laminate
The laminate with a polyamide and radically reactive group adhesive composition addresses the challenges of heat resistance and surface followability, ensuring secure and residue-free wafer processing, enhancing semiconductor manufacturing efficiency.
Patent Information
- Application Number
- PCT/JP2024/012179
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2024-03-27
- Publication Date
- 2024-11-28
AI Technical Summary
Existing temporary fixing materials for semiconductor wafers lack sufficient heat resistance and ability to follow uneven surfaces while maintaining adhesion, and often result in damage or residue during peeling, especially when exposed to high temperatures.
A laminate with a layer containing an adhesive composition of polyamide and a curable resin having radically reactive groups, which provides a 300°C elastic modulus of 1 MPa or more, enabling easy peeling and maintaining shape without residue, and can be crosslinked for enhanced heat resistance.
The laminate achieves both high heat resistance and unevenness followability, allowing for secure wafer processing and easy removal without damage, improving the productivity of electronic devices and semiconductor manufacturing.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Laminate
[0001] The present invention relates to a laminate including a layer containing an adhesive composition containing a polyamide, and more specifically to a temporary fixing material used to temporarily fix a semiconductor wafer to a support substrate (carrier) in order to perform wafer processing such as grinding, film formation, and etching on the back surface of the semiconductor wafer. The present invention also relates to a wafer manufacturing method and an electronic component manufacturing method.
[0002] Pressure-sensitive adhesive tapes are widely used in the manufacturing processes of electronic components, semiconductor components, and the like for purposes such as temporary fixation of members and components, fixation during transportation, reinforcement, protection, and masking. The pressure-sensitive adhesive compositions used in such pressure-sensitive adhesive tapes are required to have high enough adhesiveness to firmly fix adherends such as wafers and semiconductor chips during processing, while being able to be peeled off without damaging the adherend after the process is completed. Furthermore, in recent years, there has been a demand for higher-density integration of semiconductors, and it has been necessary to grind semiconductor wafers to extremely thin thicknesses in the back-grinding process. Furthermore, next-generation materials called compound semiconductors, such as SiC, have emerged, but these are harder and more brittle than silicon wafers and are considered to be extremely difficult to process. Grinding such materials to a thin thickness is even more difficult, and a method of supporting the wafer using a pressure-sensitive adhesive and a support substrate is effective. Furthermore, since wafers, pressure-sensitive adhesives, and support substrates are often exposed to high temperatures during semiconductor manufacturing processes, the pressure-sensitive adhesives that fix these support substrates and wafers are also required to have high heat resistance.
[0003] Patent Document 1 discloses a temporary fixing material that temporarily fixes a wafer and a support substrate using a photocurable acrylic ester polymer. Patent Document 2 discloses a temporary fixing material that temporarily fixes a wafer and a support substrate using a pressure-sensitive adhesive composition containing a photocurable polyimide and a maleimide group. Patent Document 3 discloses a temporary fixing material that temporarily fixes a wafer and a support substrate using a pressure-sensitive adhesive composition containing a polyimide having a siloxane skeleton. However, the temporary fixing material of Patent Document 1 has issues with heat resistance because it uses an acrylic ester polymer as the base polymer in the pressure-sensitive adhesive composition. The temporary fixing material of Patent Document 2 uses a polymer containing an imide skeleton in the pressure-sensitive adhesive composition, essentially using polyimide as the base polymer. Polyimides tend to retain carboxylic acid functional groups during the polymerization process, which increases the pressure-sensitive adhesive strength to the adherend, potentially damaging the wafer during peeling or making peeling impossible. The temporary fixing material of Patent Document 3 is not in the form of a tape but is a liquid adhesive, which requires processes such as application and drying, potentially complicating the processing process.
[0004] Patent No. 5639280 Patent No. 7261860 Patent No. 6435862
[0005] That is, temporary fixing materials are required to be able to easily bond a wafer and a support (ability to conform to the irregularities on the wafer surface), to withstand the external forces and high heat involved in the semiconductor manufacturing process (heat resistance), and to be easily peeled off after the process is completed without damaging or contaminating the adherend. Furthermore, the adhesive composition contained in the temporary fixing material crosslinks by thermal curing or photocuring, but has limited heat resistance (up to approximately 250°C), and temporary fixing materials with even higher heat resistance (up to 300°C) are needed. On the other hand, if a large amount of crosslinking agent is introduced from the beginning, separate from thermal curing or photocuring, heat resistance is improved, but this tends to impair the ability to conform to the irregularities. In other words, it is difficult to achieve both sufficient heat resistance and ability to conform to the irregularities on the wafer surface. In view of the above technical background, an object of the present invention is to provide a laminate (temporary fixing material) for use in a wafer support system, which has heat resistance and the ability to conform to the irregularities on the wafer surface. Another object of the present invention is to provide a method for manufacturing a wafer using this laminate.
[0006] As a result of extensive research, the present inventors discovered that by using a laminate including a layer containing an adhesive composition containing a polyamide as a temporary fixing material, the temporary fixing material can be easily peeled from a wafer even after exposure to a high-temperature environment, and thus completed the present invention. Furthermore, none of the patent documents discloses an adhesive composition containing a polyamide or a temporary fixing material using the same.
[0007] That is, the present invention relates to: [1] a laminate including at least a layer containing an adhesive composition, wherein the adhesive composition contains a polyamide and a curable resin having a radical reactive group, and the layer containing the adhesive composition after curing has a modulus of elasticity at 300°C of 1 MPa or more.
[0008]
[0023] Below, [2] to [7] are all preferred aspects or embodiments of the present invention. [2] The laminate according to [1], wherein the polyamide is at least one selected from the group consisting of polyesteramide, aliphatic polyamide, and polyetheresteramide. [3] The laminate according to [1] or [2], wherein the laminate is a multilayer film and is used as a temporary fixing material in a wafer support system. [4] The laminate according to [3], wherein the multilayer film includes a substrate and a device-side adhesive layer, and the device-side adhesive layer includes the adhesive composition. [5] The laminate according to any of [1] to [4], wherein the curable resin having a radical reactive group is a maleimide compound. [6] A method for manufacturing a wafer, comprising: (a) forming a laminate including a wafer, an adhesive layer, and a substrate; (b) curing the adhesive layer by heating; (c) after step (b), subjecting the wafer to heat treatment, mechanical processing treatment, chemical treatment, physical treatment, laser processing treatment, and / or film formation treatment; (d) after step (c), removing the substrate from the laminate; and (e) after step (d), removing the adhesive layer from the laminate including the wafer and the adhesive layer, wherein the adhesive layer comprises an adhesive composition including a polyamide and a curable resin having a radical reactive group, and the adhesive layer after curing in step (b) has a modulus of elasticity at 300°C of 1 MPa or more. [7] A method for manufacturing an electronic component, comprising the method for manufacturing a wafer according to [6].
[0009] The laminate of the present invention has both sufficient heat resistance and conformability to irregularities, and can be crosslinked by thermal curing to further improve its heat resistance, and can be used in wafer support systems.
[0010] The present invention relates to a laminate including at least a layer containing an adhesive composition, wherein the adhesive composition contains a polyamide and a curable resin having a radical reactive group, and the layer containing the adhesive composition after curing has a modulus of elasticity at 300°C of 1 MPa or more.
[0011] Laminate The laminate of the present invention is a laminate including at least a layer containing an adhesive composition, and is used to temporarily fix a wafer to a support (substrate). In particular, it is a laminate that comes into contact with a wafer. It is intended to be easily peeled from the wafer after wafer processing, and the layer containing the adhesive composition after curing has a 300°C elastic modulus of 1 MPa or more. The elastic modulus is preferably 1.1 MPa or more, more preferably 1.2 MPa or more. By having the elastic modulus within this range, the laminate of the present invention can achieve both sufficient heat resistance and conformability to uneven surfaces, and can also prevent adhesive residue. If the elastic modulus is less than 1 MPa, increased adhesion is likely to occur. The layer containing the adhesive composition after curing has a 300°C weight loss of preferably 2.0% or less, more preferably 0.8% or less, and even more preferably 0.4% or less. Furthermore, the 350°C weight loss is preferably 3% or less, more preferably 2% or less, and even more preferably 1.5% or less. By having the 300°C weight loss and 350°C weight loss within these ranges, the shape of the laminate can be maintained. If the weight loss at 300°C and the weight loss at 350°C are outside this range (if the weight loss at 300°C and the weight loss at 350°C are large), the shape of the laminate cannot be maintained.
[0012] The laminate of the present invention can be a multilayer film and can be used as a temporary fixing material in a wafer support system. The multilayer film can include a substrate and a device-side adhesive layer (a layer that contacts the wafer), and the device-side adhesive layer can contain the adhesive composition. The multilayer film can also include a device-side adhesive layer and a carrier-side adhesive layer (a layer that contacts the substrate), and the carrier-side adhesive layer can contain the adhesive composition.
[0013] Adhesive Composition The adhesive composition used in the present invention contains a polyamide and a curable resin having a radical reactive group. The adhesive composition is contained in the layer containing the adhesive composition in an amount of preferably 50 to 100 mass %, more preferably 80 to 100 mass %. The laminate of the present invention and the adhesive composition used in the present invention preferably do not contain an acrylic polymer.
[0014] Polyamides Examples of polyamides used in the present invention include polyesteramides, aliphatic polyamides, and polyetheresteramides.
[0015] Polyesteramide Polyesteramide is a block copolymer in which a polyester block and a polyamide block are bonded via an amide bond or an ester bond. The polyester block contains an aliphatic dicarboxylic acid and a diol compound as monomers. The aliphatic dicarboxylic acid preferably has 4 to 60 carbon atoms, and more preferably has 4 to 36 carbon atoms. Specific examples include, but are not limited to, adipic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, hexadecanedioic acid, eicosanedioic acid, and dimer acid. The polyesteramide may also contain an aromatic dicarboxylic acid unit. Examples of aromatic dicarboxylic acids include isophthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, and biphenyl-4,4'-dicarboxylic acid. Specific examples of the diol compound include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, 3-methyl-1,5-pentanediol, 2-methyl-2,4-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 2,4-heptanediol, 2,2-diethyl-1,3-propanediol, 2-ethyl-1,3-hexanediol, 2-butyl-2-ethyl-1,3-propanediol, and dimer diols derived from dimer acids, but are not limited thereto. The polyamide block contains either or both of an aliphatic dicarboxylic acid and an aliphatic diamine as monomers. The aliphatic dicarboxylic acid preferably has 4 to 60 carbon atoms, and more preferably 4 to 36 carbon atoms. Specific examples include, but are not limited to, adipic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, hexadecanedioic acid, eicosanedioic acid, and dimer acid. Aromatic dicarboxylic acid units may also be included. Examples of aromatic dicarboxylic acids include isophthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, and biphenyl-4,4'-dicarboxylic acid.The aliphatic diamine preferably has 4 to 60 carbon atoms, and more preferably has 4 to 36 carbon atoms. Specific examples include, but are not limited to, hexamethylenediamine, tetramethylenediamine, nonamethylenediamine, undecamethylenediamine, dodecamethylenediamine, methylpentamethylenediamine, 2,2,4- or 2,4,4-trimethylhexamethylenediamine, and dimer diamines derived from dimer acids. The diamine may also contain an aromatic diamine unit. Examples of aromatic diamines include 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-diaminodiphenyl ether, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminodiphenyl sulfone, 1,3-bis(4-aminophenoxy)benzene, and 1,4-bis(4-aminophenoxy)benzene. Examples of polyesteramides include block copolymers in which a polyester block and a polyamide block are bonded via an amide bond or an ester bond. Specific examples include TPAE-617 (manufactured by T&K TOKA Corporation, softening point 153°C) and TPAE-617C (manufactured by T&K TOKA Corporation, softening point 161°C).
[0016] Aliphatic Polyamides Aliphatic polyamides are polyamides containing either or both of aliphatic dicarboxylic acids and aliphatic diamines as monomers. The aliphatic dicarboxylic acids preferably have 4 to 60 carbon atoms, and more preferably 4 to 36 carbon atoms. Specific examples include, but are not limited to, adipic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, hexadecanedioic acid, eicosanedioic acid, and dimer acids. Dimer acids are dimers or hydrogenated products of unsaturated fatty acids such as oleic acid, linoleic acid, and erucic acid derived from vegetable oils such as castor oil, tall oil, soybean oil, and rapeseed oil. Aromatic dicarboxylic acid units may also be included. Examples of aromatic dicarboxylic acids include isophthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, and biphenyl-4,4'-dicarboxylic acid. The aliphatic diamines preferably have 4 to 60 carbon atoms, and more preferably 4 to 36 carbon atoms. Specific examples include, but are not limited to, hexamethylenediamine, tetramethylenediamine, nonamethylenediamine, undecamethylenediamine, dodecamethylenediamine, methylpentamethylenediamine, 2,2,4- or 2,4,4-trimethylhexamethylenediamine, and dimer diamines derived from dimer acids. Other aromatic diamine units may also be included. Examples of aromatic diamines include 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-diaminodiphenyl ether, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminodiphenyl sulfone, 1,3-bis(4-aminophenoxy)benzene, and 1,4-bis(4-aminophenoxy)benzene. Examples of aliphatic polyamides include polyamides containing 50% by weight or more of a dimer acid skeleton, and specific examples thereof include PA-100 (manufactured by T&K Toka Corporation, melting point 84°C) and TOMAID 1310 (manufactured by T&K Toka Corporation, softening point 120±5°C).
[0017] Polyetheresteramide Polyetheresteramide is a block copolymer in which polyetherester blocks and polyamide blocks are bonded via amide or ester bonds. The polyetherester block contains an aliphatic dicarboxylic acid and a diol compound as monomers, and further contains multiple ether bonds formed by condensation of diols. The aliphatic dicarboxylic acid preferably has 4 to 60 carbon atoms, and more preferably 4 to 36 carbon atoms. Specific examples include, but are not limited to, adipic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, hexadecanedioic acid, eicosanedioic acid, and dimer acid. Aromatic dicarboxylic acid units may also be included. Examples of aromatic dicarboxylic acids include isophthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, and biphenyl-4,4'-dicarboxylic acid. Specific examples of the diol compound include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, 3-methyl-1,5-pentanediol, 2-methyl-2,4-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 2,4-heptanediol, 2,2-diethyl-1,3-propanediol, 2-ethyl-1,3-hexanediol, 2-butyl-2-ethyl-1,3-propanediol, and dimer diols derived from dimer acids, but are not limited thereto. The polyamide block contains either or both of an aliphatic dicarboxylic acid and an aliphatic diamine as a monomer, and the aliphatic dicarboxylic acid preferably has 4 to 60 carbon atoms, more preferably 4 to 36 carbon atoms. Specific examples include, but are not limited to, adipic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, hexadecanedioic acid, eicosanedioic acid, and dimer acid. Additionally, an aromatic dicarboxylic acid unit may be contained.Examples of aromatic dicarboxylic acids include isophthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, and biphenyl-4,4'-dicarboxylic acid. Aliphatic diamines preferably have 4 to 60 carbon atoms, and more preferably 4 to 36 carbon atoms. Specific examples include, but are not limited to, hexamethylenediamine, tetramethylenediamine, nonamethylenediamine, undecamethylenediamine, dodecamethylenediamine, methylpentamethylenediamine, 2,2,4- or 2,4,4-trimethylhexamethylenediamine, and dimer diamines derived from dimer acids. The diamines may also contain aromatic diamine units. Examples of aromatic diamines include 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-diaminodiphenyl ether, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminodiphenyl sulfone, 1,3-bis(4-aminophenoxy)benzene, and 1,4-bis(4-aminophenoxy)benzene. Examples of polyether ester amides include block copolymers of polyether ester blocks and polyamide resins, and specific examples include PA-201 (manufactured by T&K TOKA Corporation, melting point 122°C) and TPAE-32C (manufactured by T&K TOKA Corporation, melting point 124°C).
[0018] Curable Resins Having Radical Reactive Groups The curable resins having radical reactive groups (radical curable resins) used in the present invention, when cured before wafer processing, are less likely to produce voids during heat treatment during the wafer manufacturing process, and can be easily peeled off without leaving any adhesive residue by suppressing adhesion enhancement due to high temperatures during heat treatment. Examples of the curable adhesive components include photocurable adhesive components that crosslink and cure upon light irradiation and thermosetting adhesive components that crosslink and cure upon heating. In particular, examples of the curable resins having radical reactive groups used in the present invention include thermosetting adhesive components that contain, as curing components, olefin-based curing agents, or monomers, oligomers, or polymers such as acrylic, epoxy, urethane acrylate, epoxy acrylate, silicone acrylate, or polyester acrylate, and that contain a thermal polymerization initiator. Preferred examples include bismaleimide crosslinking agents (e.g., BMI-5100 having the following chemical formula), alicyclic crosslinking agents (e.g., IRR-214K having the following chemical formula), and epoxy acrylate crosslinking agents (e.g., EBECRYL3700 having the following chemical formula). More preferably, the curable resin having a radical reactive group is a maleimide compound. The curable resin having a radical reactive group is contained in the adhesive composition in an amount of preferably 10 to 100 parts by mass, more preferably 20 to 75 parts by mass, per 100 parts by mass of polyamide.
[0019] Organic Peroxide In one embodiment, the adhesive composition used in the present invention can contain an organic peroxide as a thermal polymerization initiator. Examples of organic peroxides include those that decompose when heated to generate active radicals that initiate polymerization and curing. Specific examples include t-butylperoxy-2-ethyl hexanoate, bis(4-methylbenzoyl)peroxide, benzoyl peroxide, 1,1-bis(t-hexylperoxy)cyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, 2,2-bis(4,4-bis-(t-butylperoxy)cyclohexyl)propane, t-hexylperoxyisopropyl monocarboxylate, t-butylperoxyacetate, 2,2-bis-( t-butylperoxy)butane, 4,4-bis-(t-butylperoxy)n-butyl pentanoate, bis-t-hexyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, bis(2-t-butylperoxyisopropyl)benzene, t-butylcumyl peroxide, di-t-butyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne, and diisopropylbenzene hydroperoxide.
[0020] Among these thermal polymerization initiators, commercially available ones are not particularly limited, but suitable examples include Perbutyl O, Niper BMT, Niper BW, Perhexa HC, Perhexa C, Pertetra A, Perhexyl I, Perbutyl A, Perhexa 22, Perhexa V, Perhexyl D, Percumyl D, Perhexa 25B, Perbutyl P, Perbutyl C, Perhexyne 25B, Percumyl P (all manufactured by NOF Corporation), Perkadox 12XL25 (manufactured by Nouryon Chemical Co., Ltd.), etc. These thermal polymerization initiators may be used alone or in combination of two or more.
[0021] The amount of the organic peroxide is preferably 0.1 to 3.0 parts by mass relative to 100 parts by mass of the polyamide. The amount is more preferably 0.1 to 1.0 part by mass. When the amount of the organic peroxide is within this range, it can function sufficiently as a thermal polymerization initiator.
[0022] The adhesive composition of the present invention may contain, if desired, various thermal crosslinking agents such as melamine compounds and epoxy compounds, as well as known additives such as release agents, plasticizers, resins, surfactants, waxes, and fine particle fillers.
[0023] The release agent is not particularly limited as long as it generally exhibits a release effect. Examples include hydrocarbon compounds, silicone compounds, fluorine compounds, and polyethylene waxes, carnauba wax, montanic acid, and stearic acid, which are known as release agents for plastic materials. Among these, silicone and fluorine compounds are preferred, and silicone and fluorine compounds having functional groups crosslinkable with curable adhesives are more preferred. Silicone compounds, in particular, have excellent heat resistance, preventing scorching of adhesives even after treatment involving heating at 200°C or higher. Upon peeling, they bleed out to the adherend interface, facilitating peeling. Because the silicone compound has functional groups crosslinkable with the curable adhesive, it chemically reacts with the curable adhesive upon light irradiation or heating and is incorporated into the curable adhesive, preventing the silicone compound from adhering to the adherend and causing contamination. The inclusion of a silicone compound also prevents adhesive residue on semiconductor chips. Other examples of release agents include plasticizers. The plasticizer is not particularly limited as long as it generally reduces the adhesive strength of the adhesive material to an adherend. Examples of the plasticizer include trimellitic acid esters, pyromellitic acid esters, phthalic acid esters, and adipic acid esters.
[0024] The amount of release agent added is not particularly limited, but is appropriately determined so as to obtain a release effect. On the other hand, the amount added is controlled so as not to be excessive so as not to significantly impair the adhesive function of the adhesive composition used in the present invention. For example, it is desirable to adjust the amount added according to the peel force, with an amount of typically 0.1 to 5 parts by mass, preferably 0.1 to 3 parts by mass, and more preferably 0.1 to 1 part by mass, per 100 parts by mass of the total adhesive composition.
[0025] When a plasticizer is added, it is desirable to adjust the amount of addition according to the peel strength, typically about 5 to 50 parts by mass, preferably about 10 to 50 parts by mass, and more preferably about 20 to 40 parts by mass. In this embodiment, these release agents can be used alone or in combination.
[0026] The thickness of the layer containing the adhesive composition used in the present invention is not particularly limited, but the lower limit is preferably 5 μm and the upper limit is preferably 250 μm, and the lower limit of the thickness is more preferably 10 μm and the upper limit is more preferably 200 μm. When the thickness is within this range, the unevenness of the wafer can be absorbed, and temporary fixing to the support with sufficient strength can be performed, and when peeling off the adhesive material, the peel force can be easily adjusted to a suitable range.
[0027] In one aspect of the present invention, a tape including the laminate of the present invention is provided. Examples of such tapes include a tape having a substrate film and a layer containing the adhesive composition used in the present invention as a device-side adhesive layer (wafer-side adhesive layer). Alternatively, the tape may further include a carrier-side adhesive layer (support-side adhesive layer) on the side of the substrate film opposite the wafer-side adhesive layer, a so-called double-sided adhesive tape. In this embodiment, the adhesive strength on the support side can be appropriately adjusted, allowing the support (substrate) to be easily removed after wafer processing. The substrate film can be designed from the perspectives of the mechanical strength and handleability of the entire laminate, which is particularly advantageous from the perspective of optimizing tape performance. While the material of the substrate film is not particularly limited, plastic films are preferably used. Examples include films, sheets, mesh-like sheets, and perforated sheets made of acrylic, olefin, polycarbonate, vinyl chloride, ABS, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), nylon, urethane, polyether ether ketone (PEEK), liquid crystal polymer (LCP), polyimide, etc. From the perspective of handling, PET, PEN, or polyimide films are preferred.
[0028] Wafer There are no particular limitations on the wafer that can be temporarily fixed to a support and processed using the laminate of the present invention; any wafer typically used in semiconductor manufacturing processes can be used. Among these, wafers that require careful handling during processing due to their thinness and fragility are preferred. Here, the thinness and fragility of the wafer are assumed to occur, for example, in cases where the wafer temporarily thins during processing, causing handling problems. The laminate of the present invention is used to temporarily fix such wafers to a support. Examples of cases where a wafer temporarily becomes thin include cases where a thin wafer is processed starting from a thin wafer, cases where a relatively thick wafer is thinned during the process, and cases where the thinned wafer is further processed. The thickness of the temporarily thinned wafer is typically 1 to 200 μm. For example, in cases where a semiconductor wafer on which functional layer processing has been completed is temporarily fixed to a support with the functional layer facing the support, the opposite side (backside) of the functional layer is thin-ground, ion implantation, annealing, and electrode formation are performed on the backside, and the wafer is then separated from the support, the semiconductor wafer during the process corresponds to the wafer. As described above, wafers that are temporarily fixed using the laminate of the present invention include those whose state changes during the process.
[0029] As described above, there are no particular limitations on the wafer that can be temporarily fixed using the laminate of the present invention, but more specific examples include semiconductor wafers such as silicon wafers, compound semiconductor wafers such as SiC, AlSb, AlAs, AlN, AlP, BN, BP, BAs, GaSb, GaAs, GaN, GaP, InSb, InAs, InN, or InP, quartz wafers, sapphire, glass, mold wafers, etc. The silicon wafers and compound semiconductor wafers may be doped.
[0030] Electrical / electronic functional layers may be formed on or within the wafer. Examples of suitable functional layers include electronic circuits, capacitors, transistors, resistors, electrodes, optical elements, and MEMS, but other microdevices may also be used. The surfaces of these functional layers may have structures, typically electrodes, formed from one or more of the following materials: silicon, polysilicon, silicon dioxide, (oxy)silicon nitride, metals (e.g., copper, aluminum, gold, tungsten, and tantalum), low-k dielectrics, polymer dielectrics, and various metal nitrides and metal silicides. The surface of the wafer on which the functional layer is formed (the functional layer surface) may have raised structures such as solder bumps, metal posts, and pillars. The wafer surface may also be covered with an oxide or nitride film for the formation of the functional layer or for protection of the functional layer. The wafer surface may also be covered with a passivation film for wafer protection.
[0031] 1. A method for manufacturing a wafer, in one aspect, the present invention relates to a method for manufacturing a wafer, comprising: (a) a step of forming a laminate including a wafer, an adhesive layer, and a substrate; (b) a step of curing the adhesive layer by heating; (c) a step of subjecting the wafer to a heat treatment, a mechanical processing treatment, a chemical treatment, a physical treatment, a laser processing treatment, and / or a film formation treatment after step (b); (d) a step of removing the substrate from the laminate after step (c); and (e) a step of removing the adhesive layer from the laminate including the wafer and the adhesive layer after step (d). 2. A method for manufacturing a wafer, wherein the adhesive layer comprises an adhesive composition including a polyamide and a curable resin having a radical reactive group, and the adhesive layer after curing in step (b) has a modulus of elasticity at 300°C of 1 MPa or more.
[0032] Step (a) is a step of forming a laminate including a wafer, an adhesive layer, and a substrate, that is, a step of laminating the wafer and the substrate to temporarily fix them via the adhesive layer.
[0033] The adhesive layer may be the same as the layer containing the adhesive composition described above. Alternatively, an adhesive layer containing a photocurable adhesive component that is crosslinked and cured by light irradiation may be used.
[0034] Examples of the photocurable adhesive component include a photocurable adhesive component containing a monomer, oligomer, or polymer such as epoxy, urethane acrylate, epoxy acrylate, silicone acrylate, or polyester acrylate as a curing component, and containing a photopolymerization initiator.
[0035] Examples of the photopolymerization initiator include those that are activated by irradiation with light having a wavelength of 250 to 800 nm. Examples of such photopolymerization initiators include acetophenone derivative compounds such as methoxyacetophenone, benzoin ether compounds such as benzoin propyl ether and benzoin isobutyl ether, ketal derivative compounds such as benzyl dimethyl ketal and acetophenone diethyl ketal, phosphine oxide derivative compounds, bis(η5-cyclopentadienyl)titanocene derivative compounds, benzophenone, Michler's ketone, chlorothioxanthone, todecylthioxanthone, dimethylthioxanthone, diethylthioxanthone, α-hydroxycyclohexylphenyl ketone, and 2-hydroxymethylphenylpropane. These photopolymerization initiators may be used alone or in combination of two or more.
[0036] Wafer The wafer can be any of those described above.
[0037] Substrate The substrate (support) can be the same as the substrate described above, and preferably has sufficient strength and rigidity, and excellent heat resistance and chemical resistance. By using such a substrate, even if the wafer is thin-ground in a later process, it is possible to handle the wafer stably, and it is possible to subject the wafer to multiple and / or diverse processes without causing bending, etc. For example, a wafer on which an electronic circuit is formed can be subjected to various processes required to manufacture an electronic device having a structure in which semiconductor chips are stacked, such as TSV connection.
[0038] Materials preferably used for the substrate include silicon, sapphire, quartz, metals (e.g., aluminum, copper, steel), and various glasses and ceramics. The substrate may be composed of a single material, or may be composed of multiple materials, or may include other materials deposited on the substrate. For example, a silicon wafer may have a vapor-deposited layer of silicon nitride or the like. The substrate may also be surface-treated, such as by providing a silicone layer.
[0039] Depending on the temperature of the process to which the laminate is subjected, the substrate may be made of plastic. For example, a sheet made of plastic such as polyimide, acrylic, polyolefin, polycarbonate, vinyl chloride, ABS, polyethylene terephthalate (PET), nylon, or urethane can be preferably used as the support. Polyimide can be used because it has a certain degree of heat resistance.
[0040] In order to obtain uniformity in the thickness of the wafer after grinding, etc., it is desirable that the thickness of the substrate be uniform. For example, in order to thin a silicon wafer to 50 μm or less and keep the uniformity at ±10% or less, the variation in the thickness of the substrate should be kept to ±2 μm or less. There are no particular restrictions on the thickness of the substrate, but from the viewpoint of effectively preventing wafer curvature, it is preferably 300 μm or more, and particularly preferably 500 μm or more. From the viewpoint of reducing the total weight during handling or reducing the stress required for mechanical peeling, it is preferably 1500 μm or less, and particularly preferably 1000 μm or less.
[0041] In step (a), a laminate including a wafer, an adhesive layer, and a substrate can be obtained. By curing the adhesive layer in step (b) described below, the laminate has sufficient strength and rigidity, and can be used in various semiconductor manufacturing processes while preventing bending and breakage.
[0042] As a method for forming the laminate, the substrate, adhesive layer, and wafer can be laminated in that order. The order of lamination is not particularly limited, and these layers may be laminated at once or sequentially.
[0043] When the adhesive layer is supplied as a liquid curable adhesive material or the like, the liquid curable adhesive material or the like is applied to either or both of the wafer and the support by spin coating or the like to form a laminate of wafer / adhesive layer or adhesive layer / substrate, and then the two adhesive layers are bonded together under reduced pressure to produce a laminate including the wafer, adhesive layer, and substrate.
[0044] When the adhesive layer is supplied as a solid film, the solid film can be attached to either the wafer or the substrate, and then the other can be attached under reduced pressure to create a laminate including the wafer, adhesive layer, and substrate.
[0045] Step (b) Step (b) is a step of curing the adhesive layer by heating, that is, a step of curing the adhesive layer in the laminate obtained in step (a).
[0046] The adhesive layer (e.g., curable adhesive component) crosslinked and cured by heating has dramatically improved chemical resistance, and can be prevented from dissolving in a chemical solution even when, for example, a backside of a wafer is treated with a chemical solution in a wafer processing step. Furthermore, the crosslinked and cured curable adhesive component has an increased elastic modulus, and therefore, adhesion is less likely to increase even at high temperatures, and peeling is relatively easy.
[0047] Furthermore, for example, when an adhesive layer containing a polymer having an unsaturated double bond such as a vinyl group in a side chain and a thermal polymerization initiator that is activated by heating at about 50 to 200°C is used as the thermosetting adhesive component that is crosslinked and cured by heating, the thermosetting adhesive component can be crosslinked and cured by heating at a temperature of about 50 to 200°C for 5 to 40 minutes.
[0048] In one embodiment of the present invention, step (b) may involve curing the adhesive layer by heating at 140 to 200°C for 5 to 60 minutes. Heating at 140°C or higher for 15 minutes or longer can sufficiently cure the adhesive layer. Furthermore, while it is sufficient to cure the adhesive layer to a degree that the laminate can withstand in the wafer processing step, it is preferable from the viewpoint of cost to set the heating conditions to 180°C or 40 minutes or less.
[0049] Furthermore, since the adhesive layer contains an adhesive composition containing polyamide and a curable resin having a radical reactive group, the heating temperature (curing temperature) can be higher than conventional heating temperatures, i.e., above 160°C and up to about 300°C, thereby enabling even higher heat resistance.
[0050] Step (c) is a step of subjecting the wafer to heat treatment, mechanical processing, chemical treatment, physical treatment, laser processing, and / or film formation treatment after step (b). The stack formed through steps (a) and (b) can be subjected to at least one wafer treatment selected from heat treatment (including treatment involving heat generation; the same applies below), mechanical processing, chemical treatment, physical treatment, laser processing, and film formation treatment. In addition, the stack formed through steps (a) and (b) can also be subjected to processing required for TSV processing and for forming a structure in which TSV-processed semiconductor chips are stacked.
[0051] Examples of the heat treatment include, but are not limited to, thermal curing of the resin composition, heat drying of the resin composition, baking of the resin composition, reflow, resin sealing, and the like.
[0052] The above-mentioned machining processes typically include polishing, grinding, drilling, and cutting of the wafer, but are not limited to these and also include singulation. When grinding or polishing a wafer having electrodes formed on its surface, the surface on which the electrodes are not formed (back surface) is ground or polished. The thickness of the wafer after back surface grinding and polishing varies depending on the electronic device in which the obtained electronic device is used, but is usually set to 1 μm or more and 200 μm or less, preferably 5 μm or more and 100 μm or less, and more preferably 5 μm or more and 50 μm or less. This allows the obtained electronic device to be made thinner, thereby realizing the miniaturization of electronic devices using such electronic devices.
[0053] In this embodiment, when grinding or polishing the wafer, by laminating the wafer to a rigid support via an adhesive layer, the wafer can be ground or polished with greater processing accuracy, and after this grinding or polishing, the wafer can be subjected to further processing steps or the wafer and the adhesive layer can be easily separated without damaging the wafer.
[0054] The chemical treatment is, for example, a polishing treatment such as CMP, a treatment using an acid, an alkali, or an organic solvent, and examples thereof include plating treatments such as electrolytic plating and electroless plating, wet etching treatments using hydrofluoric acid, an aqueous solution of tetramethylammonium hydroxide (TMAH), or the like, a resist stripping process using N-methyl-2-pyrrolidone, monoethanolamine, DMSO, or the like, and a cleaning process using concentrated sulfuric acid, aqueous ammonia, aqueous hydrogen peroxide, or the like, but is not limited to these.
[0055] Examples of the physical treatment include, but are not limited to, plasma treatment, ion implantation, and laser annealing.
[0056] Examples of the laser processing include, but are not limited to, annealing, via processing, circuit formation processing by direct writing, and pre-processing for separation from the support.
[0057] Examples of the film formation process include, but are not limited to, coating processes such as spin coating, inkjet printing, and screen printing, sputtering, vapor deposition, etching, chemical vapor deposition (CVD), physical vapor deposition (PVD), resist coating / patterning, heat lamination of a resin composition film, and back metal.
[0058] In this embodiment, even though the wafer undergoes heat treatment, mechanical processing, chemical processing, physical processing, laser processing, and film formation processing during the wafer processing process, sufficient adhesive strength is maintained during wafer processing, and after the wafer processing process is completed, the wafer can be peeled from the adhesive layer without being damaged or leaving any adhesive residue when the wafer is peeled from the laminate.
[0059] After the treatment in step (c), chip bonding, wire bonding, flip-chip bonding, surface activation direct bonding, etc. may be performed. Furthermore, a dicing tape may be attached to the treated surface (preferably the ground surface) of the wafer. By attaching the dicing tape in advance, dicing can be performed quickly after peeling off the substrate and adhesive layer.
[0060] Step (d) Step (d) is a step of removing the substrate from the laminate after step (c). In step (d), the method of removing the substrate from the laminate is not particularly limited, but it is preferable to perform laser peeling or mechanical peeling because it is cost-effective and can simplify the equipment. In addition, a pre-peeling treatment may be performed in advance, and a method such as swelling or dissolution of the adhesive layer with a solvent may be appropriately adopted as a pre-peeling treatment.
[0061] In the wafer manufacturing method of the present invention, the adhesive layer after curing in step (b) has a 300°C elastic modulus of 1 MPa or more. The elastic modulus is preferably 1.1 MPa or more, more preferably 1.2 MPa or more. When the elastic modulus is within this range, the laminate of the present invention achieves both sufficient heat resistance and unevenness-following ability, and also prevents adhesive residue. When the elastic modulus is less than 1 MPa, adhesion tends to increase. When the adhesive layer after curing has a 300°C weight loss of preferably 1.1% or less, more preferably 1.0% or less. When the 300°C weight loss is within this range, the shape of the laminate can be maintained. When the 300°C weight loss is outside this range (when the 300°C weight loss is large), the shape of the laminate cannot be maintained.
[0062] Step (e) Step (e) is a step of removing the adhesive layer from a laminate including a wafer and an adhesive layer after step (d). Since the substrate is removed from the laminate through step (d), the adhesive layer can be separated from the wafer without applying excessive stress to the wafer, thereby minimizing the risk of damaging functional layers formed on the wafer. There are no particular limitations on the method for removing the adhesive layer, but considering the ease of peeling the adhesive layer, for example, peeling tape can be attached to the adhesive layer and the adhesive layer can be peeled off from the wafer together with the peeling tape. This is also advantageous in terms of cost because it does not require special equipment, etc.
[0063] Electronic Component Manufacturing Method The electronic component manufacturing method of the present invention includes the above-described wafer manufacturing method. According to the adhesive layer and wafer processing method of the present invention, the wafer can be stably processed and then subjected to subsequent processes to manufacture final products such as electronic components. When a functional layer is formed on the wafer, processes such as dicing, bonding, packaging, and sealing that are commonly used in the manufacture of electronic devices such as semiconductor devices can be carried out to manufacture final products such as electronic components.
[0064] The present invention will be specifically described below, but the present invention is not limited in any way by the following examples.
[0065] Details of the materials, ingredients, test procedures, etc. used in the Examples and Comparative Examples are as follows:
[0066] Sample Preparation Procedure (Paint Preparation) 100 parts by weight of polyamides, 25 parts by weight of a radical curing resin, and 0.8 parts by weight of a peroxide (Perbutyl P, manufactured by NOF Corporation) as a curing initiator were added to an appropriate solvent to prepare a 25 wt% adhesive paint. (Single-Layer Adhesive Film Preparation) The prepared adhesive paint was applied to the release-treated surface of a release PET film (T-15, manufactured by Mitsui Chemicals Tohcello) using a simple roll coater so that the coating thickness after drying would be 25 μm. The film was then dried at 120°C for 2 minutes in a ventilated oven to obtain a single-layer adhesive film. (Adhesive Lamination) The obtained single-layer adhesive film was laminated to a thickness of approximately 100 μm using a roll laminator while heating to 100°C to prepare a laminated adhesive film. (Adhesive Cured Product) The laminated adhesive film was heated at 180°C for 30 minutes in a nitrogen atmosphere to obtain a cured adhesive product. (Production of single-sided adhesive tape) The prepared adhesive coating was applied to the inside of a roll of polyimide film (Kapton 100EN, manufactured by Toray DuPont Co., Ltd.) using a simple roll coater so that the coating thickness after drying would be 25 μm, and the film was heated and dried at 120° C. for 2 minutes in a ventilated oven to obtain a single-sided adhesive tape. (Production of double-sided adhesive tape) A single-layer adhesive film was laminated on the polyimide surface of the obtained single-sided adhesive tape using a roll laminator while heating to 100° C., to produce a double-sided adhesive tape.
[0067] Experiments / Measurements (Weight Loss Measurement at 300°C (350°C)) A simultaneous differential thermal and thermogravimetric analyzer (TG / DTA7300, manufactured by Hitachi High-Technologies Corporation) was used to measure the weight loss of 10 mg of cured adhesive at 300°C (350°C). The measurement was carried out at a temperature increase rate of 10°C / min while flowing nitrogen gas. (300°C Storage Modulus Measurement) A dynamic viscoelasticity analyzer (RSA-G2, manufactured by TA Instruments) was used to measure the tensile storage modulus (E') of the cured adhesive at 300°C. The measurement was carried out at a temperature increase rate of 3°C / min and a frequency of 1 Hz while flowing nitrogen gas. (Evaluation of Embeddability (Follow-up Ability to Patterned Wafer)) The double-sided adhesive tape was cut into 50 mm squares and attached to a 1 mm thick glass plate while heating to 100°C on a hot plate using a hand roller. A Si wafer with a 10 μm high pattern made of polyimide was prepared and cut into 30 mm squares to obtain a patterned wafer chip. The patterned wafer chip was placed on the adhesive surface of a double-sided tape with a glass plate attached, and pressurized using a vacuum laminator at 130°C and 0.8 MPa for 2 minutes under reduced pressure. The appearance of the sample after pressurization was visually inspected to confirm the presence or absence of peeling, bubbles, or imperfect embedding. OK: No peeling or bubbles from the glass plate or patterned wafer chip, or imperfect embedding of the pattern was observed. NG: Peeling or bubbles from the glass plate or patterned wafer chip, or imperfect embedding of the pattern occurred.
[0068] Experiments / Measurements (Example 1) Aliphatic polyamide (manufactured by T&K TOKA Corporation, PA-100) was used as the polyimide, and bismaleimide (manufactured by Daiwa Chemical Industry Co., Ltd., BMI-5100) was used as the radical curable resin. (Example 2) Aliphatic polyamide (manufactured by T&K TOKA Corporation, PA-100) was used as the polyimide, and tricyclodecane dimethanol diacrylate (manufactured by Daicel Allnex Corporation, IRR 214-K) was used as the radical curable resin. (Example 3) Aliphatic polyamide (manufactured by T&K TOKA Corporation, PA-100) was used as the polyimide, and epoxy acrylate (manufactured by Daicel Allnex Corporation, EBECRYL 3700) was used as the radical curable resin. (Example 4) Polyetheresteramide (PA-201, manufactured by T&K Toka Corporation) was used as the polyimide, and bismaleimide (BMI-5100, manufactured by Daiwa Chemical Industry Co., Ltd.) was used as the radical curable resin. (Example 5) Polyetheresteramide (PA-201, manufactured by T&K Toka Corporation) was used as the polyimide, and tricyclodecane dimethanol diacrylate (IRR 214-K, manufactured by Daicel Allnex Corporation) was used as the radical curable resin. (Example 6) Aliphatic polyamide polyetheresteramide (PA-201, manufactured by T&K Toka Corporation) was used as the polyimide, and epoxy acrylate (EBECRYL 3700, manufactured by Daicel Allnex Corporation) was used as the radical curable resin. (Example 7) Polyesteramide (TPAE-617C, manufactured by T&K Toka Corporation) was used as the polyimide, and bismaleimide (BMI-5100, manufactured by Daiwa Chemical Industry Co., Ltd.) was used as the radical curable resin. (Comparative Example 1) Acrylic rubber (NV-11) was used instead of polyimides, and bismaleimide (BMI-5100, manufactured by Daiwa Chemical Industry Co., Ltd.) was used as the radical curable resin.
[0069] List of Materials Details of the materials and substrates used in the examples and comparative examples are as follows. Polyamides Aliphatic polyamide (T&K Toka, PA-100) Polyetheresteramide (T&K Toka, PA-201) Polyesteramide (T&K Toka, TPAE-617C) Acrylic rubber (NV-11) Radical curing resin Bismaleimide (Daiwa Chemical Industry, BMI-5100) Tricyclodecane dimethanol diacrylate (Daicel-Allnex, IRR 214-K) Epoxy acrylate (Daicel-Allnex, EBECRYL 3700) Curing initiator Peroxide (NOF Corporation, Perbutyl P) Film Release PET film (Mitsui Chemicals Tocello, T-15, thickness 38 μm) Polyimide film (Toray DuPont, Kapton 100EN, thickness 25 μm)
[0070] ・Physical property measurement equipment: Differential thermal and thermogravimetric simultaneous measurement device (Hitachi High-Tech, TG / DTA7300), dynamic viscoelasticity measurement device (TA Instruments, RSA-G2)
[0071] The formulations and physical property test results of each Example / Comparative Example are shown in Table 1.
[0072]
[0073] The results in Table 1 show that in the examples in which an adhesive composition containing polyamide was used, the cured product of the adhesive composition had an elastic modulus at 300°C of 1 MPa or more, a weight loss at 300°C of 0.8% or less, and a weight loss at 350°C of 3% or less, and also had good conformability to the pattern wafer. In contrast, in the comparative examples in which an adhesive composition containing an acrylic copolymer but no polyamide was used, the weight loss at 300°C was large.
[0074] According to the present invention, by using a laminate including a layer containing an adhesive composition containing a polyamide as a temporary fixing material, it can be easily peeled from a wafer even after exposure to a high-temperature environment, and at the same time, the laminate of the present invention combines sufficient heat resistance and unevenness-following ability, and can be crosslinked by thermal curing to further improve heat resistance, making it usable for wafer support systems. The present invention will greatly contribute to improving the productivity of electronic devices and has high applicability in various fields of industries that use electronic components, such as the electronic component industry, including the semiconductor process industry, the electrical and electronics industry, the transportation machinery industry, the information and communications industry, and the precision machinery industry.
Claims
1. A laminate comprising at least a layer containing an adhesive composition, the adhesive composition containing a polyamide and a curable resin having a radical reactive group, and the layer containing the adhesive composition after curing has a 300°C elastic modulus of 1 MPa or more.
2. The laminate according to claim 1, wherein the polyamide is at least one selected from the group consisting of polyesteramides, aliphatic polyamides and polyetheresteramides.
3. The laminate according to claim 1 or 2, which is a multi-layer film and is used as a temporary fixing material in a wafer support system.
4. The laminate according to claim 3, wherein the multilayer film comprises a substrate and a device-side adhesive layer, and the device-side adhesive layer comprises the adhesive composition.
5. The laminate according to claim 1 or 2, wherein the curable resin having a radical reactive group is a maleimide compound.
6. A method for manufacturing a wafer, comprising: (a) forming a laminate comprising a wafer, an adhesive layer, and a substrate; (b) curing the adhesive layer by heating; (c) subjecting the wafer to a heat treatment, a mechanical processing treatment, a chemical treatment, a physical treatment, a laser processing treatment, and / or a film formation treatment after step (b); (d) removing the substrate from the laminate after step (c); and (e) removing the adhesive layer from the laminate comprising the wafer and the adhesive layer after step (d), wherein the adhesive layer comprises an adhesive composition comprising a polyamide and a curable resin having a radical reactive group, and the adhesive layer after curing in step (b) has a 300°C elastic modulus of 1 MPa or more.
7. A method for manufacturing electronic components, comprising the method for manufacturing a wafer according to claim 6.
Citation Information
Patent Citations
Adhesive sheet for working wafer
JP2005019772A
Semiconductor device
JP2008124296A
Adhesive composition, film-shaped adhesive, adhesive sheet, and semiconductor device
JP2011042730A