Release agent composition and release sheet
A solvent-free release agent composition using specific organopolysiloxanes and catalysts addresses the challenges of high reactivity and environmental concerns, achieving strong and sustainable heavy peeling performance.
Patent Information
- Application Number
- PCT/JP2024/017707
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2024-05-14
- Publication Date
- 2024-11-28
AI Technical Summary
Conventional release agent compositions for heavy-duty applications face challenges such as high reactivity leading to gel formation, insufficient peeling force, and the need for solvents, which are harmful to the environment and human health.
A solvent-free release agent composition comprising a straight-chain or branched organopolysiloxane with three silicon-bonded alkenyl groups, a three-dimensional network organopolysiloxane, an olefin liquid, an organohydrogenpolysiloxane, and a platinum group metal catalyst, which forms a crosslinked structure without excessive reactivity and maintains a high peeling force.
The composition achieves excellent heavy peeling force, long pot life, and safety by preventing gel formation and eliminating the need for solvents, resulting in a reliable and environmentally friendly release sheet.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Release agent composition and release sheet
[0001] The present invention relates to an addition reaction curable release agent composition that provides excellent release properties, and a release sheet using the same. More specifically, the present invention relates to a release agent composition that is not a solvent-based or emulsion-based composition, and more preferably to a solventless type release agent composition.
[0002] Conventionally, in order to prevent adhesion or sticking between substrates such as paper or plastics and adhesive materials, a cured coating of an organopolysiloxane composition has been formed on the surface of the substrate to impart release properties. As a method for forming a cured organopolysiloxane coating on the surface of the substrate, a method for forming a release coating by addition reaction is widely used because of its excellent curing properties.
[0003] This method of forming a releaseable coating by addition reaction includes a type in which the organopolysiloxane composition is dissolved in an organic solvent, a type in which an emulsifier is used to disperse the organopolysiloxane composition in water to form an emulsion, and a solventless type consisting only of organopolysiloxane. However, since the solvent-based type has the disadvantage of being potentially harmful to the human body and the environment, there is a growing trend to switch from the solvent-based type to the solventless type for safety reasons.
[0004] Generally, organopolysiloxane compositions for release paper are required to have various release strengths depending on the purpose. For applications requiring strong release, three-dimensional network organopolysiloxanes called MQ resins (M units are R' 3 SiO 1/2 The Q unit is SiO 4/2 R' means a monovalent hydrocarbon group) is widely used.
[0005] However, alkenyl group-containing MQ resins are often resinous or highly viscous compounds, and when added in large quantities, they must be diluted with an organic solvent before use. Although small amounts can be used without a solvent, the heavy release effect is insufficient in this case.
[0006] Patent Document 1 discloses a release modifier comprising an organopolysiloxane resin-organopolysiloxane condensation product obtained by condensation reaction of (a1) 100 parts by weight of an MQ-type resin having a molar ratio of M units to Q units of 0.6 to 1.0 and a hydroxyl or alkoxy group content in the range of 0.3 to 2.0% by weight with (a2) 20 to 150 parts by weight of a linear polydiorganosiloxane having hydroxyl or alkoxy groups and an average degree of polymerization of 100 to 1,000. In Patent Document 1, the release force in the examples increases only 1.4 to 2.2 times at low speeds (0.3 m / min) compared to comparative examples containing no condensation product, failing to achieve a sufficient release strength. This is presumably because the hydroxyl or alkoxy group content of (a1) is low, in the range of 0.3 to 2.0% by weight, leaving few reaction sites with (a2), resulting in insufficient crosslinking due to condensation. Furthermore, since the condensation reaction between the components (a1) and (a2) is time-consuming, there is a demand for a heavy release composition that can be produced by a simpler and less expensive method.
[0007] Patent Document 2 achieves a high release strength by blending a pressure-sensitive adhesive as a release modifier into a mixture of a reactive siloxane polymer, a siloxane crosslinker, and a catalyst. However, increasing the amount of pressure-sensitive adhesive is thought to produce adhesive effects, so there is a limit to how high the release strength can be achieved, and the examples do not suggest that a sufficient high release strength is achieved. Furthermore, pressure-sensitive adhesives have high viscosity and are generally diluted in a solvent such as toluene. However, given the recent trend toward solvent-free adhesives, adding them to compositions requires replacing the solvent with an α-olefin or the like.
[0008] Patent Document 3 describes a mixture of an alkenyl group-containing MQ resin, an organofunctional siloxane with a low viscosity of 5 to 80 centipoise, and an organohydrogenpolysiloxane. Due to the high addition reactivity of the organofunctional siloxane, a crosslinked structure can be easily formed, achieving heavy release. However, when the inventors reproduced the composition, they found that due to the high reactivity, a silicone gel, believed to be an addition reaction product, formed in the composition immediately after preparation. It is believed that an imbalance in the catalyst concentration distribution occurs immediately after adding the catalyst, causing crosslinking to proceed at room temperature.
[0009] Japanese Patent Application Laid-Open No. 2010-37557 Japanese Patent Application Laid-Open No. 2007-523225 Japanese Patent Application Laid-Open No. 2017-523258
[0010] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a solvent-free release agent composition that is not too highly reactive and prevents the generation of gel after preparation, yet is capable of forming a crosslinked structure that can achieve excellent heavy release, and a release sheet on which a cured coating of the composition is formed.
[0011] In order to solve the above problems, the present invention provides a release agent composition comprising the following components (A) to (E): (A) a linear or branched organopolysiloxane having at least three silicon-bonded alkenyl groups in side chains per molecule, a viscosity at 25°C of 100 mPa·s or more, and a vinyl value of 0.05 to 0.3 mol / 100 g: 20 to 65 parts by mass per 100 parts by mass of the total of component (A) and component (B): (B) R' 3 SiO 1/2 Units and SiO 4/2 Units and / or R'SiO 3/2 an organopolysiloxane having a three-dimensional network structure and at least two silicon-bonded alkenyl groups per molecule (in each of the above formulas, R' is a substituted or unsubstituted monovalent hydrocarbon group of 1 to 12 carbon atoms which may contain an unsaturated bond): 35 to 80 parts by mass per 100 parts by mass of the components (A) and (B) combined; (C) an olefin which is liquid at 25°C: 0 to 20 parts by mass per 100 parts by mass of the components (A) and (B) combined; (D) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms per molecule: an amount such that the ratio of the number of silicon-bonded hydrogen atoms in component (D) to the total number of alkenyl groups in components (A), (B), and (C) is 0.5 to 5; and (E) a platinum group metal catalyst: an effective amount.
[0012] Such a release agent composition is a solvent-free type, does not have excessively high addition reactivity, prevents gel formation after preparation, and yet can form a crosslinked structure that can achieve excellent heavy release.
[0013] In the present invention, the component (A) is represented by the following average composition formula (1): (R 2 3 SiO 1/2 ) a (R 1 R 2 2 SiO 1/2 ) b (R 1 R 2 SiO) c (R 2 2 SiO) d (R 1 SiO 3/2 ) e (R 2 SiO 3/2 ) f (SiO 4/2 ) g (1) (wherein, R 1 each independently represents an alkenyl group; R 2 are independently an unsubstituted or substituted monovalent hydrocarbon group that does not contain an alkenyl group, and a, b, c, d, e, f, and g are each independently a number of 0 or more, and are preferably represented by the following formula: 0≦a, 0≦b, 2≦a+b, 3≦c, 50≦d, 90≦c+d≦400, 0≦e≦8, 3≦b+c+e, 0≦f≦8, 0≦g≦8, 0≦f+g≦8.
[0014] Such component (A) can provide a more preferable viscosity of the release agent composition and a more preferable release force of the cured product.
[0015] In the present invention, the component (B) is preferably represented by the following average composition formula (2): (R 4 3 SiO 1/2 ) h (R 3 R 4 2 SiO 1/2 ) i (R 3 R 4 SiO) j (R 4 2 SiO) k (R 3 SiO 3/2 ) l (R4 SiO 3/2 ) m (SiO 4/2 ) n (2) (wherein, R 3 are each independently an alkenyl group having 2 to 8 carbon atoms, and R 4 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms that is not an alkenyl group, provided that all R 4 are methyl groups, and h, i, j, k, l, m, and n are each independently a number equal to or greater than 0, provided that i+j+l>0, l+m+n>0, and h+i+j+k+l+m+n=1.
[0016] Such component (B) can provide a more preferable strong release effect.
[0017] In the present invention, the component (C) is preferably a linear monoolefin having 10 to 18 carbon atoms or a branched monoolefin having 10 or more carbon atoms.
[0018] Such a component (C) is preferable because it is possible to lower the viscosity of the release agent composition and the crosslink density does not become too high.
[0019] In the present invention, the component (D) is represented by the following average composition formula (3): (R 6 3 SiO 1/2 ) p (R 5 R 6 2 SiO 1/2 ) q (R 5 R 6 SiO) r (R 6 2 SiO) s (R 5 SiO 3/2 ) t (R 6 SiO 3/2 ) u (SiO 4/2 ) v (3) (wherein, R 5 each independently represents a hydrogen atom; R 6are independently unsubstituted or substituted monovalent hydrocarbon groups other than hydrogen atoms, and p, q, r, s, t, u, and v are each independently a number of 0 or greater, and are preferably linear or branched organohydrogenpolysiloxanes having at least two silicon-bonded hydrogen atoms in side chains per molecule, represented by the formula: 0≦p, 0≦q, 0≦p+q, 0≦r, 40≦s, 90≦r+s≦400, 0≦t≦8, 2≦q+r+t, 0≦u≦8, 0≦v≦8, 0≦u+v≦8), and having a viscosity at 25°C of 100 mPa s or greater.
[0020] If the component (D) is of this type, the release agent composition will have a more suitable viscosity, and the handling properties and coating accuracy will be more preferable.
[0021] In the present invention, it is preferable to contain 0 to 20 parts by mass of organopolysiloxane (F) represented by the following formula: where 1≦p≦20 and X is a group selected from methyl, methoxy, and vinyl groups, or an oxygen atom that provides a cyclic structure.
[0022] When such a component (F) is contained, a more suitable release agent composition can be obtained.
[0023] In the present invention, the viscosity of the release agent composition at 25° C. is preferably 50 to 1000 mPa·s.
[0024] Such a viscosity is preferable because it allows coating when forming a cured film on a substrate and results in a uniform film.
[0025] In the present invention, it is also preferable that the stripping composition does not contain a solvent.
[0026] Such a solvent-free stripping composition is preferred because it is highly safe for the human body and the environment.
[0027] The present invention also provides a release sheet having a sheet-like substrate and a cured coating formed by curing the release agent composition on one or both surfaces of the substrate.
[0028] Such a release sheet is preferable because it provides an excellent release sheet with heavy release properties.
[0029] In the present invention, the release sheet preferably has a peel strength of 3.0 N / 25 mm or greater when a 25 mm wide polyester adhesive tape is attached to the cured coating and measured at an angle of 180° and a peel rate of 0.3 m / min.
[0030] Such a release sheet is preferable because it reliably provides a strong release effect.
[0031] The release agent composition of the present invention can provide a very high release strength compared to conventional high release compositions. It also has an excellent pot life and shows little decrease in release strength over time after curing, making it useful as a material for high release release sheets. Furthermore, excellent release sheets can be provided using such a release agent composition.
[0032] As described above, there has been a need for the development of a solvent-free release agent composition that is not too highly reactive, that prevents gel formation after preparation, and that is capable of forming a crosslinked structure that can achieve excellent heavy release, as well as a release sheet on which a cured coating of the composition is formed.
[0033]
[0003] As a result of extensive research into the above-mentioned problems, the present inventors have discovered that a composition comprising (A) a linear or branched organopolysiloxane having at least three silicon-bonded alkenyl groups in side chains per molecule, a viscosity of 100 mPa s or greater at 25°C, and a vinyl value of 0.05 to 0.3 mol / 100 g, (B) a three-dimensional network organopolysiloxane resin having at least two alkenyl groups per molecule, (C) an olefin that is liquid at 25°C, (D) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms per molecule, and (E) a platinum group metal catalyst has an excellent heavy release effect, inhibits loss of release force over time after curing, and further has an excellent pot life, which has led to the completion of the present invention. In particular, by using a linear or branched organopolysiloxane having at least three silicon-bonded alkenyl groups per molecule, a viscosity of 100 mPa·s or more at 25°C, and a vinyl value of 0.05 to 0.3 mol / 100 g, the composition of the present invention can provide a solvent-free release sheet that has extremely strong release properties while not exhibiting excessively high addition reactivity.
[0034] That is, the present invention provides a release agent composition comprising the following components (A) to (E): (A) a linear or branched organopolysiloxane having at least three silicon-bonded alkenyl groups in side chains per molecule, a viscosity of 100 mPa·s or more at 25°C, and a vinyl value of 0.05 to 0.3 mol / 100 g: 20 to 65 parts by mass per 100 parts by mass of the total of component (A) and component (B): (B) R' 3 SiO 1/2 Units and SiO 4/2 Units and / or R'SiO 3/2 an organopolysiloxane having a three-dimensional network structure and at least two silicon-bonded alkenyl groups per molecule (in each of the above formulas, R' is a substituted or unsubstituted monovalent hydrocarbon group of 1 to 12 carbon atoms which may contain an unsaturated bond): 35 to 80 parts by mass per 100 parts by mass of the components (A) and (B) combined; (C) an olefin which is liquid at 25°C: 0 to 20 parts by mass per 100 parts by mass of the components (A) and (B) combined; (D) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms per molecule: an amount such that the ratio of the number of silicon-bonded hydrogen atoms in component (D) to the total number of alkenyl groups in components (A), (B), and (C) is 0.5 to 5; and (E) a platinum group metal catalyst: an effective amount.
[0035] The present invention is described in detail below, but is not limited thereto. In this specification, "Me" represents a methyl group, and "Vi" represents a vinyl group. [(A) Alkenyl Group-Containing Organopolysiloxane] Component (A) is a linear or branched organopolysiloxane that has at least three silicon-bonded alkenyl groups in side chains per molecule, has a viscosity of 100 mPa·s or more at 25°C, and a vinyl value of 0.05 to 0.3 mol / 100 g.
[0036] The component (A) is a component for adjusting the viscosity of the composition and the release strength of the cured product, and specifically, is represented by the following average composition formula (1): (R 2 3 SiO 1/2 )a (R 1 R 2 2 SiO 1/2 ) b (R 1 R 2 SiO) c (R 2 2 SiO) d (R 1 SiO 3/2 ) e (R 2 SiO 3/2 ) f (SiO 4/2 ) g (1) (wherein, R 1 each independently represents an alkenyl group; R 2 are independently unsubstituted or substituted monovalent hydrocarbon groups that do not contain alkenyl groups, and a, b, c, d, e, f, and g are each independently a number equal to or greater than 0, and are represented by the following formula: 0≦a, 0≦b, 2≦a+b, 3≦c, 50≦d, 90≦c+d≦400, 0≦e≦8, 3≦b+c+e, 0≦f≦8, 0≦g≦8, 0≦f+g≦8. Component (A) is a linear organopolysiloxane having at least three, preferably 3 to 50, and more preferably 3 to 30, silicon-bonded alkenyl groups in side chains per molecule. The organopolysiloxane should have a viscosity at 25°C of 5,000 mPa s or less, preferably 3,000 mPa s or less, and more preferably 1,500 mPa s or less. Organopolysiloxanes having a linear molecular structure in which the main chain is composed of repeating diorganosiloxane units and the molecular chain terminals are blocked with triorganosiloxy groups are preferred. A viscosity within the above upper limit is preferred because the desired heavy release effect can be achieved without reducing the crosslink density of the cured product. The lower limit is 100 mPa·s or more, preferably 200 mPa·s or more. Viscosities below the lower limit are undesirable because they may lead to the formation of a silicone gel in the composition. Furthermore, even if no silicone gel is formed, problems such as a significantly increased viscosity of the composition may occur. In the present invention, the viscosity is measured as the absolute viscosity value measured using a B-type rotational viscometer at 25°C (the same applies hereinafter).
[0037] The vinyl value of component (A) is 0.05 or more and 0.3 mol / 100g or less. If the vinyl value of component (A) is less than 0.05 mol / 100g, the curability may be reduced. On the other hand, if the vinyl value exceeds 0.3 mol / 100g, the release properties of the cured coating may be reduced. The vinyl value is particularly preferably 0.07 or more and 0.2 mol / 100g or less.
[0038] In the above formula (1), a, b, c, d, e, f, and g are each independently a number equal to or greater than 0, and satisfy the following conditions: 0≦a, 0≦b, 2≦a+b, 3≦c, 50≦d, 90≦c+d≦400, 0≦e≦8, 3<b+c+e, 0≦f≦8, 0≦g≦8, 0≦f+g≦8. Preferably, 2≦a≦20, 2≦b≦20, 4≦a+b≦20, 3≦c≦40, 55≦d≦220, 95≦c+d≦250, 0≦e≦5, 5≦b+c+e≦60, 0≦f≦5, 0≦g≦5, 0≦f+g≦5.
[0039] The alkenyl group bonded to the silicon atom preferably has 2 to 8 carbon atoms, more preferably 2 to 4 carbon atoms. Examples include vinyl groups, aryl groups, butenyl groups, pentenyl groups, hexenyl groups, and heptenyl groups, with vinyl groups being preferred. The alkenyl group bonded to the silicon atom may be present at the molecular chain terminals in addition to at the molecular chain side chains in the organopolysiloxane molecule.
[0040] The organic group bonded to the silicon atom other than the alkenyl group is not particularly limited as long as it does not contain an aliphatic unsaturated bond. For example, it can be an unsubstituted or substituted monovalent hydrocarbon group having typically 1 to 12, and preferably 1 to 10, carbon atoms. Examples of the unsubstituted or substituted monovalent hydrocarbon group include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, and heptyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; aralkyl groups such as benzyl and phenethyl; and halogenated alkyl groups in which some or all of the hydrogen atoms in these groups have been substituted with halogen atoms such as chlorine, fluorine, and bromine atoms, such as chloromethyl, 3-chloropropyl, and 3,3,3-trifluoropropyl. Alkyl groups are preferred, and methyl groups are more preferred.
[0041] The amount of component (A) is 20 to 65 parts by mass, preferably 22 to 55 parts by mass, and more preferably 25 to 50 parts by mass, per 100 parts by mass of the total of components (A) and (B). If the content of component (A) is less than the above lower limit, the viscosity of the resulting composition will be significantly increased, resulting in reduced handleability and coating accuracy. If the amount of component (A) exceeds the above upper limit, the crosslink density of the cured product will be reduced, making it difficult to achieve the desired heavy release effect.
[0042] Examples of the linear organopolysiloxane (A) include those having the structure shown below: In the formula, R is a methyl group or a vinyl group, and the component (A) may be used alone or in combination of two or more different types.
[0043]
[0044]
[0045]
[0046]
[0047]
[0048]
[0049] [(B) Three-dimensional network organopolysiloxane] Component (B) is a three-dimensional network organopolysiloxane having R' 3 SiO 1/2 Units and SiO 4/2 Units and / or R'SiO 3/2 The organopolysiloxane has a three-dimensional network structure and has at least two alkenyl groups bonded to silicon atoms per molecule (in each of the above formulas, R' is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 12 carbon atoms which may have an unsaturated bond). Component (B) is a component for imparting a heavy release effect, and specifically, is an organopolysiloxane represented by the following average composition formula (2): (R 4 3 SiO 1/2 ) h (R 3 R 4 2 SiO 1/2 ) i (R 3 R 4 SiO) j (R 4 2 SiO) k (R 3 SiO 3/2 ) l (R 4 SiO 3/2 ) m (SiO 4/2 ) n (2) (wherein, R 3 are each independently an alkenyl group having 2 to 8 carbon atoms, and R 4 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms that is not an alkenyl group, provided that all R 4 are methyl groups, and h, i, j, k, l, m, and n are each independently a number equal to or greater than 0, provided that i + j + l > 0, l + m + n > 0, and h + i + j + k + l + m + n = 1. Component (B) is preferably waxy or solid at 25°C. Here, "waxy" means a gum-like (raw rubber-like) material that exhibits almost no self-fluidity and has a viscosity of 10,000 Pa s or more, particularly 100,000 Pa s or more, at 25°C.
[0050] In the above formula (2), h, i, j, k, l, m, and n are each independently a number equal to or greater than 0, provided that i + j + l > 0, l + m + n > 0, and h + i + j + k + l + m + n = 1. Preferably, h is a number from 0 to 0.65, and more preferably from 0.2 to 0.4. i is a number from 0 to 0.12, and more preferably from 0.03 to 0.07. j is a number from 0 to 0.2, and more preferably from 0 to 0.1. k is a number from 0 to 0.2, and more preferably from 0 to 0.1. l is a number from 0 to 0.2, and more preferably from 0 to 0.1. m is a number from 0 to 0.2, and more preferably from 0 to 0.1. n is a number from 0 to 0.6, and more preferably from 0.23 to 0.6. Preferably, i+j+l is 0 to 0.5, and more preferably 0 to 0.2, and preferably l+m+n is 0.1 to 0.8, and more preferably 0.2 to 0.6.
[0051] In the above formula (2), R 3 Examples of the alkenyl group represented by the formula (R) include the silicon-bonded alkenyl groups exemplified for component (A), and vinyl groups are particularly preferred. 4 Examples of the unsubstituted or substituted monovalent hydrocarbon group other than an alkenyl group, which is represented by the following formula, include the organic groups other than the silicon-bonded alkenyl groups exemplified for component (A). Among these, a methyl group is preferred, and when all R 4 At least 80 mol %, preferably 90 to 98 mol %, of the total R 4 When the content is 80 mol % or more, the compatibility with the above-mentioned component (A) is excellent, and the release agent composition does not separate into cloudy white layers, and a uniform coating can be obtained.
[0052] The content of silicon-bonded alkenyl groups in component (B) is preferably in the range of 0.01 to 1 mol, more preferably 0.05 to 0.2 mol, and even more preferably 0.06 to 0.1 mol per 100 g of component (B). When the alkenyl group content is in the range of 0.01 to 1 mol, the crosslinking reaction proceeds sufficiently, resulting in a cured product with higher hardness.
[0053] The amount of component (B) is 35 to 80 parts by mass, preferably 40 to 60 parts by mass, and more preferably 45 to 50 parts by mass, per 100 parts by mass of the total of components (A) and (B). If the content of component (B) exceeds the above upper limit, the viscosity of the resulting composition will be significantly increased, resulting in reduced handleability and coating accuracy. If the amount of component (B) is less than the above lower limit, the crosslink density of the cured product will be reduced, making it difficult to achieve the desired high release effect.
[0054] Examples of the organopolysiloxane resin of component (B) include the following: (Me 3 SiO 1/2 ) h (ViMe 2 SiO 1/2 ) i (SiO 4/2 ) n (ViMe 2 SiO 1/2 ) i (SiO 4/2 ) n (ViMeSiO) j (Me 2 SiO) k (MeSiO 3/2 ) m (ViMe 2 SiO 1/2 ) i (Me 2 SiO) k (ViSiO 3/2 ) l (ViMe 2 SiO 1/2 ) i (Me 2 SiO) k (MeSiO 3/2 ) m (Me 3 SiO 1/2 ) h (ViMe 2 SiO 1/2 ) i (Me 2 SiO) k (MeSiO 3/2 ) m (Me 3 SiO 1/2 )h (ViMe 2 SiO 1/2 ) i (Me 2 SiO) k (ViMeSiO) j (MeSiO 3/2 ) m (In the formula, h, i, j, k, l, m, and n are as defined in the above average composition formula (2).)
[0055] Especially Me 3 SiO 1/2 , ViMe 2 SiO 1/2 and SiO 4/2 It is more preferable to use an organopolysiloxane resin composed of units. By using such an organopolysiloxane resin, the crosslinking density of the resulting cured product can be sufficiently high, making it possible to obtain the desired high release effect. Note that component (B) may be used alone or in combination of two or more types.
[0056] [(C) Liquid Olefin] Component (C) is an olefin that is liquid at 25°C. Component (C) is a so-called viscosity reducer that can reduce the viscosity of the composition by adding a small amount. There are no particular limitations on the olefin as long as it is liquid at 25°C, and it may be appropriately selected from known olefins, but monoolefins are particularly preferred. For example, in the case of diolefins, the crosslink density may be too high, which may cause peeling noise during peeling. Preferably, the component (C) is a linear monoolefin having 10 to 18 carbon atoms or a branched monoolefin having 10 or more carbon atoms.
[0057] Conventionally, methods for reducing the viscosity of organopolysiloxane compositions have been employed, such as adding a solvent or a low-viscosity organopolysiloxane component. However, the use of highly volatile solvents can be harmful to humans and the environment, making the use of solvents undesirable from a safety perspective. Furthermore, while the viscosity can also be reduced by adding a low-volatility, low-viscosity organopolysiloxane component, the inventors have found, through extensive research, that the viscosity-reducing effect is weaker than that of hydrocarbon-based compounds. Therefore, in order to reduce the viscosity by adding a low-viscosity organopolysiloxane component, it becomes necessary to add a large amount of the component, which makes it difficult to achieve the desired high release effect.
[0058] In contrast, olefins that are liquid at 25°C (particularly preferably linear monoolefins having 10 to 18 carbon atoms or branched monoolefins having 10 or more carbon atoms) have a high viscosity-reducing effect on organopolysiloxane compositions, so a small amount is sufficient to reduce the viscosity without impairing the strong release effect. Furthermore, because they contain groups (particularly olefin moieties) that are reactive with organopolysiloxane compositions (particularly SiH), they are incorporated into the cured coating and do not volatilize or migrate to the tape. Therefore, they are extremely useful for controlling the viscosity of the release agent composition.
[0059] In the present invention, the olefin may be either linear or branched, but is preferably a linear monoolefin having 10 to 18 carbon atoms or a branched monoolefin having 10 or more carbon atoms. The linear monoolefin preferably has 10 to 18 carbon atoms, more preferably 12 to 18 carbon atoms, and even more preferably 14 to 18 carbon atoms. Monoolefins having a carbon atom count within the above upper limit are preferred because they are liquid at 25°C. Furthermore, monoolefins having a carbon atom count equal to or greater than the above lower limit are less volatile and therefore more safe for humans and the environment. Examples of such linear monoolefins include 1-tetradecene, 1-hexadecene, and 1-octadecene. More specifically, commercially available products in the "Linearene" (manufactured by Idemitsu Kosan Co., Ltd.) series (e.g., "Linearene 14," "Linearene 16," and "Linearene 18") can be used.
[0060] From the viewpoint of volatility, the branched monoolefin preferably has 10 or more carbon atoms, more preferably 15 or more carbon atoms. There is no particular upper limit on the number of carbon atoms, as long as it is liquid at 25°C. It is preferably 50 or less, and more preferably 40 or less. Furthermore, when two or more branched monoolefins are mixed, such as HS Dimer A-20P exemplified below, a small amount of a branched monoolefin having more than 50 carbon atoms may be mixed. As such a branched monoolefin, for example, a commercially available product in the series under the trade name "HS Dimer" (manufactured by Toyokuni Oil Mills Co., Ltd.) represented by the following formula (e.g., trade names "A-20" and "A-20P") can be used. The component (C) may be used alone, or two or more types may be used in combination.
[0061] HS Dimer A-20 HS dimer A-20P
[0062] The blending amount of component (C) is 0 to 20 parts by mass, preferably 0.1 to 18 parts by mass, more preferably 1 to 15 parts by mass, and even more preferably 4 to 12 parts by mass, per 100 parts by mass of the combined total of components (A) and (B). If the amount of component (C) exceeds the above upper limit, the viscosity of the resulting composition will be too low, resulting in poor coatability. When component (C) is blended, it is preferable that the amount of component (C) is equal to or greater than the above lower limit, since this will provide the effect of the component (C) as a viscosity reducer.
[0063] [(D) Organohydrogenpolysiloxane] Component (D) is an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms (hereinafter referred to as SiH groups) per molecule. A known organohydrogenpolysiloxane used in addition reaction silicone compositions can be used. For example, an organohydrogenpolysiloxane represented by the following average composition formula (3): (R 6 3 SiO 1/2 ) p (R 5 R 6 2 SiO 1/2 ) q (R 5 R 6SiO) r (R 6 2 SiO) s (R 5 SiO 3/2 ) t (R 6 SiO 3/2 ) u (SiO 4/2 ) v (3) (wherein, R 5 each independently represents a hydrogen atom; R 6 are independently an unsubstituted or substituted monovalent hydrocarbon group other than a hydrogen atom, and p, q, r, s, t, u, and v are each independently a number of 0 or more, and are represented by the following expressions: 0≦p, 0≦q, 0≦p+q, 0≦r, 40≦s, 90≦r+s≦400, 0≦t≦8, 2≦q+r+t, 0≦u≦8, 0≦v≦8, 0≦u+v≦8.
[0064] Alkenyl groups contained in components (A), (B), and (C) react with SiH groups in component (D) to form a crosslinked structure. That is, component (D) functions as a crosslinking agent. Component (D) preferably has a viscosity of 1,000 mPa·s or less at 25°C, more preferably 100 to 500 mPa·s, and even more preferably 100 to 200 mPa·s. When the viscosity is within the above upper limit, the overall composition does not become highly viscous, resulting in good handleability and coating accuracy. The viscosity is the absolute viscosity measured using a Brookfield rotational viscometer at 25°C. From the perspective of crosslinking balance, the amount of component (D) blended is preferably such that the ratio of the number of SiH groups in component (D) to the total number of alkenyl groups in components (A), (B), and (C) is 0.5 to 5.0, preferably 0.7 to 3.0. If the amount of component (D) does not satisfy the above range, the crosslinking balance may become inappropriate.
[0065] In component (D), the content of the SiH group is preferably in the range of 0.1 to 2 mol, and more preferably in the range of 0.2 to 1.7 mol, per 100 g of component (D). 6The unsubstituted or substituted monovalent hydrocarbon group other than a hydrogen atom, represented by the formula (I), includes the silicon-bonded organic groups other than alkenyl groups exemplified for component (A) above. A methyl group is preferred, and when all R 6 It is preferred that at least 50 mol %, typically 60 to 100 mol %, of the total R be methyl groups. 6 When the content of the component (A) is 50 mol % or more, the compatibility with the component (B) is excellent, and the release agent composition does not become cloudy or undergo phase separation. In the average composition formula (3), p, q, r, s, t, u, and v are each independently a number equal to or greater than 0, and satisfy the following conditions: 0≦p, 0≦q, 0≦p+q, 0≦r, 40≦s, 90≦r+s≦400, 0≦t≦8, 2≦q+r+t, 0≦u≦8, 0≦v≦8, and 0≦u+v≦8. Preferably, the following conditions are satisfied: 0≦p≦20, 0≦q≦20, 0≦p+q≦20, 3≦r≦60, 50≦s≦200, 95≦r+s≦250, 0≦t≦5, 5≦q+r+t≦70, 0≦u≦5, 0≦v≦5, and 0≦u+v≦5.
[0066] Component (D) has at least two SiH groups per molecule, typically 2 to 200, and preferably 3 to 100. The SiH groups may be located at either the terminals or the middle of the molecular chain, or both. The molecular structure of the organohydrogenpolysiloxane may be linear, cyclic, branched, or a three-dimensional network structure, but the number of silicon atoms per molecule (or degree of polymerization) is typically 100 to 300, preferably about 100 to 200.
[0067] Examples of organohydrogenpolysiloxanes represented by the above average composition formula (3) include methylhydrogensiloxane-dimethylsiloxane cyclic copolymers, dimethylsiloxane-methylhydrogensiloxane copolymers both ends of which are capped with trimethylsiloxy groups, dimethylpolysiloxanes both ends of which are capped with dimethylhydrogensiloxane groups, dimethylsiloxane-methylhydrogensiloxane copolymers both ends of which are capped with dimethylhydrogensiloxy groups, and methylhydrogensiloxane-diphenylsiloxane copolymers both ends of which are capped with trimethylsiloxy groups. , a methylhydrogensiloxane-diphenylsiloxane-dimethylsiloxane copolymer both ends of which are capped with trimethylsiloxy groups, a methylhydrogensiloxane-methylphenylsiloxane-dimethylsiloxane copolymer both ends of which are capped with trimethylsiloxy groups, a methylhydrogensiloxane-dimethylsiloxane-diphenylsiloxane copolymer both ends of which are capped with dimethylhydrogensiloxy groups, a methylhydrogensiloxane-dimethylsiloxane-methylphenylsiloxane copolymer both ends of which are capped with dimethylhydrogensiloxy groups, etc. Component (D) may be used alone, or two or more types may be used in combination.
[0068] Examples of the component (D) include cyclic siloxanes or linear siloxanes represented by the following formula:
[0069]
[0070]
[0071]
[0072]
[0073] [(E) Platinum group metal catalyst] The platinum group metal catalyst of component (E) is a catalyst for promoting the addition reaction of component (A), component (B), and component (C) with component (D), and any catalyst known to those skilled in the art for promoting so-called hydrosilylation reaction can be used.Such platinum group metal catalysts include, for example, platinum-based, palladium-based, rhodium-based, and ruthenium-based catalysts, and among these, platinum-based catalysts are particularly preferred.Such platinum catalysts include, for example, chloroplatinic acid, alcohol solution or aldehyde solution of chloroplatinic acid, complexes of chloroplatinic acid with various olefins or vinylsiloxanes, and complexes of platinum with various olefins or vinylsiloxanes.
[0074] The amount of component (E) added should be what is known as an effective amount as a catalyst. For example, from an economical standpoint, while still providing a good cured coating, the amount should be in the range of 0.1 to 1000 ppm, more preferably 1 to 500 ppm, calculated as platinum group metal by mass relative to the total mass of components (A), (B), (C), and (D).
[0075] [Other Components] In addition to the above components (A) to (E), other optional components can be blended into the release agent composition of the present invention. Examples include the following components. These other components may be used either alone or in combination of two or more.
[0076] Alkenyl Group-Containing Compounds Other Than Components (A), (B), and (C) In addition to components (A), (B), and (C), the composition of the present invention may also contain an alkenyl group-containing compound that undergoes an addition reaction with component (D). Such alkenyl group-containing compounds other than components (A), (B), and (C) are preferably those that contribute to the formation of a cured product, such as organopolysiloxanes other than components (A), (B), and (C) that have at least one alkenyl group per molecule. The molecular structure may be, for example, linear, cyclic, branched, or three-dimensionally network. It is particularly preferred that the composition contain 0 to 20 parts by mass of component (F) having the following structure:
[0077] (1≦p≦20, X is a group selected from a methyl group, a methoxy group, and a vinyl group, or one which gives a cyclic structure with an oxygen atom) "One which gives a cyclic structure with an oxygen atom" means that when X is an oxygen atom, Si on the left and right sides of the formula are connected to O via a siloxane bond, forming a cyclic structure.
[0078] Addition Reaction Inhibitors: To ensure a long pot life, an addition reaction inhibitor can be incorporated into the composition of the present invention. The addition reaction inhibitor is not particularly limited as long as it has a curing inhibitory effect on the platinum group metal catalyst (E) described above, and conventionally known inhibitors can be preferably used. Examples include phosphorus-containing compounds such as triphenylphosphine; nitrogen-containing compounds such as tributylamine, tetramethylethylenediamine, and benzotriazole; sulfur-containing compounds; acetylene-based compounds such as acetylene alcohols (e.g., 1-ethynylcyclohexanol and 3,5-dimethyl-1-hexyn-3-ol); compounds containing two or more alkenyl groups; hydroperoxy compounds; and maleic acid derivatives. The degree of curing inhibitory effect of the addition reaction inhibitor varies depending on its chemical structure. Therefore, the amount of each addition reaction inhibitor used can be appropriately adjusted according to conventionally known methods. By adding an appropriate amount of addition reaction inhibitor, the release agent composition exhibits excellent long-term storage stability at room temperature and excellent heat curing properties.
[0079] Other Optional Components If necessary, known antioxidants, pigments, stabilizers, antistatic agents, defoamers, adhesion improvers, thickeners, or inorganic fillers such as silica may be blended in. The blending amounts can be appropriately selected according to conventional techniques.
[0080] [Release Agent Composition] The composition of the present invention preferably has a viscosity at 25°C of 50 to 1,000 mPa·s, more preferably 80 to 500 mPa·s. A viscosity within the above range is preferable because it can be applied to form a cured coating on a substrate and a uniform coating can be obtained. The composition of the present invention does not require a solvent, and can therefore be used as a solvent-free release agent composition.
[0081] [Method for producing the composition for release sheets] The method for producing the release agent composition of the present invention is not particularly limited, but a method in which the above components (A) to (D) and any optional components are mixed uniformly in advance and then the catalyst (E) is added immediately before use is preferred in terms of pot life.
[0082] [Release Sheet] The present invention further provides a release sheet having a sheet-like substrate and a cured coating formed by curing the release agent composition on one or both surfaces of the substrate. The coating method is not particularly limited, but for example, the composition of the present invention can be applied to one or both surfaces of a sheet-like substrate such as paper or film in an amount of 0.01 to 100 g / m using a coating method such as coating with a comma coater, lip coater, roll coater, die coater, knife coater, blade coater, rod coater, kiss coater, gravure coater, or wire bar coater, screen coating, dip coating, or cast coating. 2 After application, a cured coating can be formed on the substrate by heating for 1 to 120 seconds at a temperature in the range of 50 to 200° C. When forming release layers on both sides of the substrate, it is preferable to perform the cured coating formation operation on each side of the substrate at a time.
[0083] The sheet-like substrate includes paper and various known films. Examples of the substrate include polyethylene-laminated paper, glassine paper, high-quality paper, kraft paper, and various coated papers such as clay-coated paper, synthetic paper such as Yupo, polyethylene film, polypropylene film such as CPP and OPP, polyester film such as polyethylene terephthalate film, polyamide film, polyimide film, polylactic acid film, polyphenol film, and polycarbonate film. It may also be casting paper used in the production of artificial leather, ceramic sheets, and double-sided separators. To improve the adhesion between these substrates and the release layer (cured film), the substrate surface may be corona-treated, etched, primer-treated, or plasma-treated.
[0084] More specifically, the method for producing the release sheet is, for example, to apply the release agent composition of the present invention to a polylaminated paper substrate in an amount of 1.0 to 1.5 g / m. 2After coating, the sheet can be prepared by heating at 140°C for 30 seconds. The release sheet preferably has a peel strength of 3.0 N / 25 mm or more when a 25 mm wide polyester adhesive tape is attached to the cured film at an angle of 180° and a peel speed of 0.3 m / min. There is no particular upper limit, but if the peel strength is too high, cohesive failure may occur between the adhesive tape and the film, so it can be set to 20.0 N / 25 mm or less.
[0085] The present invention will be specifically described below using examples and comparative examples, but the present invention is not limited to these. The viscosities listed below are all values measured at 25°C using a Brookfield rotational viscometer. In the following examples, parts represent parts by mass. Hereinafter, Me and Vi represent methyl and vinyl groups, respectively.
[0086] The components used in the examples and comparative examples are as follows. Hereinafter, the vinyl value refers to the number of moles of vinyl groups per 100 g of each component, and the SiH group content refers to the number of moles of SiH groups per 100 g of each component. The viscosity is the value at 25°C. The bonding order of the siloxane units shown in parentheses is not limited to the following. Component (A) (A1) (ViMe 2 SiO 1/2 ) 2 (Me 2 SiO) 120 (ViMeSiO) 18 Vinyl value: 0.187 mol / 100 g, viscosity: 300 mPa·s (A2) (ViMe 2 SiO 1/2 ) 2 (Me 2 SiO) 95 (ViMeSiO) 3 Vinyl value: 0.068 mol / 100 g, viscosity: 200 mPa·s (A3) (ViMe 2 SiO 1/2 ) 2 (Me 2 SiO) 210 (ViMeSiO) 10 Vinyl value: 0.071 mol / 100 g, viscosity: 840 mPa·s (a4) (ViMe 2SiO 1/2 ) 2 (Me 2 SiO) 101 Vinyl value: 0.027 mol / 100 g, viscosity: 190 mPa·s (a5) (ViMe 2 SiO 1/2 ) 3 (Me 2 SiO) 157 (MeSiO 3/2 ) Vinyl value: 0.026 mol / 100 g, viscosity: 250 mPa s (a6) (ViMe 2 SiO 1/2 ) 2 (Me 2 SiO) 10 Vinyl value: 0.211 mol / 100 g, viscosity: 9.0 mPa·s (a7) (ViMe 2 SiO 1/2 ) 2 (Me 2 SiO) 60 Vinyl value: 0.039 mol / 100 g, viscosity: 100 mPa·s (B) component (B1) (Me 3 SiO 1/2 ) 0.38 (ViMe 2 SiO 1/2 ) 0.06 (SiO 4/2 ) 0.56 Vinyl value: 0.086 mol / 100 g, solid at 25°C Component (C) (C1) 1-tetradecene (Linearene 14 manufactured by Idemitsu Kosan Co., Ltd.) Vinyl value: 0.51 mol / 100 g, viscosity: 2.4 mPa·s Component (D) (D1) (Me 3 SiO 1/2 ) 2 (MeHSiO) 30 (Me 2 SiO) 70 SiH group content: 1.098 mol / 100 g, viscosity: 119 mPa・s (D2) (Me 3 SiO 1/2 ) 2 (MeHSiO) 50 (Me 2 SiO) 48SiH group content: 0.791 mol / 100 g, viscosity: 118 mPa s Component (E) (E1) catalyst: platinum-vinylsiloxane complex Component (F) (F1) (MeSiO 3/2 -ViMe 2 SiO 1/2 ) n Vinyl value: 0.53 mol / 100 g, viscosity: 25 mPa·s (G) Component (other components) (G1) Addition reaction inhibitor (pot life extender): 1-ethynylcyclohexanol
[0087] [Example 1] The above (A1) average formula: (ViMe 2 SiO 1/2 ) 2 (Me 2 SiO) 120 (ViMeSiO 1/2 ) 18 and the linear dimethylpolysiloxane represented by the average formula (Me 3 SiO 1/2 ) 0.38 (ViMe 2 SiO 1/2 ) 0.06 (SiO 4/2 ) 0.56 The xylene was removed from the mixture at 150°C under a reduced pressure of 20 mmHg or less, and the mixture was cooled. Then, 6.0 parts by mass of (C1) 1-tetradecene and (D1) an organosiloxane having the average formula: (Me 3 SiO 1/2 ) 2 (MeHSiO) 30 (Me 2 SiO) 70A transparent liquid was obtained by mixing 25.2 parts by mass of a methylhydrogenpolysiloxane represented by the formula (I), 2.8 parts by mass of (F), and 0.2 parts by mass of 1-ethynylcyclohexanol (G). (The ratio of the amount of SiH groups in component (D1) to the total amount of alkenyl groups in components (A1), (B1), and (C1), i.e., H / Vi, was 1.8.) To the mixture obtained above, the catalyst (E) was added in an amount equivalent to 100 ppm by mass of platinum relative to the total mass of components (A1), (B1), (C1), and (D1), and the mixture was stirred and mixed to obtain a transparent composition with a viscosity of 223 mPa s.
[0088] [Examples 2 to 6, Comparative Examples 1 to 4] Using the same procedure as in Example 1, components (A) and (B) were mixed to the compositions shown in Tables 1 and 2 below, and then xylene in component (B) was removed by distillation under reduced pressure. Components (C), (D), (F), and (G) were then mixed, followed by mixing with platinum catalyst (E), to obtain the compositions of Examples 2 to 6 and Comparative Examples 1 to 4. Tables 1 and 2 show the blending amounts of each component. Coated products (release sheets) were prepared using the obtained compositions using the methods described below and evaluated.
[0089] [Peeling Force] The obtained composition was applied to the surface of polyethylene laminated paper in an amount of 1.0 to 1.1 g / m 2 The resulting cured film was subjected to separator aging at 25°C for 1 day, after which a 25mm wide polyester adhesive tape (No. 31B 75 High, product name of Nitto Denko) was attached to the surface of the cured film, and the tape was heated at 70°C with a load of 20 gf / cm. 2 The tape was then adhered and aged for one day at 70°C under a load of 20 gf / cm. Thereafter, one end of the tape was peeled off, and the end was pulled at an angle of 180° to the polyethylene-laminated paper substrate at a peeling rate of 0.3 m / min, and the peel force (N / 25 mm) was measured using a tensile tester. The tensile tester used was an AGS-50G model manufactured by Shimadzu Corporation. [Residual Adhesion Rate] A 25 mm wide polyester adhesive tape (No. 31B75 High, product name manufactured by Nitto Denko) was adhered to the cured coating surface after separator aging, and the tape was then aged at 70°C under a load of 20 gf / cm. 2The tape was peeled off from the cured film, stuck to a 25 μm PET film, and pressed back and forth once with a 2 kg tape roller. The tape was then peeled off at an angle of 180° at 0.3 m / min using a tensile tester, and the force F (N / 25 mm) required for peeling was measured. For comparison, the above polyester adhesive tape was stuck to a Teflon (registered trademark) plate instead of the cured film, and the force F required for peeling was measured in the same manner as above. 0 The residual adhesive strength (%) of the polyester adhesive tape after peeling from the release layer was measured in comparison with that of the polyester adhesive tape peeled from the Teflon (registered trademark) plate, and was calculated using the formula: F / F 0 The calculation was made by multiplying the result by 0.01×100. [Presence or absence of treatment bath gel] After preparing the compositions shown in Tables 1 and 2 below excluding component (E), component (E) was added and stirred, and then it was checked whether or not any silicone gel matter had adhered to or floated on the walls of the treatment bath container or in the treatment bath. If no silicone gel matter was observed, it was marked as ◯, and if a silicone gel matter was observed, it was marked as ×. The results are shown in Tables 1 and 2.
[0090]
[0091]
[0092] The results of Examples 1 to 6 demonstrate that the release agent composition of the present invention has a viscosity of 500 mPa·s or less at 25°C, which is suitable for a solventless heavy release agent composition. The release sheets obtained using this composition have a high release force of 3.0 N / 25 mm or more. Furthermore, the use of an organopolysiloxane with a high vinyl value and side-chain alkenyl groups that suppress addition reactivity can suppress the generation of silicone gel immediately after the composition is prepared. On the other hand, systems using organopolysiloxanes with no side-chain alkenyl groups and a low vinyl value (Comparative Examples 1, 2, and 4) result in low crosslink density and therefore low release force. A system using a short-chain polyorganosiloxane containing alkenyl groups at both ends (Comparative Example 3) exhibits high release force, but its high reactivity results in the generation of silicone gel after the preparation of the treatment bath. Based on these results, the compositions shown in Comparative Examples 1 to 4 are not suitable for the applications intended by the present invention.
[0093] This specification includes the following aspects: [1]: A release agent composition comprising the following components (A) to (E): (A) a linear or branched organopolysiloxane having at least three silicon-bonded alkenyl groups in side chains per molecule, a viscosity at 25°C of 100 mPa·s or more, and a vinyl value of 0.05 or more and 0.3 mol / 100 g or less: 20 to 65 parts by mass per 100 parts by mass of the total of component (A) and component (B) below; 3 SiO 1/2 Units and SiO 4/2 Units and / or R'SiO 3/2an organopolysiloxane having a three-dimensional network structure, the organopolysiloxane having a unit, at least two silicon-bonded alkenyl groups per molecule (in each of the above formulas, R' is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 12 carbon atoms, which may have an unsaturated bond, in an amount of 35 to 80 parts by mass per 100 parts by mass of the component (A) and the component (B) combined; (C) an olefin that is liquid at 25°C, the amount being 0 to 20 parts by mass per 100 parts by mass of the component (A) and the component (B) combined; (D) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms per molecule, the amount being such that the ratio of the number of silicon-bonded hydrogen atoms in component (D) to the total number of alkenyl groups in components (A), (B), and (C) is 0.5 to 5; and (E) an effective amount of platinum group metal catalyst [2]: the component (A) is represented by the following average composition formula (1): (R 2 3 SiO 1/2 ) a (R 1 R 2 2 SiO 1/2 ) b (R 1 R 2 SiO) c (R 2 2 SiO) d (R 1 SiO 3/2 ) e (R 2 SiO 3/2 ) f (SiO 4/2 ) g (1) (wherein, R 1 each independently represents an alkenyl group; R 2 are independently an unsubstituted or substituted monovalent hydrocarbon group not containing an alkenyl group, and a, b, c, d, e, f and g are each independently a number of 0 or more, and are represented by the following formulas: 0≦a, 0≦b, 2≦a+b, 3≦c, 50≦d, 90≦c+d≦400, 0≦e≦8, 3≦b+c+e, 0≦f≦8, 0≦g≦8, 0≦f+g≦8. [3]: The stripping composition according to [1] or [2], wherein the component (B) is represented by the following average composition formula (2): (R 4 3SiO 1/2 ) h (R 3 R 4 2 SiO 1/2 ) i (R 3 R 4 SiO) j (R 4 2 SiO) k (R 3 SiO 3/2 ) l (R 4 SiO 3/2 ) m (SiO 4/2 ) n (2) (wherein, R 3 are each independently an alkenyl group having 2 to 8 carbon atoms, and R 4 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms that is not an alkenyl group, provided that all R 4 are methyl groups, and h, i, j, k, l, m, and n are each independently a number of 0 or greater, with the proviso that i+j+l>0, l+m+n>0, and h+i+j+k+l+m+n=1. [4]: The stripping composition according to any one of [1] to [3], wherein the component (C) is a linear monoolefin having 10 to 18 carbon atoms or a branched monoolefin having 10 or more carbon atoms. [5]: The stripping composition according to any one of [1] to [3], wherein the component (D) is a group represented by the following average composition formula (3): (R 6 3 SiO 1/2 ) p (R 5 R 6 2 SiO 1/2 ) q (R 5 R 6 SiO) r (R 6 2 SiO) s (R 5 SiO 3/2 ) t (R 6 SiO 3/2 ) u (SiO 4/2 ) v (3) (wherein, R 5 each independently represents a hydrogen atom; R 6 are independently an unsubstituted or substituted monovalent hydrocarbon group other than a hydrogen atom, and p, q, r, s, t, u, and v are each independently a number of 0 or greater, and are linear or branched organohydrogenpolysiloxanes having at least two hydrogen atoms bonded to silicon atoms in side chains per molecule, and having a viscosity at 25°C of 100 mPa s or greater, wherein p, q, r, s, t, u, and v are each independently a number of 0 or greater, and 0≦p, 0≦q, 0≦p+q, 0≦r, 40≦s, 90≦r+s≦400, 0≦t≦8, 2≦q+r+t, 0≦u≦8, 0≦v≦8, 0≦u+v≦8. [6]: The release agent composition according to any one of [1] to [5], which contains 0 to 20 parts by mass of an organopolysiloxane (F) represented by the following formula: However, 1≦p≦20, and X is a group selected from a methyl group, a methoxy group, and a vinyl group, or an oxygen atom that gives a cyclic structure. [7]: The release agent composition according to any one of [1] to [6], which has a viscosity of 50 to 1,000 mPa s at 25°C. [8]: The release agent composition according to any one of [1] to [7], which does not contain a solvent. [9]: A release sheet having a sheet-like substrate and a cured coating formed on one or both surfaces of the substrate by curing the release agent composition according to any one of [1] to [8].
[10] : The release sheet according to [9], which has a peel strength of 3.0 N / 25 mm or more when a 25 mm wide polyester pressure-sensitive adhesive tape is attached to the cured coating at an angle of 180° and a peel speed of 0.3 m / min.
[0094] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that exhibits similar effects is included within the technical scope of the present invention.
Claims
1. A release agent composition containing the following components (A) to (E). (A) A linear or branched organopolysiloxane having at least 3 alkenyl groups bonded to silicon atoms in one molecule, having a viscosity at 25 °C of 100 mPa·s or more, and a vinyl value of 0.05 or more and 0.3 mol / 100 g or less: 20 to 65 parts by mass with respect to a total of 100 parts by mass of the component (A) and the following component (B), (B) R' 3 SiO 1/2 units, and SiO 4/2 units and / or R'SiO 3/2 units, having at least 2 alkenyl groups bonded to silicon atoms in one molecule, and having a three-dimensional network structure (in the above formulas, R' is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 12 carbon atoms which may have an unsaturated bond): 35 to 80 parts by mass with respect to a total of 100 parts by mass of the component (A) and the component (B), (C) An olefin that is liquid at 25 °C: 0 to 20 parts by mass with respect to a total of 100 parts by mass of the component (A) and the component (B), (D) An organohydrogenpolysiloxane having at least 2 hydrogen atoms bonded to silicon atoms in one molecule: an amount such that the number ratio of the hydrogen atoms bonded to silicon atoms in the component (D) to the total number of alkenyl groups in the component (A), the component (B), and the component (C) is 0.5 to 5, and (E) A platinum group metal-based catalyst: an effective amount 2. The component (A) has the following average compositional formula (1): (R 2 3 SiO 1/2 ). a (R 1 R 2 2 SiO 1/2 ). b (R 1 R 2 SiO). c (R 2 2 SiO). d (R 1 SiO 3/2 ). e (R 2 SiO 3/2 ). f (SiO 4/2 ).g (1) (In the formula, R 1 independently represents an alkenyl group, and R 2 independently represents an unsubstituted or substituted monovalent hydrocarbon group that does not contain an alkenyl group. a, b, c, d, e, f, and g are independently numbers of 0 or more, where 0 ≤ a, 0 ≤ b, 2 ≤ a + b, 3 ≤ c, 50 ≤ d, 90 ≤ c + d ≤ 400, 0 ≤ e ≤ 8, 3 ≤ b + c + e, 0 ≤ f ≤ 8, 0 ≤ g ≤ 8, and 0 ≤ f + g ≤ 8). The release agent composition according to claim 1.
3. The release agent composition according to claim 1, wherein the component (B) is represented by the following average composition formula (2). (R 4 3 SiO 1/2 ). h (R 3 R 4 2 SiO 1/2 ). i (R 3 R 4 SiO). j (R 4 2 SiO). k (R 3 SiO 3/2 ). l (R 4 SiO 3/2 ). m (SiO 4/2 ).n (2) (In the formula, R 3 are each independently an alkenyl group having 2 to 8 carbon atoms, and R 4 are each independently a monovalent hydrocarbon group having 1 to 12 carbon atoms that is not an alkenyl group and is unsubstituted or substituted, provided that at least 80 mol% of all R 4 are methyl groups, and h, i, j, k, l, m, and n are each independently a number of 0 or more, provided that i + j + l > 0, l + m + n > 0, and h + i + j + k + l + m + n = 1).
4. The release agent composition according to claim 1, wherein the component (C) is a linear monoolefin having 10 to 18 carbon atoms or a branched monoolefin having 10 or more carbon atoms.
5. The component (D) is represented by the following average composition formula (3): (R 6 3 SiO 1/2 )(R p R 5 R 6 2 SiO 1/2 )(R q R 5 R 6 SiO)(R r R 6 2 SiO)(R s R 5 SiO 3/2 )(R t R 6 SiO 3/2 )(R u SiO 4/2 )(SiO v (3) (In the formula, R 5 independently represents a hydrogen atom, R 6 independently represents an unsubstituted or substituted monovalent hydrocarbon group other than a hydrogen atom, p, q, r, s, t, u, and v are independently numbers of 0 or more, 0 ≤ p, 0 ≤ q, 0 ≤ p + q, 0 ≤ r, 40 ≤ s, 90 ≤ r + s ≤ 400, 0 ≤ t ≤ 8, 2 ≤ q + r + t, 0 ≤ u ≤ 8, 0 ≤ v ≤ 8, 0 ≤ u + v ≤ 8), and it is a linear or branched organohydrogenpolysiloxane having at least 2 hydrogen atoms bonded to silicon atoms in the side chain in one molecule and having a viscosity at 25°C of 100 mPa·s or more. The release agent composition according to claim 1.
6. The release agent composition according to claim 1, comprising 0 to 20 parts by mass of an organopolysiloxane (F) represented by the following formula, provided that 1 ≦ p ≦ 20, X is a group selected from a methyl group, a methoxy group, and a vinyl group, or gives a cyclic structure with an oxygen atom.
7. The release agent composition according to claim 1, having a viscosity at 25°C of 50 to 1000 mPa·s.
8. The release agent composition according to claim 1, which does not contain a solvent.
9. A release sheet having a sheet-like substrate and a cured film formed by curing the release agent composition according to any one of claims 1 to 8 on one or both surfaces of the substrate surface.
10. The release sheet according to claim 9, wherein a polyester adhesive tape having a width of 25 mm is attached to the cured film, and the peel force measured at an angle of 180° and a peel rate of 0.3 m / min is 3.0 N / 25 mm or more.
Citation Information
Patent Citations
Organopolysiloxane composition
JP1995097520A
Curable siloxane composition with modified surface properties
JP2007523225A
Release modifier, release modifier composition, organopolysiloxane composition for forming releasable cured coating, and sheet-like substrate having releasable cured coating
JP2010037557A
Release modifier composition
JP2017523258A
Oil-in-water silicone emulsion composition for release film, release film, and method for producing the release film, method for adjusting coatability, and peelability in release film
JP2020139040A