Resin composition for insulating layer and insulated wire

The resin composition for insulating layers, using polyvinyl chloride with biomass-derived plasticizers and inorganic fillers, addresses the environmental impact challenge by improving insulation and flexibility, ensuring enhanced safety and workability in insulated wires.

WO2024241401A1PCT designated stage expired Publication Date: 2024-11-28SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/018836
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The increasing demand for reducing environmental impact by moving away from fossil fuels in insulating materials for electric wires has led to a decrease in insulation performance when using biomass-derived plasticizers, necessitating a resin composition that improves insulation and flexibility while minimizing environmental load.

Method used

A resin composition for insulating layers comprising polyvinyl chloride as the main component, combined with epoxidized soybean oil, acetylated castor oil, or epoxidized linseed oil as plasticizers, and an inorganic filler like clay, calcium carbonate, or talc, along with a flame retardant, optimized to maintain flexibility and enhance insulation performance.

Benefits of technology

The composition effectively reduces environmental load, improves insulation performance, and maintains flexibility, thereby enhancing the safety and workability of insulated wires.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023018836_28112024_PF_FP_ABST
    Figure JP2023018836_28112024_PF_FP_ABST
Patent Text Reader

Abstract

This resin composition for an insulating layer according to the present disclosure contains a resin component, a plasticizer, an inorganic filler, and a flame retardant. The resin component contains polyvinyl chloride as a main component. The plasticizer is epoxidized soybean oil, acetylated castor oil, epoxidized linseed oil, or a combination thereof. The content of the plasticizer is 20-100 parts by mass based on 100 parts by mass of the polyvinyl chloride. The content of the inorganic filler is 5-40 parts by mass based on 100 parts by mass of the polyvinyl chloride.
Need to check novelty before this filing date? Find Prior Art

Description

Resin composition for insulating layer and insulated wire

[0001] The present disclosure relates to a resin composition for an insulating layer and an insulated wire.

[0002] Vinyl chloride resins have excellent electrical insulation properties, voltage resistance, heat resistance, etc., and are used as insulating materials for electric wires and cables in the fields of automobiles and electrical and electronic devices. Prior art has disclosed phthalate esters, trimellitate esters, adipate polyesters, cyclohexanedicarboxylic acid esters, etc. as plasticizers for such polyvinyl chloride compositions (see Patent Document 1).

[0003] JP 2011-207973 A

[0004] The resin composition for an insulating layer of the present disclosure contains a resin component, a plasticizer, an inorganic filler, and a flame retardant, wherein the resin component is primarily composed of polyvinyl chloride, the plasticizer is epoxidized soybean oil, acetylated castor oil, epoxidized linseed oil, or a combination thereof, the content of the plasticizer is 20 parts by mass or more and 100 parts by mass or less per 100 parts by mass of the polyvinyl chloride, and the content of the inorganic filler is 5 parts by mass or more and 40 parts by mass or less per 100 parts by mass of the polyvinyl chloride.

[0005] FIG. 1 is a schematic cross-sectional view of an insulated wire according to one embodiment of the present disclosure.

[0006] [Problem to be Solved by the Present Disclosure] In recent years, with the increasing need to reduce environmental impact, there has been a desire to move away from fossil fuels in the materials field as well, and the use of biomass has been attracting attention. Biomass, such as plant seed oil, is organic matter produced by living organisms through photosynthesis from water and carbon dioxide using solar energy, and is a carbon-neutral resource that does not newly increase carbon dioxide in the atmosphere.

[0007] On the other hand, the present inventors have found that when a biomass-derived material such as seed oil is used as a plasticizer for an insulating layer, the insulating performance is reduced compared to plasticizers derived from fossil resources such as petroleum. From the viewpoint of safety, insulating materials used in electric wires are required to have good insulating performance.

[0008] An object of the present disclosure is to provide a resin composition for an insulating layer and an insulated wire that can reduce the environmental load and improve the insulating performance and flexibility of the insulating layer.

[0009] Effect of the Present Disclosure According to the present disclosure, it is possible to provide a resin composition for an insulating layer and an insulated wire that can reduce the environmental load and improve the insulating performance and flexibility of the insulating layer.

[0010] [Description of Embodiments of the Present Invention] First, embodiments of the present disclosure will be listed and described.

[0011] The resin composition for an insulating layer of the present disclosure (1) contains a resin component, a plasticizer, an inorganic filler, and a flame retardant, wherein the resin component is primarily composed of polyvinyl chloride, the plasticizer is epoxidized soybean oil, acetylated castor oil, epoxidized linseed oil, or a combination thereof, the content of the plasticizer is 20 parts by mass or more and 100 parts by mass or less per 100 parts by mass of the polyvinyl chloride, and the content of the inorganic filler is 5 parts by mass or more and 40 parts by mass or less per 100 parts by mass of the polyvinyl chloride.

[0012] The resin composition for an insulating layer can reduce environmental impact by using epoxidized soybean oil, acetylated castor oil, epoxidized linseed oil, or a combination thereof as the plasticizer. Furthermore, the resin composition for an insulating layer can improve insulating performance while maintaining good flexibility by using 20 to 100 parts by mass of plasticizer per 100 parts by mass of polyvinyl chloride, the main component of the resin component, and 5 to 40 parts by mass of inorganic filler per 100 parts by mass of polyvinyl chloride. Therefore, the resin composition for an insulating layer can reduce environmental impact and improve the insulating performance and flexibility of the insulating layer. In the present disclosure, the term "main component" refers to the component with the highest content, and may be, for example, 80% by mass or more.

[0013] (2) In the above (1), the inorganic filler may be clay, calcium carbonate, talc, magnesium carbonate, or a combination thereof. When the inorganic filler is clay, calcium carbonate, talc, magnesium carbonate, or a combination thereof, the insulating performance of the insulating layer can be further improved.

[0014] (3) In the above (1) or (2), the flame retardant may be antimony trioxide, a brominated flame retardant, or melamine cyanurate, and the content of the flame retardant may be 1 part by mass or more and 20 parts by mass or less per 100 parts by mass of the polyvinyl chloride. By using antimony trioxide, a brominated flame retardant, or melamine cyanurate, and the content of the flame retardant is 1 part by mass or more and 20 parts by mass or less per 100 parts by mass of the polyvinyl chloride, the extrusion moldability and mechanical properties of the insulating layer can be sufficiently maintained while improving the flame retardant effect.

[0015] (4) The insulated wire of the present disclosure includes a linear conductor and one or more insulating layers laminated on an outer peripheral surface of the conductor and made of the resin composition for an insulating layer according to any one of (1) to (3) above.

[0016] The insulated wire includes one or more insulating layers made of the resin composition for insulating layers, which reduces the environmental impact and improves the insulating performance and flexibility of the insulating layers, thereby improving safety and workability.

[0017] [Details of Embodiments of the Present Invention] Hereinafter, the resin composition for an insulating layer and the insulated wire according to the embodiments of the present disclosure will be described in detail with appropriate reference to the drawings.

[0018] <Resin Composition for Insulating Layer> The resin composition for insulating layer contains a resin component mainly composed of polyvinyl chloride, a plasticizer, an inorganic filler, and a flame retardant.

[0019] (Resin Component) In the resin composition for the insulating layer, the resin component is primarily composed of polyvinyl chloride, which can impart excellent insulating performance, voltage resistance, and heat resistance to the insulating layer. Examples of the polyvinyl chloride include vinyl chloride homopolymers produced by methods such as suspension polymerization, bulk polymerization, and emulsion polymerization, as well as copolymers of vinyl chloride with ethylene, propylene, vinyl acetate, (meth)acrylic esters, and the like. Mixtures of the above homopolymers or copolymers with other thermoplastic resins can also be used. Polyvinyl chloride can be used alone or in combination of two or more types.

[0020] The average degree of polymerization of polyvinyl chloride may be 1,000 or more and 3,000 or less, or 1,200 or more and 2,500 or less. When the average degree of polymerization of polyvinyl chloride is within the above range, an insulating layer having excellent flexibility and tensile strength can be formed. Here, the average degree of polymerization is a number-average degree of polymerization measured by gel permeation chromatography (GPC).

[0021] The resin component may contain a resin other than the polyvinyl chloride. The content of polyvinyl chloride in the resin component may be 80% by mass, 85% by mass, 90% by mass, 95% by mass, or 100% by mass.

[0022] (Plasticizer) When the resin composition for an insulating layer contains a plasticizer, the flexibility and processability of the insulating layer can be improved.

[0023] The plasticizer is epoxidized soybean oil, acetylated castor oil, epoxidized linseed oil, or a combination thereof. By using these biomass-derived materials as the plasticizer, the flexibility and processability of the insulating layer can be improved while reducing the environmental impact.

[0024] The viscosity of the plasticizer at 25°C may be 100 mPa·s or more and 1000 mPa·s or less, or 200 mPa·s or more and 800 mPa·s or less, from the viewpoints of migration into the polyvinyl chloride, which is the main component, and processability.

[0025] The lower limit of the plasticizer content per 100 parts by mass of polyvinyl chloride is 20 parts by mass, or may be 35 parts by mass, or 40 parts by mass. If the plasticizer content is less than 20 parts by mass, it may be difficult to improve the flexibility of the resulting insulating layer. On the other hand, the upper limit of the plasticizer content per 100 parts by mass of polyvinyl chloride is 100 parts by mass, or may be 60 parts by mass, or 55 parts by mass. If the plasticizer content exceeds 100 parts by mass, the insulating performance of the resulting insulating layer may be reduced.

[0026] (Inorganic Filler) The insulating layer resin composition contains an inorganic filler, which can improve the insulating performance of the resulting insulating layer. Various known inorganic fillers can be used as the inorganic filler, including, for example, clay, calcium carbonate, talc, magnesium carbonate, calcium hydroxide, barium sulfate, calcium sulfate, strontium sulfate, titanium dioxide, magnesium silicate, magnesium oxide, magnesium hydroxide, fumed silica, and combinations thereof. From the viewpoint of further improving the insulating performance of the resulting insulating layer, the inorganic filler may be, among these, clay, calcium carbonate, talc, magnesium carbonate, or combinations thereof.

[0027] The lower limit of the content of the inorganic filler per 100 parts by mass of polyvinyl chloride is 5 parts by mass, or may be 7 parts by mass, or may be 10 parts by mass. If the content of the inorganic filler is less than 5 parts by mass, it may be difficult to improve the insulating performance of the resulting insulating layer. On the other hand, the upper limit of the content of the inorganic filler per 100 parts by mass of polyvinyl chloride is 40 parts by mass, or may be 20 parts by mass, or may be 17 parts by mass. If the content of the inorganic filler exceeds 40 parts by mass, the flexibility of the resulting insulating layer may be reduced.

[0028] (Flame Retardant) The flame retardant imparts flame retardancy to the insulating layer using the resin composition for insulating layer. Examples of the flame retardant include halogen-based flame retardants such as chlorine-based flame retardants and bromine-based flame retardants.

[0029] Examples of the flame retardant include halogen-based flame retardants such as antimony trioxide, antimony pentoxide, zinc borate, bromine-based flame retardants, and chlorine-based flame retardants, and non-halogen-based flame retardants such as metal hydroxides, nitrogen-based flame retardants, and phosphorus-based flame retardants. The flame retardants can be used alone or in combination of two or more.

[0030] Examples of bromine-based flame retardants include decabromodiphenylethane. Examples of chlorine-based flame retardants include chlorinated paraffin, chlorinated polyethylene, chlorinated polyphenol, and perchlorpentacyclodecane. Examples of metal hydroxides include magnesium hydroxide and aluminum hydroxide. Examples of nitrogen-based flame retardants include melamine cyanurate, triazine, isocyanurate, urea, and guanidine. Examples of phosphorus-based flame retardants include metal phosphinate, phosphaphenanthrene, melamine phosphate, ammonium phosphate, phosphate ester, and polyphosphazene.

[0031] As the flame retardant, from the viewpoint of further improving the flame retardancy of the resulting insulating layer, among these, antimony trioxide, bromine-based flame retardants, or melamine cyanurate may be used.

[0032] When the flame retardant is antimony trioxide, the content of the antimony trioxide may be 1 part by mass or more and 20 parts by mass or less, or 3 parts by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the polyvinyl chloride. When the content of the antimony trioxide is within the above range, the extrusion moldability and mechanical properties of the insulating layer can be sufficiently maintained while improving the flame retardant effect.

[0033] When the flame retardant is a brominated flame retardant, the content of the brominated flame retardant may be 1 part by mass to 20 parts by mass or 3 parts by mass to 15 parts by mass relative to 100 parts by mass of the polyvinyl chloride. By having the content of the brominated flame retardant in the above range, the extrusion moldability and mechanical properties of the insulating layer can be sufficiently maintained while improving the flame retardant effect.

[0034] When the flame retardant is melamine cyanurate, the content of the melamine cyanurate may be 1 part by mass or more and 20 parts by mass or less, or 10 parts by mass or more and 20 parts by mass or less, relative to 100 parts by mass of the polyvinyl chloride. When the content of the melamine cyanurate is within the above range, the extrusion moldability and mechanical properties of the insulating layer can be sufficiently maintained while improving the flame retardant effect.

[0035] (Stabilizer) Various stabilizers can be added to the resin composition for the insulating layer to suppress thermal and oxidative degradation of polyvinyl chloride. Lead-free stabilizers that do not contain lead may be used as the stabilizer to reduce the environmental impact. Examples of lead-free stabilizers include basic inorganic acid salts or their calcined products, hydrotalcite, calcium stearate, zinc stearate, and calcium-zinc composite stabilizers. One type of stabilizer can be used alone, or two or more types can be used in combination.

[0036] (Other Components) The resin composition for insulating layer may contain, in addition to the above-mentioned resin components, plasticizer, inorganic filler, flame retardant, and stabilizer, other components such as antioxidants, crosslinking agents, ultraviolet absorbers, colorants, processability improvers, and other modifiers, either alone or in combination of two or more.

[0037] The resin composition for an insulating layer reduces the environmental load and can improve the insulating performance and flexibility of the insulating layer.

[0038] <Insulated wire> The insulated wire includes a linear conductor and one or more insulating layers formed using the resin composition for insulating layers and laminated on the outer peripheral surface of the conductor. The conductor may be one or more. Fig. 1 is a schematic cross-sectional view of an insulated wire according to one embodiment of the present disclosure. As shown in Fig. 1, the insulated wire 1 includes a linear conductor 2 and one insulating layer 3 laminated on the outer peripheral surface of the conductor 2.

[0039] [Conductor] The conductor 2 is, for example, a round wire having a circular cross section, but may also be a rectangular wire having a square cross section or a rectangular wire, or a twisted wire made by twisting together a plurality of wires.

[0040] The conductor 2 is preferably made of a metal having high electrical conductivity and high mechanical strength. Examples of such metals include copper, copper alloys, aluminum, aluminum alloys, nickel, silver, mild steel, steel, and stainless steel. The conductor 2 may be made of a wire-shaped material made of such a metal, or a multilayer structure in which such a wire-shaped material is further coated with another metal, such as a nickel-coated copper wire, a silver-coated copper wire, a copper-coated aluminum wire, or a copper-coated steel wire.

[0041] The lower limit of the average cross-sectional area of ​​the conductor 2 is 0.01 mm 2 0.1 mm 2 On the other hand, the upper limit of the average cross-sectional area of ​​the conductor 2 is 30 mm 2 25 mm 2 If the average cross-sectional area of ​​the conductor 2 is less than the above-mentioned lower limit, the volume of the insulating layer 3 relative to the conductor 2 may become large, which may reduce the volumetric efficiency of a coil or the like formed using the insulated wire 1. Conversely, if the average cross-sectional area of ​​the conductor 2 exceeds the above-mentioned upper limit, the insulating layer 3 must be made thick to sufficiently reduce the dielectric constant, which may result in the insulated wire 1 having an unnecessarily large diameter. The "average cross-sectional area" of the conductor 2 refers to the average value obtained by measuring the cross-sectional area of ​​10 arbitrary points of the conductor 2.

[0042] [Insulating Layer] The insulating layer 3 is formed on the outer peripheral surface of the conductor 2 by extrusion molding using the above-mentioned resin composition for insulating layer.

[0043] The lower limit of the volume resistivity of the insulating layer 3 is 1.0×10 15 Ω cm, and 5.0×10 15 If the volume resistivity of the insulating layer 3 is less than the above lower limit, sufficient insulating performance may not be obtained. "Volume resistivity" refers to the electrical resistance value measured by the double ring electrode method in accordance with JIS-K6271:2008.

[0044] The lower limit of the average thickness of the insulating layer 3 may be 50 μm or 100 μm. On the other hand, the upper limit of the average thickness of the insulating layer 3 may be 1500 μm or 1000 μm. If the average thickness of the insulating layer 3 is less than the lower limit, the insulating performance may be reduced. Conversely, if the average thickness of the insulating layer 3 exceeds the upper limit, the volumetric efficiency of a cable or the like formed using the insulated wire 1 may be reduced. The "average thickness" of the insulating layer 3 refers to the average value obtained by measuring the thickness at 10 arbitrary points on the insulating layer 3. If multiple insulating layers 3 are provided, the average thickness of each insulating layer 3 is calculated, and this average value is used as the average thickness.

[0045] [Method for manufacturing an insulated wire] Next, a method for manufacturing the insulated wire will be described. In the insulated wire, an insulating layer is formed by extrusion molding. The method for manufacturing the insulated wire includes a step of extrusion coating the resin composition for an insulating layer onto the outer peripheral surface of the conductor.

[0046] The insulated wire includes one or more insulating layers made of the resin composition for insulating layers, which reduces the environmental impact as described above and improves the insulating performance and flexibility of the insulating layers, thereby improving safety and workability.

[0047] [Other Embodiments] The embodiments disclosed herein should be considered to be illustrative in all respects and not restrictive. The scope of the present invention is not limited to the configurations of the above-described embodiments, but is defined by the claims, and is intended to include all modifications within the meaning and scope of the claims.

[0048] The conductor may also be formed from a stranded wire, which is made by twisting together multiple metal wires. In this case, multiple types of metal wires may be combined. The number of twists is generally seven or more.

[0049] The insulated wire may have a primer layer laminated directly on the conductor. This primer layer may be a crosslinked layer of a crosslinkable resin such as ethylene that does not contain metal hydroxide. The provision of such a primer layer can prevent deterioration over time in the peelability of the insulating layer and the conductor.

[0050] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to the following examples.

[0051] [Resin Compositions for Insulating Layer Nos. 1 to 15] Resin compositions for insulating layer Nos. 1 to 15 were prepared by mixing the main component polyvinyl chloride ("TH-1300" manufactured by Taiyo Vinyl Corporation), plasticizer, inorganic filler, stabilizer, and flame retardant in the amounts (parts by mass) shown in Table 1. In Table 1 below, "-" indicates that the corresponding component was not used.

[0052] The plasticizers used were as follows: Plasticizer: Epoxidized soybean oil ("Adeka Cizer o-130P" manufactured by ADEKA Corporation) Epoxidized linseed oil ("Adeka Cizer o-180P" manufactured by ADEKA Corporation)

[0053]

[0054] <Evaluation> The resin compositions for insulating layer Nos. 1 to 15 obtained as described above were evaluated for flexibility, flame retardancy, and insulating performance. The evaluation results are shown in Table 1.

[0055] (Evaluation of Flexibility by 2% Secant Modulus) The flexibility of resin compositions No. 1 to No. 15 for insulating layers was evaluated by 2% secant modulus. Secant modulus was measured using the following procedure. A test piece 1 mm thick and 100 mm long was prepared from each resin composition for insulating layers using a hot press machine. The test piece was then pulled in the longitudinal direction at a tensile speed of 50 mm / min using a tensile tester. The load at 2% elongation was measured and divided by the cross-sectional area. This value was then multiplied by 50 to obtain the 2% secant modulus value (MPa). Here, "secant modulus" refers to the slope of the line connecting a point on a stress-strain curve to the origin, and serves as an index of ease of strain. A smaller measured value indicates better flexibility. A secant modulus of 90 MPa or less was considered acceptable.

[0056] (Evaluation of Flame Retardancy by VW-1 Vertical Flame Retardancy Test) The flame retardancy of resin compositions for insulating layers No. 1 to No. 15 was evaluated according to the following procedure. The VW-1 vertical flame retardancy test described in UL1581 1080 was conducted. Specifically, five 40 cm electric wires were prepared, and a burner flame was applied to each sample at a 20-degree angle. The cycle of ignition for 15 seconds and a 15-second break was repeated five times. A sample was rated as passing (A) if the fire was extinguished within 60 seconds, the absorbent cotton placed underneath was not burned by falling combustion, and the kraft paper attached to the top of the sample was not burned or scorched. A sample that did not meet the passing level out of the five samples was rated as failing (B).

[0057] (Evaluation of insulating performance by volume resistivity) Test samples with a size of φ100 mm × t2.5 mm were prepared from each resin composition for insulating layer using a heat press, and electrical resistance was measured using the double ring electrode method specified in JIS-K6271:2008. Volume resistivity (Ω cm) was calculated from the measured value. 15 A value of Ω·cm or more is acceptable.

[0058] (Evaluation of Heat Aging Resistance) For the evaluation of heat aging resistance, sheets with a thickness of 1 mm were prepared from each insulating layer resin composition using a heat press, and a heat aging resistance test was carried out according to the following procedure in accordance with the UL 80°C rating standard. The sheets were punched into dumbbell shapes (JIS No. 3) and placed in each thermostatic oven set at 113°C for one week. The tensile strength and tensile elongation after placement were compared with the tensile strength and tensile elongation before placement to determine retention rates. A tensile strength retention rate of 70% or more and a tensile elongation retention rate of 65% or more were considered pass, with passing samples being rated "A" and failing samples being rated "B."

[0059] From the results in Table 1 above, it can be seen that Samples No. 3, No. 5, No. 6, No. 9, No. 10, No. 11, No. 12, No. 13, No. 14, and No. 15, which contained polyvinyl chloride as the main resin component, a plasticizer, an inorganic filler, and a flame retardant, where the plasticizer was epoxidized soybean oil, acetylated castor oil, epoxidized linseed oil, or a combination thereof, and in which the plasticizer content was 20 parts by mass or more and 100 parts by mass or less per 100 parts by mass of the polyvinyl chloride, and the inorganic filler content was 5 parts by mass or more and 40 parts by mass or less per 100 parts by mass of the polyvinyl chloride, exhibited favorable results in terms of 2% secant modulus and volume resistivity.

[0060] On the other hand, No. 1, in which the epoxidized soybean oil content was less than 20 parts by mass per 100 parts by mass of the polyvinyl chloride, exhibited a very high 2% secant modulus. Nos. 2 and 4, in which the clay content was less than 5 parts by mass per 100 parts by mass of the polyvinyl chloride, exhibited low volume resistivity. No. 7, in which the clay content was more than 40 parts by mass per 100 parts by mass of the polyvinyl chloride, exhibited a high 2% secant modulus. No. 8, in which the epoxidized soybean oil content was more than 100 parts by mass per 100 parts by mass of the polyvinyl chloride, exhibited a low volume resistivity.

[0061] The above results demonstrate that the resin composition for an insulating layer can provide an insulating layer with good insulating performance and flexibility.

[0062] 1 insulated wire 2 conductor 3 insulating layer

Claims

1. A resin composition for an insulating layer comprising a resin component, a plasticizer, an inorganic filler and a flame retardant, wherein the resin component is primarily composed of polyvinyl chloride, the plasticizer is epoxidized soybean oil, acetylated castor oil, epoxidized linseed oil or a combination thereof, the content of the plasticizer is 20 parts by mass or more and 100 parts by mass or less per 100 parts by mass of the polyvinyl chloride, and the content of the inorganic filler is 5 parts by mass or more and 40 parts by mass or less per 100 parts by mass of the polyvinyl chloride.

2. The resin composition for an insulating layer according to claim 1, wherein said inorganic filler is clay, calcium carbonate, talc, magnesium carbonate or a combination thereof.

3. The resin composition for insulating layers according to claim 1 or 2, wherein the flame retardant is antimony trioxide, a bromine-based flame retardant or melamine cyanurate, and the content of the flame retardant is 1 part by mass or more and 20 parts by mass or less per 100 parts by mass of the polyvinyl chloride.

4. An insulated wire comprising: a linear conductor; and one or more insulating layers laminated on the outer peripheral surface of the conductor and made of the resin composition for insulating layers according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Modified polyvinyl chloride cable material, preparation method thereof and cable

    CN112480573A

  • Purified acetylated derivatives of castor oil and compositions containing the same

    JP2013534924A

  • Plasticizers and plasticizing polymer compositions

    JP2015522684A

  • Synergistic blend of calcium carbonate and calcined clay

    JP2016519168A