Star-shaped styrene-grafted butadiene-isoprene modified rubber, preparation method therefor, and use thereof
Through the star-shaped structure of styrene grafted butadiene-isoprene modified rubber, the problem of insufficient rolling resistance and slippage resistance of high styrene rubber is solved, high hardness and wear resistance are achieved, and the Process and reduce costs, suitable for a variety of rubber products.
Patent Information
- Application Number
- PCT/CN2023/130991
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2023-11-10
- Publication Date
- 2024-11-28
AI Technical Summary
The existing high styrene rubber has poor rolling resistance, slip resistance and wear resistance, and has complex production processes, high cost, and low equipment utilization, making it difficult to take into account the comprehensive performance and dynamic mechanical properties of rubber.
Star styrene grafted butadiene-isoprene modified rubber is used to form a polymer chain with a star structure through homopolymerization and coupling reaction, and the styrene homopolymerization segment and butyl are connected by coupling agent. Diene-isoprene copolymerization segments form a mixing arm structure to improve the compatibility and adhesion of rubber.
Achieve high hardness, strength and branching of rubber, improve slip resistance and reduce rolling resistance, simplify process flow, reduce production costs, improve equipment utilization, and maintain good results when mixed with natural rubber performance.
Smart Images

Figure CN2023130991_28112024_PF_FP_ABST
Abstract
Description
Star-shaped styrene-grafted butadiene-isoprene modified rubber and its preparation method and application
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of Chinese patent application No. 202310589831.6 filed on May 23, 2023, the contents of which are incorporated herein by reference. Technical Field
[0003] The present invention relates to the field of rubber preparation, and in particular to a star-shaped styrene-grafted butadiene-isoprene modified rubber and a preparation method and application thereof. Background Art
[0004] A copolymer composed of isoprene or butadiene and styrene, typically containing 23-30% bound styrene. A high bound styrene content results in a copolymer with greater plasticity; conversely, a low bound styrene content results in a copolymer with greater elasticity. Copolymers with a styrene content between 45-70% in their molecular structure are generally referred to as high-styrene rubbers, while those with a bound styrene content of 70% or more are referred to as high-styrene resins. Due to the high bound styrene content in high-styrene rubber, its physical properties differ from those of general-purpose styrene-butadiene rubber. High-styrene rubber is rarely used alone. When used in combination with various synthetic or natural rubbers, it can improve the rigidity, hardness, wear resistance, tear resistance, dielectric properties, and other properties of rubber products. It is widely used in the tire, shoe, printing, and other industries, and is also highly valued for its use in the modification of synthetic plastics.
[0005] Most existing technologies use latex co-coagulation technology. Although this process can produce high-styrene rubber with good performance, the main problems of this method are: first, in terms of process, it is necessary to separately synthesize SBR-1500 or SBR-1502 latex and high-styrene resin emulsion, mix the two emulsions that pass analysis in a certain proportion, and then obtain the high-styrene rubber through coagulation and drying. The process flow is relatively long and requires two synthesis steps, such as the preparation of the aqueous phase, the oil phase, and the initiator, and degassing. Secondly, in terms of production cost, since the monomer conversion rate of the synthesized SBR-1500 or SBR-1502 latex is only 70%, unreacted monomers account for 30%, and this portion of monomers is difficult to recover in small and medium-sized production equipment, resulting in high production costs and relatively large amounts of equipment, auxiliary raw materials, personnel, time, and energy required for the polymerization reaction process. In addition, in terms of production cycle, since the synthesis temperature of the high-styrene resin emulsion is high, there is a large amount of structural gel in the polymerization kettle. The polymerization kettle used generally needs to be cleaned once after producing 10 batches, resulting in low equipment utilization.
[0006] Although high-styrene rubber can be produced through blending and copolymerization, these polymers often suffer from insufficient tensile strength and hardness, as well as poor compatibility with natural rubber and styrene-butadiene rubber. Consequently, the resulting high-styrene rubber fails to maintain optimal overall performance and improve its dynamic mechanical properties. Furthermore, the process is complex, operationally difficult, with long reaction cycles, high costs, and the tendency to gel, which can cause environmental pollution.
[0007] In the existing technology, high styrene rubber is mainly produced at home and abroad by emulsion polymerization of butadiene and styrene monomers. The rolling resistance, anti-skid and wear resistance of the prepared high styrene rubber are poor. Taking into account the comprehensive performance of rubber and improving the dynamic mechanical properties of rubber are problems that need to be solved in this field.
[0008] Summary of the Invention
[0009] The purpose of the present invention is to overcome the problems of poor rolling resistance, wet skid resistance and wear resistance of high styrene rubber in the prior art, and to provide a star-shaped styrene-grafted butadiene-isoprene modified rubber and its preparation method and application.
[0010] In order to achieve the above-mentioned object, the first aspect of the present invention provides a star-shaped styrene-grafted butadiene-isoprene modified rubber, wherein the modified rubber comprises a polymer segment from a coupling agent and a plurality of styrene homopolymer segments and butadiene-isoprene copolymer segments grafted onto the polymer segment, wherein the coupling agent is selected from polyvinyl aromatic monomers.
[0011] A second aspect of the present invention provides a method for preparing a star-shaped styrene-grafted butadiene-isoprene modified rubber, wherein the preparation method comprises:
[0012] (1) In the presence of an initiator, styrene undergoes homopolymerization to obtain an active styrene homopolymer segment;
[0013] (2) coupling the active styrene homopolymer segment with a coupling agent to obtain an active chain;
[0014] (3) In the presence of a polar activator, the active chain, butadiene and isoprene are copolymerized to obtain the star-shaped mixed arm high styrene rubber.
[0015] The third aspect of the present invention provides a star-shaped styrene-grafted butadiene-isoprene modified rubber obtained by the preparation method.
[0016] The fourth aspect of the present invention provides an application of the star-shaped styrene-grafted butadiene-isoprene modified rubber in the field of rubber processing.
[0017] Through the above technical solution, the present invention provides a star-shaped styrene-grafted butadiene-isoprene modified rubber. From the perspective of polymer chain structure, it is a branched polymer with a star-shaped structure. That is, multiple molecular chains are grafted onto the polymer segment to form different segments as branches. Similar connected molecular arms (such as polybutadiene-isoprene arms and styrene arms) are called mixed arms. In the modified rubber, the polymer segment formed by the coupling agent is equivalent to the polybutadiene-isoprene rubber and polystyrene rubber being chained together as the core, achieving the combination of different polymer molecular chains at the short-range structural level of the polymer chain, and can have good compatibility, stability and adhesion. The polymer structure is evenly distributed in the microphase and acts in coordination with each other. It has high hardness, good strength, good branching degree, and the physical properties of natural rubber, improving the rubber's anti-slip properties and reducing rolling resistance. When used in combination with various synthetic or natural rubbers, it can improve the rigidity, hardness, wear resistance, tear resistance, and dielectric properties of rubber products. It is widely used in a variety of rubber processing fields, including tires, belts, hoses, and rubber shoes, as well as other industries. The method for preparing the star-shaped styrene-grafted butadiene-isoprene-modified rubber provided by the present invention features a simple process, mild polymerization conditions, stable product performance, and excellent overall properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] FIG1 is a schematic diagram of the molecular chain structure of star-shaped styrene-grafted butadiene-isoprene modified rubber.
[0019] Description of Reference Numerals
[0020] PS stands for styrene homopolymer segment, and PIB stands for butadiene-isoprene copolymer segment. DETAILED DESCRIPTION
[0021] The endpoints of the ranges and any values disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range and individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered to be specifically disclosed herein.
[0022] A first aspect of the present invention provides a star-shaped styrene-grafted butadiene-isoprene modified rubber, wherein the modified rubber comprises a polymer segment derived from a coupling agent and a plurality of styrene homopolymer segments and butadiene-isoprene copolymer segments grafted onto the polymer segment, wherein the coupling agent is selected from polyvinyl aromatic monomers.
[0023] In the present invention, the star-shaped styrene-grafted butadiene-isoprene modified rubber provided is a branched polymer with a star-shaped structure from the perspective of the polymer chain structure, wherein the polymer segment formed by the coupling agent serves as the core, and the multiple vinyl functional groups possessed by the coupling agent provide the polymer segment with multiple vinyl groups that can further graft other branches; the butadiene-isoprene copolymer chain and the styrene homopolymer chain can be bonded to the vinyl groups on the polymer segment through the carbon-carbon double bonds contained in each, forming a butadiene-isoprene copolymer segment and a styrene homopolymer segment grafted on the polymer segment, that is, multiple molecular chains are grafted on the polymer segment to form different segments as branches, which are similarly connected molecular arms (such as polybutadiene isoprene arms and styrene arms), which are called mixed arms. In the modified rubber, the polymer chain segments formed by the coupling agent of polybutadiene-isoprene rubber and polystyrene rubber are used as the core and chained together, thereby realizing the combination of different polymer molecular chains at the short-range structural level of the polymer chain, and having good compatibility, stability and adhesion, so that the polymer structure is evenly distributed in the microphase and acts in coordination with each other, and has high hardness, good strength, good branching degree and the physical properties of natural rubber, thereby improving the rubber's anti-slip properties and reducing rolling resistance.
[0024] In the present invention, the molecular arms of the polymer are connected by polymer segments derived from a coupling agent. The coupling agent is selected from polyvinyl aromatic monomers. The polyvinyl aromatic monomers polymerize to form polymer segments with multiple molecular arms, as shown in Figure 1. Multiple linear branches are chemically bonded to the same central core, achieving molecular blending of the polymers, making the polymer structure more uniformly distributed in the microphase, and improving the physical and mechanical properties of the rubber. PS represents a styrene homopolymer segment, and PIB represents a butadiene-isoprene copolymer segment.
[0025] In some specific embodiments of the present invention, the modified rubber comprises 30-70 wt% of the styrene homopolymer segment and 30-70 wt% of the butadiene-isoprene copolymer segment, based on the combined weights of the styrene homopolymer segment and the butadiene-isoprene copolymer segment. By limiting the modified rubber to these limits, different polymer chains are combined at the short-range structural level of the polymer chain, resulting in good compatibility, stability, and adhesion. The polymer structures are evenly distributed and coordinated at the microscopic level, resulting in high hardness and strength.
[0026] In some specific embodiments of the present invention, in the modified rubber, based on the sum of the weights of the styrene homopolymer segment and the butadiene-isoprene copolymer segment, the content of the styrene homopolymer segment can be selected from 30 wt%, 40 wt%, 50 wt%, 60 wt%, 70 wt%, or any value within a range consisting of any two of the aforementioned values. The content of the butadiene-isoprene copolymer segment can be selected from 30 wt%, 40 wt%, 50 wt%, 60 wt%, 70 wt%, or any value within a range consisting of any two of the aforementioned values.
[0027] In some specific embodiments of the present invention, in the butadiene-isoprene copolymer segment, based on the total weight of the butadiene-isoprene copolymer segment, the content of the isoprene structural unit is 50-90 wt %, and the content of the butadiene structural unit is 10-50 wt %.
[0028] In some specific embodiments of the present invention, the content of the isoprene structural unit in the butadiene-isoprene copolymer segment can be selected from 50 wt%, 60 wt%, 70 wt%, 80 wt%, 90 wt%, or any value within the range consisting of any two of the above values. The content of the butadiene structural unit can be selected from 10 wt%, 20 wt%, 30 wt%, 40 wt%, 50 wt%, or any value within the range consisting of any two of the above values.
[0029] In some specific embodiments of the present invention, in the butadiene-isoprene copolymer segment, based on the total weight of the butadiene-isoprene copolymer segment, the total content of 1,4-structural units of isoprene and 1,4-structural units of butadiene is 40-80 wt%, and the total content of 3,4-structural units of isoprene and 1,2-structural units of butadiene is 20-60 wt%.
[0030] In some specific embodiments of the present invention, the total content of 1,4-structural units of isoprene and 1,4-structural units of butadiene in the butadiene-isoprene copolymer segment can be selected from 40 wt%, 50 wt%, 60 wt%, 70 wt%, 80 wt%, or any value within a range consisting of any two of the aforementioned values. The total content of 3,4-structural units of isoprene and 1,2-structural units of butadiene can be selected from 20 wt%, 30 wt%, 40 wt%, 50 wt%, 60 wt%, or any value within a range consisting of any two of the aforementioned values.
[0031] In some specific embodiments of the present invention, preferably, the coupling agent is selected from divinylbenzene.
[0032] In some specific embodiments of the present invention, in the modified liquid styrene-butadiene rubber, the amount of the coupling agent is relatively small, and the polymer segment formed by the coupling agent is used as the core. The core formed by the coupling agent is a macromolecular active species, and the macromolecular active species provides the polymer with multiple reactive active points that can further initiate polymerization of the reaction monomers, thereby initiating polymerization of the monomers to form polymer segments. The proportion of the polymer segment formed by the coupling agent itself is very small relative to the amount of the macromolecular polymer, and the content can be excluded from the polymer proportion. The amount of the coupling agent has been described in the text.
[0033] In some specific embodiments of the present invention, the number average molecular weight of the modified rubber is 100,000-600,000 g / mol, the weight average molecular weight is 200,000-1,000,000 g / mol; the molecular weight distribution index is 1.2-5, the larger the molecular weight distribution index, the better the rubber processing performance. The molecular weight distribution index of the modified rubber is 1.2-5, the processing performance is good, tanδ (0°C) is 0.22-0.27, tanδ (60°C) is 0.009-0.119, and the coupling efficiency is 60-75%.
[0034] A second aspect of the present invention provides a method for preparing a star-shaped styrene-grafted butadiene-isoprene modified rubber, wherein the preparation method comprises:
[0035] (1) In the presence of an initiator, styrene undergoes homopolymerization to obtain an active styrene homopolymer segment;
[0036] (2) coupling the active styrene homopolymer segment with a coupling agent to obtain an active chain;
[0037] (3) In the presence of a polar activator, the active chain, butadiene and isoprene are copolymerized to obtain the star-shaped mixed arm high styrene rubber.
[0038] In some specific embodiments of the present invention, the coupling reaction is a process in which the polymer segment formed by the coupling agent and the styrene homopolymer segment are bonded to the vinyl group on the polymer segment via the carbon-carbon double bond contained therein to obtain the active chain.
[0039] In some specific embodiments of the present invention, the initiator is selected from one or more of n-butyllithium, sec-butyllithium, methylbutyllithium, phenylbutyllithium, naphthalenelithium, cyclohexyllithium, and dodecyllithium, preferably n-butyllithium and / or sec-butyllithium. The amount of the initiator added is determined by the molecular weight of the designed polymer.
[0040] In some specific embodiments of the present invention, the coupling agent is selected from polyvinyl aromatic hydrocarbons, preferably divinylbenzene. During the coupling reaction, the coupling agent can be added once or multiple times. By adding the coupling agent multiple times, the coupling efficiency of the coupling agent can be improved.
[0041] In some specific embodiments of the present invention, the polar activator is selected from one or more of diethylene glycol dimethyl ether, tetrahydrofuran, ethyl ether, ethyl methyl ether, anisole, diphenyl ether, ethylene glycol dimethyl ether, triethylamine, tetramethylethylenediamine, and hexamethylphosphonic triamide, preferably one or more of diethylene glycol dimethyl ether, tetrahydrofuran, and tetramethylethylenediamine. The polymerization system of the present invention requires the addition of a polar organic compound as an activator to produce a polarization or solvation effect on the initiator, thereby reducing its degree of association and increasing the initiation reaction rate of an initiator such as n-butyllithium. The activator can also regulate the reactivity ratio of butadiene and isoprene, allowing the two to copolymerize randomly. The activator can also increase the content of 1,2-structures in the butadiene unit and 3,4-structures in the isoprene unit.
[0042] In some embodiments of the present invention, the mechanical properties of star-shaped styrene-grafted butadiene-isoprene-modified rubbers are related to the monomer ratio of styrene, isoprene, and butadiene, as well as the product molecular weight. Generally speaking, high styrene content results in higher hardness and lower elongation at break, while high isoprene and butadiene content results in lower hardness and higher elongation at break. Furthermore, the molecular weight of the single arm of the high-styrene rubber determines the product molecular weight to a certain extent, thereby influencing product performance. The single arm number average molecular weight of the styrene homopolymer segment of the present invention is 50,000-150,000 g / mol.
[0043] In some specific embodiments of the present invention, the temperature of the homopolymerization reaction is 50-80° C., the pressure of the homopolymerization reaction is 0.1-0.25 MPa, and the time of the homopolymerization reaction is 20-80 min.
[0044] In some specific embodiments of the present invention, the coupling reaction temperature is 50-80° C., the coupling reaction pressure is 0.1-0.25 MPa, and the coupling reaction time is 60-90 min.
[0045] In some specific embodiments of the present invention, the copolymerization reaction temperature is 50-80° C., the copolymerization reaction pressure is 0.1-0.25 MPa, and the copolymerization reaction time is 60-100 min.
[0046] In some specific embodiments of the present invention, the coupling efficiency of the star-shaped styrene-grafted butadiene-isoprene modified rubber polymer is 61-74%. The coupling efficiency (CE) is determined by subjecting the resulting coupling mixture to GPC analysis, where the ratio of the peak area of the polymer formed by coupling to the sum of the peak area of the polymer formed by coupling and the peak area of the copolymer remaining after coupling is the coupling efficiency. A higher coupling efficiency indicates better coupling performance of divinylbenzene, greater activity of the macromolecular active species formed, and a greater number of linear branches chemically bonded to the central core formed by divinylbenzene.
[0047] In some specific embodiments of the present invention, after the reaction is complete, the obtained polymer solution is treated with water. The amount of water used is generally 100-300 times the amount of the initiator used, preferably 150-250 times.
[0048] In some specific embodiments of the present invention, 0.5%-1% of the polymer weight of an antioxidant can be added to the obtained star-shaped styrene grafted butadiene-isoprene modified rubber, and then high-performance star-shaped styrene grafted butadiene-isoprene modified rubber is obtained through washing, dehydration and drying.
[0049] In some specific embodiments of the present invention, styrene is 30-70 parts by weight, and the mixed monomer of butadiene and isoprene is 30-70 parts by weight, wherein butadiene accounts for 10-50wt% of the mixed monomer amount, and isoprene accounts for 50-90wt% of the mixed monomer amount.
[0050] In some specific embodiments of the present invention, the initiator is 0.0005-0.002 parts by weight,
[0051] In some specific embodiments of the present invention, the molar ratio of the polar activator to the initiator is 0.1-30:1.
[0052] In some specific embodiments of the present invention, the molar ratio of the coupling agent to the initiator is 0.1-1.5:1.
[0053] In some specific embodiments of the present invention, preferably, the styrene monomer is 30-70 parts by weight, and the butadiene and isoprene mixed monomer is 30-70 parts by weight, wherein butadiene accounts for 10-50 wt% of the mixed monomer amount, and isoprene accounts for 50-90 wt% of the mixed monomer amount.
[0054] In some specific embodiments of the present invention, preferably, the initiator is 0.0007-0.002 parts by weight.
[0055] In some specific embodiments of the present invention, preferably, the molar ratio of the polar activator to the initiator is 0.2-20:1.
[0056] In some specific embodiments of the present invention, preferably, the molar ratio of the coupling agent to the initiator is 0.15-1:1.
[0057] In the present invention, the composition and structure of the modified rubber can be determined by nuclear magnetic resonance, infrared, GPC, elemental analysis, etc., or determined by preparation and feeding. The total content of the 1,4-structural unit of isoprene and the 1,4-structural unit of butadiene and the total content of the 3,4-structural unit of isoprene and the 1,2-structural unit of butadiene are measured by infrared spectroscopy.
[0058] The third aspect of the present invention provides a star-shaped styrene-grafted butadiene-isoprene modified rubber obtained by the above-mentioned preparation method, which may have the aforementioned composition and structural characteristics and will not be described in detail.
[0059] The fourth aspect of the present invention provides an application of the star-shaped styrene-grafted butadiene-isoprene modified rubber in the field of rubber processing.
[0060] The present invention will be described in detail below through examples.
[0061] Determination of molecular weight and coupling efficiency: The molecular weight and its distribution of the sample were analyzed using a Viscoteck TDA302 gel permeation chromatography (GPC) produced by Agilent Technologies, USA, with THF as the mobile phase and the test temperature at 30°C.
[0062] Fourier Transform Infrared Spectroscopy (FTIR) Analysis: Analyzed using a Nicolet 560 FTIR instrument (USA) without purification and using potassium bromide for tableting and film coating. This method is used to determine the styrene, butadiene, and isoprene content in modified rubber.
[0063] Dynamic mechanical analysis (DMA): The dynamic mechanical properties of the samples were tested using a Va3000 dynamic mechanical analysis (DMA) instrument produced by the French company 01db-Metravib, under shear conditions and a deformation amplitude of 5%.
[0064] Mechanical properties analysis: The mechanical properties of the samples were tested using a 5567 universal material testing machine produced by Instron, USA.
[0065] Mooney viscosity was measured using a MV2000 Mooney viscometer from Alpha Instruments, USA. The Mooney viscosity test was conducted in accordance with GB / T1232.1-2000.
[0066] In the following examples and comparative examples, where specific conditions are not specified, the experiments were conducted under conventional conditions or those recommended by the manufacturer. Reagents and instruments used, where the manufacturer is not specified, are commercially available. The composition and structure of the modified rubbers described in the following examples and comparative examples can be determined by nuclear magnetic resonance (NMR), infrared spectroscopy (IR), gel permeation chromatography (GPC), elemental analysis, or by preparing and feeding the materials.
[0067] Example 1
[0068] In a jacketed 15L stainless steel reactor, the system was flushed three times with argon. 4212g of cyclohexane, 468g of styrene, and 5.85mmol of n-butyllithium were added to the reactor, and the temperature was raised to 50°C for polymerization for 80 minutes. After complete monomer conversion, the temperature was raised to 80°C, and 2.34mmol of divinylbenzene was added to continue coupling. After 60 minutes of reaction, a mixture of 2.11g of tetrahydrofuran, 4212g of cyclohexane, 234g of butadiene, and 234g of isoprene was pressurized into the reactor and the reaction continued for 60 minutes. After completion of the reaction, the coupled reaction mixture was treated with water, and 100g of water and 12g of antioxidant 1010 were added and stirred. The rubber solution is subjected to wet coagulation and drying to obtain a modified rubber (in the obtained modified rubber, based on the sum of the weights of the styrene homopolymer segment and the butadiene-isoprene copolymer segment, the content of the styrene homopolymer segment is 50wt%, and the content of the butadiene-isoprene copolymer segment is 50wt%; in the butadiene-isoprene copolymer segment, based on the total weight of the butadiene-isoprene copolymer segment, the content of the isoprene structural unit is 50wt%, and the content of the butadiene structural unit is 50wt%).
[0069] Example 2
[0070] In a 15 L stainless steel reactor with a jacket, the system was replaced three times with argon. 4212 g of cyclohexane, 468 g of styrene (50 wt% of the total monomer amount), and 5.85 mmol of n-butyl lithium were added to the reactor, and the temperature was raised to 50° C. for polymerization for 80 min. After complete conversion of the monomers, the temperature was raised to 80° C., and 2.34 mmol of divinylbenzene was added to continue coupling. After the reaction was completed for 60 min, 0.339 g of tetramethylethylenediamine, 4212 g of cyclohexane, 234 g of butadiene (50 wt% of the mixed monomer amount), and 234 g of isoprene (50 wt% of the mixed monomer amount) were pressed into the reactor and the reaction was continued for 60 min. After the reaction was completed, the coupled reaction mixture was treated with water, 100 g of water and 12 g of antioxidant 1010 were added, and the mixture was stirred. The rubber solution is subjected to wet coagulation and drying to obtain a modified rubber (in the obtained modified rubber, based on the sum of the weights of the styrene homopolymer segment and the butadiene-isoprene copolymer segment, the content of the styrene homopolymer segment is 50wt%, and the content of the butadiene-isoprene copolymer segment is 50wt%; in the butadiene-isoprene copolymer segment, based on the total weight of the butadiene-isoprene copolymer segment, the content of the isoprene structural unit is 50wt%, and the content of the butadiene structural unit is 50wt%).
[0071] Example 3
[0072] In a 15L stainless steel reactor with a jacket, argon was passed through the system to replace the system three times. 4212g of cyclohexane, 468g of styrene, and 5.85mmol of n-butyl lithium were added to the polymerization reactor, and the temperature was raised to 50°C for polymerization for 80min. After the monomers were completely converted, the temperature was raised to 80°C, and 2.34mmol of divinylbenzene was added to continue coupling. After the reaction was completed for 60min, 0.392g of diethylene glycol dimethyl ether (2G), 4212g of cyclohexane and a mixture of 234g of butadiene and 234g of isoprene were pressed into the polymerization reactor and the reaction was continued for 60min. After the reaction was completed, the reaction mixture after coupling was treated with water, 100g of water was added, and 10 g of antioxidant 1076 and 5 g of antioxidant 1010 were added and stirred evenly. The rubber solution was subjected to wet coagulation and drying to obtain a modified rubber (in the obtained modified rubber, based on the sum of the weights of the styrene homopolymer segment and the butadiene-isoprene copolymer segment, the content of the styrene homopolymer segment is 50 wt%, and the content of the butadiene-isoprene copolymer segment is 50 wt%; in the butadiene-isoprene copolymer segment, based on the total weight of the butadiene-isoprene copolymer segment, the content of the isoprene structural unit is 50 wt%, and the content of the butadiene structural unit is 50 wt%).
[0073] Example 4
[0074] In a 15 L stainless steel reactor with a jacket, the system was replaced three times with argon. 4212 g of cyclohexane, 468 g of styrene, and 5.85 mmol of n-butyl lithium were added to the reactor, and the temperature was raised to 50° C. for polymerization for 80 min. After complete monomer conversion, the temperature was raised to 80° C., and 2.34 mmol of divinylbenzene was added in two portions (70 wt % of the total amount of divinylbenzene was added in the first addition, and the remaining 30 wt % was added after 30 min of reaction) to carry out a coupling reaction. After the reaction time of 80 min, a mixture of 2.11 g of tetrahydrofuran, 4212 g of cyclohexane, and 234 g of butadiene and 234 g of isoprene was pressed into the reactor, and the reaction was continued for 60 min. After the reaction was completed, the coupled reaction mixture was treated with water, and 100 g of water and 12 g of antioxidant 1010 were added and stirred. The rubber solution is subjected to wet coagulation and drying to obtain a modified rubber (in the obtained modified rubber, based on the sum of the weights of the styrene homopolymer segment and the butadiene-isoprene copolymer segment, the content of the styrene homopolymer segment is 50wt%, and the content of the butadiene-isoprene copolymer segment is 50wt%; in the butadiene-isoprene copolymer segment, based on the total weight of the butadiene-isoprene copolymer segment, the content of the isoprene structural unit is 50wt%, and the content of the butadiene structural unit is 50wt%).
[0075] Example 5
[0076] In a 15L stainless steel reactor with a jacket, argon was passed through the system to replace the system three times. 4212g of cyclohexane, 468g of styrene, and 5.85mmol of n-butyl lithium were added to the polymerization reactor, and the temperature was raised to 50°C for polymerization for 80min. After the monomers were completely converted, the temperature was raised to 80°C, and 4.68mmol of divinylbenzene was added twice (70wt% of the total amount of divinylbenzene was added in the first step, and the remaining 30wt% was added after 30min of reaction) to carry out coupling reaction. After 80min of reaction, 2.11g of tetrahydrofuran, 4212g of cyclohexane, and a mixture of 234g of butadiene and 234g of isoprene were pressed into the polymerization reactor and the reaction was continued for 60min. After the reaction was completed, the coupling was treated with water. To the reaction mixture after the reaction, 100 g of water, 10 g of antioxidant 1076 and 5 g of antioxidant 1010 were added, and the mixture was stirred evenly. The rubber solution was subjected to wet coagulation and drying to obtain a modified rubber (in the obtained modified rubber, based on the sum of the weights of the styrene homopolymer segment and the butadiene-isoprene copolymer segment, the content of the styrene homopolymer segment is 50 wt%, and the content of the butadiene-isoprene copolymer segment is 50 wt%; in the butadiene-isoprene copolymer segment, based on the total weight of the butadiene-isoprene copolymer segment, the content of the isoprene structural unit is 50 wt%, and the content of the butadiene structural unit is 50 wt%).
[0077] Example 6
[0078] In a 15L stainless steel reactor with a jacket, the system was replaced three times with argon. 4212g of cyclohexane, 468g of styrene, and 11.70mmol of n-butyl lithium were added to the polymerization reactor, and the temperature was raised to 50°C for polymerization for 80min. After the monomers were completely converted, the temperature was raised to 80°C, and 2.34mmol of divinylbenzene was added twice (70wt% of the total amount of divinylbenzene was added in the first step, and the remaining 30wt% was added after 30min of reaction) to carry out coupling reaction. After 80min of reaction, 4.22g of tetrahydrofuran, 4212g of cyclohexane, and a mixture of 234g of butadiene and 234g of isoprene were pressed into the polymerization reactor and the reaction was continued for 60min. After the reaction was completed, the coupling reaction mixture was treated with water. To the reaction mixture after coupling, 100 g of water, 10 g of antioxidant 1076 and 5 g of antioxidant 1010 were added, and the mixture was stirred evenly. The rubber solution was subjected to wet coagulation and drying to obtain a modified rubber (in the obtained modified rubber, based on the sum of the weights of the styrene homopolymer segment and the butadiene-isoprene copolymer segment, the content of the styrene homopolymer segment is 50 wt%, and the content of the butadiene-isoprene copolymer segment is 50 wt%; in the butadiene-isoprene copolymer segment, based on the total weight of the butadiene-isoprene copolymer segment, the content of the isoprene structural unit is 50 wt%, and the content of the butadiene structural unit is 50 wt%).
[0079] Example 7
[0080] In a 15L stainless steel reactor with a jacket, argon was passed through the system to replace the system three times. 5054g of cyclohexane, 562g of styrene, and 7.03mmol of n-butyl lithium were added to the polymerization reactor, and the temperature was raised to 50°C for polymerization for 80min. After the monomers were completely converted, the temperature was raised to 80°C, and 2.81mmol of divinylbenzene was added twice (70wt% of the total amount of divinylbenzene was added in the first step, and the remaining 30wt% was added after 30min of reaction) to carry out coupling reaction. After 80min of reaction, 2.54g of tetrahydrofuran, 3370g of cyclohexane, and a mixture of 187g of butadiene and 187g of isoprene were pressed into the polymerization reactor and the reaction was continued for 60min. After the reaction was completed, the coupling was treated with water. To the reaction mixture after the reaction, 100 g of water, 10 g of antioxidant 1076 and 5 g of antioxidant 1010 were added, and the mixture was stirred evenly. The rubber solution was subjected to wet coagulation and drying to obtain a modified rubber (in the obtained modified rubber, based on the sum of the weights of the styrene homopolymer segment and the butadiene-isoprene copolymer segment, the content of the styrene homopolymer segment is 60 wt %, and the content of the butadiene-isoprene copolymer segment is 40 wt %; in the butadiene-isoprene copolymer segment, based on the total weight of the butadiene-isoprene copolymer segment, the content of the isoprene structural unit is 50 wt %, and the content of the butadiene structural unit is 50 wt %).
[0081] Example 8
[0082] In a 15L stainless steel reactor with a jacket, argon was passed through the system to replace the system three times. 5475g of cyclohexane, 608g of styrene, and 7.60mmol of n-butyl lithium were added to the polymerization reactor, and the temperature was raised to 50°C for polymerization for 80min. After the monomers were completely converted, the temperature was raised to 80°C, and 3.04mmol of divinylbenzene was added twice (70wt% of the total amount of divinylbenzene was added in the first step, and the remaining 30wt% was added after 30min of reaction) to carry out coupling reaction. After the reaction for 80min, 2.74g of tetrahydrofuran, 2949g of cyclohexane, 131g of butadiene, and 196g of isoprene were pressed into the polymerization reactor and the reaction was continued for 60min. After the reaction was completed, the coupling was treated with water. To the reaction mixture after the reaction, 100 g of water, 10 g of antioxidant 1076 and 5 g of antioxidant 1010 were added, and the mixture was stirred evenly. The rubber solution was subjected to wet coagulation and drying to obtain a modified rubber (in the obtained modified rubber, based on the sum of the weights of the styrene homopolymer segment and the butadiene-isoprene copolymer segment, the content of the styrene homopolymer segment is 65 wt %, and the content of the butadiene-isoprene copolymer segment is 35 wt %; in the butadiene-isoprene copolymer segment, based on the total weight of the butadiene-isoprene copolymer segment, the content of the isoprene structural unit is 40 wt %, and the content of the butadiene structural unit is 60 wt %).
[0083] Example 9
[0084] In a 15L stainless steel reactor with a jacket, argon was passed through the system to replace the system three times. 4212g of cyclohexane, 468g of styrene, and 5.85mmol of n-butyllithium were added to the polymerization reactor, and the temperature was raised to 50°C for polymerization for 80min. After the monomers were completely converted, the temperature was raised to 80°C, and 2.34mmol of divinylbenzene was added three times (50wt% of the total amount of divinylbenzene was added for the first time, 30wt% was added after 15min, and the remaining 20wt% was added after 30min) to carry out coupling reaction. After the reaction time of 80min, 0.39g of diethylene glycol dimethyl ether (2G), a mixture of 4212g of cyclohexane and 234g of butadiene and 234g of isoprene were pressed into the polymerization reactor and the reaction was continued for 60min. After completion, the coupled reaction mixture was treated with water, 100 g of water, 10 g of antioxidant 1076 and 5 g of antioxidant 1010 were added, and the mixture was stirred evenly. The rubber solution was subjected to wet coagulation and drying to obtain a modified rubber (in the obtained modified rubber, based on the sum of the weights of the styrene homopolymer segment and the butadiene-isoprene copolymer segment, the content of the styrene homopolymer segment is 50 wt%, and the content of the butadiene-isoprene copolymer segment is 50 wt%; in the butadiene-isoprene copolymer segment, based on the total weight of the butadiene-isoprene copolymer segment, the content of the isoprene structural unit is 50 wt%, and the content of the butadiene structural unit is 50 wt%).
[0085] Example 10
[0086] In a 15L stainless steel reactor with a jacket, the system was replaced three times with argon. 4212g of pentane, 468g of styrene, and 5.85mmol of n-butyllithium were added to the polymerization reactor, and the temperature was raised to 50°C. The polymerization was carried out for 60min. After the monomers were completely converted, 2.34mmol of divinylbenzene was added twice (50wt% of the total amount of divinylbenzene was added in the first addition, and the remaining 50wt% was added after 30min of reaction) to carry out a coupling reaction. After 80min of reaction, a mixture of 2.11g of tetrahydrofuran, 4212g of pentane, 234g of butadiene, and 234g of isoprene was pressed into the polymerization reactor and the reaction was continued for 60min. After the reaction was completed, the coupling reaction was treated with water. To the reaction mixture after coupling, 100 g of water and 15 g of antioxidant 1010 were added, and the mixture was stirred evenly. The rubber solution was subjected to wet coagulation and drying to obtain a modified rubber (in the obtained modified rubber, based on the sum of the weights of the styrene homopolymer segment and the butadiene-isoprene copolymer segment, the content of the styrene homopolymer segment is 50 wt%, and the content of the butadiene-isoprene copolymer segment is 50 wt%; in the butadiene-isoprene copolymer segment, based on the total weight of the butadiene-isoprene copolymer segment, the content of the isoprene structural unit is 50 wt%, and the content of the butadiene structural unit is 50 wt%).
[0087] Comparative Example 1
[0088] In a jacketed 15L stainless steel reactor, the system was flushed three times with argon. 8424g of cyclohexane, 468g of styrene (50wt% of the total monomers), 234g of butadiene (25wt% of the total monomers), 234g of isoprene (25wt% of the total monomers), and 4.21g of tetrahydrofuran were added to the reactor. 11.70mmol of n-butyllithium was added and the reaction was heated to 50°C for 80min. After complete monomer conversion, the temperature was raised to 80°C and the reaction was continued until no free monomers remained. 2.93mmol of SnCl4 coupling agent was added to initiate the coupling reaction. After completion of the reaction, the reaction mixture was treated with water, and 100g of water and 12g of antioxidant 1010 were added with stirring. The gel was wet coagulated and dried.
[0089] Comparative Example 2
[0090] In a 15L stainless steel reactor with a jacket, the system was flushed three times with argon. 4212g of cyclohexane, 234g of styrene (25wt% of the total monomers), and 234g of butadiene (25wt% of the total monomers) were added to the reactor. Polymerization was then continued for 80 min. A mixture of 0.679g of tetramethylethylenediamine, 4212g of cyclohexane, 234g of styrene (25wt% of the total monomers), and 234g of butadiene (25wt% of the total monomers) was then added to the reactor and the reaction continued for 60 min. After complete monomer conversion, 2.93mmol of SnCl4 coupling agent was added to initiate a coupling reaction. After completion of the reaction, the coupled reaction mixture was treated with water, and 100g of water and 12g of antioxidant 1010 were added with stirring. The resulting gel was subjected to wet coagulation and drying.
[0091] Comparative Example 3
[0092] In a 15L stainless steel reactor with a jacket, the system was purged three times with argon. 4212g of cyclohexane, 234g of styrene (25wt% of the total monomers), and 234g of isoprene (25wt% of the total monomers) were added to the reactor. Polymerization was then continued for 80 min. A mixture of 0.784g of diethylene glycol dimethyl ether, 4212g of cyclohexane, 234g of styrene (25wt% of the total monomers), and 234g of isoprene (25wt% of the total monomers) was then added to the reactor and the reaction continued for 60 min. After complete monomer conversion, 2.93mmol of SnCl4 coupling agent was added to initiate a coupling reaction. After completion of the reaction, the coupled reaction mixture was treated with water, and 100g of water and 12g of antioxidant 1010 were added with stirring. The resulting gel was subjected to wet coagulation and drying.
[0093] Comparative Example 4
[0094] In a 15L stainless steel reactor with a jacket, the system was purged three times with argon. 8424g of cyclohexane, 468g of styrene (50wt% of the total monomers), 234g of butadiene (25wt% of the total monomers), 234g of isoprene (25wt% of the total monomers), and 4.21g of tetrahydrofuran were added to the reactor. 11.70mmol of n-butyllithium was added and the reaction was heated to 50°C for 80min. After complete monomer conversion, the temperature was raised to 80°C and the reaction was continued until no free monomers remained. 2.93mmol of SnCl4 was then added in two portions (80wt% of the total SnCl4 was added in the first addition, and the remaining 20wt% was added after 30min of reaction) to carry out a coupling reaction. After completion of the reaction, the coupled reaction mixture was treated with water, 100g of water and 12g of antioxidant 1010 were added, and the mixture was stirred. The gel was subjected to wet coagulation and drying.
[0095] Comparative Example 5
[0096] The high styrene rubber HS860, which has been commercialized on the market, uses styrene and butadiene as raw materials for the polymerization reaction. The difference lies in the different polymerization methods. First, high styrene resin (styrene / butadiene = 80 / 20) is prepared by emulsion polymerization, and then it is mixed with emulsion-polymerized styrene-butadiene rubber (styrene / butadiene = 23 / 77) to finally produce high styrene rubber.
[0097] Comparative Example 6
[0098] In a 15L stainless steel reactor with a jacket, the system was flushed three times with argon. 5054g of cyclohexane and 562g of styrene (60wt% of the total monomer content) were added to the reactor, along with 11.70mmol of n-butyllithium. The temperature was raised to 50°C and polymerization was carried out for 80 minutes. After complete monomer conversion, the temperature was raised to 80°C. A mixture of 4.21g of tetrahydrofuran, 1685g of cyclohexane, and 187g of isoprene (20wt% of the total monomer content) was then pressed into the reactor and the reaction continued for 60 minutes. After complete monomer conversion, 1685g of cyclohexane and 187g of butadiene (20wt% of the total monomer content) were added to the reactor. After the reaction was complete, 2.93mmol of SnCl4 coupling agent was added to carry out a coupling reaction. After completion of the reaction, the coupled reaction mixture was treated with water, and 100g of water and 12g of antioxidant 1010 were added and stirred. The gel was subjected to wet coagulation and drying.
[0099] Comparative Example 7
[0100] In a jacketed 15L stainless steel reactor, the system was flushed three times with argon. 4212g of cyclohexane, 468g of styrene (50wt% of the total monomers), 234g of butadiene (25wt% of the total monomers), 234g of isoprene (25wt% of the total monomers), and 4.21g of tetrahydrofuran were added to the reactor. 11.70mmol of n-butyllithium was added and the temperature was raised to 50°C for polymerization for 80 minutes. After complete monomer conversion, the temperature was raised to 80°C and the reaction continued until no free monomers remained. 2.93mmol of divinylbenzene was added for coupling. After completion of the reaction, the reaction mixture was treated with water, and 100g of water and 12g of antioxidant 1010 were added with stirring. The gel was wet coagulated and dried.
[0101] The high styrene rubbers obtained according to the methods of Examples 1-10 and Comparative Examples 1-7 have rubber molecular weights and microstructure contents as shown in Table 1. (Ip-1,4 and Ip-3,4 represent the 1,4-structure and 3,4-structure of isoprene, respectively; Bd-1,4 and Bd-1,2 represent the 1,4-structure and 1,2-structure of butadiene, respectively.)
[0102] Table 1
[0103] Table 1 (Continued)
[0104] Table 1 (Continued)
[0105] As can be seen from Table 1, the polar activators tetrahydrofuran, diethylene glycol dimethyl ether, and tetramethylethylenediamine can increase the content of 1,2-structures in butadiene units and 3,4-structures in isoprene units. As can be seen from the Examples, the ability of the polar activators to regulate the 1,2-structures in butadiene units and the 3,4-structures in isoprene units is greater for tetramethylethylenediamine than for diethylene glycol dimethyl ether, and greater than for tetrahydrofuran.
[0106] The test performance results of the liquid rubber obtained according to the methods of Examples 1-10 and Comparative Examples 1-7 are shown in Table 2.
[0107] Table 2
[0108] Table 2 (Continued)
[0109] Table 2 (Continued)
[0110] Table 2 (Continued)
[0111] The results in Table 2 show that, in the synthesis process of the star-shaped styrene grafted butadiene-isoprene modified rubber, a secondary feeding method (feeding the styrene homopolymer segment monomer and the butadiene-isoprene copolymer segment monomer) is adopted to synthesize the star-shaped styrene grafted butadiene-isoprene modified rubber having mixed arms (such as polystyrene arms and butadiene-isoprene copolymer arms) and different 1,2-structure contents in the butadiene unit and 3,4-structure contents in the isoprene unit. Due to the presence of the mixed arms, it is equivalent to linking the styrene homopolymer segment and the butadiene-isoprene copolymer segment with different microstructures to the same molecular chain, thereby achieving the molecular blending of the polymers, improving the properties of the rubber and its vulcanization, promoting the synergistic optimization of various product properties, and improving the hardness and dynamic mechanical properties of the product. The isoprene structural units in the polymer are very similar to those of natural rubber, giving the product properties and applications closer to those of natural rubber. This allows for better mixing with natural rubber and styrene-butadiene rubber in applications, significantly improving compatibility and reducing phase separation in the blended rubbers. Furthermore, through structural design during the polymerization process, mixing arms are formed, linking the styrene homopolymer segments and butadiene-isoprene copolymer segments with different microstructures onto the same molecular chain. This achieves molecular blending of the polymers, resulting in a uniform distribution of the polymer structures in the microphase and a coordinated interaction. This avoids the drawbacks of star-shaped styrene-grafted butadiene-isoprene modified rubber during mechanical mixing with natural rubber, such as uneven distribution, poor product quality and performance, and high energy consumption. The star-shaped high-styrene rubber of the present invention has high hardness and good strength. The formed polymer has a high degree of branching and has the physical properties of natural rubber, realizing the blending of polymers in molecular structure. When used in combination with a variety of synthetic rubbers or natural rubbers, the rigidity, hardness, wear resistance, tear resistance, dielectric properties and other properties of rubber products can be improved. The star-shaped high-styrene rubber is widely used in many rubber processing fields such as tires, belts, hoses, rubber shoes and other industries.
[0112] The method for preparing the star-shaped styrene-grafted butadiene-isoprene modified rubber provided by the present invention has the characteristics of simple process, mild polymerization conditions, high coupling efficiency, stable product performance, and good overall performance. Furthermore, a larger tanδ / 0°C value indicates better wet skid resistance of the rubber, and a smaller tanδ / 60°C value indicates lower rolling resistance of the rubber. As can be seen in Table 2, the tanδ / 0°C values of the rubbers of the examples of the present application are all better than those of the comparative examples, indicating that the rubbers of the examples have better wet skid resistance. The tanδ / 60°C values of the rubbers of the examples are all lower than those of the comparative examples, indicating that the rubbers of the examples have lower rolling resistance. Among them, Examples 1, 3, and 5 have better wet skid resistance and rolling resistance.
[0113] As can be seen from Table 2, the coupling efficiency of the embodiment is high compared to the comparative example, indicating that the coupling performance of divinylbenzene is better, the activity of the macromolecular active species formed is also larger, the number of linear branches connected to the central core formed by divinylbenzene by chemical bonds is also more, and the star-shaped polymer branching degree formed is high. As can be seen from Table 2, the performance of the embodiment is better than the comparative example in many aspects. The tensile strength and elongation at break of the embodiment are higher than those of the comparative example. The hardness of the embodiment is relatively higher. The Mooney viscosity of the embodiment is also slightly better. The permanent deformation of the embodiment is slightly lower than that of the comparative example. Therefore, it can be seen that the synthesized star-shaped styrene-grafted butadiene-isoprene modified rubber has excellent dynamic mechanical properties.
[0114] The preferred embodiments of the present invention have been described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, various simple variations of the technical solution of the present invention may be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as disclosed in the present invention and fall within the scope of protection of the present invention.
Claims
1. A star-shaped styrene-grafted butadiene-isoprene modified rubber, characterized in that: The modified rubber comprises a polymer segment derived from a coupling agent and a plurality of styrene homopolymer segments and butadiene-isoprene copolymer segments grafted onto the polymer segment, wherein the coupling agent is selected from polyvinyl aromatic monomers.
2. The modified rubber according to claim 1, characterized in that In the modified rubber, based on the sum of the weights of the styrene homopolymer segment and the butadiene-isoprene copolymer segment, the content of the styrene homopolymer segment is 30-70wt%, and the content of the butadiene-isoprene copolymer segment is 30-70wt%; Preferably, in the butadiene-isoprene copolymer segment, based on the total weight of the butadiene-isoprene copolymer segment, the content of the isoprene structural unit is 50-90wt%, and the content of the butadiene structural unit is 10-50wt%; Preferably, in the butadiene-isoprene copolymer segment, based on the total weight of the butadiene-isoprene copolymer segment, the total content of 1,4-structural units of isoprene and 1,4-structural units of butadiene is 40-80wt%, and the total content of 3,4-structural units of isoprene and 1,2-structural units of butadiene is 20-60wt%; Preferably, the coupling agent is selected from divinylbenzene.
3. The modified rubber according to claim 1 or 2, characterized in that: The number average molecular weight of the modified rubber is 100,000-600,000 g / mol, the weight average molecular weight is 200,000-1,000,000 g / mol, the molecular weight distribution index is 1.2-5, tanδ (0°C) is 0.22-0.27, tanδ (60°C) is 0.009-0.119, and the coupling efficiency is 60-75%.
4. A method for preparing a star-shaped styrene-grafted butadiene-isoprene modified rubber, characterized in that: The preparation method comprises: (1) In the presence of an initiator, styrene undergoes homopolymerization to obtain an active styrene homopolymer segment; (2) subjecting the active styrene homopolymer segment to a coupling reaction with a coupling agent to obtain an active chain; (3) In the presence of a polar activator, the active chain, butadiene and isoprene are copolymerized to obtain the star-shaped styrene-grafted butadiene-isoprene modified rubber.
5. The preparation method according to claim 4, characterized in that: The initiator is selected from one or more of n-butyl lithium, sec-butyl lithium, methylbutyl lithium, phenylbutyl lithium, naphthalene lithium, cyclohexyl lithium and dodecyl lithium, preferably selected from n-butyl lithium and / or sec-butyl lithium; Preferably, the coupling agent is selected from polyvinyl aromatic hydrocarbons, preferably divinyl benzene; Preferably, during the coupling reaction, the coupling agent can be added once or multiple times; Preferably, the polar activator is selected from one or more of diethylene glycol dimethyl ether, tetrahydrofuran, ethyl ether, ethyl methyl ether, anisole, diphenyl ether, ethylene glycol dimethyl ether, triethylamine, tetramethylethylenediamine and hexamethylphosphonic triamide, preferably selected from one or more of diethylene glycol dimethyl ether, tetrahydrofuran and tetramethylethylenediamine.
6. The preparation method according to claim 4 or 5, characterized in that: The temperature of the homopolymerization reaction is 50-80°C, the pressure of the homopolymerization reaction is 0.1-0.25MPa, and the time of the homopolymerization reaction is 20-80min; Preferably, the coupling reaction temperature is 50-80°C, the coupling reaction pressure is 0.1-0.25MPa, and the coupling reaction time is 60-90min; Preferably, the copolymerization reaction temperature is 50-80°C, the copolymerization reaction pressure is 0.1-0.25MPa, and the copolymerization reaction time is 60-100min; Preferably, the coupling efficiency of the star-shaped styrene-grafted butadiene-isoprene modified rubber is 61-74%.
7. The preparation method according to any one of claims 4 to 6, characterized in that: Styrene is 30-70 parts by weight, and the mixed monomer of butadiene and isoprene is 30-70 parts by weight, wherein butadiene accounts for 10-50wt% of the mixed monomer amount, and isoprene accounts for 50-90wt% of the mixed monomer amount; Preferably, the initiator is 0.0005-0.002 parts by weight; Preferably, the molar ratio of the polar activator to the initiator is 0.1-30:1; Preferably, the molar ratio of the coupling agent to the initiator is 0.1-1.5:
1.
8. The preparation method according to claim 7, characterized in that: The styrene monomer is 30-70 parts by weight, and the mixed monomer of butadiene and isoprene is 30-70 parts by weight, wherein butadiene accounts for 10-50wt% of the mixed monomer, and isoprene accounts for 50-90wt% of the mixed monomer; Preferably, the initiator is 0.0007-0.002 parts by weight; Preferably, the molar ratio of the polar activator to the initiator is 0.2-20:1; Preferably, the molar ratio of the coupling agent to the initiator is 0.15-1:
1.
9. The star-shaped styrene-grafted butadiene-isoprene modified rubber obtained by the preparation method according to any one of claims 4 to 8.
10. Use of the star-shaped styrene-grafted butadiene-isoprene modified rubber according to any one of claims 1 to 3 and 9 in the field of rubber processing.
Citation Information
Patent Citations
Method for synthesizing star amphiphilic rubber
CN101062964A
Star block copolymer prepared from isoprene, butadiene and styrene, and preparation method and application thereof
CN101817911A
Thermoplastic block polymers
US3949020A
Clear impact resistant thermoplastic star-block copolymers
US4180530A