By preparing tetrahydronaphthol-phosphine post-transition metal complexes, the problems of low activity of existing catalysts in ethylene polymerization at high temperatures and copolymerization of acrylate monomers were solved, realizing efficient and low-cost ethylene polymerization and copolymerization, and preparing polymers with narrow molecular weight distribution.

WO2024239969A1PCT designated stage expired Publication Date: 2024-11-28CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/091993
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-05-09
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing catalysts exhibit low activity in ethylene polymerization at high temperatures and cannot be directly copolymerized with acrylate monomers, resulting in complex and costly preparation methods.

Method used

A tetrahydronaphthol-phosphine post-transition metal complex is provided. By reacting the complex with a group VIII metal compound through a specific structural formula (I), a catalyst with good thermal stability and high ethylene polymerization activity is prepared, which can copolymerize with acrylate monomers at higher temperatures.

Benefits of technology

The high-temperature polymerization of highly reactive ethylene and copolymerization of acrylate monomers were achieved, resulting in polymers with narrow molecular weight distributions. The synthesis method is simple and low-cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024091993_28112024_PF_FP_ABST
    Figure CN2024091993_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of olefin polymerization catalysts. Disclosed are 5,6,7,8-tetrahydro-1-naphthol-phosphine post-transition metal complexes, a preparation method therefor, and the use thereof. The structure of the complexes is as shown in formula (I), in which R7-R11 are selected from hydrogen, halogens, hydroxyl, and substituted or unsubstituted C1-C15 hydrocarbyls, and R2 and R3 are selected from halogens, C1-C10 hydrocarbyls, P(R4)3, NR5R6 and OR12R13, wherein R4 is selected from substituted or unsubstituted C1-C10 hydrocarbyls, and R5, R6, R12 and R13 are selected from C1-C6 hydrocarbyls, or R5 and R6 are linked to N to form a five-membered ring or six-membered ring, or R12 and R13 are linked to O to form a five-membered ring or six-membered ring. Said complexes have good thermal stability, have relatively high ethylene polymerization activity at relatively high temperatures, and has a relatively good property of copolymerization with acrylate type monomers, prepared polymers having relatively good properties.
Need to check novelty before this filing date? Find Prior Art

Description

Tetrahydronaphthol-phosphine late transition metal complex and its preparation method and application

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of Chinese patent application No. 202310573961.0 filed on May 19, 2023, the contents of which are incorporated herein by reference. Technical Field

[0003] The present invention relates to the technical field of olefin polymerization catalysts, and in particular to a tetralinol-phosphine late transition metal complex and a preparation method and application thereof. Background Art

[0004] Polyethylene materials are widely used due to their good chemical resistance, low price, simple preparation, low density, and good mechanical properties. Among them, late transition metal catalysts have attracted widespread attention in the scientific research community due to their high ethylene homopolymerization activity, good tolerance to polar groups, and the ability to directly coordinate copolymerize olefins with polar monomers under relatively mild conditions (see, for example, S. D. Ittel, Chem Rev, 2000, 100(4), 1169-1203; H. Mu, Coord Chem Rev, 2021, 435, 213802).

[0005] In 1995, Brookhart et al. reported a class of α-diimine Ni(II) complexes that can polymerize ethylene with high activity. The cationic α-diimine palladium complexes they developed were successfully applied to the copolymerization of ethylene or propylene with acrylates. Due to the unique "β-H elimination" and "chain walking" characteristics, the polar groups in the highly branched copolymers are mostly located at the chain ends (see, for example, M. Brookhart, J Am Chem Soc, 1996, 118(1), 267-268); in 2000, Grubbs et al. developed a salicylaldehyde imine neutral nickel catalyst with good tolerance to heteroatoms, which achieved the copolymerization of ethylene and functionalized norbornene to form a linear copolymer with high insertion rate (see, for example, RH Grubbs, Science, 2000, 287, 460-462); in 2002, Drent et al. reported an electronically asymmetric neutral phosphinesulfonic acid neutral palladium complex as another classic catalyst for ethylene homo / copolymerization (see, for example, E. Drent, Chem Commun, 2002, 7, 744-745), which can catalyze the copolymerization of ethylene with a variety of simple industrial bulk polar monomers (acrylonitrile, vinyl acetate, acrylic acid and acrylates, etc.) to form linear copolymers (see, for example, E. Drent, Chem. Commun. 2002, 7, 744-745); Mecking, Nozaki, Jordon and other research groups have conducted in-depth research on the copolymerization reaction behavior and catalytic mechanism of ethylene initiated by this type of catalyst, further promoting the development of late transition metal catalysts.

[0006] However, when the above catalyst is used at high temperature, its ethylene polymerization activity is low, it cannot directly homopolymerize with ethylene and cannot be coordinated and copolymerized with acrylic esters. At the same time, its preparation method is complicated and the cost is high.

[0007] Summary of the Invention

[0008] The present invention aims to overcome the problem of low ethylene polymerization activity of catalysts in the prior art at high temperatures and to provide a tetralinol-phosphine late transition metal complex, a preparation method thereof, and applications thereof. The tetralinol-phosphine late transition metal complex has good thermal stability, high ethylene polymerization activity at relatively high temperatures, and high copolymerization performance with acrylic acid ester monomers. The resulting polymer has good properties, such as a narrow molecular weight distribution.

[0009] In order to achieve the above object, the present invention provides a tetralin-phosphine late transition metal complex, the structural formula of which is shown in formula (I):

[0010] M is selected from Group VIII metals, R7-R 11Each is independently selected from hydrogen, halogen, hydroxyl and substituted or unsubstituted C1-C15 hydrocarbon group, R2 and R3 are independently selected from halogen, C1-C10 hydrocarbon group, P(R4)3, NR5R6 and OR 12 R 13 ;

[0011] wherein R4 is selected from substituted or unsubstituted C1-C10 alkyl and substituted or unsubstituted C6-C10 aryl; R5 and R6 are each independently selected from C1-C10 hydrocarbon groups, or R5, R6 and N are connected to form a five-membered ring or a six-membered ring; R 12 and R 13 Each independently selected from C1-C10 hydrocarbon group, or R 12 、R 13 Connected with O to form a five-membered ring or a six-membered ring.

[0012] The second aspect of the present invention provides a method for preparing a tetralinol-phosphine late transition metal complex, the method comprising the following steps:

[0013] (1) reacting the compound represented by formula (II) with the compound represented by formula (III) to obtain a ligand;

[0014] (2) reacting the ligand with the M metal compound;

[0015] Wherein, the metal M in the M metal compound is selected from Group VIII metals;

[0016] In formula (III), X is halogen; R7-R 11 Each is independently selected from hydrogen, halogen, hydroxyl and substituted or unsubstituted C1-C15 hydrocarbon group, R2 and R3 are independently selected from halogen, C1-C10 hydrocarbon group, P(R4)3, NR5R6 and OR 12 R 13 , wherein R4 is selected from substituted or unsubstituted C1-C10 alkyl and substituted or unsubstituted C6-C10 aryl; R5 and R6 are each independently selected from C1-C10 hydrocarbon group, or R5, R6 and N are connected to form a five-membered ring or a six-membered ring; R 12 and R 13 Each independently selected from C1-C10 hydrocarbon group, or R 12 、R 13 Connected with O to form a five-membered ring or a six-membered ring.

[0017] The third aspect of the present invention provides an olefin polymerization method, which comprises carrying out an olefin polymerization reaction in the presence of the tetralinol-phosphine late transition metal complex provided by the present invention.

[0018] According to the technical solution of the present invention, the tetralinol-phosphine late transition metal complex has good thermal stability, high ethylene polymerization activity at higher temperatures, and high copolymerization performance with acrylic acid ester monomers. The prepared polymer has good properties, such as a narrow molecular weight distribution.

[0019] Compared with the prior art, the technical solution of the present invention has the following advantages:

[0020] (1) The synthesis method of the tetrahydronaphthol-phosphine late transition metal complex of the present invention is simple, has high yield and low cost;

[0021] (2) The tetralinol-phosphine late transition metal complex of the present invention can catalyze ethylene polymerization with high activity, has high polymerization activity at a high polymerization temperature, and can prepare linear polyethylene with adjustable relative molecular weight;

[0022] (3) The tetralinol-phosphine late transition metal complex of the present invention has high copolymerization performance with acrylic ester monomers. DETAILED DESCRIPTION

[0023] The following is a detailed description of the specific embodiments of the present invention. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention and are not intended to limit the present invention.

[0024] The structural formula of the tetralinol-phosphine late transition metal complex of the present invention is shown in formula (I),

[0025] M is selected from Group VIII metals, R7-R 11 Each is independently selected from hydrogen, halogen, hydroxyl and substituted or unsubstituted C1-C15 hydrocarbon group, R2 and R3 are independently selected from halogen, C1-C10 hydrocarbon group, P(R4)3, NR5R6 and OR 12 R 13 ;

[0026] wherein R4 is selected from substituted or unsubstituted C1-C10 alkyl and substituted or unsubstituted C6-C10 aryl; R5 and R6 are each independently selected from C1-C10 hydrocarbon, or R5, R6 and N are connected to form a five-membered ring or a six-membered ring; R 12 and R 13 Each independently selected from C1-C10 hydrocarbon group, or R 12 、R 13 Connected with O to form a five-membered ring or a six-membered ring.

[0027] In a more preferred embodiment, R7-R 11Each is independently selected from hydrogen, halogen, hydroxyl, substituted or unsubstituted C1-C15 alkyl and substituted or unsubstituted C6-C15 aryl, and the substituent is selected from halogen, hydroxyl, C1-C10 alkyl, halogenated C1-C10 alkyl, C1-C10 alkoxy or halogenated C1-C10 alkoxy.

[0028] In a more preferred embodiment, M is nickel or palladium.

[0029] In a preferred embodiment, R2 and R3 are each independently selected from halogen, C1-C8 hydrocarbon, P(R4)3, NR5R6 or OR 12 R 13 , wherein R4 is selected from substituted or unsubstituted C1-C10 alkyl and substituted or unsubstituted C6-C10 aryl; R5 and R6 are each independently selected from C1-C6 hydrocarbon group, or R5, R6 and N are connected to form a five-membered ring or a six-membered ring; R 12 and R 13 Each independently selected from C1-C6 hydrocarbon group, or R 12 、R 13 Connected with O to form a five-membered ring or a six-membered ring.

[0030] In a preferred embodiment, at least one of R2 and R3 is selected from halogen or C1-C10 hydrocarbon group.

[0031] In some embodiments, R2 and R3 are each independently selected from halogen and C1-C10 hydrocarbon group (such as C1-C10 alkyl or C6-C10 aryl).

[0032] In other embodiments, R2 is selected from halogen or C1-C8 hydrocarbon group (such as C1-C8 alkyl or C6-C8 aryl), R3 is selected from P(R4)3, NR5R6 or OR 12 R 13 , wherein R4 is selected from substituted or unsubstituted C1-C10 alkyl and substituted or unsubstituted C6-C10 aryl; R5 and R6 are each independently selected from C1-C6 hydrocarbon groups, and R5, R6 and N are connected to form a five-membered ring or a six-membered ring; R 12 and R 13 are each independently selected from C1-C10 hydrocarbon groups, and R 12 、R 13 Connected with O to form a five-membered ring or a six-membered ring.

[0033] In a preferred embodiment, when R2 and R3 are each independently selected from P(R4)3, P(R4)3 may be PMe3, PPh3 or PEt3; when R2 and R3 are each independently selected from NR5R6, NR5R6 may be pyridine (C5H5N), 2-picoline, 3-picoline or 4-picoline; when R2 and R3 are each independently selected from OR12 R 13 When, OR 12 R 13 It may be tetrahydrofuran (C4H8O), 2-methyltetrahydrofuran, 3-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran or 2,2-dimethyltetrahydrofuran.

[0034] As used herein, "Me" refers to methyl, "Ph" refers to phenyl, and "Et" refers to ethyl.

[0035] In the present invention, the "substituted" in "substituted or unsubstituted" refers to containing substituents, and the substituents here can be selected from halogen, hydroxyl, C1-C6 alkyl, halogenated C1-C6 alkyl, C1-C6 alkoxy or halogenated C1-C6 alkoxy.

[0036] In one embodiment, the C1-C6 alkyl group is selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl, n-hexyl, isohexyl or 3,3-dimethylbutyl.

[0037] Preferably, the C1-C6 alkoxy group is selected from methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, n-pentoxy, isopentoxy, n-hexoxy, isohexoxy or 3,3-dimethylbutoxy.

[0038] In the present invention, the halogen is selected from fluorine, chlorine, bromine or iodine.

[0039] In a further preferred embodiment, the tetralinol-phosphine late transition metal complex is selected from the group consisting of the following complexes:

[0040] Complex 1: Complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5;

[0041] Complex 2: Complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is phenyl, and R3 is PMe3;

[0042] Complex 3: Complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is Cl, and R3 is -OC4H8;

[0043] Complex 4: Complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is Br, and R3 is -OC4H8;

[0044] Complex 5: Complex represented by formula (I), wherein M is Ni, R7, R9 and R 10is H, R8 is methyl, R 11 is isopropyl, R2 is methyl, and R3 is -NC5H5;

[0045] Complex 6: Complex represented by formula (I), wherein M is Ni, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is phenyl, and R3 is PMe3;

[0046] Complex 7: Complex represented by formula (I), wherein M is Ni, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is Cl, and R3 is -OC4H8;

[0047] Complex 8: Complex represented by formula (I), wherein M is Ni, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is Br, and R3 is -OC4H8;

[0048] Complex 9: Complex represented by formula (I), wherein M is Pd, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5;

[0049] Complex 10: Complex represented by formula (I), wherein M is Pd, R7-R 11 is H, R2 is Cl, and R3 is PMe3;

[0050] Complex 11: a complex represented by formula (I), wherein M is Pd, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is methyl, and R3 is -NC5H5;

[0051] Complex 12: A complex represented by formula (I), wherein M is Pd, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is Cl, and R3 is PMe3.

[0052] The preparation method of the tetralinol-phosphine late transition metal complex of the present invention may include:

[0053] (1) reacting the compound represented by formula (II) with the compound represented by formula (III) to obtain a ligand represented by formula (IV);

[0054] (2) reacting the ligand with the M metal compound.

[0055] In formula (III), X is a halogen, specifically, for example, chlorine or bromine, and most preferably chlorine.

[0056] In formula (III), R7-R 11 The definition of is the same as described above.

[0057] In the method of the present invention, the metal M in the M metal compound is selected from Group VIII metals, preferably nickel or palladium.

[0058] In a preferred embodiment, the M metal compound is selected from nickel dimethyldipyridinium (Py2NiMe2), bis(1,5-cyclooctadiene) nickel (Ni(COD)2), nickel dichlorotetrapyridinium (Ni2Cl2Py4), ethylene glycol dimethyl ether nickel bromide ((DME)NiBr2), ethylene glycol dimethyl ether nickel chloride ((DME)NiCl2), dichlorobis(trimethylphosphine) nickel (NiCl2(PMe3)2), bis(pyridine)bis[(trimethylsilyl)methyl]nickel (Ni(Py)2(CH2SiMe3)2), bromo(phenyl)(N,N,N',N'-tetramethyl-1,2-ethylenediamine)nickel (NiArBr(TMEDA)), dibenzyldipyridinium nickel (Ni(CH2Ph)2Py2), phenyl(trimethylphosphine)nickel bromide (Ni One or more of PhBr(PMe3)2, phenyl(triethylphosphine)nickel chloride (NiPhCl(PEt3)2), diphenylbis(trimethylphosphine)nickel (NiPh2(PMe3)2), dichlorobis(trimethylphosphine)nickel (NiCl2(PMe3)2), dimethyldipyridine palladium (Pd(Me)2Py2), dichlorodipyridine palladium (PdCl2Py2), di(pyridine)bis[(trimethylsilyl)methyl]palladium (Pd(Py)2(CH2SiMe3)2), dibenzyldipyridine palladium (Pd(CH2Ph)2Py2), methyl-1,5-cyclooctadiene-palladium chloride (Pd(COD)ClMe) and dimethyl(N,N,N',N'-tetramethyl-1,2-ethylenediamine)palladium ((TMEDA)PdMe2).

[0059] In the method of the present invention, the reaction process of step (1) is shown in the following reaction formula:

[0060] Among them, X and R7-R 11 The definition of is the same as described above.

[0061] In the method of the present invention, the reaction process of step (2) is shown in the following reaction formula:

[0062] Among them, M, R2, R3, R7-R 11 The definition of is the same as described above.

[0063] In a preferred embodiment, the reaction of step (1) is carried out in the presence of a solvent. In a specific example, the solvent can be diethyl ether.

[0064] In a preferred embodiment, the reaction of step (2) is carried out in the presence of a reaction solvent. In a specific example, the reaction solvent can be toluene or tetrahydrofuran.

[0065] In a preferred embodiment, in step (2), the molar ratio of the M metal compound to the ligand is 1.1-1.3:1.

[0066] In a specific embodiment, the preparation process of step (1) comprises: dissolving the compound represented by formula (II) in anhydrous ether in an atmosphere of protective gas (such as nitrogen), adding n-BuLi (n-butyl lithium) solution dropwise at -78°C, and gradually returning to room temperature after the reaction; then, adding anhydrous ether solution of the compound represented by formula (III) dropwise (in an ice-water bath), slowly warming to room temperature, and stirring to react overnight. Quenching with water, extracting the organic phase with anhydrous ether, concentrating the obtained organic phase, deoxygenating by freezing cycle, adding 15mL of concentrated hydrochloric acid under a nitrogen atmosphere to react, tracking the completion of the reaction by TLC, then adding NaHCO3 aqueous solution for neutralization, quenching with water, extracting the organic phase with anhydrous ether, drying with anhydrous MgSO4, filtering, concentrating, and column chromatography to obtain the ligand represented by formula (IV).

[0067] In a specific embodiment, the preparation process of step (2) comprises: in an atmosphere of protective gas (such as nitrogen), dissolving the ligand obtained in step (1) and the M metal compound in a reaction solvent (such as toluene, tetrahydrofuran, etc.), stirring and mixing the ligand solution and the solution of the M metal compound, reacting at room temperature for 8 to 10 hours, filtering, concentrating the filtrate, adding heptane for recrystallization, and obtaining the tetralinol-phosphine late transition metal complex of the present invention.

[0068] The present invention also provides an olefin polymerization method, which comprises carrying out an olefin polymerization reaction in the presence of the tetralinol-phosphine late transition metal complex provided by the present invention.

[0069] In the olefin polymerization method of the present invention, the olefin polymerization reaction can be homopolymerization or copolymerization.

[0070] In some embodiments, the polymerization monomer is ethylene. In this embodiment, the olefin polymerization reaction is a homopolymerization of ethylene.

[0071] In other embodiments, the polymerizable monomers include ethylene and α-olefins. In this embodiment, the olefin polymerization reaction is a copolymerization reaction. The α-olefin can be a C3-C16 α-olefin, specifically, at least one selected from, but not limited to, propylene, butene, pentene, hexene, octene, and 4-methylpentene-1. As an optional example, the α-olefin can have one or more polar functional groups, such as hydroxyl groups, carboxyl groups, ester groups, and the like.

[0072] In other embodiments, the polymerization monomers include ethylene and acrylate monomers. In this embodiment, the olefin polymerization reaction is a copolymerization reaction. The general formula of the acrylate monomer is CH2=C(R 31 )CO2(R 32 ), where R 31 It can be H or a C1-C10 hydrocarbon group, which may have a branch, a ring and / or an unsaturated bond; R 32 It may be a C1-C30 hydrocarbon group, which may have a branch, a ring and / or an unsaturated bond, and R 32 Heteroatoms may be contained at any position.

[0073] When R 31 When the number of carbon atoms is 11 or more, the polymerization activity tends to be less. 31 is H or C1-C10 hydrocarbon group. 31 is H or a C1-C5 hydrocarbon group. More preferably, R 31 is H or methyl.

[0074] Similarly, when R 32 When the number of carbon atoms is greater than 30, the polymerization activity tends to be less. 32 The number of carbon atoms is 1-30, preferably 1-12, more preferably 1-8.

[0075] In addition, as R 32 The heteroatoms optionally contained in R can be selected from oxygen, sulfur, selenium, phosphorus, nitrogen, silicon, fluorine, boron, etc. Among these heteroatoms, oxygen, silicon and fluorine are preferred, and oxygen is more preferred. 32 It is also preferred.

[0076] Further preferably, specific examples of the acrylic acid ester monomers include, but are not limited to, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, toluyl (meth)acrylate, ) benzyl (meth)acrylate, hydroxyethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, 2-aminoethyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, glycidyl (meth)acrylate, oxirane (meth)acrylate, trifluoromethyl (meth)acrylate, 2-trifluoromethylethyl (meth)acrylate, perfluoroethyl (meth)acrylate, (meth)acrylamide, (meth)acryloyldimethylamide, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and the like. The above-mentioned acrylic acid ester monomers may be used alone or in combination of multiple types.

[0077] In the olefin polymerization method of the present invention, the temperature of the olefin polymerization reaction can be -78°C to 200°C, preferably -20°C to 150°C. The tetralinol-phosphine late transition metal complex of the present invention has high polymerization activity at high temperatures, and therefore the olefin polymerization method of the present invention is particularly suitable for olefin polymerization reactions at high temperatures. In some embodiments, the temperature of the olefin polymerization reaction is 30-100°C, preferably 70-100°C.

[0078] In the olefin polymerization method of the present invention, the polymerization pressure of the olefin polymerization reaction may be 0.01 to 10 MPa, preferably 0.01 to 5 MPa.

[0079] In the olefin polymerization method of the present invention, the polymerization reaction time of the olefin polymerization reaction can be 5 to 60 minutes.

[0080] In the present invention, "polymerization pressure" refers to the ethylene pressure in the polymerization system and is expressed as absolute pressure.

[0081] In the olefin polymerization method of the present invention, the polymerization is carried out by polymerizing monomers in a solvent. The polymerization solvent can be selected from one or more of alkanes, aromatic hydrocarbons, and halogenated hydrocarbons. Preferably, the polymerization solvent is selected from one or more of hexane, pentane, heptane, benzene, toluene, dichloromethane, chloroform, and dichloroethane, and more preferably one or more of hexane, toluene, and heptane.

[0082] In the present invention, alkyl refers to a straight-chain alkyl, a branched-chain alkyl or a cycloalkyl, including but not limited to: methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, tert-pentyl, neopentyl, n-hexyl, n-heptyl, n-octyl, n-decyl, cyclopropyl, cyclopentyl, cyclohexyl, 4-methylcyclohexyl, 4-ethylcyclohexyl, 4-n-propylcyclohexyl and 4-n-butylcyclohexyl.

[0083] In the present invention, examples of the aryl group include, but are not limited to, phenyl, 4-methylphenyl, 4-ethylphenyl, dimethylphenyl, and vinylphenyl.

[0084] In the present invention, alkenyl refers to straight-chain alkenyl, branched-chain alkenyl or cycloalkenyl, including but not limited to vinyl, allyl and butenyl.

[0085] In the present invention, examples of the aralkyl group include, but are not limited to, phenylmethyl, phenylethyl, phenyl-n-propyl, phenyl-isopropyl, phenyl-n-butyl, and phenyl-t-butyl.

[0086] In the present invention, examples of the alkaryl group include, but are not limited to, tolyl, ethylphenyl, n-propylphenyl, isopropylphenyl, n-butylphenyl, and tert-butylphenyl.

[0087] The following examples further illustrate the phosphine-phenol late transition metal complexes, their preparation methods, and applications of the present invention. The examples are implemented based on the technical solutions of the present invention, and provide detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following examples.

[0088] The experimental methods in the following examples, unless otherwise specified, are all conventional methods in the art; the experimental materials used in the following examples, unless otherwise specified, are all commercially available.

[0089] The analytical characterization instruments and test methods used in the following examples and comparative examples are as follows:

[0090] (1) Nuclear magnetic resonance instrument: Avance III HD 500 (500 MHz), with tetramethylsilane (TMS) as the internal standard;

[0091] (2) Polymer molecular weight and molecular weight distribution (PDI) (PDI = Mw / Mn): measured using a PL-GPC220 chromatograph with trichlorobenzene as solvent at 150°C (standard: PS, flow rate: 1.0 mL / min, column: 3×PLgel 10 μm M1×ED-B, 300×7.5 nm);

[0092] (3) Activity measurement method: The polymer was washed with hydrochloric acid ethanol solution, vacuum dried, and the weight of the polymer was measured; the polymerization activity was calculated as follows: polymer weight (g) / metal (mol) × 60 / polymerization time (min);

[0093] (4) Analysis of comonomer content of polymer: using 1 H NMR, 13 C NMR spectroscopy was performed on a 400 MHz Bruker Avance 400 NMR spectrometer using a 10 mm PASEX 13 probe. The polymer samples were dissolved in 1,2,4-trichlorobenzene at 120°C for analysis.

[0094] Example 1

[0095] Complex 1: Complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5.

[0096] Under a nitrogen atmosphere, the compound represented by formula (II) (2.32 g, 10 mmol) was dissolved in anhydrous ether (20 mL), and n-butyllithium solution (2.7 M, 4.0 mL, 11 mmol) was added dropwise at -78 ° C. The reaction gradually returned to room temperature and continued stirring for 12 h to obtain a white precipitate. Dicyclohexylphosphine chloride (10 mmol, 2.32 g) was evenly dispersed in 10 mL of anhydrous ether and added dropwise to the original reaction system under an ice-water bath. The temperature was slowly raised to room temperature and stirred overnight. The mixture was quenched with water and the organic phase was extracted with anhydrous ether. The obtained organic phase was concentrated and deoxygenated under a freeze cycle. 5 mL of concentrated hydrochloric acid was added under a nitrogen atmosphere and the reaction was reacted for 5 h. After the reaction was completed by TLC tracking, a NaHCO3 aqueous solution was added for neutralization, the mixture was quenched with water, the organic phase was extracted with anhydrous ether, dried over anhydrous MgSO4, filtered, concentrated, and column chromatography was performed to obtain ligand L1 with a yield of 31%. 1H NMR (500MHz, CDCl3, TMS): δ11.65 (s, 0.9H), 6.72-6.68 (m, 1H), 6.58-6.56 (m, 1H), 2.74-2.72 (t, J= 5.8Hz, 2H), 2.65-2.63 (t, J=6.3Hz, 2H), 2.06-1.96 (m, 4H), 1.86-1.68 (m, 12H), 1.45-1.13 (m, 10H). 13 C NMR (126MHz, CDCl3) δ163.26, 143.18, 143.16, 126.63, 126.58, 125.86, 125.79, 119.39, 119.30, 104.10, 103.39, 77.28, 77.03, 76.77, 36.01, 35.49, 29.98, 26.41, 26.31, 26.27, 26.17, 25.76, 25.27, 25.25, 24.10, 24.08, 22.78, 22.59, 22.54. 31 P NMR (202 MHz, CDCl3) δ 60.52.

[0097] In a nitrogen atmosphere, ligand L1 (0.517 g, 1.5 mmol) and metal nickel source (Py2NiMe2) (0.366 g, 1.5 mmol) were dissolved in toluene (10 mL) respectively. The ligand solution was then added dropwise into the metal nickel source solution with vigorous stirring. The mixture was reacted at room temperature for 10 h and filtered to obtain a brown-yellow solution. The solvent was concentrated and frozen at -30°C for crystallization to obtain complex 1 with a yield of 72%. 31 P NMR (202MHz,CDCl3)δ60.61.Elemental analysis test C 28 H 40 NNiOP: Theoretical calculated values ​​are: C, 67.76; H, 8.12; N, 2.82; measured values ​​are: C, 67.45; H, 8.42; N, 2.67.

[0098] A 1 L stainless steel polymerization kettle equipped with a mechanical stirrer was dried continuously at 130° C. for 6 h, evacuated while hot and replaced with N2 gas three times. 500 mL of toluene was injected into the polymerization kettle, and 5.0 mg (10 μmol) of complex 1 was added. The reaction was vigorously stirred at 70° C. while maintaining an ethylene pressure of 10 atm for 30 min. The reaction was neutralized with an ethanol solution acidified with 10 wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight-average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.

[0099] Example 2

[0100] Complex 1: Complex represented by formula (II), wherein M is Ni, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5.

[0101] A 1 L stainless steel polymerization kettle equipped with a mechanical stirrer was dried continuously at 130° C. for 6 h, evacuated while hot and replaced with N2 gas three times. 500 mL of toluene was injected into the polymerization kettle, and 5.0 mg (10 μmol) of complex 1 was added. The reaction was vigorously stirred at 80° C. while maintaining an ethylene pressure of 10 atm for 30 min. The reaction was neutralized with an ethanol solution acidified with 10 wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight-average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.

[0102] Example 3

[0103] Complex 1: Complex represented by formula (II), wherein M is Ni, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5.

[0104] A 1 L stainless steel polymerization kettle equipped with a mechanical stirrer was dried continuously at 130° C. for 6 h, evacuated while hot and replaced with N2 gas three times. 500 mL of toluene was injected into the polymerization kettle, and 5.0 mg (10 μmol) of complex 1 was added. The reaction was vigorously stirred at 100° C. while maintaining an ethylene pressure of 10 atm for 30 min. The reaction was neutralized with an ethanol solution acidified with 10 wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight-average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.

[0105] Example 4

[0106] Complex 1: Complex represented by formula (II), wherein M is Ni, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5;

[0107] A 100 mL stainless steel polymerization kettle equipped with a mechanical stirrer was dried continuously at 130° C. for 6 h, evacuated while hot and replaced with N2 gas three times. 50 mL of toluene and 0.45 mL (5 mmol) of methyl acrylate were injected into the polymerization kettle, and 5.0 mg (10 μmol) of complex 1 was added. The reaction was vigorously stirred at 70° C., maintaining an ethylene pressure of 15 atm, for 60 min. The reaction was neutralized with an ethanol solution acidified with 10 wt% hydrochloric acid to obtain an ethylene-acrylate copolymer. The polymer was dried and weighed to test the polymerization activity. The test data of the weight-average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.

[0108] Example 5

[0109] Complex 1: Complex represented by formula (II), wherein M is Ni, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5.

[0110] A 100 mL stainless steel polymerization kettle equipped with a mechanical stirrer was dried continuously at 130° C. for 6 h, evacuated while hot and replaced with N2 gas three times. 50 mL of toluene and 0.72 mL (5 mmol) of butyl acrylate were injected into the polymerization kettle, and 5.0 mg (10 μmol) of complex 1 was added. The reaction was stirred vigorously at 70° C., maintaining an ethylene pressure of 15 atm, for 60 min. The reaction was neutralized with an ethanol solution acidified with 10 wt% hydrochloric acid to obtain an ethylene-acrylate copolymer. The polymer was dried and weighed to test the polymerization activity. The test data of the weight-average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.

[0111] Example 6

[0112] Complex 4: Complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is Br, and R3 is -OC4H8.

[0113] Ligand L1 was prepared according to the method of Example 1.

[0114] Under nitrogen atmosphere, ligand L1 (0.688 g, 2 mmol) was dissolved in tetrahydrofuran, excess NaH (0.072 g, 3 mmol) was added, and the mixture was stirred at room temperature for 10 h. The NaH was removed by filtration, and a solution of nickel source (DME) NiBr2 (0.617 g, 2 mmol) in tetrahydrofuran was added dropwise. The reaction was allowed to proceed overnight at room temperature. The solvent was drained, and dichloromethane (40 mL) was added to dissolve the mixture. The filter cake was removed by filtration, and the filtrate was concentrated and recrystallized from heptane to obtain complex 4 with a yield of 72%. Elemental analysis test C 26 H 40 BrNiO2P: Theoretical calculated values ​​are: C, 56.35; H, 7.28; measured values ​​are: C, 56.74; H, 7.41.

[0115] A 1 L stainless steel polymerization kettle equipped with a mechanical stirrer was dried continuously at 130° C. for 6 h, evacuated while hot and replaced with N2 gas three times. 500 mL of toluene was injected into the polymerization kettle, and 5.5 mg (10 μmol) of complex 4 was added. The reaction was vigorously stirred at 30° C. while maintaining an ethylene pressure of 10 atm for 30 min. The reaction was neutralized with an ethanol solution acidified with 10 wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight-average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.

[0116] Example 7

[0117] Complex 4: Complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is Br, and R3 is -OC4H8.

[0118] A 1 L stainless steel polymerization kettle equipped with a mechanical stirrer was dried continuously at 130° C. for 6 h, evacuated while hot and replaced with N2 gas three times. 500 mL of toluene was injected into the polymerization kettle, and 5.5 mg (10 μmol) of complex 4 was added. The reaction was vigorously stirred at 80° C. while maintaining an ethylene pressure of 10 atm for 30 min. The reaction was neutralized with an ethanol solution acidified with 10 wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight-average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.

[0119] Example 8

[0120] Complex 4: Complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is Br, and R3 is -OC4H8.

[0121] A 100 mL stainless steel polymerization kettle equipped with a mechanical stirrer was dried continuously at 130° C. for 6 h, evacuated while hot and replaced with N2 gas three times. 50 mL of toluene and 0.45 mL (5 mmol) of methyl acrylate were injected into the polymerization kettle, and 5.5 mg (10 μmol) of complex 4 was added. The reaction was stirred vigorously at 70° C., maintaining an ethylene pressure of 15 atm, for 60 min. The reaction was neutralized with an ethanol solution acidified with 10 wt% hydrochloric acid to obtain an ethylene-acrylate copolymer. The polymer was dried and weighed to test the polymerization activity. The test data of the weight-average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.

[0122] Example 9

[0123] Complex 11: a complex represented by formula (I), wherein M is Pd, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5;

[0124] Ligand L1 was prepared according to the method of Example 1;

[0125] In a nitrogen atmosphere, ligand L1 (0.688 g, 2 mmol) was dissolved in toluene (20 mL), and metal palladium source (TMEDA) PdMe2 (0.51 g, 2 mmol) was dissolved in toluene (15 mL). The ligand solution was then dripped dropwise into the metal palladium source solution, stirred vigorously, and reacted at room temperature for 5 h. 0.6 mL of pyridine was added and the reaction was allowed to proceed overnight. The black solution was filtered and the solvent was removed in vacuo to obtain complex 11 with a yield of 77%. The elemental analysis test showed that C 28 H40 NOPPd: Theoretical calculated values ​​are: C, 61.82; H, 7.41; N, 2.57; Found values ​​are: C, 62.03; H, 7.58; N, 2.36;

[0126] A 1 L stainless steel polymerization kettle equipped with a mechanical stirrer was dried continuously at 130° C. for 6 h, evacuated while hot and replaced with N2 gas three times. 500 mL of toluene was injected into the polymerization kettle, 5.4 mg (10 μmol) of complex 11 and 40 μmol of B(C6F5)3 were added, and the reaction was vigorously stirred at 80° C. while maintaining an ethylene pressure of 10 atm for 30 min. The reaction was neutralized with an ethanol solution acidified with 10 wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight-average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.

[0127] Comparative Example 1

[0128] A 1 L stainless steel polymerization kettle equipped with a mechanical stirrer was dried continuously at 130° C. for 6 h, evacuated while hot and replaced with N2 gas three times. 500 mL of toluene was injected into the polymerization kettle, and then 5.0 ml of methylaluminoxane (MAO) (1.53 mol / L toluene solution) was added. 5.1 mg (10 μmol) of complex A (Chem Cat Chem 2022, 14, e202101736) was added. The reaction was stirred vigorously at 80° C., maintaining an ethylene pressure of 10 atm, for 30 min. The reaction was neutralized with an ethanol solution acidified with 10 wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight-average molecular weight, molecular weight distribution, polymerization activity, and comonomer content of the obtained polymer are shown in Table 1.

[0129] Complex A

[0130] Comparative Example 2

[0131] A 100 mL stainless steel polymerization kettle equipped with a mechanical stirrer was dried continuously at 130° C. for 6 h, evacuated while hot and replaced with N2 gas three times. 50 mL of toluene and 0.45 mL (5 mmol) of methyl acrylate were injected into the polymerization kettle, and 5.1 mg (10 μmol) of complex A was added. The reaction was carried out at 70° C., maintaining an ethylene pressure of 15 atm, and vigorously stirred for 60 min. The reaction was then neutralized with an ethanol solution acidified with 10 wt% hydrochloric acid to obtain an ethylene-acrylate copolymer. The polymer was dried and weighed to test the polymerization activity. The test data of the weight-average molecular weight, molecular weight distribution, polymerization activity, and comonomer content of the obtained polymer are shown in Table 1.

[0132] Comparative Example 3

[0133] Complex B was prepared according to the method disclosed in patent application CN102197040A.

[0134] Complex B

[0135] A 1 L stainless steel polymerization kettle equipped with a mechanical stirrer was dried continuously at 130° C. for 6 h, evacuated while hot and replaced with N2 gas three times. 500 mL of toluene was injected into the polymerization kettle, and 6.2 mg (10 μmol) of complex B was added. The reaction was vigorously stirred at 80° C. while maintaining an ethylene pressure of 10 atm for 30 min. The reaction was neutralized with an ethanol solution acidified with 10 wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight-average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.

[0136] Table 1

[0137] As can be seen from Table 1, the tetralinol-phosphine late transition metal complexes of the present invention have high polymerization activity at relatively high temperatures, and the polymers prepared therefrom have good properties. Specifically, a comparison of Examples 1-3, 6-7, and 9 with Comparative Examples 1 and 3 shows that the complexes of the present invention have significantly higher ethylene polymerization activity, and the prepared polyethylene has a significantly higher molecular weight and a significantly narrower molecular weight distribution. A comparison of Examples 4-5 and 8 with Comparative Example 2 shows that the complexes of the present invention have significantly higher copolymerization activity with acrylate monomers, and the prepared copolymers have a significantly higher molecular weight and a narrower molecular weight distribution.

[0138] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including combining the various technical features in any other suitable manner. These simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A tetralinol-phosphine late transition metal complex, characterized in that: Its structural formula is shown in formula (I), M is selected from Group VIII metals, R7-R 11 Each is independently selected from hydrogen, halogen, hydroxyl and substituted or unsubstituted C1-C15 hydrocarbon group, R2 and R3 are independently selected from halogen, C1-C10 hydrocarbon group, P(R4)3, NR5R6 and OR 12 R 13 ; Wherein, R4 is selected from substituted or unsubstituted C1-C10 alkyl and substituted or unsubstituted C6-C10 aryl; R5 and R6 are each independently selected from C1-C10 hydrocarbon group, or R5, R6 and N are connected to form a five-membered ring or a six-membered ring; R 12 and R 13 Each independently selected from C1-C10 hydrocarbon group, or R 12 , R 13 Connected with O to form a five-membered ring or a six-membered ring.

2. The tetralin-phosphine late transition metal complex according to claim 1, characterized in that: M is nickel or palladium.

3. The tetralin-phosphine late transition metal complex according to claim 1 or 2, characterized in that: R7-R 11 Each is independently selected from hydrogen, halogen, hydroxyl, substituted or unsubstituted C1-C15 alkyl and substituted or unsubstituted C6-C15 aryl, and the substituent is selected from halogen, hydroxyl, C1-C10 alkyl, halogenated C1-C10 alkyl, C1-C10 alkoxy or halogenated C1-C10 alkoxy.

4. The tetralin-phosphine late transition metal complex according to any one of claims 1 to 3, characterized in that: R2 and R3 are each independently selected from halogen, C1-C8 hydrocarbon, P(R4)3, NR5R6 or OR 12 R 13 , wherein R4 is selected from substituted or unsubstituted C1-C10 alkyl and substituted or unsubstituted C6-C10 aryl; R5 and R6 are each independently selected from C1-C6 hydrocarbon group, or R5, R6 and N are connected to each other to form a five-membered ring or a six-membered ring; R 12 and R 13 Each independently selected from C1-C6 hydrocarbon group, or R 12 , R 13 Connected with O to form a five-membered ring or a six-membered ring.

5. The tetralin-phosphine late transition metal complex according to any one of claims 1 to 4, characterized in that: It is selected from the group consisting of the following complexes: Complex 1: Complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5; Complex 2: Complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is phenyl, and R3 is PMe3; Complex 3: A complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is Cl, and R3 is -OC4H8; Complex 4: A complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is Br, and R3 is -OC4H8; Complex 5: A complex represented by formula (I), wherein M is Ni, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is methyl, and R3 is -NC5H5; Complex 6: A complex represented by formula (I), wherein M is Ni, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is phenyl, and R3 is PMe3; Complex 7: A complex represented by formula (I), wherein M is Ni, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is Cl, and R3 is -OC4H8; Complex 8: A complex represented by formula (I), wherein M is Ni, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is Br, and R3 is -OC4H8; Complex 9: A complex represented by formula (I), wherein M is Pd, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5; Complex 10: The complex represented by formula (I), wherein M is Pd, R7-R 11 is H, R2 is Cl, and R3 is PMe3; Complex 11: A complex represented by formula (I), wherein M is Pd, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is methyl, and R3 is -NC5H5; Complex 12: A complex represented by formula (I), wherein M is Pd, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is Cl, and R3 is PMe3.

6. A method for preparing a tetralinol-phosphine late transition metal complex, characterized in that: The method comprises the following steps: (1) reacting the compound represented by formula (II) with the compound represented by formula (III) to obtain a ligand; (2) reacting the ligand with an M metal compound; Wherein, the metal M in the M metal compound is selected from Group VIII metals; In formula (III), X is halogen; R7-R 11 Each is independently selected from hydrogen, halogen, hydroxyl and substituted or unsubstituted C1-C15 hydrocarbon group, R2 and R3 are independently selected from halogen, C1-C10 hydrocarbon group, P(R4)3, NR5R6 and OR 12 R 13 , wherein R4 is selected from substituted or unsubstituted C1-C10 alkyl and substituted or unsubstituted C6-C10 aryl; R5 and R6 are each independently selected from C1-C10 hydrocarbon groups, or R5, R6 and N are interconnected to form a five-membered ring or a six-membered ring; R 12 and R 13 Each independently selected from C1-C10 hydrocarbon group, or R 12 , R 13 Connected with O to form a five-membered ring or a six-membered ring.

7. The method according to claim 6, characterized in that The metal M is nickel or palladium.

8. The method according to claim 7, characterized in that The M metal compound is selected from one or more of dimethyldipyridinium nickel, bis(1,5-cyclooctadiene)nickel, dichlorotetrapyridinium nickel, ethylene glycol dimethyl ether nickel bromide, ethylene glycol dimethyl ether nickel chloride, dichlorobis(trimethylphosphine)nickel, bis(pyridine)bis[(trimethylsilyl)methyl]nickel, bromo(phenyl)(N,N,N',N'-tetramethyl-1,2-ethylenediamine)nickel, dibenzyldipyridinium nickel, phenyl(trimethylphosphine)nickel bromide, phenyl(triethylphosphine)nickel chloride, diphenylbis(trimethylphosphine)nickel, dichlorobis(trimethylphosphine)nickel, dimethyldipyridinium palladium, dichlorodipyridinium palladium, bis(pyridine)bis[(trimethylsilyl)methyl]palladium, dibenzyldipyridinium palladium, methyl-1,5-cyclooctadiene-palladium chloride and dimethyl(N,N,N',N'-tetramethyl-1,2-ethylenediamine)palladium.

9. The method according to any one of claims 6 to 8, characterized in that: The reaction in step (2) is carried out in the presence of a reaction solvent, which is toluene and / or tetrahydrofuran.

10. An olefin polymerization method, characterized in that: The method comprises carrying out olefin polymerization in the presence of the tetrahydronaphthol-phosphine late transition metal complex as claimed in any one of claims 1 to 5.

11. The method according to claim 10, characterized in that The olefin polymerization reaction is homopolymerization or copolymerization.

12. The method according to claim 10 or 11, characterized in that: The polymerizable monomer is ethylene.

13. The method according to claim 10 or 11, characterized in that: The polymerizable monomers include ethylene and α-olefins.

14. The method according to claim 10 or 11, characterized in that: The polymerizable monomers include ethylene and acrylic acid ester monomers.

15. The method according to claim 14, characterized in that The acrylic acid ester monomer is selected from methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, toluyl (meth)acrylate, benzyl (meth)acrylate, At least one of hydroxyethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, 2-aminoethyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, glycidyl (meth)acrylate, oxirane (meth)acrylate, trifluoromethyl (meth)acrylate, 2-trifluoromethylethyl (meth)acrylate, perfluoroethyl (meth)acrylate, (meth)acrylamide, (meth)acryloyldimethylamide, 2-hydroxybutyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate.

16. The method according to any one of claims 10 to 15, characterized in that: The temperature of the olefin polymerization reaction is 30-100°C.

Citation Information

Patent Citations

  • Novel metal complex, and method for producing alpha-olefin polymer and method for producing alpha-olefin / (meth)acrylate copolymer each using the metal complex

    CN102197040A

  • Naphthol skeleton phenol-phosphine neutral nickel catalyst preparation method and application in preparing ethylene / vinyl polar monomer co-polymer

    CN109320558A

  • Metal complex, catalyst component for olefin polymerization and catalyst for olefin polymerization containing the metal complex, and method for producing olefin polymer and copolymer using the metal complex