Lithium-rich manganese-based positive electrode material, preparation method therefor, and use thereof
Through the coating technology of doped niobium oxide and lithium phosphate, the problem of low structural instability and conductivity of lithium-rich manganese-based positive electrode materials during circulation is solved, and the high capacity and voltage retention performance is improved. It is suitable for lithium Application of ion batteries.
Patent Information
- Application Number
- PCT/CN2023/111876
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2023-08-09
- Publication Date
- 2024-11-28
AI Technical Summary
During the charging and discharging process, lithium-rich manganese-based positive electrode materials have problems such as low electronic and ion conductivity and poor structural stability, which leads to the gradual attenuation of the discharge specific capacity and average voltage as the number of cycles increases, limiting its commercial application.
The rock salt structure is formed by doping niobium oxide, and the inner layer of lithium phosphate and the outer layer of full surface are coated to limit the production of lattice oxygen, prevent structural transformation and decrease in manganese valence, and improve the stability and capacity maintenance of the material.
The capacity maintenance and circulation performance of lithium-rich manganese-based positive electrode materials is significantly improved, and the voltage maintenance performance is voltage maintenance. The discharge capacity of 1C can reach more than 244mAh/g, the discharge capacity of 5C can reach more than 210mAh/g, and the capacity retention rate can reach 91.1 after 400 cycles. %above.
Smart Images

Figure CN2023111876_28112024_PF_FP_ABST
Abstract
Description
A lithium-rich manganese-based positive electrode material and its preparation method and application Technical Field
[0001] The present application belongs to the technical field of lithium-ion batteries and relates to a lithium-rich manganese-based positive electrode material and a preparation method and application thereof. Background Art
[0002] Layered lithium-rich manganese-based cathode materials offer distinct advantages, such as high specific capacity, high energy density, and environmental friendliness, making them the ideal choice for next-generation commercial cathode materials. However, these materials often suffer from low electronic and ionic conductivity and poor structural stability. This leads to a gradual decay in discharge specific capacity and average voltage with increasing cycle number during charge and discharge, a major limitation to their commercialization.
[0003] Among them, the positive electrode material is an important factor in determining a series of key indicators of lithium batteries, such as energy density, cycle performance, and cost. Precursors are the main raw materials for preparing battery positive electrode materials. Currently, the discharge capacity of most commercial lithium batteries is less than 200mAh / g, and the operating voltage generally does not exceed 4.3V. However, lithium-rich manganese-based positive electrode materials have an operating voltage range of 2.0-4.8V and a discharge capacity exceeding 250mAh / g, making them an excellent choice for achieving a high specific energy of 400Wh / kg for lithium-ion batteries.
[0004] During charging, the release of lattice oxygen destabilizes the transition metal elements on the surface of the material, forming a spinel-like structure. This spinel structure gradually permeates the interior of the material, causing the discharge voltage to continue to drop. Furthermore, the release of oxygen lowers the valence of the transition metal manganese, causing it to dissolve, thus reducing capacity.
[0005] CN111640931A discloses a method for preparing a lithium-rich manganese-based positive electrode material, comprising the following steps: S1, preparing a magnesium-doped precursor by a carbonate co-precipitation method: dissolving nickel salt, manganese salt and magnesium salt in water to obtain a mixed metal salt solution, and injecting the mixed metal salt solution and a precipitant solution into a reactor respectively, adjusting the pH value with a complexing agent, reacting for 24-120 hours to generate a precipitate, and washing, drying, crushing and sieving the precipitate to obtain a precursor; S2, mixing the precursor with a lithium source and calcining: after fully grinding and mixing the precursor and the lithium source, sintering to obtain the positive electrode material.
[0006] CN105489842A discloses a lithium-rich manganese-based positive electrode material and a preparation method thereof, the preparation method comprising the following steps: (1) preparing a precursor; (2) dissolving a lithium source and an organic acid or a sugar substance in water, dripping the obtained solution into the precursor for reaction, and heating to form a gel after the dripping is completed; (3) drying the gel, grinding, sieving, calcining, cooling, and then crushing and sieving to obtain the lithium-rich manganese-based positive electrode material.
[0007] The above scheme uses a coprecipitation method, where a salt solution, an alkaline solution, and a complexing agent solution are separately introduced into a reactor containing a base liquid and a protective gas for constant temperature coprecipitation. After the reaction, the overflow is subjected to solid-liquid separation, aging, centrifugation, and drying to obtain a spherical precursor material. This application uses doping and double-layer coating to reduce the voltage and capacity decay problems of lithium-rich manganese-based positive electrode materials.
[0008] Summary of the Invention
[0009] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0010] The purpose of the present application is to provide a lithium-rich manganese-based positive electrode material and its preparation method and application. The present application forms a rock salt structure by doping niobium oxide to prevent structural transformation; an inner layer of lithium phosphate is coated to supplement the lithium source; and an outer layer is coated on the entire surface to limit the reaction of lattice oxygen.
[0011] To achieve the purpose of this application, this application adopts the following technical solutions:
[0012] In a first aspect, an embodiment of the present application provides a method for preparing a lithium-rich manganese-based positive electrode material, the preparation method comprising the following steps:
[0013] (1) mixing a nickel source, a cobalt source, and a manganese source to obtain a ternary liquid, adding the ternary liquid, liquid alkali, and ammonia water to the bottom liquid in parallel for a coprecipitation reaction to obtain precursor particles, and mixing the precursor particles with a lithium source for one-step sintering to obtain a single-fired material;
[0014] (2) mixing the calcined material and the ethanol solution of Nb2O5, and reacting the mixture with the lithium phosphate solution after annealing to obtain the inner layer coated lithium-rich manganese-based positive electrode material;
[0015] (3) The inner layer coated lithium-rich manganese-based positive electrode material is mixed with a nickel source, heated and stirred, and then the obtained solid is mixed with an ethanol solution of NaBH4 and stirred to obtain the lithium-rich manganese-based positive electrode material.
[0016] In the lithium-rich manganese-based positive electrode material prepared by the method described in the embodiment of the present application, Nb2O5 is doped to convert the layered structure of the outer layer into a rock salt structure, thereby preventing the lithium-rich manganese-based layered structure from transforming into a spinel structure. The inner layer of Li2PO4 is coated, and since oxygen reacts with free lithium ions to form Li2O, lithium is continuously replenished to slow down capacity decay. Then, the entire surface of the outer layer of niobium is coated to limit the generation of lattice oxygen, thereby increasing the initial capacity and preventing defects such as voltage decay and thermal effect runaway.
[0017] In one embodiment, the molar ratio of the nickel source, cobalt source and manganese source in step (1) is x:y:c, wherein x+y+c=1, 0.1 <x≤0.4,0≤y≤0.2,0.5≤c≤0.8。
[0018] In one embodiment, the concentration of the ternary solution is 1.6 to 2.4 mol / L, for example, 1.6 mol / L, 1.8 mol / L, 2 mol / L, 2.2 mol / L or 2.4 mol / L.
[0019] In one embodiment, the alkali solution includes sodium hydroxide solution and / or potassium hydroxide solution.
[0020] In one embodiment, the concentration of the alkali solution is 9-12 mol / L, for example, 9 mol / L, 10 mol / L, 11 mol / L or 12 mol / L.
[0021] In one embodiment, the concentration of the ammonia solution is 7 to 10 mol / L, for example, 7 mol / L, 8 mol / L, 9 mol / L or 10 mol / L.
[0022] In one embodiment, the pH of the base solution in step (1) is 9 to 12, for example, 9, 10, 11 or 12.
[0023] In one embodiment, the ammonia concentration of the base solution is 1-8 g / L, for example, 1 g / L, 2 g / L, 4 g / L, 5 g / L or 8 g / L.
[0024] In one embodiment, the pH of the coprecipitation reaction is 9-13, for example, 9, 10, 11, 12 or 13.
[0025] In one embodiment, the stirring speed of the coprecipitation reaction is 200-380 rpm, for example, 200 rpm, 250 rpm, 280 rpm, 320 rpm or 380 rpm.
[0026] In one embodiment, the particle size of the precursor particles is 7 to 25 μm, for example, 7 μm, 10 μm, 15 μm, 20 μm or 25 μm.
[0027] In one embodiment, the lithium source includes lithium carbonate.
[0028] In one embodiment, the temperature of the one-step sintering is 750-850°C, for example, 750°C, 780°C, 800°C, 820°C or 850°C.
[0029] In one embodiment, the one-step sintering time is 10 to 15 hours, for example, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours or 15 hours.
[0030] In one embodiment, the concentration of the Nb2O5 ethanol solution in step (2) is 2-5%, for example, 2%, 3%, 4% or 5%.
[0031] In one embodiment, the annealing treatment is performed at a temperature of 500-700° C., for example, 500° C., 550° C., 600° C., 650° C., or 700° C.
[0032] In one embodiment, the annealing treatment time is 5 to 8 hours, for example, 5 hours, 6 hours, 7 hours or 8 hours.
[0033] In one embodiment, the reaction temperature in step (2) is 400-600°C, for example, 400°C, 450°C, 500°C, 550°C or 600°C.
[0034] In one embodiment, the reaction time is 2 to 4 hours, for example, 2 hours, 2.5 hours, 3 hours, 3.5 hours or 4 hours.
[0035] In one embodiment, the nickel source in step (3) comprises a mixed solution of NiCl2 and anhydrous ethanol.
[0036] In one embodiment, the temperature of the heating and stirring is 110-130°C, for example, 110°C, 115°C, 120°C, 125°C or 130°C.
[0037] In one embodiment, the atmosphere for heating and stirring comprises a nitrogen atmosphere.
[0038] In one embodiment, the heating and stirring time is 1.5 to 3 hours, for example, 1.5 hours, 1.8 hours, 2 hours, 2.5 hours or 3 hours.
[0039] In one embodiment, the stirring time is 1.5 to 3 hours, for example, 1.5 hours, 1.8 hours, 2 hours, 2.5 hours or 3 hours.
[0040] In a second aspect, an embodiment of the present application provides a lithium-rich manganese-based positive electrode material, which is prepared by the method described in the first aspect.
[0041] In one embodiment, the lithium-rich manganese-based positive electrode material includes a lithium-rich manganese-based core and a double-layer coating layer of a polycrystalline rock salt structure disposed on the surface of the lithium-rich manganese-based core.
[0042] In a third aspect, an embodiment of the present application provides a positive electrode plate, which comprises the lithium-rich manganese-based positive electrode material as described in the second aspect.
[0043] In a fourth aspect, an embodiment of the present application provides a lithium-ion battery, wherein the lithium-ion battery comprises the positive electrode sheet as described in the third aspect.
[0044] Compared with the prior art, this application has the following beneficial effects:
[0045] (1) The present application forms a rock salt structure by doping niobium oxide to prevent structural transformation; an inner layer of lithium phosphate is coated to supplement the lithium source; and an outer layer is coated on the entire surface to limit the reaction of lattice oxygen, thereby significantly improving the capacity retention, cycle performance, and voltage retention performance of the lithium-rich manganese-based positive electrode material.
[0046] (2) The lithium-rich manganese-based positive electrode material prepared by the method described in this application can produce a battery with a 1C discharge capacity of more than 244 mAh / g, a 5C discharge capacity of more than 210 mAh / g, and a capacity retention rate of more than 91.1% after 400 (1C) cycles.
[0047] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of this application, they are used to explain the technical solution of this article and do not constitute a limitation to the technical solution of this article.
[0049] FIG1 is a SEM image of the lithium-rich manganese-based positive electrode material described in Example 1 of the present application. DETAILED DESCRIPTION
[0050] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.
[0051] Example 1
[0052] (1) A sulfate solution A containing nickel ions, cobalt ions and manganese ions with a total ion concentration of 2 mol / L is prepared, wherein the molar ratio of nickel ions, cobalt ions and manganese ions is 20:10:70, an industrial liquid alkali with a concentration of 10 mol / L is used as a precipitant solution B, and a 9 mol / L ammonia solution is used as a complexing agent solution C. A bottom liquid D is prepared in a reactor, the pH of the bottom liquid D is controlled at 10, the ammonia concentration of D is 5 g / L, and the temperature of D is 30-60°C; and nitrogen is introduced as a protective gas, and the mixed salt solution A, the precipitant solution B and the complexing agent solution C are mixed. The bottom liquid is added in parallel, and a co-precipitation reaction is carried out at a normal stirring paddle speed of 300 rpm to obtain seed particles with a particle size of 12 μm and a target particle size D50. The obtained spherical nickel manganese zirconium precursor is centrifuged, washed, dried, and subjected to treatments such as magnetic foreign matter removal to obtain spherical precursor particles. The reacted material is centrifuged and washed in a centrifuge, and then dried at a certain temperature. The precursor powder is pre-calcined at 400°C for 5 hours, and then uniformly mixed with Li2CO3 powder according to the element ratio, and calcined at 800°C in an air atmosphere for 12 hours to obtain LMR;
[0053] (2) LMR was dispersed in a 3% (Nb2O5) ethanol solution, the suspension was ultrasonically stirred and dried, and then annealed at 600°C for 6 h (N-LMR). N-LMR was added to a lithium phosphate solution and heated to 500°C for 3 h to obtain an inner layer-coated lithium-rich manganese-based cathode material (LN-LMR);
[0054] (3) LN-LMR was added to NiCl2·6H2O and anhydrous ethanol solution and nitrogen was introduced to protect the temperature, raised to 120°C and stirred for 2 hours, and then washed and dried, and then added to NaBH4 anhydrous ethanol solution and continued to stir for 2 hours, and then washed and dried to obtain the lithium-rich manganese-based positive electrode material. The SEM image of the lithium-rich manganese-based positive electrode material is shown in Figure 1. It can be seen from Figure 1 that the lithium-rich manganese-based positive electrode material in this embodiment is a polycrystalline rock salt structure double-layer coated lithium-rich manganese-based positive electrode material.
[0055] Example 2
[0056] This embodiment provides a lithium-rich manganese-based positive electrode material, and the preparation method of the lithium-rich manganese-based positive electrode material is as follows:
[0057] This embodiment provides a lithium-rich manganese-based positive electrode material, and the preparation method of the lithium-rich manganese-based positive electrode material is as follows:
[0058] (1) A sulfate solution A containing nickel ions, cobalt ions and manganese ions with a total ion concentration of 2 mol / L is prepared, wherein the molar ratio of nickel ions, cobalt ions and manganese ions is 30:10:60, an industrial liquid alkali with a concentration of 10.5 mol / L is used as a precipitant solution B, and a 9.2 mol / L ammonia solution is used as a complexing agent solution C. A bottom liquid D is prepared in a reactor, the pH of the bottom liquid D is controlled at 10, the ammonia concentration of D is 5.5 g / L, and the temperature of D is 30-60°C; and nitrogen is introduced as a protective gas, and the mixed salt solution A, the precipitant solution B and the complexing agent solution C are mixed. Solution C was added to the bottom liquid in parallel, and a co-precipitation reaction was carried out at a normal stirring paddle speed of 320 rpm to obtain seed particles with a particle size of 15 μm and a target particle size D50. The obtained spherical nickel manganese zirconium precursor was centrifuged, washed, dried, and subjected to treatments such as magnetic foreign matter removal to obtain spherical precursor particles. The reacted material was centrifuged and washed, and then dried at a certain temperature. The precursor powder was pre-calcined at 400 ° C for 5 h, and then uniformly mixed with Li2CO3 powder according to the element ratio, and calcined at 820 ° C in air atmosphere for 12 h to obtain LMR;
[0059] (2) LMR was dispersed in a 3.5% (Nb2O5) ethanol solution, the suspension was ultrasonically stirred and dried, and then annealed at 630°C for 6 h (N-LMR). The N-LMR was added to a lithium phosphate solution and heated to 520°C for 3 h to obtain an inner layer-coated lithium-rich manganese-based cathode material (LN-LMR);
[0060] (3) LN-LMR was added to NiCl2·6H2O and anhydrous ethanol solution and nitrogen was introduced to protect the temperature, raised to 120°C and stirred for 2 hours, then washed and dried, and then added to NaBH4 anhydrous ethanol solution and continued to stir for 2 hours, and then washed and dried to obtain the lithium-rich manganese-based positive electrode material.
[0061] Example 3
[0062] The only difference between this embodiment and embodiment 1 is that the concentration of the Nb2O5 ethanol solution is 1%, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0063] Example 4
[0064] The only difference between this embodiment and embodiment 1 is that the concentration of the Nb2O5 ethanol solution is 6%, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0065] Example 5
[0066] The only difference between this embodiment and embodiment 1 is that the annealing temperature in step (2) is 400° C., and the other conditions and parameters are exactly the same as those in embodiment 1.
[0067] Example 6
[0068] The only difference between this embodiment and embodiment 1 is that the annealing temperature in step (2) is 800° C., and the other conditions and parameters are exactly the same as those in embodiment 1.
[0069] Comparative Example 1
[0070] The only difference between this comparative example and Example 1 is that the inner layer is not doped with Nb2O5, and the other conditions and parameters are exactly the same as those in Example 1.
[0071] Comparative Example 2
[0072] The only difference between this comparative example and Example 1 is that the inner layer coating of Li2PO4 is not performed, and the other conditions and parameters are exactly the same as those in Example 1.
[0073] Comparative Example 3
[0074] The only difference between this comparative example and Example 1 is that no outer coating is performed, and other conditions and parameters are exactly the same as those in Example 1.
[0075] Comparative Example 4
[0076] The only difference between this comparative example and Example 1 is that a commercially available lithium-rich manganese-based precursor is used, and other conditions and parameters are exactly the same as those in Example 1.
[0077] Performance testing:
[0078] The electrode materials, acetylene black, and polyvinylidene fluoride prepared in the Examples and Comparative Examples were added dropwise to N-methyl-2-pyridine to prepare a solution. The solution was then evenly applied to aluminum foil, dried, and punched into thin sheets. The battery electrode, elemental sodium sheet, glass fiber separator, electrolyte (NaClO4) gasket, spring, and battery case were assembled into button cells in an Ar glove box. Performance testing was performed, and the test results are shown in Table 1.
[0079] Table 1
[0080] As can be seen from Table 1, according to Examples 1-2, the lithium-rich manganese-based positive electrode material prepared by the method described in the present application can produce a battery with a 1C discharge capacity of more than 244 mAh / g, a 5C discharge capacity of more than 210 mAh / g, and a capacity retention rate of more than 91.1% after 400 (1C) cycles.
[0081] By comparing Example 1 with Examples 3-4, it can be seen that during the preparation process of the lithium-rich manganese-based positive electrode material described in the present application, the concentration of the Nb2O5 ethanol solution will affect the performance of the obtained lithium-rich manganese-based positive electrode material. When the concentration of the Nb2O5 ethanol solution is controlled at 2-5%, the performance of the lithium-rich manganese-based positive electrode material is better. If the concentration of the Nb2O5 ethanol solution is too low, the outer coating layer is thin and uneven. If the concentration of the Nb2O5 ethanol solution is too high, the coating layer is complete but too thick.
[0082] By comparing Example 1 with Examples 5-6, it can be seen that in the preparation process of the lithium-rich manganese-based positive electrode material described in the present application, the temperature of the annealing treatment will affect the performance of the obtained lithium-rich manganese-based positive electrode material. The annealing treatment temperature is controlled at 500-700°C, and the performance of the obtained lithium-rich manganese-based positive electrode material is better. If the annealing treatment temperature is too low, the internal crystal structure defects cannot be eliminated. If the annealing treatment temperature is too high, the material itself will be damaged, the mechanical properties of the material will deteriorate, and microcracks will be easily generated inside.
[0083] From the comparison between Example 1 and Comparative Example 1, it can be seen that in the lithium-rich manganese-based positive electrode material described in the present application, Nb2O5 doping converts the layered structure of the outer layer into a rock salt structure, preventing the lithium-rich manganese-based layered structure from transforming into a spinel structure.
[0084] From the comparison between Example 1 and Comparative Example 2, it can be seen that in the lithium-rich manganese-based positive electrode material described in the present application, the inner layer of Li2PO4 is coated, and since oxygen and free lithium ions generate Li2O, lithium is continuously replenished to slow down capacity decay.
[0085] From the comparison between Example 1 and Comparative Example 3, it can be seen that in the lithium-rich manganese-based positive electrode material described in the present application, the outer layer is coated on the entire surface, which limits the generation of lattice oxygen, increases the initial capacity, and thus prevents defects such as voltage decay and thermal effect runaway.
[0086] From the comparison between Example 1 and Comparative Example 4, it can be seen that the method described in the present application produces loose spherical precursor particles, which is more conducive to Nb2O5 doping in the prepared positive electrode material, and further facilitates the transformation of the outer layer layer structure into a rock salt structure.
[0087] The applicant declares that the above is only a specific implementation method of the present application, but the protection scope of the present application is not limited thereto. Technical personnel in the relevant technical field should understand that any changes or substitutions that can be easily thought of by technical personnel in the relevant technical field within the technical scope disclosed in this application fall within the protection scope and disclosure scope of this application.
Claims
1. A method for preparing a lithium-rich manganese-based positive electrode material, the preparation method comprising the following steps: (1) mixing a nickel source, a cobalt source and a manganese source to obtain a ternary liquid, adding the ternary liquid, liquid alkali and ammonia water to the bottom liquid in parallel for a coprecipitation reaction to obtain precursor particles, and mixing the precursor particles with a lithium source for one-step sintering to obtain a single-fired material; (2) mixing a calcined material and an ethanol solution of Nb2O5, and reacting the mixture with a lithium phosphate solution after annealing to obtain an inner layer coated lithium-rich manganese-based positive electrode material; (3) The inner layer coated lithium-rich manganese-based positive electrode material is mixed with a nickel source, and after heating and stirring, the obtained solid is mixed with an ethanol solution of NaBH4 and stirred to obtain the lithium-rich manganese-based positive electrode material.
2. The preparation method according to claim 1, wherein The molar ratio of the nickel source, cobalt source and manganese source in step (1) is x:y:c, wherein x+y+c=1, 0.1 <x≤0.4,0≤y≤0.2,0.1<x≤0.4,0≤y≤0.2,0.5≤c≤0.8; Optionally, the concentration of the ternary solution is 1.6 to 2.4 mol / L; Optionally, the alkali solution includes sodium hydroxide solution and / or potassium hydroxide solution; Optionally, the concentration of the alkali solution is 9 to 12 mol / L; Optionally, the concentration of the ammonia water is 7 to 10 mol / L.
3. The preparation method according to claim 1 or 2, wherein: The pH of the base solution in step (1) is 9 to 12; Optionally, the ammonia concentration of the base solution is 1 to 8 g / L; Optionally, the pH of the coprecipitation reaction is 9 to 13; Optionally, the stirring speed of the coprecipitation reaction is 200 to 380 rpm; Optionally, the particle size of the precursor particles is 7 to 25 μm; Optionally, the lithium source comprises lithium carbonate; Optionally, the one-step sintering temperature is 750-850°C; Optionally, the one-step sintering time is 10 to 15 hours.
4. The preparation method according to any one of claims 1 to 3, wherein The concentration of the Nb2O5 ethanol solution in step (2) is 2-5%.
5. The preparation method according to any one of claims 1 to 4, wherein: The temperature of the annealing treatment in step (2) is 500-700° C. Optionally, the annealing treatment time is 5 to 8 hours.
6. The preparation method according to any one of claims 1 to 5, wherein: The reaction temperature in step (2) is 400-600° C. Optionally, the reaction time is 2 to 4 hours.
7. The preparation method according to any one of claims 1 to 6, wherein: The nickel source in step (3) comprises a mixed solution of NiCl2 and anhydrous ethanol; Optionally, the temperature of the heating and stirring is 110 to 130° C.; Optionally, the atmosphere for heating and stirring includes a nitrogen atmosphere; Optionally, the heating and stirring time is 1.5 to 3 hours; Optionally, the stirring time is 1.5 to 3 hours.
8. A lithium-rich manganese-based positive electrode material, wherein the lithium-rich manganese-based positive electrode material is prepared by the method according to any one of claims 1 to 7.
9. The lithium-rich manganese-based positive electrode material according to claim 8, wherein: The lithium-rich manganese-based positive electrode material comprises a lithium-rich manganese-based core and a double-layer coating layer with a polycrystalline rock salt structure arranged on the surface of the lithium-rich manganese-based core. 10 . A positive electrode plate, comprising the lithium-rich manganese-based positive electrode material according to claim 9 . 11 . A lithium ion battery, comprising the positive electrode sheet according to claim 10 .
Citation Information
Patent Citations
High-nickel positive electrode material with rock salt phase thin layer on primary particle surface layer and preparation method thereof
CN111740096A
Preparation method of niobium modified lithium-rich manganese-based material, positive electrode material and lithium ion battery
CN113184923A
Electrode material, and preparation method and application thereof
CN113745478A
Modified lithium-rich manganese-based positive electrode material and preparation method thereof
CN113823786A
Lithium nickel manganese oxide positive electrode material as well as preparation method and application thereof
CN114843501A
Cited By
Synthesis method of solid electrolyte and carbon composite coated lithium-rich manganese-based positive electrode material
CN119581538A
Lithium-rich manganese-based material for all-solid-state battery as well as preparation method and application of lithium-rich manganese-based material
CN119706967A
Positive electrode material, secondary battery and electric device
CN119833604A
Double-layer coated full-concentration gradient positive electrode material and preparation method and application thereof
CN121097043A