Substrate for sic semiconductor devices, sic bonded substrate, sic polycrystalline substrate, and method for producing sic polycrystalline substrate
The SiC bonded substrate, featuring a high-quality SiC single crystal epitaxial layer bonded to a low-cost SiC polycrystalline substrate with a heat treatment process to correct warpage, addresses the cost and warpage issues in SiC semiconductor devices, improving manufacturing efficiency and reducing substrate warpage.
Patent Information
- Application Number
- PCT/JP2024/017618
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-25
- Filing Date
- 2024-05-13
- Publication Date
- 2024-11-28
AI Technical Summary
The high manufacturing cost and warpage issues associated with SiC single crystal substrates hinder the practical application of SiC semiconductor devices, particularly in high-voltage and high-output electronic devices, due to slow crystal growth rates and high processing costs, as well as substrate warpage during thinning processes like back grinding, which can lead to transportation errors and processing table issues.
A SiC bonded substrate is developed using a high-quality SiC single crystal epitaxial layer bonded to a low-cost SiC polycrystalline substrate, with a unique bonding method and heat treatment process to correct warpage, reducing substrate warpage to 0.17 mm/inch or less after back grinding, thereby addressing cost and manufacturing efficiency concerns.
The approach significantly reduces substrate warpage during back grinding, preventing transportation errors and processing table issues, while maintaining the benefits of high-quality SiC single crystal performance, thus enhancing manufacturing efficiency and reducing costs.
Smart Images

Figure JP2024017618_28112024_PF_FP_ABST
Abstract
Description
Substrate for SiC semiconductor device, SiC bonded substrate, SiC polycrystalline substrate, and method for manufacturing SiC polycrystalline substrate
[0001] The present invention relates to a silicon carbide (hereinafter sometimes referred to as "SiC") polycrystalline substrate and a method for manufacturing the same, a SiC bonded substrate obtained by bonding a SiC single crystal substrate to a SiC polycrystalline substrate, and a substrate for a SiC semiconductor device in which a SiC single crystal epitaxial layer and a semiconductor circuit are formed on a SiC bonded substrate.
[0002] SiC is a wide bandgap semiconductor with a wide bandgap of 2.2 to 3.3 eV, and due to its excellent physical and chemical properties, it has been researched and developed as an environmentally resistant semiconductor material. In recent years, SiC has attracted attention as a material for power devices such as high-voltage, high-output electronic devices and high-frequency electronic devices, as well as short-wavelength optical devices in the blue to ultraviolet wavelength range, and research and development into this material has been intensified. However, the difficulty of producing high-quality large-diameter single crystals of SiC has hindered the practical application of SiC devices.
[0003] To solve this problem, an improved Lely process has been developed, which uses a SiC single crystal substrate as a seed crystal and performs sublimation recrystallization. This improved Lely process allows SiC single crystals to be grown while controlling the crystal polytype (4H-SiC, 6H-SiC, 15R-SiC, etc.), carrier type, and impurity concentration. This technique significantly reduces the crystal defect density, and has led to the practical application of Schottky barrier diodes (SBDs) and field-effect transistors (MOSFETs) on these substrates.
[0004] However, in the improved Lely process using a SiC single crystal substrate as a seed crystal, the production cost of the SiC single crystal substrate is high due to the slow crystal growth rate and the high processing costs involved in processing the SiC single crystal ingot into wafers through steps mainly consisting of cutting and polishing. This high production cost has also been a factor that has hindered the practical application of SiC devices, and there has been a strong demand for the development of technology that can provide inexpensive SiC substrates for semiconductor device applications, particularly for high-voltage, high-power electronic devices.
[0005] Therefore, a technology has been proposed for manufacturing a semiconductor substrate (hereinafter sometimes referred to as a "SiC bonded substrate") that combines a low-cost support substrate portion with a high-quality SiC single crystal by using a high-quality SiC single crystal only for the device formation layer portion and fixing it to a support substrate (a material having the strength, heat resistance, and cleanliness sufficient to withstand the device manufacturing process: for example, a SiC polycrystalline substrate) using a bonding method that does not involve the formation of an oxide film at the bonding interface (see, for example, Patent Document 1). In particular, SiC bonded substrates using SiC polycrystalline as a support substrate are advantageous over single-crystal SiC substrates in that they enable lower manufacturing costs while taking advantage of the properties of SiC single crystal when applied to power devices. As SiC single crystal substrates become more widespread, SiC bonded substrates, which can be manufactured more inexpensively, are attracting increasing attention.
[0006] Meanwhile, problems related to substrate warpage have become apparent during device fabrication processes using SiC single crystal substrates. Generally, the degree of substrate warpage is of great importance during device fabrication processes. This is because a substrate with significant warpage can cause errors in the automatic device transport process or prevent the substrate from being held on the processing table. Furthermore, even if the substrate can be held on the processing table, a significant substrate warpage can prevent the substrate from being sufficiently flat. For example, during the exposure process (lithography process), a portion of the substrate surface may be out of focus, resulting in an inability to form a clear mask image. The impact of this defocusing phenomenon is greater the finer the circuit. Furthermore, substrate warpage can also be a concern due to reduced yields during the dicing and package assembly processes. In response to this, for example, Patent Document 2 provides a SiC single crystal substrate having a surface in which processing damage has been removed from the front and back surfaces of the substrate by CMP or diamond polishing, and the SiC single crystal substrate has small warpage as explained by strain and residual stress obtained by Raman spectroscopy and X-ray analysis. Also, Patent Document 3 provides a SiC polycrystalline molded body with small warpage as explained by residual stress values measured by X-ray analysis.
[0007] JP 2015-15401 A JP 2015-59073 A JP 2021-54666 A
[0008] Substrate warpage can also occur during thinning processes, such as backgrinding (BG), after mounting a surface circuit pattern in the fabrication process of vertical power devices, where the current flow direction is the substrate thickness direction. This thinning process requires removing approximately 40 to 60% of the original substrate thickness. For example, for a 6-inch diameter SiC single crystal substrate, the thickness after thinning by grinding is approximately 150 to 200 μm compared to a substrate thickness of 350 μm, resulting in a large amount of grinding. Therefore, a grinding process with high processing efficiency is generally adopted. In semiconductor device substrates using unbonded SiC single crystal substrates, substrate warpage is kept to approximately 1 mm or less, and no problems due to the above-mentioned warpage occur. In contrast, in the case of SiC bonded substrates, which are formed by bonding a SiC polycrystalline substrate and a SiC single crystal substrate, warpage exceeds 1 mm after backgrinding, potentially resulting in problems due to warpage, such as substrate transport errors in subsequent processes and inability to hold the substrate on the processing table. In particular, when the amount of back grinding exceeds the thickness of the substrate, the amount of warpage becomes extremely large. This is thought to be because the substrate becomes thinner, the rigidity of the substrate itself becomes smaller, and the balance of internal stresses becomes unbalanced.
[0009] This warpage during back grinding occurs because a processing damage layer is generated on the back surface of the substrate due to the grinding process, and the difference in the state of the processed surfaces on the front and back of the substrate causes the Twyman effect, resulting in significant warpage of the substrate. On the other hand, chemical mechanical polishing (CMP), which does not involve a processing damage layer, is less likely to cause significant warpage of the substrate, but the polishing speed is about 1 / 100 of that of grinding, which is very slow and expensive. Therefore, back grinding is essential for thinning substrates, rather than polishing.
[0010] Therefore, from the viewpoints of cost and manufacturing efficiency, if it were possible to provide a substrate that is less likely to warp during backgrinding, assuming that only backgrinding would be used for thinning, the process window for grinding that can achieve the desired processed state would be widened, and it would be easier to optimize the backgrinding design in the device manufacturing process.
[0011] The present invention has been made in view of these problems, and has an object to provide a SiC semiconductor device substrate having a structure in which a SiC polycrystalline substrate and a SiC single crystal substrate are bonded together, a SiC bonded substrate, a SiC polycrystalline substrate, and a method for manufacturing a SiC polycrystalline substrate, which are capable of sufficiently suppressing the amount of warpage of the substrate after backside grinding.
[0012] In order to solve the above-mentioned problems, the substrate for a SiC semiconductor device of the present invention is a substrate for a SiC semiconductor device comprising a support substrate made of SiC polycrystal, a SiC single crystal substrate bonded to a surface of the support substrate, a SiC single crystal epitaxial layer formed on the surface of the SiC single crystal substrate, and components of a semiconductor element formed on the SiC single crystal epitaxial layer, stacked in this order, wherein the surface of the support substrate that is not bonded to the SiC single crystal substrate is a ground surface, and the amount of warpage of the ground surface relative to the diameter of the ground surface is 0.17 mm / inch or less.
[0013] In order to solve the above-mentioned problems, the SiC bonded substrate of the present invention is a SiC bonded substrate obtained by stacking a support substrate made of SiC polycrystal and a SiC single crystal substrate bonded to a surface of the support substrate, wherein a surface of the support substrate that is not bonded to the SiC single crystal substrate is back-ground to grind 40 to 60% of the thickness of the support substrate to form a ground surface, and the amount of warpage of the ground surface relative to the diameter of the ground surface is 0.17 mm / inch or less.
[0014] In order to solve the above-mentioned problems, the SiC polycrystalline substrate of the present invention is a SiC bonded substrate formed by stacking a support substrate made of SiC polycrystal and a SiC single crystal substrate bonded to a surface of the support substrate, and the SiC polycrystalline substrate is used as the support substrate, wherein the surface of the support substrate that is not bonded to the SiC single crystal substrate is back-ground to grind 40 to 60% of the thickness of the support substrate to form a ground surface, and the amount of warpage of the ground surface relative to the diameter of the ground surface is 0.17 mm / inch or less.
[0015] In order to solve the above-mentioned problems, the present invention provides a method for manufacturing a SiC polycrystalline substrate, in which a support substrate made of SiC polycrystal and a SiC single crystal substrate bonded to a surface of the support substrate are stacked together, and the method uses the support substrate as the support substrate for a SiC bonded substrate, the method comprising: a film formation step of forming a SiC polycrystalline film on a seed substrate; a separation step of separating the seed substrate and the SiC polycrystalline film after the film formation step; a heat treatment step of heat treating the SiC polycrystalline film by maintaining it at a temperature of 1600°C or higher but lower than 2000°C after the separation step; and a grinding / polishing step of grinding and polishing the SiC polycrystalline film to process it into the support substrate after the heat treatment step, wherein the heat treatment is performed while the SiC polycrystalline film is maintained in a state warped opposite to the warp of the SiC polycrystalline film.
[0016] According to the present invention, it is possible to provide a substrate for a SiC semiconductor device having a structure in which a SiC polycrystalline substrate and a SiC single crystal substrate are bonded together, a SiC bonded substrate, a SiC polycrystalline substrate, and a method for manufacturing a SiC polycrystalline substrate, which are capable of sufficiently suppressing the amount of warpage of the substrate after backside grinding.
[0017] 7A and 7B. FIG. 7B is a schematic perspective view of a SiC polycrystalline substrate. FIG. 7A is a schematic perspective view of a SiC polycrystalline substrate. FIG. 7B is a schematic perspective view of a SiC bonded substrate. FIG. 7C is a schematic perspective view of a SiC bonded substrate. FIG. 7C is a schematic cross-sectional view of a substrate for a SiC semiconductor device. FIG. 7D is a schematic cross-sectional view of a MOSFET, which is an example of a SiC semiconductor device. FIG. 7E is a flowchart showing an example of a method for manufacturing a support substrate and a SiC bonded substrate. FIG. 7F is a flowchart showing an example of a method for manufacturing a SiC semiconductor device. FIG. 7F is a schematic side view showing a method for correcting warpage of a SiC polycrystalline film. FIG. 7F is a schematic side view showing a method for correcting warpage of a SiC polycrystalline film, which is a different aspect from that of FIGS. 7A and 7B. FIG. 7F is a schematic side view showing a method for correcting warpage of a SiC polycrystalline film, which is a different aspect from that of FIGS. 7A, 7B, 8A and 8B. FIG. 7F is a schematic view showing a method for correcting warpage of a SiC polycrystalline film, which is a different aspect from that of FIGS. 7A, 7B, 8A and 8B. 7A, 7B, 8A, 8B, 9A, and 9B are schematic diagrams showing a method for correcting warpage of a SiC polycrystalline film, which is different from the method shown in FIGS.
[0018] Hereinafter, an example of an embodiment of the present invention will be described in detail with reference to the drawings, but the present invention is not limited to this embodiment.
[0019] [SiC Polycrystalline Substrate] The SiC polycrystalline substrate is used as a support substrate for a SiC bonded substrate, which is a laminate of a support substrate made of SiC polycrystal and a SiC single crystal substrate bonded to the surface of the support substrate. For example, as shown in FIG. 1A, it is a SiC polycrystalline substrate 1 formed of polycrystalline SiC deposited by CVD. The SiC polycrystalline substrate 1 is disc-shaped with a thickness of 200 μm to 500 μm and a diameter of 4 to 8 inches. For example, it is formed into a 6-inch disc with a thickness of approximately 350 μm. The SiC polycrystalline of the SiC polycrystalline substrate 1 is composed of 4H—SiC crystal, 6H—SiC crystal, or 3C—SiC crystal, or a mixture thereof. One inch is 25.4 mm.
[0020] For example, if the surface 11 of the SiC polycrystalline substrate 1 is the surface that bonds with the SiC single crystal substrate, then the surface 12 opposite to the surface 11 is the surface that does not bond with the SiC single crystal substrate, and in the process of manufacturing the SiC semiconductor device, the opposite surface 12 is back-ground to thin the SiC polycrystalline substrate 1. Note that the opposite surface 12 may be the surface that bonds with the SiC single crystal substrate, in which case the surface 11 becomes the surface that does not bond with the SiC single crystal substrate, and the surface 11 is back-ground.
[0021] By performing back-grinding on SiC polycrystalline substrate 1, the thickness of SiC polycrystalline substrate 1 is ground by 40 to 60% to form ground surface 13 (the state of SiC polycrystalline substrate 1A in FIG. 1B ). In this state, the amount of warpage of ground surface 13 relative to the diameter of ground surface 13 is 0.17 mm / inch or less.
[0022] By keeping the amount of warpage at 0.17 mm / inch or less, problems caused by warpage, such as substrate transport errors in subsequent processes and the inability to hold the substrate on the processing table, can be prevented.
[0023] For example, if the SiC polycrystalline substrate 1 is a disk-shaped substrate having a diameter of 4 inches, 6 inches, or 8 inches, the diameters of the ground surface 13 will also be 4 inches, 6 inches, and 8 inches, respectively. A warpage of 0.17 mm / inch or less means that the warpage per inch is 0.17 mm or less, and is a value rounded to one decimal place. When the diameter of the ground surface 13 is 4 inches, the warpage of the ground surface 13 is 0.7 mm or less, when the diameter of the ground surface 13 is 6 inches, the warpage of the ground surface 13 is 1.0 mm or less, and when the diameter of the ground surface 13 is 8 inches, the warpage of the ground surface 13 is 1.4 mm or less.
[0024] In order to more reliably prevent problems caused by warpage, such as substrate transport errors in later processes and the inability to hold the substrate on the processing table, it is preferable that the amount of warpage of the ground surface 13 be 1.0 mm or less when the SiC polycrystalline substrate 1 is, for example, a disk-shaped substrate having a diameter of 6 to 8 inches. That is, by keeping the amount of warpage at 0.17 mm / inch or less, problems caused by warpage, such as substrate transport errors in later processes and the inability to hold the substrate on the processing table, can be more reliably prevented for currently mainstream disk-shaped SiC polycrystalline substrates 1 having a diameter of 6 inches or less.
[0025] When the SiC polycrystalline substrate 1 is subjected to back-grinding to grind the thickness of the SiC polycrystalline substrate 1 by 40 to 50% to form the ground surface 13, it is preferable that the amount of warpage of the ground surface 13 relative to the diameter of the ground surface 13 is 0.085 mm / inch or less.
[0026] By keeping the amount of warpage at 0.085 mm / inch or less, problems caused by warpage, such as substrate transport errors in subsequent processes and the inability to hold the substrate on the processing table, can be more reliably prevented.
[0027] For example, if the SiC polycrystalline substrate 1 is a disk-shaped substrate having a diameter of 4 inches, 6 inches, or 8 inches, the diameters of the ground surface 13 are also 4 inches, 6 inches, and 8 inches, respectively. A warpage of 0.085 mm / inch or less means, rounded to one decimal place, that the warpage of the ground surface 13 is 0.3 mm or less when the diameter of the ground surface 13 is 4 inches, 0.5 mm or less when the diameter of the ground surface 13 is 6 inches, and 0.7 mm or less when the diameter of the ground surface 13 is 8 inches. Furthermore, even when the diameter of the ground surface 13 is 12 inches, the warpage of the ground surface 15 is 1.0 mm or less ( FIG. 2B ), which is a level that can prevent problems caused by warpage, such as substrate transport errors in subsequent processes and inability to hold the substrate on the processing table.
[0028] In order to more reliably prevent problems caused by warpage, such as substrate transport errors in subsequent processes and the inability to hold the substrate on the processing table, it is more preferable that the amount of warpage of the grinding surface 13 be 0.5 mm or less, for example, when the SiC polycrystalline substrate 1 is disk-shaped and has a diameter of 6 to 8 inches.
[0029] In the process of thinning the SiC polycrystalline substrate 1, approximately 40 to 60% of the original thickness of the SiC polycrystalline substrate 1 is removed by back-grinding, but the extent to which the SiC polycrystalline substrate 1 is thinned depends on the tolerance for thickness variations in the SiC semiconductor device and the density of the device to be mounted.
[0030] Here, the SiC polycrystalline substrate 1 can be ground using a grinder with a grindstone of No. 5000 to No. 8000. The ground surface after grinding has a surface roughness Ra of 1 nm to 5 nm.
[0031] The amount of warpage of the ground surface 13 can be measured using a shape measuring device such as a three-dimensional measuring device.
[0032] [SiC Bonded Substrate] As shown in Fig. 2A, the SiC bonded substrate 3 includes a SiC polycrystalline substrate 1 and a SiC single crystal substrate 2 bonded to the surface of the SiC polycrystalline substrate 1. The SiC single crystal substrate 2 is made of single crystal SiC and has a diameter of 4 to 8 inches, the same as that of the SiC polycrystalline substrate 1. There are no particular limitations on the thickness, but the thickness may be, for example, approximately 0.5 µm to 2.0 µm. The SiC bonded substrate 3 is formed by using a high-quality SiC single crystal substrate 2 for the portion that will form the components of a semiconductor device and bonding this to the SiC polycrystalline substrate 1, which serves as a support substrate, thereby providing a substrate that combines a low-cost support substrate portion with a high-quality SiC single crystal.
[0033] Back surface 14 of SiC polycrystalline substrate 1, which is the surface not bonded to SiC single crystal substrate 2, is back-ground in the process of manufacturing the SiC semiconductor device, thereby thinning SiC polycrystalline substrate 1. By back-grinding SiC polycrystalline substrate 1, the thickness of SiC polycrystalline substrate 1 is ground by 40 to 60% to form ground surface 15 (the state of SiC bonded substrate 3A in FIG. 2B ). In this state, the amount of warpage of ground surface 15 relative to the diameter of ground surface 15 is 0.17 mm / inch or less. Note that opposite surface 12 corresponds to back surface 14, and ground surface 13 corresponds to ground surface 15.
[0034] By keeping the amount of warpage at 0.17 mm / inch or less, problems caused by warpage, such as substrate transport errors in subsequent processes and the inability to hold the substrate on the processing table, can be prevented.
[0035] For example, if the SiC polycrystalline substrate 1 is a disk-shaped substrate having a diameter of 4 inches, 6 inches, or 8 inches, the diameters of the ground surface 15 are also 4 inches, 6 inches, and 8 inches, respectively. A warpage of 0.17 mm / inch or less means, rounded to one decimal place, that the warpage of the ground surface 15 is 0.7 mm or less when the diameter of the ground surface 15 is 4 inches, that the warpage of the ground surface 15 is 1.0 mm or less when the diameter of the ground surface 15 is 6 inches, and that the warpage of the ground surface 15 is 1.4 mm or less when the diameter of the ground surface 15 is 8 inches.
[0036] In order to more reliably prevent problems caused by warpage, such as substrate transport errors in later processes and the inability to hold the substrate on the processing table, it is preferable that the amount of warpage of the ground surface 15 be 1.0 mm or less when the SiC polycrystalline substrate 1 is, for example, a disk-shaped substrate having a diameter of 6 to 8 inches. That is, by keeping the amount of warpage at 0.17 mm / inch or less, problems caused by warpage, such as substrate transport errors in later processes and the inability to hold the substrate on the processing table, can be more reliably prevented for currently mainstream disk-shaped SiC polycrystalline substrates 1 having a diameter of 6 inches or less.
[0037] When the SiC polycrystalline substrate 1 is subjected to back-grinding to grind the thickness of the SiC polycrystalline substrate 1 by 40 to 50% to form the ground surface 15, it is preferable that the amount of warpage of the ground surface 15 relative to the diameter of the ground surface 15 is 0.085 mm / inch or less.
[0038] By keeping the amount of warpage at 0.085 mm / inch or less, problems caused by warpage, such as substrate transport errors in subsequent processes and the inability to hold the substrate on the processing table, can be more reliably prevented.
[0039] For example, if the SiC polycrystalline substrate 1 is a disk-shaped substrate having a diameter of 4 inches, 6 inches, or 8 inches, the diameters of the grinding surface 15 are also 4 inches, 6 inches, and 8 inches, respectively. A warpage of 0.085 mm / inch or less means, rounded to one decimal place, that the warpage of the grinding surface 15 is 0.3 mm or less when the diameter of the grinding surface 15 is 4 inches, 0.5 mm or less when the diameter of the grinding surface 15 is 6 inches, and 0.7 mm or less when the diameter of the grinding surface 15 is 8 inches. Furthermore, even when the diameter of the grinding surface 15 is 12 inches, the warpage of the grinding surface 15 is 1.0 mm or less, which is a level that can prevent problems caused by warpage, such as substrate transport errors in subsequent processes and inability to hold the substrate on the processing table.
[0040] In order to more reliably prevent problems caused by warpage, such as substrate transport errors in subsequent processes and the inability to hold the substrate on the processing table, it is more preferable that the amount of warpage of the grinding surface 15 be 0.5 mm or less, for example, when the SiC polycrystalline substrate 1 is disk-shaped and has a diameter of 6 to 8 inches.
[0041] 3, the substrate 6 for a SiC semiconductor device is a substrate formed by laminating, in this order, a SiC polycrystalline substrate 1, a SiC single crystal substrate 2 bonded to the surface of the SiC polycrystalline substrate 1, a SiC single crystal epitaxial layer 4 formed on the surface of the SiC single crystal substrate 2, and components 5 of a semiconductor element formed on the SiC single crystal epitaxial layer 4. Here, the components 5 of the semiconductor element are not particularly limited, but may be, for example, a source electrode 51, a gate electrode 52, a gate insulating film 53, and a N + The substrate 6 for a SiC semiconductor device is a substrate in a state before being divided into individual pieces.
[0042] Ground surface 16, which is the surface of SiC polycrystalline substrate 1 that is not bonded to SiC single crystal substrate 2, is back-ground in the process of manufacturing a SiC semiconductor device, thereby thinning SiC polycrystalline substrate 1. By back-grinding SiC polycrystalline substrate 1, ground surface 16 is formed by grinding 40% to 60% of the SiC polycrystalline substrate 1 to reduce its thickness, and the amount of warping of ground surface 16 relative to the diameter of ground surface 16 is 0.17 mm / inch or less. Ground surface 16 corresponds to ground surfaces 13 and 15.
[0043] By keeping the amount of warpage at 0.17 mm / inch or less, problems caused by warpage, such as substrate transport errors in subsequent processes and the inability to hold the substrate on the processing table, can be prevented.
[0044] For example, if the SiC polycrystalline substrate 1 is a disk-shaped substrate having a diameter of 4 inches, 6 inches, or 8 inches, the diameters of the ground surface 16 are also 4 inches, 6 inches, and 8 inches, respectively. A warpage of 0.17 mm / inch or less means, rounded to one decimal place, that the warpage of the ground surface 16 is 0.7 mm or less when the diameter of the ground surface 16 is 4 inches, that the warpage of the ground surface 16 is 1.0 mm or less when the diameter of the ground surface 16 is 6 inches, and that the warpage of the ground surface 16 is 1.4 mm or less when the diameter of the ground surface 16 is 8 inches.
[0045] In order to more reliably prevent problems caused by warpage, such as substrate transport errors in later processes and the inability to hold the substrate on the processing table, it is preferable that the amount of warpage of the ground surface 16 be 1.0 mm or less when the SiC polycrystalline substrate 1 is, for example, a disk-shaped substrate having a diameter of 6 to 8 inches. That is, by keeping the amount of warpage at 0.17 mm / inch or less, problems caused by warpage, such as substrate transport errors in later processes and the inability to hold the substrate on the processing table, can be more reliably prevented for currently mainstream disk-shaped SiC polycrystalline substrates 1 having a diameter of 6 inches or less.
[0046] [SiC Semiconductor Device] The SiC semiconductor device 7 of this embodiment is obtained by dividing the substrate for a SiC semiconductor device. As shown in Figure 4, a semiconductor device for a vertical power device in which the current flows in the thickness direction of the substrate has a structure in which a drain electrode 8 is formed as a back electrode on the ground surface 16 of the substrate for a SiC semiconductor device 6.
[0047] [Method for Manufacturing SiC Polycrystalline Substrate] Next, a method for manufacturing a SiC polycrystalline substrate will be described. This manufacturing method is for manufacturing a SiC polycrystalline substrate 1 used as a support substrate in a SiC bonded substrate 3 formed by stacking a SiC polycrystalline substrate 1 serving as a support substrate and a SiC single crystal substrate 2 bonded to the surface of the SiC polycrystalline substrate 1, and includes a film formation step, a separation step, a heat treatment step, and a grinding / polishing step, which will be described below. Figure 5 is a flowchart of an example of a method for manufacturing the SiC polycrystalline substrate 1 and SiC bonded substrate 3 serving as a support substrate, showing steps S10 to S80.
[0048] <Step S10 (Film Forming Step)> In the method for manufacturing the SiC polycrystalline substrate 1, a SiC polycrystalline film is formed on a seed substrate in step S10. The seed substrate is made of carbon, silicon, or the like, and a SiC polycrystalline film is formed on the base substrate by a CVD method or the like.
[0049] <Step S20 (Separation Step)> Next, in step S20, the seed substrate and the SiC polycrystalline film are separated. For example, the base substrate on which the SiC polycrystalline film has been formed can be removed by burning or dissolving with acid.
[0050] <Step S30 (Heat Treatment Step)> In this embodiment, an object is to suppress warpage of the SiC semiconductor device substrate 6 that occurs when the SiC polycrystalline substrate 1 is thinned by the back grinding process (step S110) described later, and for this purpose, a heat treatment step is performed.
[0051] After the separation process, the SiC polycrystalline film, once separated from the seed substrate, develops warpage of several tens of micrometers even before back-grinding. The direction of warpage of the SiC polycrystalline film after this separation process can be determined using a shape measuring device such as the above-mentioned three-dimensional measuring device, as well as various simple measurements and visual inspection. In the heat treatment process, the SiC polycrystalline film is heat-treated in a state where the warpage has been corrected. The warpage is corrected by maintaining a state in which a force is applied to the SiC polycrystalline film in the direction opposite to the direction of the warpage of the SiC polycrystalline film.
[0052] For example, the SiC polycrystalline film may be placed on a correction tool capable of correcting warpage of the SiC polycrystalline film, and a weight may be applied from above to correct the shape so that a force is applied in the direction opposite to the warpage of the SiC polycrystalline film (e.g., so that the SiC polycrystalline film warps in the direction opposite to the warpage of the SiC polycrystalline film), and the heat treatment may be performed while maintaining this state. By performing the heat treatment while applying stress to the SiC polycrystalline film using the correction tool, it is possible to alleviate the internal stress of the SiC polycrystalline film so as to suppress warpage of the SiC polycrystalline film after the grinding process described below.
[0053] The correction jig is not particularly limited as long as it has a shape that can correct the warpage of the SiC polycrystalline film. Furthermore, the correction jig may be made of materials such as graphite or alumina. As an example, FIGS. 7A and 7B show schematic side views illustrating a method for correcting warpage of a SiC polycrystalline film 100. In FIG. 7A, the disk-shaped SiC polycrystalline film 100 is warped with a concave center and an upright periphery. The film has a convex spherical surface 110 that protrudes downward from the center and a concave spherical surface 120 opposite the spherical surface 110 that is concave downward from the center. The SiC polycrystalline film 100 is placed on the correction jig 200 so that the spherical surface 110 of the SiC polycrystalline film 100 is in contact with the correction surface 210 of the correction jig 200. Furthermore, a weight 300 is placed on the SiC polycrystalline film 100 so that the spherical surface 120 of the SiC polycrystalline film 100 is in contact with the spherical surface 310 of the weight 300 (FIG. 7B). Heat treatment is performed while maintaining this state.
[0054] The correction surface 210 of the correction jig 200 is a convex spherical surface that protrudes upward, and if the diameter of the SiC polycrystalline film 100 is 6 inches, the radius of curvature of the correction surface 210 may be 5.0 m or less, and is preferably 4.5 m to 3.0 m from the viewpoint of effectively correcting the warpage of the SiC polycrystalline film 100. Furthermore, the center 220 of the correction surface 210 protrudes the most on the correction surface 210, and from the viewpoint of effectively correcting the warpage of the SiC polycrystalline film 100, it is preferable that the center 220 protrudes 0.6 mm to 0.8 mm from the outer periphery 230 of the correction surface 210.
[0055] The weight may be of any shape or weight as long as it can be placed so that the entire spherical surface 110 of the SiC polycrystalline film 100 is in close contact with the entire correction surface 210 of the correction jig 200. Materials such as graphite and alumina may also be used as the weight. For example, the spherical surface 310 of the weight 300 may be a concave spherical surface that is concave upward, and may have a concave spherical shape that matches the convex spherical shape of the correction surface 210. By forming the spherical surface 310 in such a shape, scratches and the like can be prevented from occurring in the SiC polycrystalline film 100. To achieve such a shape that matches the spherical shape, the radius of curvature of the spherical surface 310 may be 5.0 m or less, and from the viewpoint of effectively correcting the warpage of the SiC polycrystalline film 100, it is preferable that the radius of curvature be 4.5 m to 3.0 m. Furthermore, the center 320 of the spherical surface 310 is the most recessed portion of the spherical surface 310, and from the viewpoint of effectively correcting the warpage of the SiC polycrystalline film 100, it is preferable that the center 320 is recessed from the outer periphery 330 of the spherical surface 310 by 0.6 mm to 0.8 mm.
[0056] The weight of the weight 300 is not particularly limited as long as it is placed so that the entire spherical surface 110 of the SiC polycrystalline film 100 is in close contact with the entire correction surface 210 of the correction jig 200. For example, if the thickness of the SiC polycrystalline film 100 is 1.0 mm or less, the weight of the weight 300 may be 3 kg or more and 8 kg or less, and preferably 4 kg or more and 6 kg or less. If the weight of the weight 300 is less than 3 kg, the warpage of the SiC polycrystalline film 100 may not be sufficiently corrected. Furthermore, if the weight of the weight 300 exceeds 8 kg, the SiC polycrystalline film 100 may crack.
[0057] 8A and 8B are schematic side views showing a method for correcting warpage of a SiC polycrystalline film 100, different from that shown in FIGS. 7A and 7B. Unlike the case shown in FIGS. 7A and 7B, the SiC polycrystalline film 100 is placed on a correcting jig 200a with its spherical surface 120 facing downward so as to contact the correcting surface 210a of the correcting jig 200a. Furthermore, a weight 300a is placed on the SiC polycrystalline film 100 so that the spherical surface 110 of the SiC polycrystalline film 100 contacts the spherical surface 310a of the weight 300a (FIG. 8B). Heat treatment may be performed while maintaining this state.
[0058] The correction surface 210a of the correction jig 200a is a downwardly concave spherical surface, and if the diameter of the SiC polycrystalline film 100 is 6 inches, the radius of curvature of the correction surface 210a may be 5.0 m or less, and is preferably 4.5 m to 3.0 m from the viewpoint of effectively correcting the warpage of the SiC polycrystalline film 100. Furthermore, the center 220a of the correction surface 210a is the most concave on the correction surface 210a, and from the viewpoint of effectively correcting the warpage of the SiC polycrystalline film 100, it is preferable that the center 220a be 0.6 mm to 0.8 mm recessed from the outer periphery 230a of the correction surface 210a.
[0059] Furthermore, the spherical surface 310a of the weight 300a may be a convex spherical surface that protrudes downward, and may have a convex spherical shape that matches the concave spherical shape of the correcting surface 210a. By matching the spherical shape in this way, scratches and other damage to the SiC polycrystalline film 100 can be prevented. To achieve this matching shape, the radius of curvature of the spherical surface 310a needs only to be 5.0 m or less, and from the viewpoint of effectively correcting the warpage of the SiC polycrystalline film 100, it is preferably 4.5 m to 3.0 m. Furthermore, the center 320a of the spherical surface 310a is the most protruding part of the spherical surface 310a, and from the viewpoint of effectively correcting the warpage of the SiC polycrystalline film 100, it is preferable that the center 320a protrudes 0.6 mm to 0.8 mm from the outer periphery 330a of the spherical surface 310a.
[0060] For example, if the thickness of the SiC polycrystalline film 100 is 1.0 mm or less, the weight of the weight 300a should be 3 kg or more and 8 kg or less, and preferably 4 kg or more and 6 kg or less. If the weight of the weight 300a is less than 3 kg, it may not be possible to sufficiently correct the warpage of the SiC polycrystalline film 100. If the weight of the weight exceeds 8 kg, the SiC polycrystalline film 100 may crack.
[0061] To correct the warpage of the SiC polycrystalline film 100, it is effective to apply a force in the direction opposite to the warpage of the SiC polycrystalline film 100 by, for example, pressing the periphery of the SiC polycrystalline film 100 with a weight to warp the SiC polycrystalline film 100 in the opposite direction. For this purpose, a weight 300b may be placed on the ring-shaped jig 400 shown in FIG. 9A to press the periphery of the SiC polycrystalline film 100 (FIG. 9B). Furthermore, by using the ring-shaped jig 400, it is not necessary to machine the lower surface of the weight into a spherical shape, so that a weight 300b with a flat lower surface 310b, which can be easily fabricated, can be used. The ring jig 400 can be made of materials such as graphite or alumina. Alternatively, a weight with a ring-shaped lower surface may be used so as to contact only the periphery of the SiC polycrystalline film 100.
[0062] Furthermore, the correction of warpage of the SiC polycrystalline film 100 can be performed simultaneously on a plurality of SiC polycrystalline films 100. For example, as shown in Fig. 10, a plurality of carbon sheets 500 may be inserted between and stacked on top of the plurality of SiC polycrystalline films 100, and the warpage may be corrected using a correction jig 200 and a weight 300. By interposing the carbon sheets 500 between the SiC polycrystalline films 100, adhesion between the SiC polycrystalline films 100 due to sublimation and recrystallization of the surfaces of the SiC polycrystalline films 100 when the SiC polycrystalline films 100 are heat-treated can be suppressed or prevented.
[0063] As shown by dotted line L in Figures 7B, 8B, 9B, and 10, in any case, the warpage of SiC polycrystalline film 100 can be reliably corrected by stacking correcting jig 200, SiC polycrystalline film 100, and weight 300 so that the center of spherical surface 110 of SiC polycrystalline film 100, the center of correction surface 210 of correcting jig 200, and the center of spherical surface 310 of weight 300 are on the same straight line and so that this straight line (dotted line L in Figures 7B, 8B, 9B, and 10) is parallel to the vertical direction.
[0064] The heat treatment process is performed after the separation process of step S20 and before the back-grinding process (step S110). Heat treatment of the SiC polycrystalline substrate 1 is possible, for example, before the back-grinding process in the manufacturing process of the SiC polycrystalline substrate, the manufacturing process of the SiC bonded substrate 3, or the manufacturing process of the SiC semiconductor device substrate 6. However, as described below, if the heat treatment temperature of the SiC polycrystalline film exceeds 1700°C, sublimation and recrystallization of SiC on the surface of the SiC polycrystalline substrate will begin, causing surface deterioration. For this reason, it is preferable to perform the heat treatment during the manufacturing process of the SiC polycrystalline substrate. In particular, performing the heat treatment before the grinding process of the SiC polycrystalline substrate (step S40) allows defects such as surface deterioration caused by the heat treatment to be eliminated in the grinding process (step S40). Furthermore, the heat treatment process can reduce warpage after back-grinding.
[0065] In step S30, the SiC polycrystalline film after the separation step is heat-treated by holding it at a temperature of 1600° C. or higher but lower than 2000° C. This step may be a step of holding the SiC polycrystalline film at a temperature between 1700° C. and 1800° C. for 3 hours or longer.
[0066] The higher the heat treatment temperature of the SiC polycrystalline film, the smaller the warpage of the substrate after back-grinding tends to be. Heat treatment relieves internal stress during film formation of the SiC polycrystalline substrate, thereby reducing substrate warpage. Heat treatment temperatures below 1600°C are less effective in improving the warpage of the substrate after back-grinding. Heat treatment temperatures above 1700°C initiate sublimation and recrystallization of SiC from the surface layer of the SiC polycrystalline film, while temperatures above 1800°C tend to cause excessive sublimation and recrystallization of SiC. Heat treatment temperatures above 2000°C may also form crater-like pores or depressions measuring several micrometers to several tens of micrometers in size in the surface layer of the SiC polycrystalline film, which may cause problems in the formation of the back electrode, and are therefore undesirable. Preferably, the polycrystalline film is heat-treated at a temperature between 1700°C and 1800°C.
[0067] The holding time for holding the SiC polycrystalline film at 1600°C or higher and lower than 2000°C is preferably 3 hours or longer. If the holding time is less than 3 hours, the effect of improving the warpage of the substrate after backside polishing may be small. There is no particular upper limit to the holding time, but 30 hours or shorter is preferred. If the holding time exceeds 30 hours, the effect will not increase any further, and the longer the holding time, the greater the disadvantage in terms of manufacturing costs. The holding time is preferably 20 hours or longer and 30 hours or shorter.
[0068] The atmosphere of the SiC polycrystalline film during the heat treatment is preferably at least one of an inert gas atmosphere such as argon (Ar) or nitrogen (N), or a vacuum atmosphere, so as to prevent unnecessary reactions such as oxidation. For example, it is desirable that the heat treatment furnace used for the heat treatment is in a state where an inert gas is flowing, and the flow rate is not limited as long as the furnace is sufficiently filled with the inert gas. The heat treatment may be performed using an atmosphere-controlled heating furnace or the like.
[0069] <Steps S40 (Grinding Step), S50 (Polishing Step)> In step S40, the SiC polycrystalline film is ground to a predetermined thickness. Then, in step 50, the surface of the SiC polycrystalline film is polished. After these grinding and polishing steps, the SiC polycrystalline substrate is ready to be bonded to SiC single crystal substrate 2, which is SiC polycrystalline substrate 1 according to this embodiment and can be used as a support substrate.
[0070] [Method of Manufacturing SiC Bonded Substrate] <Steps S60 to S80> Steps S60 to S80 are steps for manufacturing a SiC bonded substrate. In step S60, the above-described SiC polycrystalline substrate 1 is bonded to a separately prepared SiC single crystal substrate 2 (bonding step). The SiC single crystal substrate 2 may be manufactured using a hydrogen atom ablation delamination technique (also known as Smart Cut (registered trademark)) as described in Patent Document 1, in which a thick SiC single crystal substrate is bonded to a support substrate (step 60), and then separated to produce a thin SiC single crystal substrate 2 on the support substrate (step 70). Then, in step S80, a polishing step is performed to polish the surface of the SiC single crystal substrate 2, resulting in a SiC bonded substrate 3 comprising the SiC polycrystalline substrate 1 and the SiC single crystal substrate 2.
[0071] The SiC single crystal substrate 2 to be bonded may be a SiC single crystal produced by the improved Lely process, or a SiC single crystal formed by using the CVD method.
[0072] [Method of Manufacturing SiC Semiconductor Device] Next, a method of manufacturing a SiC semiconductor device will be described. FIG. 6 is a flowchart showing an example of a method of manufacturing a SiC semiconductor device 7, illustrating steps S90 to S140. In step S90, a SiC single crystal epitaxial layer 4 is epitaxially grown on the surface of a SiC single crystal substrate 2. In step S100, a circuit pattern, such as a semiconductor element component 5, is formed on the surface of the SiC single crystal epitaxial layer 4, and a surface protective layer is formed with a resin or the like to protect the circuit pattern. Then, in step S110, the back surface side opposite the surface on which the circuit pattern is formed is ground to thin the SiC polycrystalline substrate 1 and form a ground surface 16 (back grinding process). The substrate in the state in which the process up to step S110 has been completed is the substrate 6 for a SiC semiconductor device shown in FIG. 3. After step S110, in step S120, a drain electrode 8 is formed as a back surface electrode on the ground surface 16 of the substrate 6 for a SiC semiconductor device, resulting in a SiC semiconductor device 7. Before forming the back electrode, the ground surface 16 may be subjected to surface processing such as polishing.
[0073] Thereafter, in step S130, the surface protection layer protecting the circuit pattern of the SiC semiconductor device 7 is removed, and in step S140, dicing is performed by cutting the SiC semiconductor device 7 using a rotating diamond blade or the like to form dies.
[0074] The process flow from manufacturing the SiC polycrystalline substrate 1 to manufacturing the semiconductor is as shown in steps S10 to S140, but existing inspection and processing steps such as contact hole formation and probe inspection may also be performed as appropriate.
[0075] In the manufacturing process of the SiC semiconductor device 7, after the components 5 of the semiconductor element are formed on the SiC single crystal epitaxial layer 4, back-grinding is performed to remove the backside. In particular, the SiC semiconductor device 7 is often used in vertical power devices in which the current flows in the thickness direction of the substrate. Therefore, a thinning process using back-grinding is performed after the surface circuit pattern is mounted in the fabrication process of the vertical power device. This process requires removing approximately 40 to 60% of the original thickness of the SiC polycrystalline substrate 1. For example, for a 6-inch diameter SiC polycrystalline substrate with a substrate thickness of 350 μm, approximately 150 to 200 μm is removed by grinding. This results in a large amount of SiC polycrystalline grinding, and grinding is generally used because it has a higher thinning efficiency than polishing. For example, in a substrate for a SiC semiconductor device using a SiC single crystal substrate 2 that is not bonded to a SiC polycrystalline substrate, warpage of the substrate after thinning the SiC single crystal substrate 2 by back-grinding can be suppressed to approximately 1 mm or less. By keeping the warpage within this range, it becomes possible to process the substrate without any problems in subsequent processes. In contrast, in the case of using a SiC bonded substrate 3 in which a SiC polycrystalline substrate 1 and a SiC single crystal substrate 2 are bonded together, and after thinning the SiC polycrystalline substrate 1 by back-grinding, the warpage of the substrate significantly exceeds 1.0 mm, for example, in the case of a conventional technique in which no heat treatment step is performed.
[0076] In this embodiment, by performing a heat treatment step between the separation step and the grinding step, it is possible to suppress the warpage of the substrate after the thinning process of the SiC polycrystalline substrate by back-grinding to approximately 1.0 mm or less.
[0077] The present invention will be explained in more detail below by showing examples, but the present invention is not limited to the following examples in any way.
[0078] Example 1 Fabrication of SiC Polycrystalline Substrate 1 A disk-shaped carbon seed substrate was used as a base substrate, and a 2 mm thick SiC polycrystalline film was formed on the surface of the base substrate by chemical vapor deposition (CVD) (step S10). Methylchlorosilane was used as the source gas, and hydrogen and nitrogen gases were used as the carrier gas. The growth temperature in this chemical vapor deposition was 1400°C. The base substrate was then heated and removed in an air atmosphere at 1000°C by a combustion method, producing a disk-shaped SiC polycrystalline film 100 with a diameter of 6 inches (step S20).
[0079] This SiC polycrystalline film 100 was heat-treated using an atmosphere-controlled heating furnace (step S30). The heating temperature was 1700°C, the heating temperature was maintained for 24 hours, and the furnace atmosphere was an argon gas atmosphere. During the heat treatment, the warpage of the SiC polycrystalline film 100 was corrected using a graphite correction jig 200, a graphite ring-shaped jig 400, and a graphite weight 300b. First, the SiC polycrystalline film 100 was placed on the correction jig 200, whose upper surface served as the correction surface 210. The radius of curvature of the correction surface 210 was 4 m, and a convex spherical surface 110 with a protruding center of the SiC polycrystalline film 100 was placed on this correction surface 210. A ring-shaped jig 400 having an outer diameter of 150 mm, an inner diameter of 100 mm, and a thickness of 2 mm was placed on the SiC polycrystalline film 100 thus placed on the correcting jig 200, and a cylindrical weight 300b weighing 4 kg was further placed on the ring-shaped jig 400. By arranging the film in this manner, the spherical surface 110 of the SiC polycrystalline film 100 was deformed so as to be in close contact with the correcting surface 210, and a force was applied in the direction opposite to the direction of warpage of the SiC polycrystalline film 100, thereby maintaining the warped state in the opposite direction during heat treatment. The warpage direction of the SiC polycrystalline film 100 before being placed on the correcting jig 200 can be determined using a shape measuring device such as the three-dimensional measuring device described above, as well as by various simple measurements and visual inspection.
[0080] Thereafter, the surface of the SiC polycrystalline film 100 was ground and polished to be flattened (steps S40 and S50), thereby obtaining a SiC polycrystalline substrate 1 having a diameter of 6 inches (approximately 150 mm) and a thickness of 350 μm.
[0081] <Fabrication of SiC bonded substrate 3> The manufactured SiC polycrystalline substrate 1 was used to fabricate a SiC bonded substrate 3. A disk-shaped substrate of 4H polytype with a thickness of 350 μm, a diameter of 6 inches (approximately 150 mm), and a <0001> principal plane orientation, manufactured by the improved Lely process, was used as the SiC single crystal substrate 2 to be bonded to the SiC polycrystalline substrate 1. Note that the SiC bonded substrate 3 was fabricated using a hydrogen atom ablation delamination technique (also known as Smart Cut (registered trademark)) described in Patent Document 1.
[0082] (Step S60) Hydrogen ions were implanted into the bonding surface of the SiC single crystal substrate 2 to be bonded to the SiC polycrystalline substrate 1, forming a hydrogen ion implanted layer at a depth of 1.0 μm from the bonding surface. The SiC single crystal substrate 2 and the SiC polycrystalline substrate 1 were attracted by an electrostatic chuck and set in the chamber. Next, the electrostatic chuck was moved to align the relative positions of the SiC single crystal substrate 2 and the SiC polycrystalline substrate 1 so that the two substrates would contact in the correct positional relationship during the room-temperature bonding process. Next, the chamber was filled with 2×10 -6 The chamber was evacuated to a vacuum of 100 Pa. Next, an argon neutral atomic beam was uniformly irradiated onto the entire surfaces to be bonded of the SiC single crystal substrate 2 and the SiC polycrystalline substrate 1 using a FAB gun, removing any oxide films or adsorption layers from both surfaces to be bonded, exposing and activating the bonds. Next, while maintaining the vacuum at room temperature, the electrostatic chuck was moved within the chamber, bringing the surfaces to be bonded of the SiC single crystal substrate 2 and the SiC polycrystalline substrate 1 into contact with each other in the vacuum state within the chamber, directly bonding them through covalent bonds, thereby obtaining a bonded substrate.
[0083] (Step S70) Next, using a furnace, the bonded substrate was heated to 1000°C in an inert atmosphere filled with argon gas to form a microbubble layer in the hydrogen ion implanted layer, and the SiC single crystal substrate 2 was separated at the microbubble layer, and the thin plate-shaped SiC single crystal substrate 2 having a thickness of 1.0 μm was transferred to the SiC polycrystalline substrate 1.
[0084] (Step S80) The surface of the SiC single crystal substrate 2 exposed in step S70 was polished by CMP to be smooth, thereby obtaining a SiC bonded substrate 3.
[0085] <Fabrication of SiC Semiconductor Device Substrate 6> Next, a SiC semiconductor device substrate 6 was fabricated. Using the SiC bonded substrate 3 fabricated by the above method, a 20 μm-thick SiC single crystal epitaxial layer 4 was formed on the surface of the SiC single crystal substrate 2 by chemical vapor deposition (Step S90). Then, a circuit pattern was formed on the surface of the SiC single crystal epitaxial layer 4 as a component 5 of a semiconductor device and protected with a resin or the like (Step S100). Then, back grinding was performed by grinding the exposed surface of the SiC polycrystalline substrate 1 to form a ground surface 16 (Step S110). For back grinding, a DISCO grinder was used to grind the back surface of the SiC polycrystalline substrate 1. A 7000-grit grinding wheel with a diameter of 200 mm was used for grinding.
[0086] <Measurement of Warpage of Ground Surface 16> The warpage of the SiC semiconductor device substrate 6 was measured using a three-dimensional measuring instrument, EMS-3D 300XY, manufactured by COMS Corporation. First, the ground surface 16 of the SiC semiconductor device substrate 6 was suction-attached to the non-entire chucking surface, and the SiC semiconductor device substrate 6 was held with the semiconductor element components 5 facing upward. Height difference data within the ground surface 16 was acquired, and the warpage was then calculated as the sum of the maximum and minimum distances from the reference plane. The warpage was measured before grinding in step S110, and when the backside grinding amount of the SiC polycrystalline substrate 1 in step S110 was 150 μm (43% of the thickness of the SiC polycrystalline substrate 1), 175 μm (50% of the thickness of the SiC polycrystalline substrate 1), and 200 μm (57% of the thickness of the SiC polycrystalline substrate 1). The measurement results are shown in Table 1.
[0087] The non-full surface is an adsorption surface that can adsorb and hold one or three points on the measurement surface, the surface being the target for measuring warpage, without changing the original shape of the substrate. Since the entire surface is not adsorbed, the use of the non-full surface makes it possible to measure warpage.
[0088] Example 2 In Example 2, the warpage of the SiC polycrystalline substrate 1 produced in Example 1 was evaluated. First, to evaluate the backside grinding, the SiC polycrystalline substrate 1 was subjected to a back-grinding process under the same conditions as in step S110 in Example 1. Furthermore, the warpage of the ground surface 13 was measured for the opposite surface 12 of the SiC polycrystalline substrate 1 before the back-grinding process, and for the opposite surface 12 and the ground surface 13 when the backside grinding amount of the SiC polycrystalline substrate 1 was 150 μm (43% of the thickness of the SiC polycrystalline substrate 1), 175 μm (50% of the thickness of the SiC polycrystalline substrate 1), and 200 μm (57% of the thickness of the SiC polycrystalline substrate 1) by suction and holding the opposite surface 12 and the ground surface 13 with the non-entire suction surface. The measurement results are shown in Table 1.
[0089] [Example 3] [Example 4] In Example 3, the radius of curvature of the correction surface 210 of the correction tool 200 in the heat treatment step was changed to 3.5 m. In Example 4, the heat treatment temperature in the heat treatment step was changed to 1800°C. The warpage of SiC polycrystalline substrates 1 fabricated under the same conditions as those for fabricating the SiC polycrystalline substrate 1 in Example 1 was evaluated. As in Example 2, a back-grinding process was performed, and the opposite surface 12 and the ground surface 13 were sucked and held by the non-entire chucking surface, and the warpage of the opposite surface 12 and the ground surface 13 was measured. That is, the warpage of the ground surface 13 was measured when the surface 12 opposite to the state of the SiC polycrystalline substrate 1 before the back-grinding process, and when the back-grinding amount of the SiC polycrystalline substrate 1 was 150 μm (43% of the thickness of the SiC polycrystalline substrate 1), 175 μm (50% of the thickness of the SiC polycrystalline substrate 1), and 200 μm (57% of the thickness of the SiC polycrystalline substrate 1). The measurement results are shown in Table 1.
[0090] Comparative Example 1 Except for not performing the heat treatment step of step S30, a SiC polycrystalline substrate 1, a SiC bonded substrate 3, and a substrate 6 for a SiC semiconductor device were manufactured in the same manner as in Example 1, and the warpage of the manufactured substrate 6 for a SiC semiconductor device was measured. The measurement results are shown in Table 1.
[0091] Comparative Example 2 The warpage of the SiC polycrystalline substrate 1 produced in Comparative Example 1 was measured in the same manner as in Example 2. The measurement results are shown in Table 1.
[0092] Comparative Example 3 The warpage of the SiC bonded substrate 3 fabricated in Comparative Example 1 was measured. Specifically, the SiC bonded substrate 3 was subjected to back-grinding under the same conditions as in step S110 of Example 1. Furthermore, the warpage of the back surface 14 of the SiC bonded substrate 3 before back-grinding and the ground surface 15 of the SiC bonded substrate 3 with back-grinding amounts of 150 μm (43% of the thickness of the SiC polycrystalline substrate 1), 175 μm (50% of the thickness of the SiC polycrystalline substrate 1), and 200 μm (57% of the thickness of the SiC polycrystalline substrate 1) were measured. The warpage measurements were performed by suction-holding the back surface 14 and ground surface 15 on the non-entire suction surface. The measurement results are shown in Table 1.
[0093] Comparative Example 4 In Comparative Example 4, the correcting jig 200, the ring-shaped jig 400, and the weight 300b were not used in the heat treatment process, and the heat treatment was performed without correcting the warpage of the SiC polycrystalline film 100. The SiC polycrystalline substrate 1 was fabricated under the same conditions as those for fabricating the SiC polycrystalline substrate 1 in Example 1, and the warpage of the SiC polycrystalline substrate 1 was evaluated. The opposite surface 12 of the SiC polycrystalline substrate 1 before back-grinding and the ground surface 13 after back-grinding as in Example 2 were suction-held on the non-entire chucking surface, and the warpage of the opposite surface 12 and the ground surface 13 was measured. The measurement results are shown in Table 1.
[0094]
[0095] (Results and Discussion) The SiC semiconductor device substrate 6 is composed of a SiC polycrystalline substrate 1, a SiC single crystal substrate 2, a SiC single crystal epitaxial layer 4, and a semiconductor element component 5. Among these, the thickness of the SiC polycrystalline substrate 1 is sufficiently greater than the others, and the SiC polycrystalline substrate 1 is directly processed during backgrinding. Therefore, it can be seen that the SiC polycrystalline substrate 1 has a large effect on warpage. Furthermore, the results in Table 1 show that, for the SiC semiconductor device substrate 6, the SiC bonded substrate 3, and the SiC polycrystalline substrate 1, the degree of warpage after backgrinding ("after backgrinding" in Table 1) was significantly greater than the warpage before backgrinding ("before backgrinding" in Table 1). This indicates that the warpage of the substrate caused by backgrinding requires improving the warpage of the SiC polycrystalline substrate 1 after backgrinding. Comparing Examples 1 to 4 and Comparative Examples 1 to 4 in Table 1, results were obtained in which the warpage could be improved by subjecting the SiC polycrystalline substrate 1 to heat treatment.
[0096] In Comparative Examples 1 to 3, the heat treatment step was not performed on the SiC semiconductor device substrate 6, the SiC bonded substrate 3, and the SiC polycrystalline substrate 1, and therefore the warpage after backgrinding exceeded 1 mm in each case. Furthermore, the warpage after backgrinding of the SiC semiconductor device substrate 6, the SiC bonded substrate 3, and the SiC polycrystalline substrate 1 was approximately the same. From these results, it is inferred that the SiC polycrystalline substrate 1 is the essential cause of the warpage after backgrinding of the SiC semiconductor device substrate 6. Furthermore, the results of Examples 1 to 4 show that the warpage after backgrinding of the SiC semiconductor device substrate 6 can also be improved by improving the warpage of the SiC polycrystalline substrate 1 alone after backgrinding by heat treatment.
[0097] Furthermore, by performing heat treatment while maintaining the state in which the warpage of the SiC polycrystalline film 100 has been corrected using the correction jig 200, the ring-shaped jig 400, and the weight 300b, i.e., while applying a force in the direction opposite to the direction of the warpage of the SiC polycrystalline film 100, the degree of warpage was improved compared to when heat treatment was performed without correcting the warpage of the SiC polycrystalline film 100 (Examples 1 to 4, Comparative Example 4).
[0098] As described above, this embodiment can reduce the warpage of a 6-inch substrate to 1 mm or less when the backside is ground by backgrinding, and this embodiment can provide a manufacturing method that can achieve this by a heat treatment process characterized by a long time and high temperature, and is therefore industrially useful. The heat treatment conditions that can reduce the warpage of a 6-inch substrate after backgrinding by backgrinding to 1 mm or less are a heat treatment temperature of 1600°C or higher and lower than 2000°C, and a temperature holding time of 3 hours or longer. Furthermore, by performing heat treatment while maintaining a state in which the warpage of the SiC polycrystalline film is corrected, the warpage of the substrate after backgrinding by backgrinding can be further alleviated.
[0099] 1, 1A... SiC polycrystalline substrate, 2... SiC single crystal substrate, 3, 3A... SiC bonded substrate, 4... SiC single crystal epitaxial layer, 5... constituent element of semiconductor element, 6... SiC semiconductor device substrate, 7... SiC semiconductor device, 8... drain electrode, 11... front surface, 12... opposite surface, 13, 15, 16... ground surface, 14... back surface, 51... source electrode, 52... gate electrode, 53... gate insulating film, 54... N + Source, 55...P well, 100...SiC polycrystalline film, 110, 120...spherical surface, 200, 200a...correction jig, 210, 210a...correction surface, 220, 220a, 320, 320a...center, 230, 230a...periphery, 300, 300a, 300b...weight, 310, 310a...spherical surface, 310b...lower surface, 330, 330a...periphery, 400...ring-shaped jig, 500...carbon sheet.
Claims
1. A substrate for a SiC semiconductor device comprising, in order, a support substrate made of SiC polycrystal, a SiC single crystal substrate bonded to a surface of the support substrate, a SiC single crystal epitaxial layer formed on the surface of the SiC single crystal substrate, and components of a semiconductor element formed on the SiC single crystal epitaxial layer, wherein a surface of the support substrate that is not bonded to the SiC single crystal substrate is a ground surface, and the amount of warping of the ground surface relative to the diameter of the ground surface is 0.17 mm / inch or less.
2. The substrate for a SiC semiconductor device according to claim 1, wherein the amount of warping of the ground surface is 1.0 mm or less.
3. A SiC bonded substrate comprising a support substrate made of SiC polycrystal and a SiC single crystal substrate bonded to a surface of the support substrate, the surface of the support substrate not bonded to the SiC single crystal substrate being back-ground to remove 40 to 60% of the thickness of the support substrate to form a ground surface, wherein the amount of warping of the ground surface relative to the diameter of the ground surface is 0.17 mm / inch or less.
4. The SiC bonded substrate according to claim 3, wherein the amount of warping of the ground surface is 1.0 mm or less.
5. A SiC bonded substrate according to claim 3, wherein, when a surface of said support substrate not bonded to said SiC single crystal substrate is back-ground to grind away 40 to 50% of the thickness of said support substrate to form a ground surface, the amount of warping of said ground surface relative to the diameter of said ground surface is 0.085 mm / inch or less.
6. A SiC polycrystalline substrate used as a support substrate in a SiC bonded substrate formed by stacking a support substrate made of SiC polycrystal and a SiC single crystal substrate bonded to the surface of the support substrate, wherein the surface of the support substrate that is not bonded to the SiC single crystal substrate is back-ground to grind the thickness of the support substrate by 40 to 60% to form a ground surface, and the warp of the ground surface relative to the diameter of the ground surface is 0.17 mm / inch or less.
7. The SiC polycrystalline substrate according to claim 6, wherein the amount of warping of the ground surface is 1.0 mm or less.
8. A SiC polycrystalline substrate according to claim 6, wherein, when a surface of the support substrate not to be joined to the SiC single crystal substrate is back-ground to remove 40 to 50% of the thickness of the support substrate to form a ground surface, the amount of warping of the ground surface relative to the diameter of the ground surface is 0.085 mm / inch or less.
9. A method for manufacturing a SiC polycrystalline substrate, in which a support substrate made of SiC polycrystal and a SiC single crystal substrate bonded to a surface of the support substrate are stacked together to form a SiC bonded substrate, the method comprising: a film formation step of forming a SiC polycrystalline film on a seed substrate; a separation step of separating the seed substrate and the SiC polycrystalline film after the film formation step; a heat treatment step of heat treating the SiC polycrystalline film by maintaining the temperature at or above 1600°C and below 2000°C after the separation step; and a grinding / polishing step of grinding and polishing the SiC polycrystalline film to process it into the support substrate after the heat treatment step, wherein the heat treatment step involves heat treating the SiC polycrystalline film while maintaining a state in which a force is applied to the SiC polycrystalline film in a direction opposite to the direction of warping of the SiC polycrystalline film.
10. A method for producing a SiC polycrystalline substrate as described in claim 9, wherein in the heat treatment step, a force in the opposite direction is applied to the SiC polycrystalline film placed on a correction jig.
11. The method for producing a SiC polycrystalline substrate according to claim 9, wherein the heat treatment step is a step of holding the SiC polycrystalline film at a temperature between 1700° C. and 1800° C. for 3 hours or more.
Citation Information
Patent Citations
Semiconductor substrate manufacturing method
JP2015015401A
Internal stress evaluation method of silicon carbide single crystal wafer, and prediction method of warp of silicon carbide single crystal wafer
JP2015059073A
POLYCRYSTALLINE SiC COMPACT AND PRODUCTION METHOD THEREOF
JP2021054666A
Semiconductor substrate manufacturing method
JP2017112336A
Silicon carbide single crystal substrate, silicon carbide epitaxial substrate and silicon carbide semiconductor device manufacturing method
JP2020181994A