

[0028] In the present disclosure, the cross-sectional outer dimension of an MQO nanofiber refers to the shortest distance passing through the center of a cross section transverse to the longitudinal direction of the MQO nanofiber. The cross-sectional shape of an MQO nanofiber is not particularly limited, but can be approximated, for example, by a rectangle (rectangle, square, etc.) or an ellipse (flattened circle, perfect circle, etc.). When an MQO nanofiber is in the form of a nanoribbon, the cross-sectional shape can be approximated by a rectangle, and the cross-sectional outer dimension can correspond to the length of the short side of the rectangle. When an MQO nanofiber is in the form of a nanofilament, the cross-sectional shape can be approximated by a flattened circle, and the cross-sectional outer dimension can correspond to the length of the short diameter of the flattened circle.

[0029] In the present disclosure, MQO is a solid content. MQO may typically be in the form of particles (or powder).

[0030] The mixture after the reaction (also referred to as a reaction mixture) may be subjected to appropriate post-treatment, such as washing, impact (including shear force), drying (e.g., freeze-drying or heat drying), or pulverization.

[0031] Washing may be carried out using a protic solvent. The same explanation as above may be applied to the protic solvent, and the reaction mixture may be washed with, for example, water or alcohol as the protic solvent. After washing, a separation operation (centrifugation and / or decantation) may be carried out. The washing and separation operations may be repeated until the pH of the supernatant after centrifugation is, for example, 8 or less.

[0032] Optionally, instead of or in addition to the above washing, washing may be carried out using an aqueous solution of a metal salt. The metal salt may be, for example, a halide (fluoride, chloride, bromide, iodide) of an alkali metal (Li, Na, K, etc.), typically LiCl, NaCl, KCl, etc. Specifically, washing may be carried out using, for example, an aqueous solution of a metal salt having a molar concentration of 1 to 10. After washing, a separation operation (centrifugation and / or decantation) may be carried out. In this case, too, the washing and separation operations may be repeated as necessary until the pH of the supernatant after centrifugation becomes, for example, 8 or less.

[0033] Impact such as vibration and / or ultrasound may be applied during and / or after washing. This can promote the dispersion of MQO particles (e.g., nanofibers / nanoflakes, hereinafter the same). If the MQO particles are aggregated, they can be broken down. This effect is particularly pronounced when impact is applied during washing with an aqueous solution of a metal salt (it is believed that metal cations derived from the metal salt penetrate into the gaps between the aggregates and break them down). Impact can be applied using, for example, one or more of a handshake, an automatic shaker, a mechanical shaker, a vortex mixer, a homogenizer, an ultrasonic bath, etc.

[0034] Since the MQO particles are a solid component, a separation operation can be carried out at any appropriate time to remove unnecessary liquid components, if any. As a final separation operation, for example, a drying operation, typically freeze-drying or thermal drying, may be carried out. Freeze-drying can be carried out, for example, by freezing a mixture containing the MQO particles and a liquid component at any appropriate temperature (e.g., −40° C.) and then drying under reduced pressure. Thermal drying can be carried out, for example, by drying a mixture containing the MQO particles and a liquid component at a temperature of 25° C. or higher (e.g., 200° C. or lower) under atmospheric pressure or under reduced pressure. Pulverization can be carried out using, for example, a mortar and pestle combination, an IKA mill, or the like, without particular limitation. Pulverization may also be carried out after drying.

[0035] As a result, MQO particles can be obtained as a material containing MQO. MQO is represented by formula (1), but the material containing MQO (typically, MQO particles) does not necessarily have to consist solely of the constituent elements of formula (1). While not limiting the present disclosure, the material containing MQO may optionally have at least one type of modification or terminal T present on its surface selected from the group consisting of hydroxyl groups, chlorine atoms, oxygen atoms, methane atoms, and nitrogen atoms. Furthermore, the material containing MQO (typically, MQO particles) may have two or more layers, and at least one type selected from the group consisting of ammonium ions (e.g., quaternary ammonium cations) and metal cations (e.g., alkali metal ions, alkaline earth metal ions) may be present between these layers.

[0036] The particle size of the MQO particles may be, for example, 0.01 nm or more, in particular 0.1 nm or more, or even 1 nm or more, and / or may be, for example, less than 1000 nm, in particular 100 nm or less, or even 50 nm or less. Such particles may also be referred to as nanoparticles.

[0037] The particle form of MQO is nanofibers and / or two-dimensional materials. The two-dimensional materials include one or more of nanoflakes and stacks of nanoflakes. In this embodiment, the two-dimensional materials are not limited to only nanoflakes and stacks of nanoflakes.

[0038] Nanofibers may also be referred to as nanowires. In the present disclosure, "nanofiber" refers to a solid object extending in the longitudinal direction, the cross-sectional dimensions of which perpendicular to the longitudinal direction (cross-sectional external dimensions) are on the nano-order (i.e., 1 nm or more and less than 1000 nm) or even smaller, sub-nano-order (less than 1 nm, for example, 0.1 nm or more and less than 1 nm). The longitudinal length of a nanofiber is not limited to the nano-order (i.e., 1 nm or more and less than 1000 nm), but may also be on the micron order (1 μm or more and less than 1000 μm). The cross-sectional external dimensions of a nanofiber may be, for example, 0.1 nm or more, particularly 1 nm or more, and may be, for example, 100 nm or less, particularly 50 nm or less, and preferably 15 nm or less.

[0039] In the present disclosure, the term "two-dimensional material" refers to a solid object having a two-dimensionally extending surface (also referred to as a plane or two-dimensional sheet surface) and a thickness that is relatively small compared to the maximum dimension of the surface (which may correspond to the "in-plane dimension" of a particle), with the thickness being on the nano-order (i.e., 1 nm or more but less than 1000 nm) or even smaller, on the sub-nano-order (less than 1 nm, for example, 0.1 nm or more but less than 1 nm). The in-plane dimension is not limited to the nano-order (i.e., 1 nm or more but less than 1000 nm) and may be on the micron-order (1 μm or more but less than 1000 μm). As described above, two-dimensional materials include one or more of nanoflakes and stacks of nanoflakes. Nanoflakes may also be referred to as nanosheets or two-dimensional (nano)sheets. The thickness of one layer of nanoflakes may be, for example, 0.01 nm or more, particularly 0.8 nm or more, and may be, for example, 20 nm or less, particularly 3 nm or less. The in-plane dimensions of the nanoflakes may be, for example, 0.1 μm or more, in particular 1 μm or more, and may be, for example, 200 μm or less, in particular 40 μm or less. The nanoflakes may be composed of an aggregate of nanofibers.

[0040] The stack of nanoflakes may also be referred to as a multi-layer MQO. The distance (interlayer distance or gap size) between two adjacent nanoflakes (or two adjacent layers of MQO) is not particularly limited.

[0041] Each of the above dimensions can be determined as a number-average dimension (number average of at least 40 dimensions) based on a photograph observed with a scanning electron microscope (SEM), a transmission electron microscope (TEM), or an atomic force microscope (AFM) (after processing by a method such as focused ion beam (FIB) if necessary), or as a distance in real space calculated from the position in reciprocal lattice space of the (002) plane measured by X-ray diffraction (XRD).

[0042] However, it should be noted that in the present disclosure, the MQO is not limited to the above forms and may have any suitable form.

[0043] Research by the present inventors has revealed that materials (nanofibers and / or two-dimensional materials) containing MQO can adsorb large amounts of methane. The methane adsorbent of this embodiment is made of a material containing MQO and therefore has the ability to adsorb methane. It should be noted that the methane adsorbent of this embodiment may be made of a material containing MQO, and may have any suitable form.

[0044] A material containing MQO may typically have a peak in an X-ray diffraction (XRD) pattern where the diffraction angle 2θ is in the range of 2° to 12° inclusive. Although the present disclosure is not bound by any theory, it is believed that the fact that a material containing MQO has a peak in an XRD pattern where 2θ is in the range of 2° to 12° inclusive means that such MQO has a crystal structure different from that of well-known metal oxides.

[0045] In the present disclosure, an XRD pattern is a pattern (the vertical axis represents intensity and the horizontal axis represents 2θ) obtained by scanning in the θ-axis direction with an XRD analyzer using CuKα radiation (approximately 1.54 Å) as characteristic X-rays, and may also be referred to as an “XRD profile.” Peaks in an XRD pattern can be identified visually or by using software used with the XRD analyzer.

[0046] The methane adsorbent of this embodiment, in other words, the material containing MQO, has a relatively large specific surface area. More specifically, the BET specific surface area of ​​the material containing MQO is 50 m 2 The BET specific surface area can be greater than 80 m / g. The BET specific surface area is calculated using the BET equation from the isothermal adsorption curve of nitrogen gas or other suitable gases (e.g., krypton (Kr) gas, etc.) at liquid nitrogen temperature (77 K). The BET specific surface area can be, for example, 80 m 2 / g or more, and the upper limit is not particularly limited, but for example, 400 m 2 / g or less. In order to obtain a larger specific surface area, it is preferable to perform freeze-drying. That is, a preferred form of the methane adsorbent of this embodiment is a freeze-dried powder.

[0047] Although this embodiment is not limited to this embodiment, for example, the material of this embodiment (more specifically, MQO) has a Raman shift of at least 275 to 295 cm in a Raman spectrum using a laser with a wavelength of 514 nm. -1 , 435-455cm -1 , and 665-745 cm -1 It may have a peak at the position

[0048] Although this embodiment is not limited to this embodiment, for example, the material of this embodiment (more specifically, MQO) has a Raman shift of 140 to 160 cm in a Raman spectrum using a laser with a wavelength of 514 nm. -1 , 275-295cm -1 , 435-455cm -1 , and 665-745 cm -1 It may have a peak at a position of 140 to 160 cm -1 is the peak of the anatase type.

[0049] Although this embodiment is not limited thereto, for example, the material of this embodiment (more specifically, MQO) has a crystal structure of anatase type, lepidocrocite type, or a mixture of these. More preferably, it has a crystal structure of lepidocrocite type.

[0050] Although this embodiment is not limited to this embodiment, for example, the material of this embodiment (more specifically, MQO) has a Raman shift of at least 275 to 295 cm in a Raman spectrum using a laser with a wavelength of 514 nm. -1 , 435-455cm -1 , and 665-745 cm -1 and when the intensities of the respective peaks are X, Y, and Z, X is the largest.

[0051] Although this embodiment is not limited thereto, more preferably, the material of this embodiment (more specifically, MQO) has a Raman shift of at least 180 to 200 cm in a Raman spectrum using a laser with a wavelength of 514 nm. -1 , 275-295cm -1 , 375-395cm -1 , 435-455cm-1 , and 665-745 cm -1 and when the intensities of the respective peaks are V, X, Y, Z, and W, X is the largest.

[0052] In this disclosure, the Raman spectrum is measured with a Raman spectrometer using a 514 nm laser as an excitation light source (the vertical axis represents intensity, and the horizontal axis represents Raman shift). Peaks in the Raman spectrum can be identified visually or by using software used with the Raman spectrometer.

[0053] Furthermore, the MQO-containing material may contain unreacted first and / or second raw materials as impurities, and may also contain substances derived from the first, second, and / or protic solvents. For example, when a quaternary ammonium salt is used as the second raw material, N may be present (residual) in any form in the MQO-containing material. While not limiting this embodiment, the MQO-containing material may contain ammonium ions or tetramethylammonium ions. Furthermore, for example, when a MAX raw material is used as the first raw material, the MQO-containing material in this disclosure may contain a relatively small amount of residual A atoms, for example, 10% by mass or less relative to the original A atoms. The amount of residual A atoms may preferably be 8% by mass or less, more preferably 6% by mass or less. However, even if the amount of residual A atoms exceeds 10% by mass, this may not be a problem depending on the usage conditions, etc.

[0054] To obtain a material containing MQO with higher purity, it is preferable to repeat washing and centrifugation multiple times and recover the supernatant after the final centrifugation. The supernatant can be used as is, appropriately diluted with a liquid medium, or dried and then mixed with a liquid medium to form a slurry containing MQO particles. Such a slurry can be used to prepare a film, which can then be used as the methane adsorbent of this embodiment.

[0055] (Embodiment 2: Methane Adsorption Apparatus) This embodiment relates to a methane adsorption apparatus (or methane adsorption device, hereinafter the same).

[0056] The methane adsorption device of this embodiment includes the methane adsorbent described above in Embodiment 1. The same explanation as in Embodiment 1 can be applied to the methane adsorbent.

[0057] 1 , a methane adsorption device 10 may include a main body 3 defining a space 1 in which the material (not shown) described above in Embodiment 1 is disposed, an inlet 5 through which a methane-containing gas can flow into the space 1, and an outlet 7 through which a methane-containing gas can flow from the space 1. The methane-containing gas may be any gas that contains methane gas, and may consist of methane gas or may contain other gases in addition to methane gas. The inlet 5 and the outlet 7 may be provided at any appropriate locations and may be separate ( FIG. 1 ) or may be common.

[0058] Without limiting this embodiment, the methane adsorption device may be used to store and / or transport methane.

[0059] According to this embodiment, the methane adsorption device can adsorb methane by using the methane adsorbent described above in the first embodiment.

[0060] Although the methane adsorbent and the methane adsorption device according to certain embodiments of the present disclosure have been described in detail above, various modifications of the present disclosure are possible. Note that the materials of the present disclosure may be manufactured by methods different from those described in the above-described embodiments.

[0061] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples, and can be practiced with appropriate modifications within the scope of the above-mentioned and below-mentioned aims, and all such modifications are included in the technical scope of the present invention.

[0062] (Example 1) Preparation of a slurry containing TiCO First, titanium diboride (TiB 21 g of ethanol (manufactured by Alfa Aesar) and 10 mL of 25% by weight tetramethylammonium hydroxide (TMAH) aqueous solution (manufactured by Alfa Aesar) were added to the container. A stirrer tip with a length (35 mm) approximately equal to the inner diameter of the circular bottom of the container was placed therein. The container was maintained at 80°C in an oil bath, and the mixture in the container was stirred with the stirrer tip for 120 hours, allowing the reaction to proceed. The reaction mixture in the container was then transferred to a centrifuge tube. The solids were then precipitated by centrifugation at 3500 G for 5 minutes. (i) After centrifugation, the supernatant was discarded. (ii) 40 mL of ethanol (manufactured by Fisher Chemical) was added to the remaining sediment in the centrifuge tube, and the mixture was dispersed using a vortex mixer for 5 minutes (reslurry). (iii) The centrifugation was repeated under the same conditions as above. These steps (i) to (iii) were repeated until the pH of the supernatant reached 8 or below. After repeating the process three times, the pH of the supernatant became 8 or less, so the supernatant was discarded and the repeating process was terminated. 40 mL of pure water was added to the remaining sediment in the centrifuge tube, and the mixture was shaken and stirred for 5 minutes using a vortex mixer. Then, the mixture was centrifuged at 3500 G for 30 minutes using a centrifuge, and the supernatant was collected as a sample slurry. The resulting sample slurry corresponds to a slurry containing TiCO (see the analysis results below).

[0063] - Film Preparation 1 mL of the sample slurry prepared above was taken and mixed with 20 mL of pure water, and then shaken for 5 minutes using an automatic shaker. The resulting mixture was suction filtered overnight using a Nutsche filter. A membrane filter (Durapore, pore size 0.22 μm, manufactured by Merck Ltd.) was used for the suction filtration. After suction filtration, the precursor film on the filter was dried overnight at 80 ° C in a vacuum oven, and the filter was removed to obtain a film (free-standing film).

[0064] Analysis: The film (freestanding film) obtained in the same manner as above was analyzed by X-ray photoelectron spectroscopy (XPS). Peaks corresponding to Ti 2p, C 1s, O 1s, and N 1s were observed in the obtained XPS spectrum, and thus Ti, C, O, and N were detected. Since N is thought to be a residual component of the raw material TMAH, the material of the freestanding film is thought to be composed of Ti, C, and O. Furthermore, the XRD profile of the film (freestanding film) obtained in the same manner as above was measured using an XRD device (MiniFlex, manufactured by Rigaku Corporation) (characteristic X-rays: CuKα = 1.54 Å). The obtained XRD pattern is shown in Figure 2. As can be seen from Figure 2, this material had a (001) plane peak at 2θ = 7.9° and a (002) plane peak at 2θ = 15.6°. This suggests that this material has a periodic structure different from that of known metal oxides. The sample slurry prepared above was dropped onto an appropriate porous substrate, dried, and observed using an SEM. The resulting SEM images are shown in Figures 4 and 5. Figures 4 and 5 show SEM images of different locations of the sample slurry. In the SEM image of Figure 4, nanofibers with diameters (widths in the SEM image) of approximately several μm to 20 μm were observed. In the SEM image of Figure 5, as shown in the gray area on the lower left, nanoflakes extending two-dimensionally were observed, with the nanofibers bonding to each other.

[0065] Preparation of dry powder: An ultrasonic probe was immersed in the sample slurry prepared above, and ultrasonic treatment was performed for 15 minutes. The obtained slurry was freeze-dried (freezed in liquid nitrogen and then vacuum-dried) to produce a dry powder.

[0066] BET specific surface area: The dried powder obtained above was subjected to a degassing treatment by heat treatment under reduced pressure at 60°C for 1 hour, then at 100°C for 1 hour, and then at 150°C for 6 hours. After the degassing treatment, the adsorption isotherm of nitrogen gas at liquid nitrogen temperature (77K) was measured for the dried powder obtained. As a result, the BET specific surface area (SSA) of the dried powder was 100 m 2 / g.

[0067] Evaluation of Adsorption Performance The dried powder obtained above was subjected to degassing treatment in a vacuum at 180°C for 2 hours. Thereafter, it was adsorbed on methane (CH4) at room temperature in a pressure range from atmospheric pressure (101.3 kPa) to approximately 4 MPa. 4 The adsorption amount of gas was measured. The results are shown in Figure 3. In Figure 3, the vertical axis represents the mass (%) of gas adsorption relative to the mass of the dry powder before adsorption, and the horizontal axis represents the pressure (absolute pressure).

[0068] Comparative Example 1 Comparative Example 1 is a Ti-based MXene. 3 C 2 T x Regarding.

[0069] Preparation of dry powder (a) Preparation of MAX particles (precursor of MXene particles) TiC powder, Ti powder, and Al powder (all manufactured by Kojundo Chemical Laboratory Co., Ltd.) were mixed in a molar ratio of 2:1:1 in a ball mill containing zirconia balls for 24 hours. The resulting mixed powder was fired at 1350°C for 2 hours in an Ar atmosphere. The fired body (block) thus obtained was pulverized with an end mill to a maximum dimension of 40 μm or less. As a result, TiC powder was obtained as MAX particles. 3 AlC 2 particles were obtained.

[0070] (b) Etching of precursor (ACID method) Ti prepared by the above method 3 AlC 2 Using particles (powder), etching was performed under the following etching conditions to remove Ti 3 AlC 2 A solid-liquid mixture (slurry) containing solid components derived from the powder was obtained. (Etching conditions) Precursor: Ti 3 AlC 2 (Sieved through a 45 μm mesh) Etching solution composition: 49% HF 6 mL H 2 O 18 mL HCl (12 M) 36 mL Precursor input amount: 3.0 g Etching container: 100 mL Eye Boy Etching temperature: 35°C Etching time: 24 h Stirrer rotation speed: 400 rpm

[0071] (c) Post-etching cleaning The above slurry was divided into two parts and placed in two 50 mL centrifuge tubes, respectively. After centrifuging at 3500 G using a centrifuge, the supernatant was discarded. 40 mL of pure water was added to the remaining precipitate in each centrifuge tube, and the tubes were centrifuged again at 3500 G to separate and remove the supernatant. This procedure was repeated 11 times. After the final centrifugation, the supernatant was discarded, and Ti 3 C 2 T x - Water medium clay was obtained.

[0072] (d) Li intercalation Ti prepared by the above method 3 C 2 T x The clay was stirred for 12 hours at 20°C to 25°C under the following conditions using LiCl as the Li-containing compound, and the mixture was subjected to Li intercalation. (Li intercalation conditions) 3 C 2 T x - Water medium clay (MXene after washing): solid content 0.75 g LiCl: 0.75 g Intercalation container: 100 mL Eye Boy Temperature: 20 ° C or higher and 25 ° C or lower (room temperature) Time: 10 h Stirrer rotation speed: 800 rpm

[0073] (e) Delamination The above Ti 3 C 2 T x (i) 40 mL of pure water was added to the water medium clay, followed by stirring for 15 minutes on a shaker. (ii) The mixture was centrifuged at 3,500 G, and (iii) the supernatant was collected as a single-layer MXene-containing solution. These steps (i) to (iii) were repeated a total of four times to obtain a single-layer MXene-containing supernatant. This supernatant was then centrifuged at 4,300 G for two hours using a centrifuge, after which the supernatant was discarded, yielding a single-layer / few-layer MXene-containing clay as a single-layer / few-layer MXene-containing sample.

[0074] (f) Preparation of Slurry Containing MXene Particles This MXene-containing clay and pure water were mixed in appropriate amounts to prepare a sample slurry with a solid concentration (MXene particle concentration) of 34 mg / mL. The obtained sample slurry was 3 C 2 T x ) particles (MXene-water dispersion).

[0075] (g) Preparation of dry powder: An ultrasonic probe was immersed in the sample slurry prepared above, and ultrasonic treatment was performed for 15 minutes. The obtained slurry was freeze-dried (freezed in liquid nitrogen and then vacuum-dried) to produce a dry powder.

[0076] Evaluation of Adsorption Performance After degassing the dried powder prepared above in the same manner as in Example 1, the powder was subjected to adsorption of methane (CH4) at room temperature in a pressure range from atmospheric pressure (101.3 kPa) to approximately 4 MPa. 4 The amount of adsorption of HCl was measured, and the results are shown in Figure 3.

[0077] In FIG. 3, it can be seen that the dry powder of Example 1 adsorbed more methane than the dry powder of Comparative Example 1 at all pressures, demonstrating that it has a higher methane adsorption capacity.

[0078] The methane adsorbent of the present disclosure is capable of adsorbing methane and can be used, for example, in a methane adsorption device.

[0079] This application claims priority to U.S. Application No. 63 / 467,383, filed May 18, 2023, the entire contents of which are incorporated herein by reference.

[0080] REFERENCE SIGNS LIST 1 space 3 main body 5 inlet 7 outlet 10 methane adsorption device

Claims

1. The formula: MQ a O b (In the formula, M is at least one element selected from the group consisting of Groups 3, 4, 5, 6, and 7; Q is at least one element selected from the group consisting of Groups 12, 13, 14, 15, and 16 (excluding O); a is 0 or more and 2 or less; and b is 0 or more and 2 or less.

2. The methane adsorbent according to claim 1, which has an X-ray diffraction pattern with a peak at a diffraction angle 2θ in the range of 2° or more and 12° or less.

3. BET specific surface area is 50m 2 The methane adsorbent according to claim 1 or 2, wherein the methane adsorbent has a molecular weight of 1000 or more and a molecular weight of 1000 or more.

4. In the Raman spectrum using a laser with a wavelength of 514 nm, the Raman shift is 140 to 160 cm -1 , 275-295cm -1 , 435-455cm -1 , and 665-745 cm -1 The methane adsorbent according to any one of claims 1 to 3, having a peak at the position 5. The methane adsorbent according to any one of claims 1 to 4, which has a crystal structure of anatase type or lepidocrocite type, or a mixture of these.

6. The methane adsorbent according to any one of claims 1 to 4, having a lepidocrocite-type crystal structure.

7. In the Raman spectrum using a laser with a wavelength of 514 nm, the Raman shift is at least 180 to 200 cm -1 , 275-295cm -1 , 375-395cm -1 , 435-455cm -1 , and 665-745 cm -1 The methane adsorbent according to any one of claims 1 to 6, wherein, when the intensities of the respective peaks are V, X, Y, Z, and W, X is the largest.

8. The methane adsorbent according to any one of claims 1 to 7, wherein M is Ti, Q is C, and a is not 0.

9. The methane adsorbent of any one of claims 1 to 8, wherein the material contains ammonium ions.

10. The methane adsorbent of claim 9, wherein the ammonium ion is a tetramethylammonium ion.

11. The methane adsorbent according to any one of claims 1 to 10, which is a freeze-dried powder.

12. A methane adsorption device comprising the methane adsorbent according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Dispersion and coating agent

    JP2006225623A

  • Electrode catalyst for fuel cell and manufacturing method thereof

    JP2011253626A

  • Metal complex, and adsorbing material and occluding material each comprising the same

    JP2013040128A

  • Method of producing hybrid titania powder, hybrid titania powder, function-imparting liquid, and product

    JP2013139386A

  • Nanowire structure, production method thereof, ion-exchange material, photocatalytic material, and metal immobilization material

    JP2020189775A