Thermosetting composition, curing method for same, prepreg including same, and high-frequency circuit board

The thermosetting composition of reactive branched organopolysiloxanes and aromatic/cycloolefin polymers addresses the brittleness and moldability issues of existing compositions, achieving superior dielectric and thermal performance for high-frequency circuit boards.

WO2024241961A1PCT designated stage expired Publication Date: 2024-11-28DOW TORAY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017763
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-05-14
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Current thermosetting compositions with reactive branched organopolysiloxanes and polyphenylene ether (PPE) resins exhibit excellent dielectric properties and heat resistance but suffer from brittleness and poor moldability, making them unsuitable for high-frequency circuit boards that require both mechanical strength and processability.

Method used

A thermosetting composition comprising reactive branched organopolysiloxanes consisting only of difunctional and trifunctional siloxane units, combined with aromatic polymers and cycloolefin polymers, which includes a thermal radical initiator and an optional organic solvent, to produce a cured product with reduced brittleness and improved moldability, dielectric properties, and high heat resistance.

Benefits of technology

The resulting cured product demonstrates low dielectric constant and loss tangent, high elastic modulus at elevated temperatures, and excellent heat resistance, making it suitable for high-frequency circuit boards and electronic devices, while maintaining good moldability and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

[Problem] To provide: a thermosetting composition that is cured by heating, largely adjustable in terms of physical properties, and gives a cured product having excellent dielectric characteristics, molding processability, heat resistance, and elastic modulus / toughness; and a use thereof. [Solution] A thermosetting composition and a use thereof, the thermosetting composition comprising: (A) a reactive branched organopolysiloxane consisting only of (R2SiO2 / 2) and (RSiO3 / 2) units; (B) an aromatic macromolecule / cycloolefin polymer having a reactive functional group; and (C) a thermal radical initiator.
Need to check novelty before this filing date? Find Prior Art

Description

Thermosetting composition, curing method thereof, prepreg containing same, and high-frequency circuit board

[0001] The present invention relates to a thermosetting composition that can be cured by heating and comprises a specific DT-type siloxane resin having reactive functional groups and an aromatic polymer. The cured product obtained from the thermosetting composition of the present invention has excellent dielectric properties, particularly low relative permittivity and dielectric loss tangent, a high modulus of elasticity at high temperatures, and excellent heat resistance. These excellent properties make the composition suitable for use as a material for next-generation high-frequency circuit boards and as a coating material for electrical and electronic devices that require high insulation and heat resistance.

[0002] Due to their high heat resistance and excellent chemical stability, silicone resins have been used as coating agents, potting agents, insulating materials, etc. for electronic and electrical devices. Among silicone resins, many thermosetting silicone compositions containing reactive branched organopolysiloxanes have been reported.

[0003] In recent years, remarkable advances in information network technology have made it necessary to transmit large volumes of information at high speed while maintaining high quality, necessitating faster processing speeds for electronic devices. In addition to the already introduced 5G (fifth-generation mobile communication system) technology, in anticipation of future 6G technology, digital signals are becoming shorter in wavelength and higher in frequency to transmit large volumes of signals at high speed. Because signal degradation due to dielectric loss is significant in these high-frequency ranges, it is necessary to reduce the dielectric loss of insulating materials. Numerous resin materials with lower dielectric loss have been proposed as alternatives to epoxy resins, which are currently the primary choice. Among these, polyphenylene ether (PPE) resins have been widely considered as insulating materials for circuit boards of electrical and electronic devices that use high frequencies due to their excellent dielectric properties, such as dielectric constant and dielectric loss tangent, and their high heat resistance. (See, for example, Patent Documents 1 to 3.)

[0004] Compositions in which a reactive branched organopolysiloxane is added to a PPE resin have also been investigated. Patent Document 4 discloses a thermosetting composition comprising a reactive branched organopolysiloxane consisting only of trifunctional siloxane units (T units) and tetrafunctional siloxane units (Q units) and a PPE, while Patent Document 5 discloses a thermosetting composition comprising a reactive branched organopolysiloxane containing monofunctional siloxane units (M units) as an essential component and a PPE.

[0005] The cured products obtained from all of these compositions have excellent dielectric properties such as dielectric loss tangent and heat resistance. However, these cured products have characteristics such as high brittleness or low hardness, which poses problems in moldability.

[0006] That is, although cured products comprising reactive branched organopolysiloxanes and PPEs and having excellent dielectric properties and heat resistance have been disclosed, it is difficult to say that thermosetting compositions and cured products thereof that satisfy both hardness and moldability requirements have been adequately disclosed.

[0007] Japanese Patent Application Laid-Open No. 2015-44934 No. WO2019-130735 No. 2021-31612 No. WO2017-67123 No. WO2017-67124

[0008] The present invention has been made to solve the above-mentioned problems, and provides a thermosetting composition which, when heated, gives a cured product having excellent dielectric properties, in particular low relative dielectric constant and dielectric dissipation factor, and excellent heat resistance, and which also has good moldability, and uses thereof.

[0009] The present invention was made to solve the above-mentioned problems, and was completed based on the discovery that a thermosetting composition containing a reactive branched organopolysiloxane consisting only of difunctional siloxane units (D units) and trifunctional siloxane units (T units), and at least one compound selected from an aromatic polymer having a reactive functional group and a cycloolefin polymer having a reactive functional group, gives a cured product that has low dielectric properties, particularly low relative dielectric constant and dielectric dissipation factor, and excellent heat resistance, and furthermore, the brittleness of the cured product is significantly suppressed, thereby simultaneously satisfying good moldability of the curable composition.

[0010] The aromatic polymer having a reactive functional group and the cycloolefin polymer having a reactive functional group according to the present invention are preferably polymers that have a reactive functional group but have a low polar group concentration, excellent heat resistance, and low relative dielectric constant and dielectric loss tangent, and from the viewpoint of technical effect, PPE having a reactive functional group is particularly preferred.

[0011] More specifically, the present invention provides a compound comprising: (A) (R 2 SiO 2/2 ) and (RSiO 3/2 (A) is a reactive branched organopolysiloxane consisting only of 10 to 90 parts by mass of a reactive branched organopolysiloxane consisting only of 10 to 90 parts by mass of a reactive functional group selected from the group consisting of aromatic polymers having reactive functional groups and cycloolefin polymers having reactive functional groups, wherein R is a monovalent substituent not containing silicon atoms and has a reactive functional group containing at least one carbon-carbon double bond in the molecule; (B) 10 to 90 parts by mass of at least one compound selected from the group consisting of aromatic polymers having reactive functional groups and cycloolefin polymers having reactive functional groups, wherein the sum of components (A) and (B) is 100 parts by mass; and (C) a thermal radical initiator in an amount of 0.1 to 5 parts by mass per 100 parts by mass of the sum of components (A) and (B).

[0012] The component (B) may be a PPE having a reactive functional group at the molecular chain end.

[0013] The component (B) may be a PPE having at least one reactive functional group selected from an alkenyl group and a (meth)acrylate group at the molecular chain terminal.

[0014] The component (A) has at least one reactive functional group selected from an alkenyl group and a (meth)acrylate group in the molecule, and (R 2 SiO 2/2 ) and (RSiO 3/2 Preferably, the reactive branched organopolysiloxane is a reactive branched organopolysiloxane consisting solely of R) units (wherein R is a group as defined above).

[0015] The component (A) has at least one reactive functional group selected from an alkenyl group and a (meth)acrylate group in the molecule, and at least one aromatic hydrocarbon group having 6 to 10 carbon atoms in the molecule, and (R 2 SiO 2/2 ) and (RSiO 3/2 Preferably, the reactive branched organopolysiloxane is a reactive branched organopolysiloxane consisting solely of R) units (wherein R is a group as defined above).

[0016] The thermosetting composition of the present invention may further contain (D) an organic solvent. The content of component (D) may be in the range of 10 to 1000 parts by mass per 100 parts by mass of the total of components (A), (B), and (C).

[0017] The component (A) is preferably a reactive branched organopolysiloxane represented by the following formula (1): (R 1 R 2 SiO 2 / 2 ) a (R 3 SiO 3 / 2 ) b (1) (wherein, R 1 is a group represented by the following formula (2), and R 2 is an unsubstituted or fluorine-substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and R 3 is R 1 , R 2 a, an alkoxy group, and a hydroxyl group, and a and b are numbers that satisfy the following conditions: 0<a, 0<b, a+b=1, 0.05≦a / (a+b)≦0.8, and at least one R 1 and at least one aromatic hydrocarbon group having 6 to 10 carbon atoms.) X—(CH2) y -* (2) (wherein y is a number of 0 or more and 6 or less, X is one or more reactive functional groups selected from a vinyl group and a (meth)acrylate group, and * is a bonding site with silicon.)

[0018] In the reactive branched organopolysiloxane represented by the formula (1), 3 may be an aromatic hydrocarbon group having 6 to 10 carbon atoms.

[0019] In the reactive branched organopolysiloxane represented by the above formula (1), X may be a vinyl group.

[0020] The reactive branched organopolysiloxane represented by the above formula (1) preferably has an average of two or more X groups per molecule.

[0021] The present invention further provides a cured product of the above-mentioned thermosetting composition. Also, the present invention provides a prepreg containing the above-mentioned cured product of the thermosetting composition and a fibrous reinforcing material.

[0022] The present invention further provides a high-frequency circuit board comprising a laminate of one or more sheets of the above prepreg.

[0023] The present invention further provides a method for curing and molding a thermosetting composition, comprising at least the following steps: step (i): removing component (D) from a thermosetting composition containing component (D) at a temperature in the range of about 80-100°C under atmospheric pressure or reduced pressure; and step (ii): subsequent to step (i), curing the thermosetting composition at a temperature of 150°C or higher and processing it into a desired shape.

[0024] The present invention further provides a method for producing a prepreg, which comprises impregnating a fibrous reinforcing material with a thermosetting composition containing the above-mentioned component (D), and then removing component (D) to cure the thermosetting composition.

[0025] The thermosetting composition of the present invention contains, as its main components, a reactive branched organopolysiloxane composed solely of difunctional siloxane units (D units) and trifunctional siloxane units (T units), and at least one compound selected from an aromatic polymer having a reactive functional group and a cycloolefin polymer having a reactive functional group. Because the two components have good affinity with each other, the curable composition and the heat-cured product exhibit good transparency upon removal of the organic solvent. Furthermore, the brittleness of the cured product is significantly reduced, thereby simultaneously achieving good moldability of the thermosetting composition of the present invention. Meanwhile, the cured product obtained by the present invention exhibits good heat resistance and a very high modulus of elasticity even at high temperatures of 200°C or higher. Furthermore, the cured product obtained by the present invention has low relative permittivity and dielectric loss tangent, exhibiting excellent dielectric properties. Therefore, the thermosetting composition of the present invention is useful as an insulating material for circuit boards in devices for transmitting digital signals at high speed and large capacity, particularly in electric and electronic devices that use high frequencies.

[0026] The thermosetting composition of the present invention will be described in more detail below. The thermosetting composition of the present invention has (A) a reactive functional group containing at least one carbon-carbon double bond in the molecule, and (R 2 SiO 2/2 ) and (RSi 3/2 The composition comprises, as essential components, (A) a reactive branched organopolysiloxane consisting only of (B) units (wherein R is a monovalent substituent not containing a silicon atom), (B) at least one compound selected from aromatic polymers having reactive functional groups and cycloolefin polymers having reactive functional groups, and (C) a thermal radical initiator, and optionally (D) an organic solvent.

[0027] [Component (A)] Component (A) has a reactive functional group containing at least one carbon-carbon double bond in the molecule, (R 2 SiO 2/2 ) and (RSiO 3/2The branched structure of the organosiloxane is a reactive branched organopolysiloxane consisting only of (R) units (wherein R is a monovalent substituent that does not contain a silicon atom). The branched structure increases the mechanical strength of the cured product and reduces the dielectric constant. 2 SiO 2/2 The siloxane unit represented by (RSiO 3/2 ) are sometimes called "T units," and organopolysiloxanes composed only of these siloxane units are sometimes called "DT-type siloxane resins." Component (A) must be composed only of D units and T units; organopolysiloxanes that do not contain D units, for example, those that are composed only of T units, may result in poor moldability of the resulting cured product. Furthermore, trifunctional (R 3 SiO 1/2 ) and siloxane units (M units) represented by SiO 4/2 When the siloxane unit (Q unit) represented by the formula (I) is contained, the heat resistance may decrease, and the compatibility with other components and mechanical strength (particularly elastic modulus and toughness) may decrease.

[0028] In the formula, R is a monovalent substituent that does not contain a silicon atom and is a monovalent organic group, an alkoxy group, or a hydroxyl group that may contain a heteroatom other than a silicon atom selected from oxygen (O), nitrogen (N), and a halogen atom, and is preferably a monovalent hydrocarbon group, an alkoxy group, or a hydroxyl group that may contain a heteroatom selected from oxygen (O), nitrogen (N), and a halogen atom. Specifically, the monovalent substituent represented by R includes reactive functional groups containing a carbon-carbon double bond, such as alkenyl groups and (meth)acrylate groups; unsubstituted or halogen-substituted alkyl, cycloalkyl, arylalkyl, and aryl groups; and an alkoxy group or a hydroxyl group, and at least one of all R is a reactive functional group containing a carbon-carbon double bond. Furthermore, among all R, monovalent substituents other than reactive functional groups containing a carbon-carbon double bond are preferably aromatic hydrocarbon groups having 6 to 10 carbon atoms, such as methyl groups or phenyl groups, from an industrial perspective. As described below, it is particularly preferred that at least one of all R is an aromatic hydrocarbon group.

[0029] The reactive functional group contained in component (A) is preferably a functional group whose reaction is accelerated by heating, specifically a reactive functional group containing a carbon-carbon double bond. This functional group is preferably one or more groups selected from an alkenyl group and a (meth)acrylate group. Preferred examples of the alkenyl group include aliphatic alkenyl groups having 2 to 8 carbon atoms. Specific examples include vinyl, allyl, 1-butenyl, 1-pentenyl, and 1-hexenyl groups, with vinyl, allyl, and 1-hexenyl groups being particularly preferred. Meanwhile, both acrylate and methacrylate groups are applicable as the (meth)acrylate group. Considering reactivity, acrylate groups are preferred.

[0030] Furthermore, it is preferable that component (A) has at least one aromatic hydrocarbon group having 6 to 10 carbon atoms in the molecule. The presence of this functional group improves affinity with component (B), contributing to improved moldability of the thermosetting composition of the present invention and improved mechanical strength of the cured product derived therefrom. The aromatic hydrocarbon group having 6 to 10 carbon atoms that can be used here is preferably a monovalent group, and specific examples include phenyl, tolyl, ethylphenyl, and naphthyl groups, with phenyl being particularly preferred.

[0031] The component (A) can be a reactive branched organopolysiloxane represented by the following formula (1): (R 1 R 2 SiO 2 / 2 ) a (R 3 SiO 3 / 2 ) b (1) (wherein, R 1 is a group represented by the following formula (2), and R 2 is an unsubstituted or fluorine-substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and R 3 is R 1 , R 2 a, an alkoxy group, and a hydroxyl group, and a and b are numbers that satisfy the following conditions: 0<a, 0<b, a+b=1, 0.05≦a / (a+b)≦0.8, and at least one R 1 and at least one aromatic hydrocarbon group having 6 to 10 carbon atoms.) X—(CH2) y -* (2) (wherein y is a number of 0 or more and 6 or less, X is one or more reactive functional groups selected from a vinyl group and a (meth)acrylate group, and * is a bonding site with silicon.)

[0032] The (meth)acrylate group represented by X in the above formula (2) is represented by the following formula (3). (3) (wherein, R 4 is a hydrogen atom or a methyl group, and ** is the linking group (CH2) yis a bonding site with the divalent linking group.) Furthermore, y, which defines the divalent linking group, is a number of 0 to 6, preferably 0 to 4, and more preferably 0, 3, and 4. That is, preferred examples of reactive functional groups in the reactive branched organopolysiloxane of component (A) include vinyl groups, 1-hexenyl groups, methacryloxypropyl groups, and acryloxypropyl groups. Of these, from the standpoint of being able to design a cured product that exhibits a low dielectric dissipation factor, vinyl groups and 1-hexenyl groups are particularly preferred reactive functional groups.

[0033] On the other hand, the substituent R 2 is an unsubstituted or fluorine-substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, preferably a group selected from unsubstituted or fluorine-substituted alkyl, cycloalkyl, arylalkyl, and aryl groups having 1 to 10 carbon atoms. Examples of the alkyl group include methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, sec-butyl, pentyl, hexyl, and octyl, with methyl and hexyl being particularly preferred. Examples of the cycloalkyl group include cyclopentyl and cyclohexyl. Examples of the arylalkyl group include benzyl and phenylethyl. Examples of the aryl group include phenyl and naphthyl. Examples of the fluorine-substituted monovalent hydrocarbon group include 3,3,3-trifluoropropyl and 3,3,4,4,5,5,6,6,6-nonafluorohexyl, with 3,3,3-trifluoropropyl being preferred.

[0034] In addition, the substituent R 3 is R 1 , R 2 The substituent R is a group selected from an alkoxy group, an alkoxy group, and a hydroxyl group. Examples of the alkoxy group include a methoxy group, an ethoxy group, and a propoxy group. 3 is R 2 , an alkoxy group, and a hydroxyl group; 2Among these, aromatic hydrocarbon groups having 6 to 10 carbon atoms are particularly preferred from the viewpoint of the mechanical properties of the cured product obtained by heat curing the composition of the present invention.

[0035] Specific examples of the reactive branched organopolysiloxane, component (A) of the present invention, include polysiloxanes composed of the following combinations of siloxy units: where D is a dimethylsiloxy unit; Vi is a methylvinylsiloxy unit, D Hex is a methylhexenylsiloxy unit, D A is RMeSiO 2/2 a methylacryloxyalkylsiloxy unit represented by the formula: D MA is RMeSiO 2/2 T is a methylsiloxy unit, T Ph is a phenylsiloxy unit, T Vi is a vinylsiloxy unit, T Hex is a hexenylsiloxy unit, T A is RSiO 3/2 an acryloxyalkylsiloxy unit represented by T MA is RSiO 3/2 It should be noted that Me represents a methyl group, and in the examples of combinations below, the specific number of each siloxy unit is omitted.

[0036] Examples of combinations of siloxy units constituting reactive branched organopolysiloxanes: DD Vi T Ph , D.D. Vi T.T. Ph , D Vi T.T. Ph , D Vi T.D. Vi T Ph , D.D. Hex T Ph , D.D. Hex T.T. Ph , D Hex T.T. Ph , D Hex T.D. Hex T Ph , D.D. A TPh , D.D. A T.T. Ph , D A T.T. Ph , D A T.D. A T Ph , D.D. MA T Ph , D.D. MA T.T. Ph , D MA T.T. Ph , D MA T.D. MA T Ph , D.T. Vi , D.T. Hex , D.T. Vi T Ph , D.T. Hex T Ph , D.T. A , D.T. MA , D.T. A T Ph , D.T. MA T Ph

[0037] Among the above examples of combinations, D Vi T Ph , D Hex T Ph , D A T Ph , D MA T Ph The reactive branched organopolysiloxane represented by the following formula can be preferably used.

[0038] In the above formula (1), a and b define the ratio of difunctional siloxane units (D units) and trifunctional siloxane units (T units) in the reactive branched organopolysiloxane. Specifically, the ratio of D units, a / (a+b), preferably satisfies the following condition: 0.05≦a / (a+b)≦0.8. A more preferred range for the ratio of D units is 0.1≦a / (a+b)≦0.5. If the ratio of D units is less than the above-mentioned lower limit, the cured product obtained by heat curing the composition of the present invention may be highly brittle and may have poor curability. On the other hand, if the ratio of D units exceeds the above-mentioned upper limit, the resulting cured product may also be highly brittle.

[0039] Although there are no particular limitations on the molecular weight of the reactive branched organopolysiloxane of the present invention, it is recommended that the weight-average molecular weight, measured by gel permeation chromatography (GPC) in terms of standard polystyrene, be 1,000 to 5,000. In particular, a weight-average molecular weight of 1,000 to 3,000 is particularly desirable. This characteristic allows for the production of a cured product with low brittleness and good mechanical strength upon heat curing.

[0040] The reactive branched organopolysiloxane preferably has an average of 10 to 40, and more preferably 10 to 30, silicon atoms per molecule.

[0041] Furthermore, the reactive branched organopolysiloxane of the present invention has, on average, at least one of the aforementioned reactive functional groups per molecule. From the standpoint of ensuring sufficient reactivity with component (B), which will be described later, it is preferable that the number of reactive functional groups per molecule is, on average, more than one, preferably 2 to 8, and more preferably 2 to 4.

[0042] [Component (B)] Component (B) is at least one compound selected from aromatic polymers having reactive functional groups and cycloolefin polymers having reactive functional groups. This component contributes to improving the heat resistance of the cured product obtained by heat curing of the curable composition, particularly increasing the elastic modulus at high temperatures, and also contributes to reducing the dielectric constant by taking advantage of the characteristics of its low polarity skeleton.

[0043] Component (B) may be an aromatic polymer, a cycloolefin polymer, or a mixture thereof, as long as it has a reactive functional group. That is, component (B) may be a single compound or a mixture of multiple compounds, and when used in combination with component (A), it can improve the physical properties of the cured product, reduce the dielectric constant, and impart low dielectric properties. Note that component (B) having an aromatic polymer skeleton and component (B) having a cycloolefin polymer skeleton can be appropriately selected depending on the application, physical properties, and desired dielectric constant of the cured product. In a preferred embodiment of the present invention, a mixture ratio of components (B) having different skeletons can be adjusted to achieve the desired properties.

[0044] [Aromatic Polymer Having Reactive Functional Group] While there are no limitations on the location of the reactive functional group in the aromatic polymer having a reactive functional group (component (B)), from the viewpoint of good reaction control, an aromatic polymer having a reactive functional group at the molecular chain end is preferred. Here, the term "aromatic polymer" refers to a polymer whose main chain is composed of aryl groups and heteroatom-containing groups connecting them, specifically linking groups such as ether groups, thioether groups, ester groups, thioester groups, amide groups, imide groups, urethane groups, thiourethane groups, urea groups, thiourea groups, and acid anhydride groups. Among these linking groups, the lower the polarity, the more preferable it is for reducing the dielectric constant. Therefore, ether bonds are the recommended linking group. That is, preferred component (B) includes polymers having aryl groups and ether bonds as main structural units, with polyphenylene ether (PPE) being the preferred polymer. In particular, PPE having a reactive functional group at the molecular chain end is a particularly preferred polymer.

[0045] Here, the PPE is formed from repeating units consisting of phenylene groups and ether bonds, but may contain copolymerization component units other than the phenylene ether unit structure, as long as the functions and effects of the present invention are not impaired. Specifically, PPE having a substituent, such as poly(2,6-dimethyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2-methyl-6-phenyl-1,4-phenylene ether), or poly(2,6-dichloro-1,4-phenylene ether), as well as PPE copolymers such as copolymers of 2,6-dimethylphenol and other phenols (e.g., 2,3,6-trimethylphenol, 2-methyl-6-butylphenol, etc.), and PPE copolymers obtained by coupling 2,6-dimethylphenol with biphenols or bisphenols, can also be used as component (B) of the present invention.

[0046] The reactive functional group of the aforementioned component (B) is preferably a functional group whose reaction is accelerated by heating, as with component (A), and specifically, is preferably one or more functional groups selected from an alkenyl group and a (meth)acrylate group. Preferred examples of the alkenyl group include alkenyl groups having 2 to 8 carbon atoms. Specific examples include vinyl groups, allyl groups, 1-butenyl groups, 1-pentenyl groups, 1-hexenyl groups, and styryl groups, with vinyl groups, allyl groups, and styryl groups being particularly preferred. Meanwhile, both acrylate groups and methacrylate groups are applicable as the (meth)acrylate group. Considering reactivity, acrylate groups are more preferred.

[0047] That is, in the present invention, recommended component (B) includes PPE having vinyl groups at both molecular chain terminals, PPE having a vinyl group at one molecular chain terminal, PPE having allyl groups at both molecular chain terminals, PPE having an allyl group at one molecular chain terminal, PPE having a styryl group at both molecular chain terminals, PPE having a styryl group at one molecular chain terminal, PPE having an acrylate group at both molecular chain terminals, PPE having an acrylate group at one molecular chain terminal, PPE having a methacrylate group at both molecular chain terminals, and PPE having a methacrylate group at one molecular chain terminal. Among these, PPE having reactive functional groups at both molecular chain terminals is preferred, and specifically, PPE having styryl groups at both molecular chain terminals, PPE having acrylate groups at both molecular chain terminals, and PPE having methacrylate groups at both molecular chain terminals are preferred component (B). As component (B), a widely used methacrylate-terminated PPE (product name: SA9000) manufactured by Sabic Innovative Plastics can also be used.

[0048] The molecular weight of the aromatic polymer having a reactive functional group, component (B), is not particularly limited, but it is recommended that the weight-average molecular weight, measured by gel permeation chromatography (GPC) in terms of standard polystyrene, be 1,000 to 5,000. A weight-average molecular weight of 1,000 to 3,000 is particularly desirable. This characteristic allows for the production of a cured product with low brittleness and good mechanical strength upon heat curing.

[0049] [Cycloolefin Polymer Having Reactive Functional Group] Component (B) may be a polymer having a cycloolefin ring structure as its basic skeleton, and a portion or all of the polymer may be a cycloolefin polymer having a reactive functional group. Specifically, the cycloolefin polymer of component (B) is a (co)polymer having, as an essential structural unit, a repeating unit derived from a cycloolefin having the reactive functional group in the molecule. The cycloolefin monomer (cyclic olefin compound) constituting the cycloolefin polymer (B) usable in the present invention is not particularly limited, and is a compound having a polymerizable carbon-carbon double bond capable of chain polymerization (metathesis ring-opening polymerization, addition polymerization, etc.) and having an alicyclic structure such as a monocyclic ring, a polycyclic ring, a fused polycyclic ring, a bridged ring, or a polycyclic ring formed by combining these. The cycloolefin monomer constituting component (B) of the present invention may be the cyclic olefin monomer described in paragraphs 0037 to 0063 of WO 2006 / 0118261. In addition, the cycloolefin polymers that can be used in the present invention include those disclosed in JP 2015-067671, JP 2014-162172, JP 2015-160326, JP 2015-123671, JP 2015-123670, JP 2014-205727, JP 2014-177568, JP 2018-034422, JP 2018-035257, JP 2017-125176, JP 2017-125175, JP 2017-125174, etc., and can be used without particular limitation. Cycloolefin polymers obtained by the structures, monomers, and synthesis examples disclosed in these documents can be used as part or all of component (B) of the present invention.

[0050] Component (B) may contain an aromatic polymer having a reactive functional group and a cycloolefin polymer having a reactive functional group in a mixing ratio of 100:0 to 0:100. For example, component (B) that is a cycloolefin polymer may be selected from the viewpoint of further improving the dielectric properties while maintaining good heat resistance and thermal stability of the resulting cured product, prepreg, or printed wiring board, or improving the impregnation of a sheet-like fiber substrate or the like with the curable resin composition when producing a prepreg. Alternatively, component (B) that is an aromatic polymer, such as polyphenylene ether (PPE) having a reactive functional group at the molecular chain end, may be selected from the viewpoint of the mechanical properties and low dielectric constant of the cured product.

[0051] The mixing ratio (parts by mass) of component (A) to component (B) in the thermosetting composition of the present invention is in the range of 10 to 90 parts by mass of (A) to 10 to 90 parts by mass of (B), where the sum of components (A) and (B) is 100 parts by mass. This mixing ratio significantly affects the properties of the cured product, so it is preferable to design it within this range depending on the intended use of the cured product. Specifically, increasing the component (A) / component (B) ratio tends to decrease the relative dielectric constant and dielectric loss tangent. Meanwhile, mechanical properties, particularly the modulus of elasticity at high temperatures, tend to increase by increasing the component (A) / component (B) ratio, although this depends on the type and content of reactive functional groups in component (A). Therefore, by adjusting this mixing ratio, the mechanical properties and dielectric properties of the resulting cured product can be tuned to the desired range.

[0052] [Use of Other Organic Resins in Combination] While the main components in the thermosetting composition of the present invention are components (A) and (B), reactive organic resins other than component (B) can be used in combination as long as the technical effects of the present invention are not impaired. For example, in the present invention, component (B) can be used in combination with one or more organic resins (B') selected from epoxy resins, polyimide resins, liquid crystal polymers, maleimide resins (including so-called BT resins), and polybutadiene resins. Since these organic resins are optional components, their amounts are not particularly limited. However, one or more organic resins may be used in an amount of 0 to 500 parts by weight, 0 to 250 parts by weight, or 0 to 100 parts by weight per 100 parts by weight of component (B), and this is preferred. Furthermore, in order to improve the compatibility of these organic resins with component (A) and component (B), a compatibilizer (B") selected from modified polyolefins, modified elastomers, compounds having a polar group and an unsaturated carbon bond capable of contributing to a polymerization reaction in the molecule, and the like may be contained.

[0053] The epoxy resin may be one or more selected from glycidyl ether epoxy resins such as phenol novolac epoxy resins, cresol novolac epoxy resins, bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol A novolac epoxy resins, bisphenol F novolac epoxy resins, brominated bisphenol A epoxy resins, brominated bisphenol F epoxy resins, and hydrogenated bisphenol A epoxy resins, alicyclic epoxy resins, glycidyl ester epoxy resins, glycidyl amine epoxy resins, isocyanurate epoxy resins, and epoxy resins having an alicyclic olefin structure or a fluorene structure. From the viewpoint of further improving the mechanical strength of the resulting cured product, at least one selected from bisphenol A epoxy resins and bisphenol A novolac epoxy resins may be selected.

[0054] Examples of polyimide resins include those described in paragraphs 0008 to 0011 of JP 2009-120696 A, and can be obtained by reacting a tetracarboxylic acid anhydride, diimide, or monoimide (hereinafter abbreviated as tetracarboxylic acid anhydride, etc.) with a diamine. The reaction of a tetracarboxylic acid anhydride, etc. with a diamine can be carried out using a generally known method, and commercially available products can also be used. The polyimide resin may be a linear polyimide.

[0055] The liquid crystal polymer is not particularly limited, but examples thereof include those described in paragraphs 0023 to 0029 of JP 2008-19400 A, which are melt-processable polymers capable of forming an optically anisotropic molten phase. The type of liquid crystal polymer is not particularly limited, but is preferably an aromatic polyester or an aromatic polyester amide, and may be a polyester partially containing an aromatic polyester or an aromatic polyester amide in the same molecular chain.

[0056] The maleimide resin is not particularly limited, but examples thereof include those described in paragraphs 0009 to 0013 of JP-A No. 2006-124494, which are maleimide resins obtained from a maleimide compound (X) having two or more maleimide groups in the molecule. The scope of maleimide resins also includes a mixture of the maleimide compound (X) and a triazine resin obtained by reacting a cyanate ester compound (Y) with the maleimide compound (X) (bismaleimide triazine resin (BT resin)).

[0057] Examples of the maleimide compound (X) include bis(4-maleimidophenyl)methane, 2,2-bis{4-(4-maleimidophenoxy)-phenyl}propane, bis(3,5-dimethyl-4-maleimidophenyl)methane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, bis(3,5-diethyl-4-maleimidophenyl)methane, 2,2'-bis[4-(4-maleimidophenoxy)phenyl]propane, polyphenylmethane maleimide, m-phenylene bismaleimide, p-phenylene bismaleimide, 3,3'-dimethyl- Examples of suitable bismaleimides include 5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 4,4'-diphenylether bismaleimide, 4,4'-diphenylsulfone bismaleimide, 1,3-bis(3-maleimidophenoxy)benzene, 1,3-bis(4-maleimidophenoxy)benzene, 1,6'-bismaleimido-(2,2,4-trimethyl)hexane, 1,2-bismaleimidoethane, 1,6-bismaleimidohexane, and polytetramethylene oxide-bis(4-maleimidobenzoate).

[0058] The cyanate ester compound (Y) is not particularly limited as long as it is a cyanate ester compound having two or more cyanate groups in one molecule, and examples thereof include 1,3- or 1,4-dicyanate benzene, 1,3,5-tricyanate benzene, 1,3-, 1,4-, 1,6-, 1,8-, 2,6- or 2,7-dicyanate naphthalene, 1,3,6-tricyanate naphthalene, 4,4-dicyanate biphenyl, bis(4-cyanate phenyl)methane, bis(3,5-dimethyl-4-cyanate phenyl)methane, 2,2-bis(4-cyanate phenyl)propane, 2,2-bis(3,5-dibromo-4-cyanate phenyl)propane, 2,2-bis(3, Examples of the cyanate ester compound include cyanate ester compounds obtained by reacting cyanogen halide with cyanogen halide and 5-dimethyl-4-cyanatephenyl)propane, bis(4-cyanatephenyl)ether, bis(4-cyanatephenyl)thioether, bis(4-cyanatephenyl)sulfone, tris(4-cyanatephenyl)phosphite, tris(4-cyanatephenyl)phosphate, oligomers (novolak, hydroxyl group-containing thermoplastic resins (hydroxypolyphenylene ether, hydroxypolystyrene, hydroxypolycarbonate, etc.)), and the like; and cyanate ester compounds obtained by reacting cyanogen halide with a polyfunctional phenol in which phenol is bonded via dicyclopentadiene.

[0059] The polybutadiene resin is not particularly limited, and examples thereof include 1,4-polybutadiene, 1,2-polybutadiene, terminal acrylate-modified polybutadiene, and terminal urethane methacrylate-modified polybutadiene.

[0060] [Component (C)] Component (C) is a thermal radical initiator that functions as a catalyst to accelerate the curing reaction by heating. Any compound that decomposes upon heating to generate free radical species can be used as component (C) of the present invention, regardless of its chemical structure. Typically, organic peroxides that decompose to generate oxygen radicals and azo compounds that decompose to generate carbon radicals are well known, and either group of compounds can be used alone or in combination of two or more. It is also possible to use an organic peroxide and an azo compound in combination.

[0061] Known organic peroxides are broadly classified according to their chemical structure into (I) diacyl peroxides, (II) peroxydicarbonates, (III) peroxyesters, (IV) peroxyketals, (V) dialkyl peroxides, (VI) hydroperoxides, and (VII) others. Specific examples of compounds classified as (I) include dibenzoyl peroxide and dilauroyl peroxide, compounds classified as (II) include di(2-ethylhexyl)peroxydicarbonate, compounds classified as (III) include tert-butyl peroxyacetate and tert-butyl peroxylaurate, compounds classified as (IV) include 1,1-di(tert-butylperoxy)cyclohexane and normal butyl-4,4-(tert-butylperoxy)valerate, compounds classified as (V) include dicumyl peroxide, di-tert-butyl peroxide and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, and compounds classified as (VI) include cumene hydroperoxide, diisopropylbenzene hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide and di-tert-butyl hydroperoxide, but are not limited to these.

[0062] Known azo compounds are broadly classified into (I) azonitriles, (II) azoesters, (III) azoamides, and (IV) others, depending on their chemical structure. Specific examples of compounds classified into (I) include 2,2-azobis(2-methylbutyronitrile), 1,1-azobis(cyclohexane-1-carbonitrile), and 2,2-azobis(isobutyronitrile). Examples of compounds classified into (II) include dimethyl-2,2-azobis(isobutyrate). Examples of compounds classified into (III) include 2,2-azobis[N-(2-propenyl)-2-methylpropionamide] and 2,2-azobis(N-butyl-2-methylpropionamide]. Examples of compounds classified into (IV) include 2,2-azobis[2-(2-imidazolin-2-yl)propane], but are not limited to these.

[0063] The activity of the above-mentioned compounds is defined by the half-life temperature associated with decomposition in the temperature range used in the reaction, and is usually 10 hours half-life temperature (T 10h ) and 1-minute half-life temperature (T 1m In the present invention, taking into consideration the temperature range when the thermosetting composition described later is cured, T 10h is 110°C or higher and T 1m It is preferable to use as component (C) a compound that satisfies at least one of the conditions that the temperature of the component (C) is 170° C. or higher. When two or more compounds are used in combination, it is preferable that at least one of them satisfies this condition.

[0064] In view of the above conditions, it is desirable that component (C) of the present invention contains at least one compound selected from the group of compounds broadly classified as dialkyl peroxides and hydroperoxides. Specific examples of compounds that are preferably used include dicumyl peroxide, ditertiary butyl peroxide, 2,5-dimethyl-2,5-di(tertiary butylperoxy)hexyne-3, di(2-tertiary butylperoxyisopropyl)benzene, cumene hydroperoxide, diisopropylbenzene hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, ditertiary butyl hydroperoxide, and paramenthane hydroperoxide.

[0065] The content of component (C) in the present invention is an amount that is 0.1 to 5 parts by mass per 100 parts by mass of the total of the above components (A) and (B). A preferred content is 0.1 to 3 parts by mass, and more preferably 0.3 to 1 part by mass. If the content of this component is less than 0.1 part by mass, the time required for the curing reaction of the thermosetting composition described below will be longer, and there is a concern that the degree of cure in the cured product will be non-uniform. On the other hand, if the content exceeds 5 parts by mass, there is a high possibility that component (C) will remain even after the curing reaction is complete, which will have an adverse effect on the heat resistance, mechanical properties, etc. of the cured product.

[0066] [Component (D)] Component (D) is an organic solvent that serves as an auxiliary for mixing components (A), (B), and (C) to prepare a uniform curable composition. By removing component (D) from the system after mixing the raw materials constituting the curable composition, a uniform and highly transparent composition can be prepared. In addition to the above-mentioned purpose, component (D) also functions to adjust the film thickness of the coating film derived from the curable composition. While this component is an optional component, considering the above-mentioned function, it is practically desirable to use it at the stage of mixing the various components. As such an organic solvent, any organic solvent that has conventionally been blended in various organopolysiloxane-based curable compositions can be used without particular limitation.

[0067] Suitable examples of the organic solvent include (poly)alkylene glycol monoalkyl ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-propyl ether, diethylene glycol mono-n-butyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-n-butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, and dipropylene glycol mono-n-butyl ether; (Poly)alkylene glycol monoalkyl ether acetates such as methyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate (PGMEA), and propylene glycol monoethyl ether acetate; other ethers such as diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, and diethylene glycol diethyl ether; ketones such as methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, 2-heptanone, 3-heptanone, 4-heptanone, 5-methyl-3-heptanone, 2,4-dimethyl-3-pentanone, and 2,6-dimethyl-4-heptanone; alkyl lactate esters such as methyl 2-hydroxypropionate and ethyl 2-hydroxypropionate;Ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutylpropionate, ethyl acetate, n-propyl acetate, i-propyl acetate, n-butyl acetate, i-butyl acetate, n-pentyl formate, i-pentyl acetate, n-butyl propionate, butyric acid Other esters such as ethyl butyrate, n-propyl butyrate, i-propyl butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, and ethyl 2-oxobutanoate; aromatic hydrocarbons such as toluene, xylene, mesitylene, cumene, propylbenzene, diethylbenzene, and 1,3-diisopropylbenzene; and aromatic ethers such as anisole, phenetole, 2-methoxytoluene, 3-methoxytoluene, 4-methoxytoluene, 3,4-dimethoxytoluene, and 1,4-bis(methoxymethyl)benzene. Component (D) may be used alone, or multiple components (D) may be used in combination, taking into consideration the miscibility with components (A) to (C).

[0068] The content of component (D) is 0 to 1,000 parts by mass per 100 parts by mass of the total of components (A), (B), and (C) of the present invention. That is, component (D) does not have to be included in the present thermosetting composition, but it is preferable to include this component in order to efficiently prepare a uniform and transparent curable composition. The amount used may be 10 to 1,000 parts by mass, and is preferably 10 to 200 parts by mass, per 100 parts by mass of the total of components (A), (B), and (C).

[0069] [Other Additives] The thermosetting composition of the present invention may contain, if desired, other additives in addition to the above-described components (A) to (D). Examples of additives include, but are not limited to, those listed below.

[0070] [Crosslinking Agent] The thermosetting composition of the present invention may contain a component capable of chemically reacting with component (B) as a crosslinking agent in order to control the crosslink density and adjust the physical properties, particularly the mechanical properties and dielectric properties, of the resulting cured product, or to adjust the efficiency of the curing reaction. Suitable examples of such a component include silicon-containing compounds and non-silicon-containing compounds, but silicon-containing compounds are preferred in terms of their affinity with component (A) and the heat resistance of the resulting cured product. More specifically, silicon-containing compounds having multiple reactive functional groups, such as those found in component (A), are preferred, and silicon-containing compounds having multiple reactive functional groups, such as one or more selected from alkenyl groups and (meth)acrylate groups, can be used.

[0071] Examples of silicon-containing compounds suitable for use as crosslinking agents include tetramethyl-tetravinyl-cyclotetrasiloxane, tetrakis(dimethylvinylsiloxy)silane, polymethylvinylsiloxane terminated at both ends with trimethylsilyl, copolymer of trimethylsilyl-dimethyl / methylvinylsiloxane terminated at both ends with dimethylvinylsilyl-dimethyl / methylvinylsiloxane, copolymer of dimethylvinylsilyl-dimethyl / methylvinylsiloxane terminated at both ends with 1,3-dimethyl-1,3-divinyl-1,3-diphenyldisiloxane, 1,5-divinyl-3,3-diphenyl-1,1,5,5-tetramethyltrisiloxane, copolymer of trimethylsilyl-methylphenyl / methylvinylsiloxane terminated at both ends with dimethylvinylsilyl-polymethylphenylsiloxane, copolymer of dimethylvinylsilyl-dimethyl / diphenylsiloxane terminated at both ends with dimethylvinylsilyl, etc. These compounds can be used alone or in combination of two or more types.

[0072] There are no significant limitations on the amount of crosslinking agent added to the thermosetting composition of the present invention, but it is preferably in the range of 1 to 100 parts by mass, 1 to 50 parts by mass, or 1 to 10 parts by mass relative to 100 parts by mass of component (A).

[0073] [Adhesion Imparting Agent] An adhesion imparting agent can be added to the thermosetting composition of the present invention in order to improve the adhesion or adhesion to a substrate in contact with the composition. When the curable composition of the present invention is used for applications requiring adhesion or adhesion to a substrate, such as a coating agent or a sealant, it is preferable to add an adhesion imparting agent to the thermosetting composition of the present invention. Any known adhesion imparting agent can be used as this adhesion imparting agent, as long as it does not inhibit the curing reaction of the composition of the present invention.

[0074] Examples of adhesion promoters that can be used in the present invention include organosilanes having a trialkoxysiloxy group (e.g., trimethoxysiloxy group, triethoxysiloxy group) or a trialkoxysilylalkyl group (e.g., trimethoxysilylethyl group, triethoxysilylethyl group) and a hydrosilyl group or an alkenyl group (e.g., vinyl group, allyl group), or organosiloxane oligomers having a linear, branched or cyclic structure and about 4 to 20 silicon atoms; organosilanes having a trialkoxysiloxy group or a trialkoxysilylalkyl group and a methacryloxyalkyl group (e.g., 3-methacryloxypropyl group), Silanes or organosiloxane oligomers having a linear, branched, or cyclic structure and having about 4 to 20 silicon atoms; organosilanes or organosiloxane oligomers having a linear, branched, or cyclic structure and having about 4 to 20 silicon atoms, each having a trialkoxysiloxy group or trialkoxysilylalkyl group and an epoxy group-bonded alkyl group (e.g., 3-glycidoxypropyl group, 4-glycidoxybutyl group, 2-(3,4-epoxycyclohexyl)ethyl group, 3-(3,4-epoxycyclohexyl)propyl group); organic compounds having two or more trialkoxysilyl groups (e.g., trimethoxysilyl group, triethoxysilyl group);Examples thereof include reaction products of aminoalkyltrialkoxysilanes and epoxy group-bonded alkyltrialkoxysilanes, and epoxy group-containing ethyl polysilicates. Specific examples thereof include vinyltrimethoxysilane, allyltrimethoxysilane, allyltriethoxysilane, hydrogentriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 1,6-bis(trimethoxysilane), silyl)hexane, 1,6-bis(triethoxysilyl)hexane, 1,3-bis[2-(trimethoxysilyl)ethyl]-1,1,3,3-tetramethyldisiloxane, a reaction product of 3-glycidoxypropyltriethoxysilane and 3-aminopropyltriethoxysilane, a condensation reaction product of a silanol group-blocked methylvinylsiloxane oligomer and 3-glycidoxypropyltrimethoxysilane, a condensation reaction product of a silanol group-blocked methylvinylsiloxane oligomer and 3-methacryloxypropyltriethoxysilane, and tris(3-trimethoxysilylpropyl)isocyanurate;

[0075] The amount of adhesion promoter added to the thermosetting composition of the present invention is not particularly limited, but is preferably in the range of 0.01 to 5 parts by mass, or 0.01 to 2 parts by mass, per 100 parts by mass of the total of components (A) to (C), in order not to promote the curing characteristics of the curable composition or discoloration of the cured product.

[0076] [Additional Optional Additives] Other additives may be added to the thermosetting composition of the present invention or its cured product, if desired, in addition to or instead of the crosslinking agent and adhesion promoter described above. Usable additives include flame retardants, heat stabilizers, weather stabilizers, antistatic agents, slip agents, antiblocking agents, antifogging agents, lubricants, dyes, pigments, natural oils, synthetic oils, waxes, organic or inorganic filler leveling agents, silane coupling agents not included in the adhesion promoters listed above, heat absorbers, antioxidants, polymerization inhibitors, fillers (functional fillers such as reinforcing fillers, insulating fillers, and thermally conductive fillers), and fibrous reinforcing materials such as glass cloth. Furthermore, a thixotropic agent may be added to the composition of the present invention, if necessary, especially when used as a sealing material. Furthermore, thermoplastic resins or thermosetting resins other than the above components (A), (B), (B'), and (B'') may be added to the composition to the extent that the object of the present invention is not impaired, and the amount added is appropriate.

[0077] [Method of Molding and Curing Thermosetting Composition] The thermosetting composition of the present invention typically contains component (D), an organic solvent. However, it is desirable that the cured product obtained from this composition does not contain component (D). Therefore, it is preferable to prepare a thermosetting composition containing components (A) to (C) by first preparing a thermosetting composition containing components (A) to (D) and then removing component (D). In other words, it is preferable to mix component (D) with components (A) to (C), and then remove it from the composition after a uniform and transparent composition containing components (A) to (C) is obtained.

[0078] Specifically, a method for molding and curing a thermosetting composition is recommended, which includes at least the following steps (i) and (ii): (i) removing component (D) from the thermosetting composition of the present invention (where the amount of component (D) is not 0 parts by mass) at a temperature in the range of about 80-100°C under normal pressure or reduced pressure; and (ii) curing the thermosetting composition at a temperature of 150°C or higher and processing it into a desired shape following step (i).

[0079] As described above, additives can be added to or impregnated into the thermosetting composition of the present invention as needed. If the prepared composition has sufficient fluidity, it can be molded by applying the composition to a desired substrate or by pouring it into a mold of a desired shape. On the other hand, if the composition does not have sufficient fluidity, it can be processed into the desired shape by a method such as press molding.

[0080] In step (i), the organic solvent (component (D)) is removed from the curable composition molded by the above-described method by a commonly known method. Therefore, the thermosetting composition used in this production method is a composition containing the organic solvent (component (D)).

[0081] The method for removing component (D) in step (i) is not particularly limited. Specific examples of methods for removing component (D) at normal pressure include heating on a hot plate, heating in an oven, and heating in a press. Meanwhile, methods for removing component (D) under reduced pressure include heating in a vacuum oven and heating in a vacuum press. A temperature range of approximately 80-100°C is recommended for this step, and more specifically, a temperature range in which thermal curing of the composition hardly occurs is preferred. While it is desirable for the organic solvent to be completely removed in this step, it is practically acceptable for a small amount of organic solvent (D), for example, 0.1 to 10 parts by mass or less per 100 parts by mass of the total of components (A) to (C), to remain.

[0082] In step (ii), the thermosetting composition prepared above, containing almost no component (D), is thermally cured at a temperature of 150°C or higher while maintaining the desired shape. This step can be performed under normal pressure; however, if step (i) is performed under reduced pressure, the temperature can be raised and step (ii) can be performed under reduced pressure. Furthermore, even if component (D) remains at the end of step (i), step (ii) can be performed under reduced pressure, which is both possible and desirable. Taking into account the glass transition temperature of component (B), a temperature of 150°C or higher is strongly recommended for this step; however, this temperature can be adjusted appropriately, taking into account the half-life temperature of component (C) described above. The time required for step (ii) is typically 1 to 5 hours. Practically, the temperature range may be 150 to 300°C, 150 to 270°C, or 150 to 250°C. Furthermore, the time required for step (ii) (curing time) is typically 1 to 5 hours. During curing, it is possible and preferable to cure in two stages, for example, by changing the temperature conditions from low to high.

[0083] The present invention also encompasses cured products obtained from the thermosetting composition containing the above components (A) to (C).

[0084] [Prepreg] Meanwhile, by impregnating the present thermosetting composition (provided the amount of component (D) is not 0 parts by mass) with a fibrous reinforcing material and then removing component (D), an uncured composition, commonly referred to as a prepreg, containing a reactive branched organopolysiloxane, at least one compound selected from an aromatic polymer having a reactive functional group and a cycloolefin polymer having a reactive functional group, and a fibrous reinforcing material as its main components is obtained. This prepreg is also encompassed by the present invention. The resulting prepreg can be converted into a fibrous reinforcing material-containing cured product by subjecting it to the heat curing process described above. The amount of fibrous reinforcing material is typically 30 to 200 parts by mass, preferably 40 to 150 parts by mass, per 100 parts by mass of the total of components (A) to (C).

[0085] Furthermore, the present invention also encompasses a high-frequency circuit board comprising a laminate in which one or more prepregs prepared by the above-described method are laminated.

[0086] More specifically, the prepreg may be formed by combining the thermosetting composition according to the present invention (provided that the amount of component (D) is not 0 parts by mass) with a sheet-like fiber substrate. The method for producing the prepreg is not particularly limited, and various known methods can be applied. For example, there is a method including a step of impregnating a sheet-like fiber substrate with the thermosetting composition containing component (D) to obtain an impregnated body, and a step of heating the obtained impregnated body to dry the solvent contained in the varnish.

[0087] The impregnation of the sheet-like fiber substrate with the thermosetting composition can be carried out, for example, by applying a thermosetting composition containing a predetermined amount of component (D) to the sheet-like fiber substrate by a known method such as spray coating, dip coating, roll coating, curtain coating, die coating, or slit coating, and then, if necessary, overlaying a protective film thereon and pressing from above with a roller or the like. Furthermore, the process of heating the impregnated body to dry the solvent contained in the thermosetting composition containing component (D) is not particularly limited, but examples include drying in air or nitrogen using a blower dryer in a batch process, or drying by passing through a heating furnace in a continuous process. For example, after impregnating the sheet-like fiber substrate with the thermosetting composition containing component (D), the resulting impregnated body is heated to a predetermined temperature, whereby the solvent contained in the composition (= component (D)) evaporates, and a prepreg is obtained.

[0088] The fibers constituting the sheet-like fiber substrate usable in the prepreg of the present invention are not particularly limited, but examples thereof include organic fibers such as PET (polyethylene terephthalate) fibers, aramid fibers, polyamide (nylon) fibers, and liquid crystal polyester fibers; and inorganic fibers such as glass fibers, carbon fibers, alumina fibers, tungsten fibers, molybdenum fibers, titanium fibers, steel fibers, boron fibers, silicon carbide fibers, and silica fibers. Among these, organic fibers and glass fibers are preferred, with aramid fibers, liquid crystal polyester fibers, and glass fibers being particularly preferred. As glass fibers, fibers such as E-glass, NE-glass, S-glass, D-glass, H-glass, and T-glass can be suitably used.

[0089] The impregnation of the sheet-like fiber substrate with the thermosetting composition containing component (D) is carried out, for example, by immersion and coating. The impregnation process may be repeated multiple times as needed. These sheet-like fiber substrates can be used alone or in combination of two or more. The amount used is selected appropriately as desired, but is typically in the range of 30 to 200 mass%, preferably 40 to 150 mass%, and more preferably 40 to 120 mass% of the prepreg or laminate. This range is advantageous in that the dielectric properties and mechanical strength of the resulting laminate are well balanced.

[0090] The thickness of the prepreg according to the present invention is selected appropriately depending on the intended use, but is usually 0.001 to 10 mm, preferably 0.005 to 1 mm, and more preferably 0.01 to 0.5 mm. This range is suitable because it allows for sufficient shaping during lamination and the mechanical strength, toughness, and other properties of the laminate obtained by curing.

[0091] The prepreg according to the present invention may be formed into a metal-clad laminate by laminating a metal foil on at least one surface thereof and heat-curing the laminate using a lamination press, etc. Examples of the metal foil include copper foil, aluminum foil, nickel foil, gold foil, silver foil, and stainless steel foil.

[0092] [Uses] The thermosetting composition of the present invention is useful as a material for forming insulating layers constituting various articles, particularly electronic and electrical devices, taking advantage of the dielectric properties of the cured product obtained after curing, and is particularly useful as an insulating material for circuit boards of electrical and electronic devices that utilize high frequencies. Furthermore, the thermosetting composition of the present invention can also be used as a composition for insulating coating agents, taking advantage of its excellent coating properties.

[0093] The present invention will be further described below based on examples, but the present invention is not limited to the following examples.

[0094] The preparation and evaluation of the thermosetting composition of the present invention, and the preparation and evaluation of the cured product thereof will be described in detail with reference to examples.

[0095] [Preparation of Thermosetting Composition and Cured Product] A predetermined amount of an aromatic polymer having reactive functional groups and a thermal radical initiator were added to a 50% solids toluene solution of a reactive branched organopolysiloxane to prepare a homogeneous toluene solution of the curable composition. Using a rotary evaporator, more than 90% of the toluene in the solution was removed to prepare a transparent, high-concentration varnish. This was sandwiched between two polyimide films and the toluene was completely removed over 3 hours in a vacuum press set at 100°C. The press was heated to 200°C for 2 hours, then further heated to 220°C for 2 hours, yielding a light brown cured product approximately 0.5 mm thick.

[0096] [Appearance of Thermosetting Composition] The thermosetting composition (the high-concentration varnish) was visually observed, and the appearance including transparency was evaluated.

[0097] [Mechanical properties of cured product: moldability] The practical toughness of the cured product was evaluated using the following three-point scale based on the presence or absence of cracks in the cured product sheet prepared by the above method and its shape retention ability due to stress when peeled from the polyimide (PI) film. A: No cracks were observed, and the shape retention was good when peeled from the PI film. B: Some cracks were observed, and cracks occurred when peeled from the PI film. C: The sheet cracked when peeled from the PI film, making it difficult to prepare a homogeneous test piece.

[0098] [Mechanical Properties of Cured Product: Tensile Modulus and Glass Transition Temperature] A test piece approximately 50 mm long and approximately 5 mm wide was cut out from the cured product sheet prepared by the above method to prepare a test piece for measurement. Using a dynamic viscoelasticity analyzer RSA-G2 manufactured by TA Instrument, dynamic viscoelasticity was measured in tension mode under the following conditions to determine the storage modulus (E': MPa) and glass transition temperature (Tg: C). Measurement conditions: Frequency: 1 Hz, strain: 0.1%, heating rate: 3°C / min

[0099] [Mechanical properties of cured product: elongation at break, strength at break, and toughness] Test pieces similar to those used for dynamic viscoelasticity measurement were prepared from the cured product sheets prepared by the method described above. The test pieces were elongated at 25°C and a tensile speed of 5 mm / min using an Autograph AGS-X manufactured by Shimadzu Corporation, and the elongation at break and strength at break were recorded. Toughness (kJ / m3 ) was calculated by integrating the area under the stress-strain curve for every 0.004% elongation.

[0100] [Dielectric Constant and Dielectric Loss Tangent] A test piece approximately 80 mm long and approximately 1.5 mm wide was cut from the cured product sheet prepared by the above method to prepare a measurement test piece. The measurement test piece was placed in an oven at 80°C and dried for 1 hour. The relative dielectric constant (Dk) and dielectric loss tangent (Df) at 10 GHz were measured by the cavity resonance method using a network analyzer N5222B manufactured by Keysight Technologies and a cavity resonator (CP531) manufactured by Kanto Electronics Application Development Co., Ltd., under an environment of 23°C ± 2°C and a relative humidity of 50 ± 5%.

[0101] [Examples and Comparative Examples] Using the following components, thermosetting compositions having the compositions (parts by mass, excluding toluene as a solvent) shown in Table 1 were prepared. Vi Me 2 (CH 2 =CH)SiO 1/2 Unit, D Hex is Me(CH 2 =CH(CH 2 ) 4 ) SiO 2/2 Unit, D MA is Me(CH 2 =C(CH 3 ) CO 2 (CH 2 ) 3 ) SiO 2/2 Unit, D Vi is Me(CH 2 =C H )SiO 2/2 Unit, D Me Me 2 SiO 2/2 Unit, T Ph is C 6 H 5 SiO 3/2 (A-1): D Hex 0.23 T Ph 0.77 (A-2): D (average number of reactive groups: 6.9) MA 0.19 T Ph 0.81(A-3): D Vi 0.21 T Ph 0.79 (A-4)*: T Vi 0.2 T Ph 0.8 (Average number of reactive groups: 19) (A-5)*:M Vi 0.15 D Me 0.36 T Ph 0.49 (average number of reactive groups: 2.9) (B-1): Polyphenylene ether resin modified with methacrylate at both ends (SABIC, SA9000) (C-1): Di(2-t-butylperoxyisopropyl)benzene (NOF Corporation, Perbutyl P) *(A-4) and (A-5) are main agents for comparative experiments that are not DT-type siloxane resins.

[0102]

[0103] As shown in Table 1, the thermosetting composition of the present invention exhibited high transparency and also exhibited good moldability. It was confirmed that the cured product obtained from this composition had a high glass transition temperature exceeding 200°C and a high elastic modulus at high temperatures, demonstrating excellent heat resistance. Furthermore, the dielectric properties were also good. In particular, the cured product of the present invention obtained using a specific branched organopolysiloxane having alkenyl groups (DT-type siloxane resin) exhibited an extremely low dielectric tangent, suggesting its usefulness as an insulating material for circuit boards in electric and electronic devices that utilize high frequencies. Meanwhile, the cured product obtained from this composition exhibited high toughness; the toughness of the cured products obtained in Examples 1 and 2 was 64 and 72 kJ / m, respectively. 3 It was.

[0104] On the other hand, the cured product obtained from a composition that did not contain a branched organopolysiloxane (Comparative Example 1) had a low modulus of elasticity at high temperatures (200°C) and failed to achieve a sufficiently low dielectric dissipation factor. Furthermore, the composition containing a reactive branched organopolysiloxane consisting only of trifunctional siloxane units (T units) (Comparative Example 2) exhibited poor moldability. Furthermore, the composition containing a reactive branched organopolysiloxane that contained monofunctional siloxane units (M units) as an essential component exhibited good moldability, but the resulting cured product had insufficient heat resistance. These comparative experimental results confirmed that the combined use of component (A) according to the present invention with component (B) is necessary to achieve excellent dielectric properties, moldability, and heat resistance in a cured product using a thermosetting composition.

[0105] [Synthesis Example: Synthesis of Cycloolefin Polymer (B-2)] 225 ml of dicyclopentadiene (containing approximately 10% cyclopentadiene trimer), 0.54 g of diethylaluminum chloride, 0.99 g of a 70% solution of 1,3-dichloro-2-propanol in dicyclopentadiene, 1.9 ml of a 0.6 mol / L solution of tridodecylammonium molybdate in dicyclopentadiene, and 0.84 ml of a 8.2% solution of benzylidenebis(tricyclohexylphosphine)ruthenium dichloride in dichloromethane were charged in this order using a syringe into a thoroughly nitrogen-purged glass reaction vessel and vigorously stirred for 10 seconds. This reaction solution was preheated to 60°C and placed in a U-shaped resin spacer (5 mm thick) designed to have an internal volume of 20 × 20 × 0.5 cm3, and press-molded for 5 minutes to obtain poly(dicyclopentadiene).

[0106] Example V A thermosetting composition is obtained in the same manner as in Example 1, except that the same mass of poly(dicyclopentadiene) obtained by the above Synthesis Example is used instead of component (B-1) in Example 1. The cured product obtained by curing the thermosetting composition in the same manner as in Example 1 is expected to have a low dielectric constant and excellent physical strength and moldability.

Claims

1. (A) (R 2 SiO 2/2 ) and (RSiO 3/2 (A) a reactive branched organopolysiloxane consisting only of A) units, 10 to 90 parts by mass (wherein R is a monovalent substituent not containing a silicon atom and having a reactive functional group containing at least one carbon-carbon double bond in the molecule); (B) 10 to 90 parts by mass (the sum of components (A) and (B) is 100 parts by mass) of at least one compound selected from aromatic polymers having reactive functional groups and cycloolefin polymers having reactive functional groups); and (C) a thermal radical initiator in an amount of 0.1 to 5 parts by mass per 100 parts by mass of the combined total of components (A) and (B).

2. The thermosetting composition according to claim 1, wherein component (B) is a polyphenylene ether having reactive functional groups at the molecular chain terminals.

3. The thermosetting composition according to claim 1, wherein component (B) is a polyphenylene ether having at least one reactive functional group selected from an alkenyl group and a (meth)acrylate group at the molecular chain terminal.

4. Component (A) has at least one reactive functional group selected from an alkenyl group and a (meth)acrylate group in the molecule, (R 2 SiO 2/2 ) and (RSiO 3/2 2. The thermosetting composition according to claim 1, which is a reactive branched organopolysiloxane consisting only of R) units, wherein R is a group as defined above.

5. Component (A) has at least one reactive functional group selected from an alkenyl group and a (meth)acrylate group in the molecule, and at least one aromatic hydrocarbon group having 6 to 10 carbon atoms in the molecule, (R 2 SiO 2/2 ) and (RSiO 3/2 2. The thermosetting composition according to claim 1, which is a reactive branched organopolysiloxane consisting only of R) units, wherein R is a group as defined above.

6. The thermosetting composition of claim 1, further comprising (D) an organic solvent.

7. The thermosetting composition according to claim 1, wherein component (A) is a reactive branched organopolysiloxane represented by the following formula (1): (R 1 R 2 SiO 2 / 2 ) a (R 3 SiO 3 / 2 ) b (1) (wherein, R 1 is a group represented by the following formula (2), R 2 is an unsubstituted or fluorine-substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, R 3 is R 1 , R 2 a, an alkoxy group, and a hydroxyl group; a and b are numbers that satisfy the following conditions: 0<a, 0<b, a+b=1, 0.05≦a / (a+b)≦0.8; and at least one R 1 and at least one aromatic hydrocarbon group having 6 to 10 carbon atoms.) X-(CH2) y -* (2) (wherein, y is a number from 0 to 6, X is one or more reactive functional groups selected from a vinyl group and a (meth)acrylate group, and * is a bonding site with silicon.) 8. In the reactive branched organopolysiloxane represented by the above formula (1), R 3 The thermosetting composition according to claim 7, wherein is an aromatic hydrocarbon group having 6 to 10 carbon atoms.

9. The thermosetting composition according to claim 7, wherein in the reactive branched organopolysiloxane represented by the above formula (1), X is a vinyl group.

10. The thermosetting composition according to claim 7, wherein the reactive branched organopolysiloxane represented by formula (1) has an average of two or more X groups per molecule.

11. A cured product of the thermosetting composition according to any one of claims 1 to 10.

12. A prepreg comprising a cured product of the thermosetting composition according to any one of claims 1 to 10 and a fibrous reinforcing material.

13. A high-frequency circuit board comprising a laminate of one or more sheets of the prepreg according to claim 12.

14. A method for curing and molding the thermosetting composition according to claim 6, comprising at least the steps of: step (i): removing component (D) from the thermosetting composition according to claim 6 at normal pressure or reduced pressure in the temperature range of about 80-100°C; and step (ii): subsequent to step (i), curing the thermosetting composition at a temperature of 150°C or higher and processing it into a desired shape.

15. A method for producing a prepreg, comprising impregnating the thermosetting composition of claim 6 with a fibrous reinforcing material, then removing component (D) and curing the thermosetting composition.

Citation Information

Patent Citations

  • Polyphenylene ether resin composition and mixture

    JP2021031612A

  • Resin composition and uses thereof in high-frequency circuit board

    WO2015169002A1

  • Polyphenyl ether resin composition and use thereof in high-frequency circuit substrate

    WO2017067123A1

  • Polyphenyl ether resin composition and use thereof in high-frequency circuit substrate

    WO2017067124A1

  • Thermosetting vinyl organosilicon resin composition and application thereof in high-frequency circuit board