Thermally conductive filler, two-component silicone potting compound comprising thermally conductive filler, and preparation method for two-component silicone potting compound

Two-component silicone potting is solved by using mesoporous alumina-loaded nanocopper particles and coated with silica, combining low viscosity vinyl polydimethylsiloxane and crosslinking agent in silicone potting, a two-component silicone potting is solved. The problem of insufficient thermal conductivity of glue achieves higher thermal conductivity and lower electrical conductivity, which is suitable for sealing materials for electronic components.

WO2024239424A1PCT designated stage expired Publication Date: 2024-11-28GOLOHO POLYMER (JIANGXI) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/104400
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2023-06-30
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The existing two-component silicone potting adhesives have poor thermal conductivity, which makes it difficult to meet the thermal conductivity requirements in electronic components. At the same time, the thermal conductivity of thermally conductive materials is high, affecting their application.

Method used

Mesoporous alumina is used as thermal filler and nanocopper particles are loaded on its surface, and the silicon dioxide layer is coated to improve thermal conductivity while reducing electrical conductivity, combining low viscosity vinyl polydimethylsiloxane and appropriate The crosslinker ratio is optimized to optimize colloidal performance.

Benefits of technology

It significantly improves the thermal conductivity of silicone potting, reduces viscosity and electrical conductivity, enhances fluidity and mechanical properties, and is suitable for sealing materials in the electronics industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023104400_28112024_PF_FP_ABST
    Figure CN2023104400_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the field of silicone potting compounds, and in particular to a thermally conductive filler, a two-component silicone potting compound comprising the thermally conductive filler, and a preparation method for the two-component silicone potting compound. The thermally conductive filler comprises mesoporous alumina. Nano-copper particles are loaded on at least part of the surface of mesoporous alumina. At least part of the surface of the mesoporous alumina and nano-copper particles is coated with a layer of silicon oxide. According to the present application, by introducing nano-copper particles and a silicon oxide coating into a thermally conductive filler, the thermal conductivity of the thermally conductive filler is effectively enhanced without affecting the electrical conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

A thermally conductive filler, a two-component silicone potting compound containing the same, and a preparation method thereof Technical Field

[0001] The present invention relates to the field of organosilicon potting adhesives, and in particular to a thermally conductive filler, a two-component organosilicon potting adhesive containing the same, and a preparation method thereof. Background Art

[0002] Silicone potting compounds offer excellent resistance to high and low temperatures, water, electricity, radiation, and weathering. The vulcanization process produces no byproducts and exhibits minimal shrinkage. They are widely used in the electronics, automotive, and medical industries as moisture-proof, dust-proof, corrosion-resistant, and cushioning materials.

[0003] With the development of the electronics industry, electronic components are becoming increasingly miniaturized and densely packed. To ensure the proper functioning of these components, higher requirements are placed on thermally conductive materials. Two-component addition-type silicone rubber, due to its inherent properties, fulfills the role of thermal conductivity and sealing. When preparing addition-type silicone encapsulants, the thermal conductivity is often enhanced by increasing the amount of thermally conductive filler.

[0004] As the proportion of thermally conductive fillers increases, the viscosity of the silicone potting compound increases and its leveling properties decrease, which makes it difficult to degas during application and difficult to fill the tiny gaps in the device. This affects the thermal conductivity of the potting compound and its protective effect on the device during use, thus becoming a common problem in high thermal conductivity silicone potting compounds.

[0005] Therefore, improving the thermal conductivity of thermally conductive fillers in silicone potting compounds is key to solving these problems, but the electrical conductivity of the thermally conductive material also needs to be considered. Commonly used high-thermal conductivity materials such as metal, carbon fiber, graphite, and graphene, while having extremely high thermal conductivity, also have high electrical conductivity, making them difficult to use in electronic sealing materials.

[0006] Therefore, how to select thermally conductive fillers in silicone potting adhesives is the key to improving the thermal conductivity of two-component silicone potting adhesives. Summary of the Invention

[0007] The present invention aims to overcome the defect of poor thermal conductivity of the two-component organosilicon potting adhesive in the prior art and provides a thermally conductive filler, a two-component organosilicon potting adhesive containing the same and a preparation method thereof.

[0008] To achieve the above-mentioned purpose, the present invention is implemented through the following technical solutions:

[0009] In a first aspect, the present invention first provides a thermally conductive filler.

[0010] The thermally conductive filler comprises mesoporous alumina;

[0011] At least a portion of the surface of the mesoporous alumina is loaded with nano-copper particles;

[0012] At least a portion of the surface of the mesoporous aluminum oxide and the nano-copper particles is covered with a silicon dioxide layer.

[0013] In the prior art, the thermal conductive fillers used to improve the thermal conductivity of silicone potting compounds are mainly selected from metal oxides and metal nitrides. Aluminum oxide is the most widely used in organic potting compounds because it has a higher thermal conductivity coefficient among metal oxides, is cheap, and has excellent insulation properties. However, the thermal conductivity coefficient of aluminum oxide is still only maintained at 30 W·m -1 ·K -1 Compared with metal materials and carbon materials, its thermal conductivity is still relatively low. Therefore, in order to improve the thermal conductivity of organic potting glue, the amount of aluminum oxide added can only be further increased. However, the large amount of thermal conductive material added will cause other properties of organic potting glue (leveling and mechanical properties) to decline to varying degrees, which seriously affects its own use.

[0014] The thermal conductive filler provided in this application is also based on alumina material, but a certain amount of nano-copper particles are loaded on the surface of the alumina. Therefore, compared with alumina, the thermal conductivity of metallic copper can be as high as 398 W·m -1 ·K -1 Therefore, the addition of nano copper particles can effectively improve the thermal conductivity of the overall thermal conductive filler to a certain extent.

[0015] However, conventional alumina fillers (such as spherical alumina) have a relatively smooth surface, which makes it easy for the nano-copper particles to fall off the alumina surface during loading, making it difficult for the nano-copper particles to adhere. Therefore, in this application, mesoporous silica is used to increase the contact area between the nano-copper particles and the alumina surface, thereby allowing the nano-copper particles to better adhere to the alumina surface. Actual tests have shown that thermally conductive fillers containing mesoporous alumina have significantly better thermal conductivity than thermally conductive fillers containing traditional spherical alumina.

[0016] While the addition of nano-copper particles can effectively improve the thermal conductivity of thermally conductive fillers, the applicant has discovered that, despite a low nano-copper content, they significantly increase the conductivity of the overall potting compound, hindering its application in the electronics industry. Therefore, the present invention coats at least a portion of the surface of the mesoporous alumina and nano-copper particles with a layer of silicon dioxide. Silicon dioxide has a lower resistivity than alumina, so the silicon dioxide coating of both surfaces shields the conductivity of the nano-copper particles and prevents oxidation by oxygen, thereby reducing their thermal conductivity.

[0017] Therefore, in summary, the present application combines aluminum oxide, nano-copper particles, and silicon dioxide to obtain a thermally conductive material with higher thermal conductivity and lower electrical conductivity. This can effectively reduce the amount of thermally conductive filler used in silicone sealants and effectively improve the sealant's leveling and mechanical properties.

[0018] Preferably, the preparation method of the thermally conductive filler is as follows:

[0019] (1) reacting alumina with an etching solution to obtain spherical mesoporous alumina;

[0020] (2) placing mesoporous alumina in a solution containing a copper precursor and a silica precursor with an alkoxy group, uniformly dispersing the solution, and then adding an acidic reducing agent to reduce the copper precursor to obtain nano-copper particles, and hydrolyzing the silica precursor to form polysiloxane, thereby coating the mesoporous alumina and the nano-copper particles, and obtaining mesoporous alumina loaded with nano-copper particles and polysiloxane;

[0021] (3) The mesoporous alumina loaded with nano-copper particles and polysiloxane is washed, dried, and thermally decomposed under the protection of an inert gas to obtain the thermal conductive filler.

[0022] During the preparation process, the thermally conductive filler of the present invention is first etched on aluminum oxide using an etching solution. The etching solution can be an acid solution or an alkaline solution, both of which have a good etching effect on aluminum oxide. This allows the filler to react on the surface of the aluminum oxide, thereby forming a mesoporous structure on the surface.

[0023] Subsequently, the mesoporous alumina is placed in a solution containing a copper precursor and a silica precursor with an alkoxy group, and an acidic reducing agent is added after uniform dispersion. The copper precursor is reduced under the action of the acidic reducing agent to form nano-copper particles. A portion of these nano-copper particles is embedded in the pores on the surface of the mesoporous alumina, and a portion is free in the solution. Since the formed nano-copper particles can coordinate with the silica precursor with an alkoxy group, the nano-copper particles are coated. At the same time, since the silica precursor contains alkoxy groups, it will undergo a hydrolysis reaction under acidic conditions, thereby forming a cross-linked polysiloxane structure after hydrolysis, and wrapping the alumina and nano-copper particles together, so that the alumina can achieve effective loading of the nano-copper particles.

[0024] Finally, the alumina loaded with nano-copper particles and polysiloxane is thermally decomposed to decompose the organic structure in the polysiloxane to form silicon dioxide, further reducing the electrical conductivity of the overall thermal conductive filler.

[0025] Preferably, the copper precursor includes any one of copper chloride, copper sulfate and copper acetate.

[0026] Preferably, the alumina is spherical alumina.

[0027] This application gives priority to the use of spherical alumina fillers. While improving the thermal conductivity of the colloid, spherical alumina fillers are easier to disperse than irregularly shaped thermal conductive fillers, are evenly dispersed in the colloid system, are not easy to settle, and are conducive to reducing viscosity.

[0028] Preferably, the silicon dioxide precursor is obtained by a hydrosilylation reaction between an alkoxysilane containing a silicon-hydrogen structure and N-vinyl pyrrolidone.

[0029] In order to enhance the coordination effect between the silica precursor and the nano-copper particles, the present invention introduces a pyrrolidone structure into the silica precursor, thereby further enhancing the coordination and coating effects on the nano-copper particles.

[0030] Preferably, the alkoxysilane containing a silicon-hydrogen structure includes any one of trimethoxysilane, methyldimethoxysilane, triethoxysilane, and methyldiethoxysilane.

[0031] Preferably, the acidic reducing agent is any one of citric acid, ascorbic acid, oxalic acid and oxalic acid.

[0032] In a second aspect, the present invention further provides a two-component silicone potting compound comprising component A and component B;

[0033] The component A includes vinyl polydimethylsiloxane, polydimethylsiloxane, color paste and catalyst;

[0034] The B component includes vinyl polydimethylsiloxane, polydimethylsiloxane, a crosslinking agent and an inhibitor;

[0035] At least one of the components A and B contains the thermally conductive filler as described above.

[0036] Preferably, the viscosity of the vinyl polydimethylsiloxane is 100-300 mPa·s, and the viscosity of the polydimethylsiloxane is 5-200 mPa·s.

[0037] In order to effectively solve the fluidity problem, this application first gives priority to using low-viscosity vinyl polydimethylsiloxane as the base glue to improve its fluidity by lowering the overall viscosity of the product.

[0038] Preferably, the

[0039] Preferably, the cross-linking agent includes cross-linking agent I and cross-linking agent II;

[0040] The crosslinking agent I is a hydrogen-terminated silicone oil with a hydrogen content of 0.1-0.5%;

[0041] The crosslinking agent II is a hydrogenated silicone oil with a hydrogen content of 0.4-0.8%.

[0042] Preferably, the catalyst is a platinum catalyst with a content of 3000 ppm.

[0043] Preferably, the inhibitor includes one or more of 1-hexynyl-1-cyclohexanol, 2-phenyl-3-butynyl-2-ol, 3,5-dimethyl-1-hexynyl-3-ol, 2-methyl-3-butynyl-2-ol and vinyl ring.

[0044] Preferably, component A and component B are composed;

[0045] The component A comprises the following raw materials in parts by weight: 5-10 parts of vinyl polydimethylsiloxane, 5-10 parts of polydimethylsiloxane, 80-90 parts of the thermal conductive filler, 0.01-0.05 parts of color paste, and 0.1-0.3 parts of catalyst;

[0046] The component B comprises the following raw materials in parts by weight: 10-15 parts of vinyl polydimethylsiloxane, 2-5 parts of polydimethylsiloxane, 80-90 parts of the thermal conductive filler, 2-5 parts of crosslinking agent I, 0.2-0.5 parts of crosslinking agent II, and 0.001-0.01 parts of inhibitor.

[0047] Preferably, the mass ratio of component A to component B is 1:1.

[0048] In a third aspect, the present invention further provides a method for preparing the two-component silicone potting compound as described above.

[0049] The following steps are involved:

[0050] Preparation of component A: vinyl polydimethylsiloxane, polydimethylsiloxane, and the thermal conductive filler are added to a kettle at once, stirred and heated. After the temperature rises to 120°C, the temperature is maintained and vacuum is applied. After stirring for 2 hours, the mixture is stopped and cooled. After the temperature drops to room temperature, the color paste and catalyst are added. The mixture is stirred for 30 minutes while maintaining a vacuum degree of -0.08 MPa to obtain component A.

[0051] Preparation of component B: vinyl polydimethylsiloxane, polydimethylsiloxane, and the thermal conductive filler are put into a kettle at one time, stirred and heated. After the temperature rises to 120°C, the temperature is maintained and vacuum is applied. After stirring for 2 hours, the mixture is stopped and cooled. After the temperature drops to room temperature, a cross-linking agent and an inhibitor are added, and the vacuum degree is maintained at -0.08 MPa and stirred for 30 minutes to obtain component B.

[0052] By adopting the above preparation method, the preparation process is simple and the production efficiency is high. During production, low-boiling substances in the raw materials are effectively removed by high-temperature removal, which effectively improves the aging resistance of the product and extends its service life.

[0053] Therefore, this application has the following beneficial effects:

[0054] (1) This application effectively improves the thermal conductivity of a thermally conductive filler without affecting its electrical conductivity by introducing nano-copper particles and silica coatings into the thermally conductive filler;

[0055] (2) This application uses low-viscosity vinyl polydimethylsiloxane, which can effectively control the viscosity of the prepared potting glue. At the same time, the appropriate ratio of end-hydrogen silicone oil and side-hydrogen silicone oil is used to enhance the toughness of the colloid, thereby improving the performance of the colloid and protecting the packaged devices;

[0056] (3) This application uses spherical thermal conductive fillers to significantly reduce the viscosity of the system, slow down the separation of oil and powder, and improve the anti-settling effect, fluidity and thermal conductivity of the system. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] FIG1 is an electron microscope photograph of the thermal conductive filler B1 of the present invention. Implementation Method

[0058] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. Those skilled in the art will be able to implement the present invention based on these descriptions. Furthermore, the embodiments of the present invention described below are generally only a portion of the embodiments of the present invention, rather than all of the embodiments. Therefore, all other embodiments derived by those skilled in the art based on the embodiments of the present invention without inventive effort should fall within the scope of protection of the present invention.

[0059]

Preparation of silica precursor

[0060] Preparation of silica precursor A1: 12.2 g (100 mmol) of trimethoxysilane and 11.1 g (100 mmol) of N-vinylpyrrolidone were dissolved in 100 ml of toluene, and 3000 ppm of platinum catalyst (Karstedt catalyst) was added thereto. After reflux reaction for 5 h, the reaction was stopped, 1 g of activated carbon was added to the reaction solution, and stirring was continued for 30 min. The filtrate was filtered to obtain the filtrate, and the filtrate was subjected to reduced pressure rotary evaporation to obtain silica precursor A1. The reaction formula is shown in the following formula (1):

[0061]

[0062] Formula (1).

[0063] Preparation of silica precursor A2: 16.4 g (100 mmol) of trimethoxysilane and 11.1 g (100 mmol) of N-vinylpyrrolidone were dissolved in 100 ml of toluene, and 3000 ppm of platinum catalyst (Karstedt catalyst) was added thereto. After reflux reaction for 5 h, the reaction was stopped, 1 g of activated carbon was added to the reaction solution, and stirring was continued for 30 min. The filtrate was filtered to obtain the filtrate, and the filtrate was subjected to reduced pressure rotary evaporation to obtain silica precursor A2. The reaction formula is shown in the following formula (2):

[0064]

[0065] Formula (2).

[0066]

Preparation of thermal conductive filler

[0067] Thermal conductive filler B1, the preparation method thereof is as follows:

[0068] (1) Immersing the spherical alumina in a 0.005 mol / L sodium hydroxide solution at room temperature for 15 min, allowing the spherical alumina to react with the sodium hydroxide for 30 min, and then filtering and washing to obtain spherical mesoporous alumina;

[0069] (2) 500 g of mesoporous alumina was placed in a solution containing 2 L of 30 g of copper sulfate pentahydrate and 46.6 g (0.2 mol) of silica precursor A1, and dispersed evenly to form a suspension. Then, 40 g of citric acid was added and continued to be stirred and dispersed. The mixture was then heated to 75 ° C and stirred for 2 h to reduce the copper sulfate to obtain nano-copper particles and hydrolyze the silica precursor to form polysiloxane, thereby coating the mesoporous alumina and the nano-copper particles. The mesoporous alumina loaded with nano-copper particles and polysiloxane was filtered to obtain the mesoporous alumina.

[0070] (3) The mesoporous alumina loaded with nano-copper particles and polysiloxane was washed, dried, and heated to 400° C. for thermal decomposition for 3 h under nitrogen protection to obtain the thermal conductive filler B1, an electron microscope photograph of which is shown in FIG1 .

[0071] The preparation method of thermal conductive filler B2 is basically the same as that of thermal conductive filler B1, except that the silica precursor A1 in step (2) is replaced by silica precursor A2, and the rest remains unchanged.

[0072] Example 1

[0073] Preparation of component A: 20 parts by weight of vinyl polydimethylsiloxane, 7 parts of polydimethylsiloxane, and 70 parts of thermally conductive filler B1 were added to a kettle at once, stirred, and heated. After the temperature reached 120°C, the temperature was maintained and vacuumed. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature returned to room temperature, 0.06 parts of color paste and 0.5 parts of catalyst were added. The mixture was stirred for 30 minutes while maintaining a vacuum of -0.08 MPa to obtain component A.

[0074] Preparation of component B: 18 parts of vinyl polydimethylsiloxane, 5 parts of polydimethylsiloxane, and 70 parts of thermal conductive filler B1 were added into a kettle at one time, stirred and heated. After the temperature rose to 120°C, the temperature was maintained and vacuum was applied. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature dropped to room temperature, 4.2 parts of cross-linking agent I, 0.6 parts of cross-linking agent II, and 0.1 parts of inhibitor were added. The vacuum degree was maintained at -0.08 MPa and stirred for 30 minutes to obtain component B.

[0075] Example 2

[0076] Preparation of component A: 15 parts by weight of vinyl polydimethylsiloxane, 10 parts of polydimethylsiloxane, and 75 parts of thermally conductive filler B1 were added to a kettle at once, stirred, and heated. After the temperature reached 120°C, the temperature was maintained and vacuumed. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature returned to room temperature, 0.08 parts of color paste and 0.5 parts of catalyst were added. The mixture was stirred for 30 minutes while maintaining a vacuum of -0.08 MPa to obtain component A.

[0077] Preparation of component B: 19 parts of vinyl polydimethylsiloxane, 2 parts of polydimethylsiloxane, and 75 parts of thermal conductive filler B1 were added into a kettle at one time, stirred and heated. After the temperature rose to 120°C, the temperature was maintained and vacuum was applied. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature dropped to room temperature, 4 parts of cross-linking agent I, 0.6 parts of cross-linking agent II, and 0.1 parts of inhibitor were added. The vacuum degree was maintained at -0.08 MPa and stirred for 30 minutes to obtain component B.

[0078] Example 3

[0079] Preparation of component A: 16 parts by weight of vinyl polydimethylsiloxane, 8 parts of polydimethylsiloxane, and 80 parts of thermally conductive filler B1 were added to a kettle at once, stirred, and heated. After the temperature reached 120°C, the temperature was maintained and vacuumed. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature returned to room temperature, 0.08 parts of color paste and 0.5 parts of catalyst were added. The mixture was stirred for 30 minutes while maintaining a vacuum of -0.08 MPa to obtain component A.

[0080] Preparation of component B: 16 parts of vinyl polydimethylsiloxane, 4 parts of polydimethylsiloxane, and 80 parts of thermal conductive filler B1 were added into a kettle at one time, stirred and heated. After the temperature rose to 120°C, the temperature was maintained and vacuum was applied. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature dropped to room temperature, 4.3 parts of cross-linking agent I, 0.5 parts of cross-linking agent II, and 0.1 parts of inhibitor were added. The vacuum degree was maintained at -0.08 MPa and stirred for 30 minutes to obtain component B.

[0081] Example 4

[0082] Preparation of component A: 16 parts by weight of vinyl polydimethylsiloxane, 8 parts of polydimethylsiloxane, and 85 parts of non-thermal conductive filler B1 were added to a kettle at once, stirred, and heated. After the temperature reached 120°C, the temperature was maintained and vacuumed. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature returned to room temperature, 0.08 parts of color paste and 0.5 parts of catalyst were added. The mixture was stirred for 30 minutes while maintaining a vacuum of -0.08 MPa to obtain component A.

[0083] Preparation of component B: 16 parts of vinyl polydimethylsiloxane, 4 parts of polydimethylsiloxane, and 85 parts of thermal conductive filler B1 were added into a kettle at one time, stirred and heated. After the temperature rose to 120°C, the temperature was maintained and vacuum was applied. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature dropped to room temperature, 3 parts of cross-linking agent I, 0.7 parts of cross-linking agent II, and 0.1 parts of inhibitor were added. The vacuum degree was maintained at -0.08 MPa and stirred for 30 minutes to obtain component B.

[0084] Example 5

[0085] Preparation of component A: 17 parts by weight of vinyl polydimethylsiloxane, 8 parts of polydimethylsiloxane, and 85 parts of thermally conductive filler B1 were added to a kettle at once, stirred, and heated. After the temperature reached 120°C, the temperature was maintained and vacuumed. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature returned to room temperature, 0.12 parts of color paste and 0.5 parts of catalyst were added. The mixture was stirred for 30 minutes while maintaining a vacuum of -0.08 MPa to obtain component A.

[0086] Preparation of component B: 17 parts of vinyl polydimethylsiloxane, 4 parts of polydimethylsiloxane, and 85 parts of thermally conductive filler B1 were added into a kettle at one time, stirred and heated. After the temperature rose to 120°C, the temperature was maintained and vacuum was applied. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature dropped to room temperature, 4.3 parts of cross-linking agent I, 0.5 parts of cross-linking agent II, and 0.1 parts of inhibitor were added. The vacuum degree was maintained at -0.08 MPa and stirred for 30 minutes to obtain component B.

[0087] Example 6

[0088] Preparation of component A: 20 parts by weight of vinyl polydimethylsiloxane, 5 parts of polydimethylsiloxane, and 90 parts of thermally conductive filler B1 were added to a kettle at once, stirred, and heated. After the temperature reached 120°C, the temperature was maintained and vacuumed. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature returned to room temperature, 0.1 parts of color paste and 0.3 parts of catalyst were added. The mixture was stirred for 30 minutes while maintaining a vacuum of -0.08 MPa to obtain component A.

[0089] Preparation of component B: 15 parts of vinyl polydimethylsiloxane, 4 parts of polydimethylsiloxane, and 90 parts of thermal conductive filler B1 were added into a kettle at one time, stirred and heated. After the temperature rose to 120°C, the temperature was maintained and vacuum was applied. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature dropped to room temperature, 5.5 parts of cross-linking agent I, 0.2 parts of cross-linking agent II, and 0.05 parts of inhibitor were added. The vacuum degree was maintained at -0.08 MPa and stirred for 30 minutes to obtain component B.

[0090] Example 7

[0091] Preparation of component A: 18 parts by weight of vinyl polydimethylsiloxane, 9 parts of polydimethylsiloxane, and 85 parts of thermally conductive filler B1 were added to a kettle at once, stirred, and heated. After the temperature reached 120°C, the temperature was maintained and vacuumed. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature returned to room temperature, 0.08 parts of color paste and 0.6 parts of catalyst were added. The mixture was stirred for 30 minutes while maintaining a vacuum of -0.08 MPa to obtain component A.

[0092] Preparation of component B: By weight, 20 parts of vinyl polydimethylsiloxane, 4 parts of polydimethylsiloxane, and 85 parts of thermal conductive filler B1 were added into a kettle at one time, stirred and heated. After the temperature rose to 120°C, the temperature was maintained and vacuum was applied. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature dropped to room temperature, 5 parts of cross-linking agent I, 0.3 parts of cross-linking agent II, and 0.01 parts of inhibitor were added. The vacuum degree was maintained at -0.08 MPa and stirred for 30 minutes to obtain component B.

[0093] Example 8

[0094] Preparation of component A: 17 parts by weight of vinyl polydimethylsiloxane, 8 parts of polydimethylsiloxane, and 85 parts of thermally conductive filler B2 were added to a kettle at once, stirred, and heated. After the temperature reached 120°C, the temperature was maintained and vacuumed. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature returned to room temperature, 0.12 parts of color paste and 0.5 parts of catalyst were added. The mixture was stirred for 30 minutes while maintaining a vacuum of -0.08 MPa to obtain component A.

[0095] Preparation of component B: 17 parts of vinyl polydimethylsiloxane, 4 parts of polydimethylsiloxane, and 85 parts of thermally conductive filler B2 were put into a kettle at one time, stirred and heated. After the temperature rose to 120°C, the temperature was maintained and vacuum was applied. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature dropped to room temperature, 4.3 parts of cross-linking agent I, 0.5 parts of cross-linking agent II, and 0.1 parts of inhibitor were added. The vacuum degree was maintained at -0.08 MPa and stirred for 30 minutes to obtain component B.

[0096] Comparative Example 1

[0097] Preparation of component A: 17 parts by weight of vinyl polydimethylsiloxane and 85 parts of inorganic thermally conductive filler were added to a kettle at once, stirred and heated. After the temperature reached 120°C, the temperature was maintained and vacuum was applied. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature returned to room temperature, 0.12 parts of color paste and 0.5 parts of catalyst were added. The vacuum was maintained at -0.08 MPa and stirred for 30 minutes to obtain component A.

[0098] Preparation of component B: 17 parts of vinyl polydimethylsiloxane and 85 parts of inorganic thermal conductive filler were put into a kettle at one time by weight, stirred and heated, and after the temperature rose to 120°C, the temperature was maintained and vacuumed. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature dropped to room temperature, 4.3 parts of cross-linking agent I, 0.5 parts of cross-linking agent II and 0.1 parts of inhibitor were added, and the vacuum degree was maintained at -0.08 MPa and stirred for 30 minutes to obtain component B.

[0099] The difference from Example 5 is that polydimethylsiloxane was not added to observe its influence.

[0100] Comparative Example 2

[0101] Preparation of component A: 16 parts by weight of vinyl polydimethylsiloxane, 8 parts of polydimethylsiloxane, and 185 parts of inorganic thermally conductive filler were placed in a kettle at once, stirred, and heated. After the temperature reached 120°C, the temperature was maintained and vacuumed. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature returned to room temperature, 0.08 parts of color paste and 0.5 parts of catalyst were added. The mixture was stirred for 30 minutes while maintaining a vacuum of -0.08 MPa to obtain component A.

[0102] Preparation of component B: 16 parts of vinyl polydimethylsiloxane, 4 parts of polydimethylsiloxane, and 185 parts of inorganic thermal conductive filler were put into a kettle at one time, stirred and heated. After the temperature rose to 120°C, the temperature was maintained and vacuumed. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature dropped to room temperature, 6.3 parts of cross-linking agent I, 0.8 parts of cross-linking agent II, and 0.1 parts of inhibitor were added. The vacuum degree was maintained at -0.08 MPa and stirred for 30 minutes to obtain component B.

[0103] Comparative Example 3

[0104] Preparation of component A: 17 parts by weight of vinyl polydimethylsiloxane, 8 parts of polydimethylsiloxane, and 85 parts of spherical alumina were added to a kettle at once, stirred, and heated. After the temperature reached 120°C, the temperature was maintained and vacuum was applied. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature returned to room temperature, 0.12 parts of color paste and 0.5 parts of catalyst were added. The mixture was stirred for 30 minutes while maintaining a vacuum of -0.08 MPa to obtain component A.

[0105] Preparation of component B: 17 parts of vinyl polydimethylsiloxane, 4 parts of polydimethylsiloxane, and 85 parts of spherical alumina B1 were put into a kettle at one time, stirred and heated. After the temperature rose to 120°C, the temperature was maintained and vacuum was applied. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature dropped to room temperature, 4.3 parts of cross-linking agent I, 0.5 parts of cross-linking agent II, and 0.1 parts of inhibitor were added. The vacuum degree was maintained at -0.08 MPa and stirred for 30 minutes to obtain component B.

[0106] Comparative Example 4

[0107] Preparation of component A: 17 parts by weight of vinyl polydimethylsiloxane, 8 parts of polydimethylsiloxane, and 100 parts of spherical alumina were added to a kettle at once, stirred, and heated. After the temperature reached 120°C, the temperature was maintained and vacuum was applied. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature returned to room temperature, 0.12 parts of color paste and 0.5 parts of catalyst were added. The mixture was stirred for 30 minutes while maintaining a vacuum of -0.08 MPa to obtain component A.

[0108] Preparation of component B: 17 parts of vinyl polydimethylsiloxane, 4 parts of polydimethylsiloxane, and 100 parts of spherical alumina B1 were put into a kettle at one time, stirred and heated. After the temperature rose to 120°C, the temperature was maintained and vacuumed. After stirring for 2 hours, the mixture was stopped and cooled. After the temperature dropped to room temperature, 4.3 parts of cross-linking agent I, 0.5 parts of cross-linking agent II, and 0.1 parts of inhibitor were added. The vacuum degree was maintained at -0.08 MPa and stirred for 30 minutes to obtain component B.

[0109] Table 1: Component ratios of silicone potting compounds in Examples 1 to 5 and Comparative Example 1

[0110]

[0111] Performance testing: The following performance tests were performed on components A and B of the silicone potting adhesives prepared in Examples 1 to 8 and Comparative Examples 1 to 4 and the cured colloids. Specific test data are shown in Table 2.

[0112] Viscosity: Test the viscosity of components A and B separately according to GB / T2794-2013.

[0113] Leveling: After mixing components A and B in a mass ratio of 1:1, accurately weigh 20g of the adhesive on a smooth horizontal glass plate and measure the leveling diameter after 10 minutes.

[0114] Thermal conductivity: Mix components A and B in a mass ratio of 1:1 and solidify to obtain a colloid. Test the thermal conductivity according to GB / T10297-2015.

[0115] Toughness: Mix components A and B in a mass ratio of 1:1 and solidify to obtain a colloid. Cut the colloid into thin slices 2-3 mm thick, fold it in half, and observe whether it can be broken.

[0116] Table 2: Test data of the silicone potting compound prepared in Examples 1 to 5 and Comparative Example 1

[0117]

[0118] Combining the data from Examples 1-8 and Table 2, it can be seen that as the amount of inorganic thermally conductive filler increases, the thermal conductivity and viscosity of the resulting potting compound increase, while the leveling property decreases. Comparing various performance factors, the ratio of components A to B in Example 5 is more optimal.

[0119] Combining the data of Comparative Examples 1 to 4 and Table 2, it can be seen that when polydimethylsiloxane is not added to the system of Comparative Example 1, the leveling property of the obtained potting glue is obviously affected, resulting in poor fluidity. Due to the inappropriate ratio of the cross-linking agent in Comparative Example 2, the toughness of the colloid is poor, and it cannot meet the protective effect of the packaged device. After the prepared thermal conductive filler is replaced with spherical alumina in equal amount in Comparative Example 3, its thermal conductivity is greatly reduced, which is not conducive to the heat dissipation of electrical components. After the amount of spherical alumina added in Comparative Example 3 is greatly increased, its thermal conductivity is still not significantly improved. On the contrary, its viscosity, leveling and toughness are significantly reduced.

Claims

1. A thermally conductive filler, characterized in that: The thermally conductive filler comprises mesoporous alumina; At least a portion of the surface of the mesoporous alumina is loaded with nano-copper particles; At least a portion of the surface of the mesoporous aluminum oxide and the nano-copper particles is covered with a silicon dioxide layer.

2. The thermally conductive filler according to claim 1, wherein: The preparation method of the thermally conductive filler is as follows: (1) reacting alumina with an etching solution to obtain spherical mesoporous alumina; (2) placing mesoporous alumina in a solution containing a copper precursor and a silica precursor with an alkoxy group, uniformly dispersing the solution, and then adding an acidic reducing agent to reduce the copper precursor to obtain nano-copper particles, and hydrolyzing the silica precursor to form polysiloxane, thereby coating the mesoporous alumina and the nano-copper particles, and obtaining mesoporous alumina loaded with nano-copper particles and polysiloxane; (3) The mesoporous alumina loaded with nano-copper particles and polysiloxane is washed, dried, and thermally decomposed under the protection of an inert gas to obtain the thermal conductive filler.

3. The thermally conductive filler according to claim 2, wherein: The silicon dioxide precursor is obtained by reacting alkoxysilane with a silicon-hydrogen structure with N-vinyl pyrrolidone through a silicon-hydrogen addition reaction.

4. A two-component silicone potting compound, characterized in that: Includes component A and component B; The component A includes vinyl polydimethylsiloxane, polydimethylsiloxane, color paste and catalyst; The B component includes vinyl polydimethylsiloxane, polydimethylsiloxane, a crosslinking agent and an inhibitor; At least one of the components A and B contains the thermally conductive filler according to any one of claims 1 to 3.

5. The two-component silicone potting adhesive according to claim 4, characterized in that: The cross-linking agent includes cross-linking agent I and cross-linking agent II; The crosslinking agent I is a hydrogen-terminated silicone oil with a hydrogen content of 0.1-0.5%; The crosslinking agent II is a hydrogenated silicone oil with a hydrogen content of 0.4-0.8%.

6. The two-component silicone potting adhesive according to claim 4, characterized in that: The catalyst is a platinum catalyst, and its content is 3000ppm.

7. The two-component silicone potting adhesive according to claim 4, characterized in that: The inhibitor includes one or more of 1-hexynyl-1-cyclohexanol, 2-phenyl-3-butynyl-2-ol, 3,5-dimethyl-1-hexynyl-3-ol, 2-methyl-3-butynyl-2-ol and vinyl ring.

8. The two-component silicone potting adhesive according to claim 5, characterized in that: It consists of component A and component B; The component A comprises the following raw materials in parts by weight: 15-20 parts of vinyl polydimethylsiloxane, 5-10 parts of polydimethylsiloxane, 70-90 parts of the thermal conductive filler according to any one of claims 1 to 3, 0.06-0.12 parts of color paste, and 0.3-0.6 parts of catalyst; The component B comprises the following raw materials in parts by weight: 15-20 parts of vinyl polydimethylsiloxane, 2-5 parts of polydimethylsiloxane, 70-90 parts of the thermally conductive filler according to any one of claims 1 to 3, 4-6 parts of crosslinking agent I, 0.2-0.7 parts of crosslinking agent II, and 0.05-0.1 parts of inhibitor.

9. The two-component silicone potting adhesive according to claim 8, characterized in that: The mass ratio of component A to component B is 1:

1.

10. A method for preparing a two-component silicone potting compound according to any one of claims 4 to 9, characterized in that: The following steps are involved: Preparation of component A: vinyl polydimethylsiloxane, polydimethylsiloxane, and the thermally conductive filler according to any one of claims 1 to 3 are added to a kettle at once, stirred and heated, and after the temperature rises to 120° C., the temperature is maintained and vacuumed. After stirring for 2 hours, the mixture is stopped and cooled. After the temperature drops to room temperature, the color paste and catalyst are added, and the vacuum degree is maintained at -0.08 MPa and stirred for 30 minutes to obtain component A. Preparation of component B: vinyl polydimethylsiloxane, polydimethylsiloxane, and the thermally conductive filler according to any one of claims 1 to 3 are added into a kettle at once, stirred and heated, and after the temperature rises to 120°C, the temperature is maintained and vacuum is applied. After stirring for 2 hours, the mixture is stopped and cooled. After the temperature drops to room temperature, a cross-linking agent and an inhibitor are added, and the vacuum degree is maintained at -0.08 MPa and stirred for 30 minutes to obtain component B.

Citation Information

Patent Citations

  • Modified alumina composite material, copper-coated substrate and preparation method of copper-coated substrate

    CN104371274A

  • Nano copper oxide loaded mesoporous-alumina hollow microspheres and preparation and application thereof

    CN108704644A

  • Heat-conducting filler, thermal interface material and preparation method of heat-conducting filler and thermal interface material

    CN115678105A

  • Method for manufacturing silica-coated metallic composite powder, and silica-coated metallic composite powder

    JP2003013106A

  • Method for manufacturing metal particle composite

    JP2010253436A