Foaming composition, and polyurethane foam and preparation method therefor

By using new foaming compositions of hydrocarbons, fluorine-containing compounds and water, the existing polyurethane foam foaming agent has been solved, and the polyurethane with low cost, low GWP value and high thermal insulation properties has been achieved. Foam.

WO2024239911A1PCT designated stage expired Publication Date: 2024-11-28QUANZHOU YUJI ADVANCED MATERIALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/090055
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-04-26
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The existing polyurethane foam's foam's GWP value is higher than 150, which cannot meet environmental protection requirements. At the same time, the high density of polyurethane foam leads to an increase in material costs.

Method used

A new foaming composition is adopted, including hydrocarbons, fluorine-containing compounds and water, with a mass fraction of hydrocarbons ranging from 20-90%, a mass fraction of fluorine-containing compounds ranging from 10-80%, and a mass fraction of water ranging from 0.1-15%. , the GWP value is less than 25, and is used to prepare polyurethane foam with a density less than 30 kg/m3 and a thermal conductivity less than 20 mW/m·k.

Benefits of technology

The environmentally friendly foaming agent composition with low GWP value is achieved, which reduces the density and thermal conductivity of the polyurethane foam, improves the insulation and insulation performance, reduces material costs, and improves the compressive strength and dimensional stability of the foam.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2024090055-FTAPPB-I100001
    Figure PCTCN2024090055-FTAPPB-I100001
  • Figure PCTCN2024090055-FTAPPB-I100002
    Figure PCTCN2024090055-FTAPPB-I100002
Patent Text Reader

Abstract

The present application discloses a foaming composition, comprising a hydrocarbon, a fluorinated compound (CnH2n-mOzXm), and water, wherein: the mass fraction of the hydrocarbon is 20-90%, preferably 30-70%; the mass fraction of the CnH2n-mOzXm is 10-80%, preferably 30-60%; the mass fraction of the water is 0.1-15%, preferably 0.5-5%; in the CnH2n-mOzXm, n is an integer of 3-10; z is 0 or 1; and n≤m≤2n. The present application further provides a polyurethane foam and a preparation method therefor. In the foaming composition provided by the present application, the GWP value of the hydrocarbon is smaller than 25, the GWP value of the fluorinated compound is smaller than 10, and the water is converted into CO2 during the preparation of the polyurethane foam, and the GWP value of CO2 is 1. Therefore, the GWP value of the foaming agent composition provided by the present application is less than 25 which is far less than an environmental protection value of 150 required by policies, and the foaming agent composition is an ideal environmentally friendly foaming agent composition.
Need to check novelty before this filing date? Find Prior Art

Description

Foaming composition, polyurethane foam and preparation method thereof Technical Field

[0001] The present application relates to the field of foamed thermal insulation materials, and in particular to a foaming composition, polyurethane foam and a preparation method thereof. Background Art

[0002] Rigid polyurethane foam, due to its excellent thermal insulation properties, is widely used in a variety of applications, including cold storage, water heaters, and pipe insulation. With the international community's demand for zero ozone depletion potential (ODP) and low global warming potential (GWP) for blowing agents used in the production of rigid polyurethane foam, traditional chlorofluorocarbon (CFC) blowing agents are being phased out, while hydrocarbon blowing agent technology, represented by cyclopentane, is gaining popularity. Currently, the primary blowing agent used in polyurethane foam production is a multi-component blowing agent consisting of a mixture of cyclopentane, isopentane, pentafluoropropane (HFC-245fa), pentafluorobutane (HFC-365mfc), and tetrafluoroethane (HFC-134a).

[0003] Currently, the zero ozone depletion potential (ODP) of the multi-component foaming agent composed of a mixture of cyclopentane, isopentane, pentafluoropropane (HFC-245fa), pentafluorobutane (HFC-365mfc), and tetrafluoroethane (HFC-134a) can meet environmental protection requirements, but the global warming potential (GWP) is generally around 500 (when the pentane / fluorocarbon ratio is about 1:1), which is much greater than the GWP limit of 150, and therefore cannot meet the GWP value requirements. In addition, when using this type of multi-component foaming agent, in order to meet the compressive strength and dimensional stability of the polyurethane foam, the density of the polyurethane foam must be higher than 30kg / m 3 , the density is relatively large, so when manufacturing unit volume of polyurethane foam, more materials (such as foaming agent, dry white material, etc.) are required, which increases the cost of raw materials.

[0004] Summary of the Invention

[0005] The present application aims to solve the technical problems existing in the prior art. The purposes of the present invention are: 1) to provide an environmentally friendly foaming agent composition, that is, the obtained foaming agent composition has a global warming potential (GWP) of less than 25, which is far less than the requirement of 150 stipulated by national laws and regulations; 2) to provide a method for preparing polyurethane foam using the obtained foaming agent composition, wherein the prepared polyurethane foam has the characteristics of low molded density and low thermal conductivity.

[0006] The present application provides a foaming composition, comprising a hydrocarbon compound, a fluorine-containing compound (C n H 2n-m O z X m ) and water, in the foaming composition, the mass fraction of the hydrocarbon is 20-90%, the Cn H 2n-m O z X m The mass fraction of the water is 0.1-15%, and the mass fraction of the water is 10-80%. n H 2n-m O z X m wherein n is an integer of 3-10; z is 0 or 1; n≤m≤2n, and X is a halogen.

[0007] Furthermore, X is selected from at least one of F, Cl, Br, and I, and when X comprises two or more elements, F accounts for more than 50 mol% of X.

[0008] Furthermore, the fluorine-containing compound is selected from one or more of 3,3,3-trifluoropropene, cis-1,3,3,3-tetrafluoropropene, trans-1,3,3,3-tetrafluoropropene, trans-1,1,1,3,3,3-hexafluoro-2-butene, cis-1,1,1,3,3,3-hexafluoro-2-butene, 1-chloro-2,3,3-trifluoropropene, 2-chloro-3,3,3-trifluoropropene, 1-chloro-2,3,3,3-tetrafluoropropene, perfluorobutanone, perfluoropentanone, perfluorohexanone, methyl perfluoroheptyl ketone, cis-1-chloro-3,3,3-trifluoropropene and trans-1-chloro-3,3,3-trifluoropropene.

[0009] Furthermore, hydrocarbons, C n H 2n-m O z X m and water, in the foaming composition, the mass fraction of the hydrocarbon is 20-90%, the C n H 2n-m O z X m The mass fraction of the cellulose acetate is 10-80%, and the mass fraction of the water is 0.1-15%.

[0010] Furthermore, the GWP value of the foaming composition is less than 25.

[0011] Furthermore, the hydrocarbons include a first hydrocarbon and a second hydrocarbon, and the boiling point of the first hydrocarbon is lower than the boiling point of the second hydrocarbon.

[0012] Furthermore, the mass ratio of the first hydrocarbon to the second hydrocarbon is (1-50):10.

[0013] Further, the first hydrocarbon is n-butane, isobutane or neopentane;

[0014] The second hydrocarbon is selected from any one of cyclopentane, n-pentane and isopentane.

[0015] Furthermore, the fluorine-containing compound includes a first fluorine-containing compound and a second fluorine-containing compound, and the boiling point of the first fluorine-containing compound is lower than the boiling point of the second fluorine-containing compound.

[0016] Furthermore, the mass ratio of the first fluorine-containing compound to the second fluorine-containing compound is (1-50):10.

[0017] Further, the first fluorine-containing compound is selected from any one of 3,3,3-trifluoropropene, cis-1,3,3,3-tetrafluoropropene, perfluorobutanone, 2-chloro-3,3,3-trifluoropropene, trans-1,3,3,3-tetrafluoropropene or trans-1,1,1,3,3,3-hexafluoro-2-butene;

[0018] The second fluorine-containing compound is selected from any one of perfluoropentanone, perfluorohexanone, methyl perfluoroheptyl ketone, 1-chloro-2,3,3-trifluoropropene, 1-chloro-2,3,3,3-tetrafluoropropene, cis-1,1,1,3,3,3-hexafluoro-2-butene, cis-1-chloro-3,3,3-trifluoropropene or trans-1-chloro-3,3,3-trifluoropropene.

[0019] The present application provides a polyurethane foam, wherein the raw materials thereof include the aforementioned foaming composition.

[0020] Furthermore, the raw materials of the polyurethane foam also include polyols, organic polyisocyanates and additives.

[0021] Furthermore, the mass ratio of the auxiliary agent, the foaming agent composition and the polyol is (0.01-0.2):(0.3-3):1, preferably (0.03-0.1):(0.5-2):1; or

[0022] The mass ratio of the auxiliary agent, the foaming agent composition and the organic polyisocyanate is (0.01-0.3):(0.25-4):1, preferably (0.03-0.2):(0.5-2):1.

[0023] Furthermore, the density of the polyurethane foam is less than 30.0 kg / m 3 ;or

[0024] The thermal conductivity of the polyurethane foam is less than 20.0 mW / m·K.

[0025] The present application provides a method for preparing polyurethane foam, which comprises the following steps:

[0026] Providing the aforementioned blowing agent composition;

[0027] Mixing polyols and additives to prepare dry white material;

[0028] Mixing the foaming agent composition, water and dry white material under closed conditions at room temperature to obtain a white material liquid;

[0029] The organic polyisocyanate is mixed with the white liquid to react and prepare the polyurethane foam liquid;

[0030] The polyurethane foam liquid is formed into polyurethane foam of the desired shape through extrusion or spraying.

[0031] Furthermore, the foaming agent composition, water and the dry white material are mixed under closed conditions at room temperature for 0.5-24 hours; or

[0032] The organic polyisocyanate and the white material liquid are mixed and reacted for 0.1-4 hours.

[0033] The foaming composition provided herein has a GWP value of less than 25 for hydrocarbons and less than 10 for fluorine-containing compounds. Water converts into CO2 during the preparation of polyurethane foam, and CO2 has a GWP value of 1. Therefore, the GWP value of the foaming agent composition provided herein is less than 10, far below the environmental protection value of 150 required by policy, making it an ideal environmentally friendly foaming agent composition.

[0034] Compared to existing polyurethane foams, the polyurethane foam prepared with the blowing agent composition provided in this application has a significantly lower mold density (more than 15% lower than the density of polyurethane foam prepared with existing cyclopentane blowing agent compositions, and more than 5% lower than the density of polyurethane foam plastics currently prepared with ternary blowing agent compositions). When producing an equal volume of polyurethane foam, less raw materials (blowing agent composition + dry white material) are required, thereby reducing the manufacturing cost of the polyurethane foam. The polyurethane foam prepared with the blowing agent composition provided in this application has a lower thermal conductivity and better thermal insulation performance, which is beneficial for reducing the energy consumption of refrigeration equipment. In addition, the polyurethane foam liquid prepared with the blowing agent composition provided in this application has better fluidity, more uniform density distribution, smoother surface, better foam compression strength and dimensional stability, resulting in better overall performance of the resulting polyurethane foam. Therefore, the polyurethane foam prepared with the blowing agent composition provided in this application has a low mold density, low thermal conductivity, high compression strength and demolding performance, that is, the polyurethane foam prepared with the blowing agent composition provided in this application has better overall performance. DETAILED DESCRIPTION

[0035] The following description of exemplary embodiments of the present application includes various details of the embodiments of the present application to facilitate understanding, and should be considered as merely exemplary. Therefore, those skilled in the art will recognize that various changes and modifications may be made to the embodiments described herein without departing from the scope and spirit of the present application. Similarly, for the sake of clarity and conciseness, descriptions of well-known functions and structures are omitted in the following description.

[0036] The present application provides a foaming composition, comprising a hydrocarbon compound, a fluorine-containing compound (C n H 2n-m O z X m ) and water, in the foaming composition, the mass fraction of the hydrocarbon is 20-90%, preferably 30-70%, the C n H 2n-m O z X m The mass fraction of the water is 0.1-15%, preferably 0.5-5%. n H 2n-m O z X m wherein n is an integer of 3-10; z is 0 or 1; n≤m≤2n, and X is a halogen.

[0037] Furthermore, X is selected from at least one of F, Cl, Br, and I, and when X comprises two or more elements, F accounts for more than 50 mol% of X.

[0038] In some embodiments, X is F.

[0039] In some embodiments, X is Cl.

[0040] In some embodiments, X is Br.

[0041] In some embodiments, X is 1.

[0042] In some embodiments, X is F and Cl.

[0043] In some embodiments, X is F and Br.

[0044] In some embodiments, X is F and I.

[0045] In some embodiments, X is F, Cl, and I.

[0046] In some embodiments, X is F, Br, and I.

[0047] In some embodiments, X is F, Cl, Br, and I.

[0048] In some embodiments, C n H 2n-m O z X m For fluoroolefins.

[0049] In some embodiments, C n H 2n-m O z X m It is a fluorinated ketone.

[0050] In some embodiments, the value of n can be 3, 4, 5, 6, 7, 8, 9 or 10, etc.

[0051] The present application provides a foaming composition comprising hydrocarbons, fluorine-containing compounds (C n H 2n-m O z X m ) and water, in the foaming composition, the mass fraction of the hydrocarbon is 20-90%, preferably 30-70%, the mass fraction of the fluorine-containing compound is 10-80%, preferably 30-60%, and the mass fraction of the water is 0.1-15%, preferably 0.5-5%.

[0052] In some embodiments, the mass fraction of the hydrocarbon is 20-90%.

[0053] In some embodiments, the mass fraction of the hydrocarbon is 30-70%.

[0054] In some embodiments, the mass fraction of the hydrocarbon is 30-80%.

[0055] In some embodiments, the mass fraction of the hydrocarbon is 30-90%.

[0056] Specifically, the mass fraction of the hydrocarbon may be 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85% or 90%.

[0057] In some embodiments, the mass fraction of the fluorine-containing compound is 10-80%.

[0058] In some embodiments, the mass fraction of the fluorine-containing compound is 30-60%.

[0059] In some embodiments, the mass fraction of the fluorine-containing compound is 30-70%.

[0060] In some embodiments, the mass fraction of the fluorine-containing compound is 30-80%.

[0061] Specifically, the mass fraction of the fluorine-containing compound can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%.

[0062] In some embodiments, the mass fraction of water is 0.1-15%.

[0063] In some embodiments, the mass fraction of water is 0.5-5%.

[0064] In some embodiments, the mass fraction of water is 0.5-10%.

[0065] In some embodiments, the mass fraction of water is 0.5-15%.

[0066] Specifically, the mass fraction of water can be 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5% or 15%.

[0067] In the present application, the GWP value of the foaming composition is less than 10, for example, it may be 9.

[0068] In the present application, the hydrocarbons include a first hydrocarbon and a second hydrocarbon, and the boiling point of the first hydrocarbon is lower than that of the second hydrocarbon.

[0069] The first hydrocarbon is a low-boiling-point hydrocarbon, and its boiling point is less than or equal to 20° C. For example, the boiling point may be 20° C., 19° C., 18° C., 17° C., 16° C., 15° C., 14° C., 13° C., 12° C., 11° C., 10° C., etc.

[0070] The second hydrocarbon is a high-boiling-point hydrocarbon, and its boiling point is greater than 20° C. For example, it can be 21° C., 22° C., 23° C., 24° C., 25° C., 26° C., 27° C., 28° C., etc.

[0071] In the present application, the mass ratio of the first hydrocarbon compound to the second hydrocarbon compound is (1-50):10, preferably (3-30):10.

[0072] Specifically, the mass ratio of the first hydrocarbon to the second hydrocarbon may be 3:10, 4:10, 5:10, 6:10, 7:10, 8:10, 9:10, 10:10, 11:10, 12:10, 13:10, 14:10, 15:10, 16:10, 17:10, 18:10, 19:10, 20:10, 21:10, 22:10, 23:10, 24:10, 25:10, 26:10, 27:10, 28:10, 29:10, or 30:10.

[0073] In the present application, the first hydrocarbon is n-butane, isobutane or neopentane, preferably n-butane;

[0074] The second hydrocarbon compound is selected from any one of cyclopentane, n-pentane, or isopentane, preferably cyclopentane.

[0075] Specifically, the boiling point of n-butane is -0.5°C.

[0076] Specifically, the boiling point of the isobutane is -10.5°C.

[0077] Specifically, the boiling point of cyclopentane is 49.2°C.

[0078] Specifically, the boiling point of n-pentane is 36°C.

[0079] Specifically, the boiling point of the neopentane is 9.5°C.

[0080] Specifically, the boiling point of isopentane is 27.8.

[0081] In the present application, the fluorine-containing compound is selected from one or more of 3,3,3-trifluoropropene, cis-1,3,3,3-tetrafluoropropene, trans-1,3,3,3-tetrafluoropropene, trans-1,1,1,3,3,3-hexafluoro-2-butene, 1-chloro-2,3,3-trifluoropropene, 2-chloro-3,3,3-trifluoropropene, 1-chloro-2,3,3,3-tetrafluoropropene, perfluorobutanone, perfluoropentanone, perfluorohexanone, methyl perfluoroheptyl ketone, cis-1,1,1,3,3,3-hexafluoro-2-butene, cis-1-chloro-3,3,3-trifluoropropene and trans-1-chloro-3,3,3-trifluoropropene.

[0082] In the present application, the fluorine-containing compound includes a first fluorine-containing compound and a second fluorine-containing compound, and the boiling point of the first fluorine-containing compound is lower than that of the second fluorine-containing compound.

[0083] The first fluorine-containing compound is a low-boiling-point fluorine-containing compound, and its boiling point is less than or equal to 15° C. For example, its boiling point can be 15° C., 14° C., 13° C., 12° C., etc.

[0084] The second fluorine-containing compound is a high-boiling-point fluorine-containing compound, and its boiling point is greater than 15° C. For example, its boiling point may be 20° C., 25° C., 30° C., 40° C., etc.

[0085] In the present application, the mass ratio of the first fluorine-containing compound to the second fluorine-containing compound is (1-50):10, preferably (3-30):10.

[0086] Specifically, the mass ratio of the first fluorine-containing compound to the second fluorine-containing compound can be 3:10, 4:10, 5:10, 6:10, 7:10, 8:10, 9:10, 10:10, 11:10, 12:10, 13:10, 14:10, 15:10, 16:10, 17:10, 18:10, 19:10, 20:10, 21:10, 22:10, 23:10, 24:10, 25:10, 26:10, 27:10, 28:10, 29:10, or 30:10.

[0087] In the present application, the first fluorine-containing compound is selected from any one of 3,3,3-trifluoropropene, cis-1,3,3,3-tetrafluoropropene, perfluorobutanone, 2-chloro-3,3,3-trifluoropropene, trans-1,3,3,3-tetrafluoropropene or trans-1,1,1,3,3,3-hexafluoro-2-butene, preferably trans-1,3,3,3-tetrafluoropropene;

[0088] The second fluorine-containing compound is selected from any one of perfluoropentanone, perfluorohexanone, 1-chloro-2,3,3-trifluoropropene, 1-chloro-2,3,3,3-tetrafluoropropene, methyl perfluoroheptyl ketone, cis-1,1,1,3,3,3-hexafluoro-2-butene, cis-1-chloro-3,3,3-trifluoropropene or trans-1-chloro-3,3,3-trifluoropropene, preferably perfluorohexanone or trans-1-chloro-3,3,3-trifluoropropene.

[0089] Specifically, the boiling point of the 3,3,3-trifluoropropene is -17°C.

[0090] Specifically, the boiling point of the cis-1,3,3,3-tetrafluoropropene is 9.6°C.

[0091] Specifically, the boiling point of the trans-1,3,3,3-tetrafluoropropene is -19°C.

[0092] Specifically, the boiling point of the trans-1-chloro-3,3,3-trifluoropropene is 19°C.

[0093] Specifically, the boiling point of cis-1-chloro-3,3,3-trifluoropropene is 39°C.

[0094] Specifically, the boiling point of the 1-chloro-2,3,3-trifluoropropene is 54°C.

[0095] Specifically, the boiling point of the 2-chloro-3,3,3-trifluoropropene is 15°C.

[0096] Specifically, the boiling point of the cis-1-chloro-2,3,3,3-tetrafluoropropene is 15°C.

[0097] Specifically, the boiling point of the trans-1-chloro-2,3,3,3-tetrafluoropropene is 19°C.

[0098] Specifically, the boiling point of the perfluorobutanone is 0°C.

[0099] Specifically, the boiling point of the perfluoropentanone is 26.9°C.

[0100] Specifically, the boiling point of perfluorohexanone is 49°C.

[0101] Specifically, the boiling point of the methyl perfluoroheptyl ketone is 57°C.

[0102] Specifically, the boiling point of the cis-1,1,1,3,3,3-hexafluoro-2-butene is 33.4°C.

[0103] Specifically, the boiling point of the trans-1,1,1,3,3,3-hexafluoro-2-butene is 7.5°C.

[0104] In the present application, the boiling point of the foaming composition is -19°C to 55°C, preferably -10°C to 40°C.

[0105] Specifically, the boiling point of the foaming composition can be -19°C, -18°C, -17°C, -16°C, -15°C, -14°C, -13°C, -12°C, -11°C, -10°C, -9°C, -8°C, -7°C, -6°C, -5°C, -4°C, -3°C, -2°C, -1°C, 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 40°C, 45°C, 50°C or 55°C.

[0106] In some embodiments, in the foaming composition, the first hydrocarbon is n-butane, the second hydrocarbon is cyclopentane, the first fluorine-containing compound is trans-1-chloro-3,3,3-trifluoropropene, and the second fluorine-containing compound is perfluorohexanone.

[0107] The present application provides a polyurethane foam, the raw materials of which include the aforementioned foaming composition.

[0108] The raw materials of the polyurethane foam further include polyol, organic polyisocyanate and auxiliary agents.

[0109] The present application provides a polyurethane foam, which is composed of the aforementioned foaming composition, polyol, organic polyisocyanate and additives.

[0110] In some embodiments, the mass ratio of the auxiliary agent, the foaming agent composition and the polyol is (0.01-0.2):(0.3-3):1, preferably (0.03-0.1):(0.5-2):1.

[0111] Specifically, when the content of the polyol is 1 part by weight, the content of the auxiliary agent is 0.01-0.2 parts by weight, preferably 0.03-0.1 parts by weight, and the content of the foaming agent composition is 0.3-3 parts by weight, preferably 0.5-2 parts by weight.

[0112] Specifically, when the content of the polyol is 1 part by weight, the content of the auxiliary agent can be 0.01 part by weight, 0.02 part by weight, 0.03 part by weight, 0.04 part by weight, 0.05 part by weight, 0.06 part by weight, 0.07 part by weight, 0.08 part by weight, 0.09 part by weight, 0.1 part by weight, 0.11 part by weight, 0.12 part by weight, 0.13 part by weight, 0.14 part by weight, 0.15 part by weight, 0.16 part by weight, 0.17 part by weight, 0.18 part by weight, 0.19 part by weight or 0.2 part by weight.

[0113] Specifically, when the content of the polyol is 1 part by weight, the content of the foaming agent composition can be 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight or 3 parts by weight.

[0114] In some embodiments, the mass ratio of the auxiliary agent, the foaming agent composition and the organic polyisocyanate is (0.01-0.3):(0.25-4):1, preferably (0.03-0.2):(0.5-3):1.

[0115] Specifically, when the content of the organic polyisocyanate is 1 part by weight, the content of the auxiliary agent is 0.01-0.3 parts by weight, preferably 0.03-0.2 parts by weight, and the content of the foaming agent composition is 0.25-4 parts by weight, preferably 0.5-3 parts by weight.

[0116] Specifically, when the content of the organic polyisocyanate is 1 part by weight, the content of the auxiliary agent can be 0.01 part by weight, 0.02 part by weight, 0.03 part by weight, 0.04 part by weight, 0.05 part by weight, 0.06 part by weight, 0.07 part by weight, 0.08 part by weight, 0.09 part by weight, 0.1 part by weight, 0.11 part by weight, 0.12 part by weight, 0.13 part by weight, 0.14 part by weight, 0.15 part by weight, 0.16 part by weight, 0.17 part by weight, 0.18 part by weight, 0.19 part by weight, 0.2 part by weight, 0.21 part by weight, 0.22 part by weight, 0.23 part by weight, 0.24 part by weight, 0.25 part by weight, 0.26 part by weight, 0.27 part by weight, 0.28 part by weight, 0.29 part by weight or 0.3 part by weight.

[0117] Specifically, when the content of the organic polyisocyanate is 1 part by weight, the content of the blowing agent composition can be 0.25 parts by weight, 0.3 parts by weight, 0.35 parts by weight, 0.4 parts by weight, 0.45 parts by weight, 0.5 parts by weight, 0.55 parts by weight, 0.6 parts by weight, 0.65 parts by weight, 0.7 parts by weight, 0.75 parts by weight, 0.8 parts by weight, 0.85 parts by weight, 0.9 parts by weight, 0.95 parts by weight, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight or 4 parts by weight.

[0118] In the present application, the auxiliary agent is selected from one or more of a cross-linking agent, a catalyst, a foam stabilizer, an antioxidant, a flame retardant, and a pigment.

[0119] In the present application, the polyol is selected from one or both of polyether polyol and polyester polyol.

[0120] In the present application, the polyether polyol is selected from one or more of polyether diol, polyether triol, polyether tetraol, pentahydroxy polyether and polyether sorbitol, mannitol and sucrose alcohol.

[0121] The polyester polyol is selected from phthalic acid or phthalic anhydride or its ester, adipic acid, halogenated phthalic acid and polyols such as ethylene glycol, propylene glycol, diethylene glycol, trimethylolpropane, pentaerythritol and the like, and is condensed (or transesterified) or polymerized.

[0122] In the present application, the organic polyisocyanate is selected from one or more of hexamethylene diisocyanate (HDI), 2,2,4-trimethylhexane diisocyanate (TMHDI, methylcyclohexylene diisocyanate (TDI), dicyclohexylmethylene diisocyanate (MDI), isophorone diisocyanate (IPDI), xylylene diisocyanate (XDI), m- or p-1,4-methylbenzylidene diisocyanate (m or p-TMXDI for short), ethylene isocyanate (TMI), and furan diisocyanate.

[0123] In the present application, the catalyst is an organic tertiary amine and a metal salt catalyst, specifically N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl) ether, triethylenediamine, N,N,N',N'-tetramethylethylenediamine, triethylamine, N-ethylmorpholine, N-methylmorpholine, N,N-dimethylbenzylamine, N,N,N',N",N"-pentamethyldiethylenetriamine, N,N'-diethylpiperazine, N,N'-diethyl-2-methylpiperazine, N,N-dimethylethanolamine, triethanolamine, organic tin compounds, alkali metal and alkaline earth metal salt compounds, etc.

[0124] In some embodiments, among the raw materials of the polyurethane foam, the auxiliary agent is N,N-dimethylcyclohexylamine and a silicone surfactant, the polyol is a mixture of a polyether polyol with glycerol as an initiator, a polyether polyol with sorbitol as an initiator, and a polyether polyol with sucrose as an initiator; and the organic polyisocyanate is MDI.

[0125] In the present application, the density of the polyurethane foam is less than 30.0 kg / m 3 , for example, it can be 28.0kg / m 3 .

[0126] The thermal conductivity of the polyurethane foam is less than 20.0 mW / m·K, for example, 18.6 mW / m·K.

[0127] The present application provides a method for preparing polyurethane foam, which comprises the following steps:

[0128] Step 1: providing the aforementioned foaming agent composition;

[0129] Step 2: Mix the polyol and the additive to prepare a dry white material;

[0130] Step 3: mixing the foaming agent composition, water and dry white material under closed conditions at room temperature to obtain a white material liquid;

[0131] Step 4: mixing the organic polyisocyanate with the white liquid to react and prepare the polyurethane foam liquid;

[0132] Step 5: The polyurethane foam liquid is molded into polyurethane foam of a desired shape by extrusion or spraying.

[0133] In step three, the foaming agent composition, water and the dry white material are mixed under closed conditions at room temperature for 0.5-24 hours, for example, 0.5 hours, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours or 24 hours.

[0134] The mixing reaction time of the organic polyisocyanate and the white liquid is 0.1-4h, for example, it can be 0.1h, 0.2h, 0.3h, 0.4h, 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1h, 1.1h, 1.2h, 1.3h, 1.4h, 1.5h, 1.6h, 1.7h, 1.8h, 1.9h, 2h, 2.1h, 2.2h, 2.3h, 2.4h, 2.5h, 2.6h, 2.7h, 2.8h, 2.9h, 3h, 3.1h, 3.2h, 3.3h, 3.4h, 3.5h, 3.6h, 3.7h, 3.8h, 3.9h or 4h.

[0135] The GWP value of all components in the foaming agent composition provided in this application is less than 10, which is much lower than the environmental protection value of 150 required by the policy, and is an ideal environmentally friendly foaming agent composition. The foaming composition of this application adopts a specific formula composition so that the foaming composition has a suitable boiling point and a lower GWP. Because if the boiling point of the foaming agent composition is too low, such as below -20°C, it cannot be used normally at room temperature because the foaming speed is too fast; if the boiling point of the foaming agent composition is too high, such as above 60°C, after foaming, the foaming agent in the pores will become liquid, and the vapor pressure is low, and it is difficult to ensure the dimensional stability of the foam, so it is not suitable for making ultra-low density foam. The components in the foaming agent composition provided in this application have a small relative molecular weight and a low boiling point, and the density of the prepared polyurethane foam is less than 30.0kg / m 3 , thermal conductivity is less than 20.0mW / m·K.

[0136] Compared with existing polyurethane foam plastics, the polyurethane foam prepared using the foaming agent composition provided by the present application has a significantly lower molding density (more than 5%). When manufacturing polyurethane foam plastics of equal volume, less raw materials are required, thereby reducing manufacturing costs. Moreover, due to the low thermal conductivity and good thermal insulation effect, a smaller volume of polyurethane foam can be used to achieve the same thermal insulation effect, further reducing the total weight of the insulation product. In addition, the ODP of the foaming agent composition provided by the present application is zero or almost zero, and the GWP is less than 25, which can fully meet environmental protection requirements. Furthermore, the polyurethane foam prepared using the foaming agent composition provided by the present application has a low thermal conductivity, good foam thermal insulation performance, which is beneficial to reducing the energy consumption of refrigeration equipment, and the polyurethane foam liquid has good fluidity, and it is easy to achieve uniform density distribution, smooth surface, and better foam compression strength and dimensional stability during construction.

[0137] Example

[0138] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods.

[0139] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0140] Example 1

[0141] The preparation process of polyurethane foam is as follows:

[0142] 1) A polyol (mixed with 25 g of polyether polyol 450L, having a hydroxyl value of 500 mgKOH / g, and 45 g of polyester polyol PS-3152, having a hydroxyl value of 315 mgKOH / g) and an additive (mixed with 12 g of flame retardant TCPP, 1 g of catalyst PCS, and 2 g of surfactant AK 8803) were mixed to prepare a dry white material.

[0143] 2) 15 g of n-butane, 25 g of cyclopentane, 30 g of trans-1,3,3,3-tetrafluoropropene, 25 g of trans-1-chloro-3,3,3-trifluoropropene, and 3 g of water were mixed at room temperature (15-25° C.) under sealed conditions (1-3 atm pressure) for 1 hour to obtain a foaming composition.

[0144] 3) 150 g of polyisocyanate (polyisocyanate PM200) was added to the foaming composition and mixed evenly to allow the polyisocyanate and the foaming composition to undergo a preliminary polymerization reaction to obtain a polyurethane foam liquid.

[0145] 4) The resulting polyurethane foam was hydraulically squeezed into a sheet mold using a screw extruder and foamed at room temperature for 4 hours. The mold was then disassembled to obtain a polyurethane foam profile of suitable shape and structure. The parameters of the profile are shown in Table 1.

[0146] The difference between Examples 2 to 5 and Example 1 is only the mass ratio of the first hydrocarbon to the second hydrocarbon. See Table 1 for details.

[0147] The difference between Example 6 to Example 9 and Example 1 is only the mass ratio of the first fluorine-containing compound to the second fluorine-containing compound. See Table 1 for details.

[0148] The only difference between Example 10 and Example 1 is the type of the first hydrocarbon. See Table 1 for details.

[0149] The difference between Example 11 to Example 13 and Example 1 is that the contents of the first hydrocarbon compound, the second hydrocarbon compound, the first fluorine-containing compound, and the second fluorine-containing compound are different. Details are shown in Table 1.

[0150] The difference between Example 14 and Example 15 is the water content, as shown in Table 1 for details.

[0151] The difference between Example 16 to Example 18 and Example 1 lies in the different types of the first hydrocarbon compound, the second hydrocarbon compound, the first fluorine-containing compound and the second fluorine-containing compound. See Table 1 for details.

[0152] The difference between Comparative Example 1 and Example 1 is that there is no fluorine-containing compound, as shown in Table 1 for details.

[0153] The difference between Comparative Example 2 and Example 1 is that there is no hydrocarbon, as shown in Table 1 for details.

[0154] The difference between Comparative Example 3 and Example 1 is that there is no water. See Table 1 for details.

[0155] The difference between Comparative Example 4 and Example 1 lies in the different contents of the first hydrocarbon compound, the second hydrocarbon compound, the first fluorine-containing compound, the second fluorine-containing compound and water. Details are shown in Table 1.

[0156] The difference between Comparative Example 5 and Example 1 is that there is no second hydrocarbon compound. See Table 1 for details.

[0157] The difference between Comparative Example 6 and Example 1 is that there is no second fluorine-containing compound, as shown in Table 1 for details.

[0158] Table 1 shows the material conditions and parameters of each embodiment and comparative example

[0159] Summary: It can be seen from the above table that the foam density and thermal conductivity of the foamed material prepared by the foaming composition of this application are relatively small, wherein the foam density is between 26.1 and 28.0 kg / m 3The thermal conductivity is in the range of 16.8 to 18.2 mW / m·K, and the GWP value can be as low as below 25, or even below 10.

[0160] Although the embodiments of the present application are described above, the present application is not limited to the above-mentioned specific embodiments and application fields. The above-mentioned specific embodiments are merely illustrative and instructive, and not restrictive. A person of ordinary skill in the art, guided by this specification and without departing from the scope of protection of the claims of this application, may also devise various forms, all of which fall within the scope of protection of this application.

Claims

1. A foaming composition, wherein Including hydrocarbons, fluorinated compounds (C n H 2n-m O z X m ) and water, in the foaming composition, the mass fraction of the hydrocarbon is 20-90%, the C n H 2n-m O z X m The mass fraction of the water is 0.1-15%, and the mass fraction of the water is 10-80%. n H 2n-m O z X m wherein n is an integer of 3-10; z is 0 or 1; n≤m≤2n, and X is a halogen.

2. The foaming composition according to claim 1, wherein The X is selected from at least one of F, Cl, Br and I, and when X comprises two or more elements, the F element accounts for more than 50 mol% of X.

3. The foaming composition according to claim 1, wherein The fluorine-containing compound is selected from one or more of 3,3,3-trifluoropropylene, cis-1,3,3,3-tetrafluoropropylene, trans-1,3,3,3-tetrafluoropropylene, trans-1,1,1,3,3,3-hexafluoro-2-butene, perfluorohexanone, cis-1,1,1,3,3,3-hexafluoro-2-butene, 2-chloro-3,3,3-trifluoropropylene, 1-chloro-2,3,3-trifluoropropylene, 1-chloro-2,3,3,3-tetrafluoropropylene, perfluorobutanone, perfluoropentanone, perfluorohexanone, methyl perfluoroheptyl ketone, cis-1-chloro-3,3,3-trifluoropropylene and trans-1-chloro-3,3,3-trifluoropropylene.

4. The foaming composition according to any one of claims 1 to 3, wherein From hydrocarbons, C n H 2n-m O z X m and water, in the foaming composition, the mass fraction of the hydrocarbon is 20-90%, the C n H 2n-m O z X m The mass fraction of the argon is 10-80%, and the mass fraction of the water is 0.1-15%.

5. The foaming composition according to any one of claims 1 to 3, wherein The GWP value of the foaming composition is less than 25.

6. The foaming composition according to claim 1, wherein The hydrocarbons include a first hydrocarbon and a second hydrocarbon, and a boiling point of the first hydrocarbon is lower than a boiling point of the second hydrocarbon.

7. The foaming composition according to claim 6, wherein The mass ratio of the first hydrocarbon to the second hydrocarbon is (1-50):

10.

8. The foaming composition according to claim 6, wherein The first hydrocarbon is n-butane, isobutane or neopentane; The second hydrocarbon is selected from any one of cyclopentane, n-pentane and isopentane.

9. The foaming composition according to any one of claims 1 to 3, wherein The fluorine-containing compound includes a first fluorine-containing compound and a second fluorine-containing compound, and a boiling point of the first fluorine-containing compound is lower than a boiling point of the second fluorine-containing compound.

10. The foaming composition according to claim 9, wherein The mass ratio of the first fluorine-containing compound to the second fluorine-containing compound is (1-50):

10.

11. The foaming composition according to claim 9, wherein The first fluorine-containing compound is selected from any one of 3,3,3-trifluoropropene, cis-1,3,3,3-tetrafluoropropene, perfluorobutanone, 2-chloro-3,3,3-trifluoropropene, trans-1,3,3,3-tetrafluoropropene or trans-1,1,1,3,3,3-hexafluoro-2-butene; The second fluorine-containing compound is selected from any one of perfluoropentanone, perfluorohexanone, methyl perfluoroheptyl ketone, 1-chloro-2,3,3-trifluoropropene, 1-chloro-2,3,3,3-tetrafluoropropene, cis-1,1,1,3,3,3-hexafluoro-2-butene, cis-1-chloro-3,3,3-trifluoropropene or trans-1-chloro-3,3,3-trifluoropropene.

12. A polyurethane foam, wherein: The raw materials include the foaming composition described in any one of claims 1 to 11.

13. The polyurethane foam according to claim 12, wherein: The raw materials of the polyurethane foam also include polyol, organic polyisocyanate and auxiliary agent.

14. The polyurethane foam according to claim 13, wherein: The mass ratio of the auxiliary agent, the foaming agent composition and the polyol is (0.01-0.2):(0.3-3):1; or The mass ratio of the auxiliary agent, the foaming agent composition and the organic polyisocyanate is (0.01-0.3):(0.25-4):

1.

15. The polyurethane foam according to claim 12, wherein: The density of the polyurethane foam is less than 30.0 kg / m 3 ;or The thermal conductivity of the polyurethane foam is less than 20.0 mW / m·K.

16. A method for preparing polyurethane foam, wherein: The steps include: Providing a blowing agent composition according to any one of claims 1 to 11; Mixing polyols and additives to prepare dry white material; Mixing the foaming agent composition, water and dry white material under closed conditions at room temperature to obtain white material liquid; The organic polyisocyanate is mixed with the white liquid to react, so as to obtain the polyurethane foam liquid; The polyurethane foam liquid is formed into polyurethane foam of a desired shape through extrusion or spraying.

17. The preparation method according to claim 16, wherein: The foaming agent composition, water and the dry white material are mixed in a closed condition at room temperature for 0.5-24 hours; or The organic polyisocyanate and the white liquid are mixed and reacted for 0.1-4 hours.

Citation Information

Patent Citations

  • Foaming agent composition, polyurethane foam and manufacturing method thereof

    CN104262670A

  • Polyurethane reaction composition for negative pressure foaming and method for preparing polyurethane foam by using composition

    CN105985503A

  • Foaming agent composition, polyurethane reaction composition and polyurethane foam and application thereof

    CN107266699A

  • Foaming composition, polyurethane foam and preparation method thereof

    CN116285306A

  • Tri-blend blowing agent composition for polymeric foam

    US20230122141A1