Power storage device packaging material
The packaging material for power storage devices, featuring an adhesive layer with acid-modified polyolefin and polyfunctional isocyanate compounds, addresses the durability issue against electrolytes by providing enhanced adhesion and stability across temperatures, ensuring the integrity of power storage devices.
Patent Information
- Application Number
- PCT/JP2024/018232
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-19
- Filing Date
- 2024-05-16
- Publication Date
- 2024-11-28
AI Technical Summary
Conventional packaging materials for power storage devices lack sufficient durability against electrolyte solutions, particularly in lithium-ion batteries, where adhesives are required to maintain integrity and performance across varying temperatures.
A packaging material comprising an adhesive layer with acid-modified polyolefin and a polyfunctional isocyanate compound, specifically designed with a cured product structure that includes a metal layer and a heat-fusible resin layer, providing enhanced durability and adhesion properties through a controlled crosslinked structure and solvent system.
The packaging material exhibits excellent durability against electrolyte solutions and maintains high peel strength at room and elevated temperatures, ensuring the integrity of power storage devices even after immersion in aggressive solvents.
Smart Images

Figure JP2024018232_28112024_PF_FP_ABST
Abstract
Description
Packaging materials for energy storage devices
[0001] The present disclosure relates to packaging materials for electrical storage devices, which are used in various industrial product fields such as electrical, automotive, and industrial fields.
[0002] Acid-modified polyolefins, obtained by grafting organic acids having unsaturated double bonds onto low-polarity polyolefins, have a highly polar acid-modified moiety and a low-polarity polymer backbone. For this reason, acid-modified polyolefins are used as a primer for coating polyolefin resins such as polypropylene, which have traditionally been considered difficult to bond, and as a raw material for adhesives for bonding polyolefins to each other or to polar materials such as metals.
[0003] The typical battery packaging material used for laminated batteries has a three-layer structure centered around aluminum foil, with adhesive between each layer. The three layers are the substrate layer that forms the exterior of the laminated battery after assembly; the barrier layer, made of aluminum foil or stainless steel foil, that prevents the penetration of moisture and air; and the sealant layer, which insulates the barrier layer from contact with the electrodes and electrolyte and heat-seals the outer periphery. Each layer may consist of two or more layers. Of these, the sealant layer that comes into contact with the electrolyte is made of an olefin-based film such as polypropylene film, and the adhesive to the aluminum foil is made of a polyurethane-based adhesive crosslinked with an acid-modified polymer, such as an acid-modified polyolefin or an acid-modified styrene-based elastomer, using an isocyanate-based crosslinking agent.
[0004] Among these, adhesives composed of acid-modified polyolefins and isocyanate-based crosslinkers have been widely used in recent years due to their high adhesive strength. For example, Japanese Patent Application Laid-Open Nos. 2010-92703 and 2014-89985 describe packaging materials for battery cases in which an unstretched thermoplastic resin film layer and an aluminum foil layer are bonded via an adhesive layer containing a polyolefin resin having a carboxy group and a multifunctional isocyanate compound. As described in Japanese Patent Application Laid-Open Nos. 2010-92703 and 2014-89985, adhesives composed of such acid-modified polyolefins and isocyanate-based crosslinkers are primarily used as adhesive solutions by dissolving them in a solvent. Battery packaging materials are produced using a dry lamination method, in which the adhesive solution is applied to aluminum foil or a film for a sealant layer, dried, and then the aluminum foil and the film for a sealant layer are bonded together.
[0005] Lithium-ion battery electrolytes contain ethylene carbonate, which readily dissolves lithium-ion electrolytes. Therefore, adhesives used in battery packaging materials must be durable against electrolytes containing ethylene carbonate. Furthermore, because ethylene carbonate's melting point is slightly higher than room temperature, it is rarely used alone; instead, it is used in combination with other solvents to maintain the electrolyte's liquid state. Recently, for new applications such as electric vehicles, electrolyte compositions that can be used over a wider temperature range have been explored, and new solvents such as propyl propionate are sometimes used in combination. Therefore, adhesives used in battery packaging materials must also be durable against solvents with polarity similar to that of polyolefins, such as propyl propionate.
[0006] In applications as packaging materials for electricity storage devices, such as battery packaging materials, adhesives are required to have durability against electrolytes (hereinafter also referred to as "electrolyte resistance"). An object of one embodiment of the present disclosure is to provide a packaging material for electricity storage devices that has excellent durability against electrolytes.
[0007] Means for solving the above problems include the following aspects. <1> A packaging material for an electricity storage device, comprising: an adhesive layer, a metal layer bonded to one side of the adhesive layer, and a heat-sealable resin layer bonded to the other side of the adhesive layer, wherein the adhesive layer is a cured product of an adhesive composition containing an acid-modified polyolefin and a polyfunctional isocyanate compound and / or a derivative thereof, and the acid-modified polyolefin has an acid value of 5 mg KOH / g to 16 mg KOH / g, a weight-average molecular weight of 70,000 to 120,000, and a melting point of 60°C to 85°C. <2> The packaging material for an electricity storage device according to <1>, wherein the polyfunctional isocyanate compound and / or derivative thereof includes at least two types of polyfunctional isocyanate compounds and / or derivatives thereof. <3> The packaging material for an electricity storage device according to <2>, wherein the polyfunctional isocyanate compound includes an alicyclic polyfunctional isocyanate compound and an aliphatic polyfunctional isocyanate compound. <4> The packaging material for an electricity storage device according to <3>, wherein the alicyclic polyfunctional isocyanate compound is selected from the group consisting of hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, norbornane diisocyanate, and combinations thereof, and the aliphatic polyfunctional isocyanate compound is selected from the group consisting of pentamethylene diisocyanate, hexamethylene diisocyanate, and combinations thereof. <5> The packaging material for an electricity storage device according to any one of <1> to <4>, wherein a ratio of the number of moles of isocyanate groups in the polyfunctional isocyanate compound to the number of moles of carboxy groups in the acid-modified polyolefin (number of moles of isocyanate groups / number of moles of carboxy groups) is 1.5 to 10, and wherein the acid anhydride structure (-CO-O-CO-) is contained in the carboxy groups at 2 moles per mole of the acid anhydride structure. <6> The packaging material for an electricity storage device according to any one of <1> to <5>, wherein the adhesive composition further comprises a solvent, and the solvent is a mixed solvent containing an alicyclic organic solvent and a ketone organic solvent. <7> The packaging material for an electricity storage device according to <6>, wherein a weight ratio of the alicyclic organic solvent to the ketone organic solvent (weight of the alicyclic organic solvent / weight of the ketone organic solvent) is 2 / 8 to 8 / 2.<8> The packaging material for an electricity storage device according to any one of <1> to <7>, wherein the acid-modified polyolefin has a melt flow rate of 21 g / 10 min to 31 g / 10 min at 130°C under a load of 2.16 kg. <9> LiPF in a mixed solvent of ethylene carbonate (EC) and diethylene carbonate (DEC) (volume ratio 1 / 1). 6 <1> The packaging material for an electricity storage device according to any one of <1> to <8>, wherein, after immersion for 7 days at 85°C in an electrolyte solution containing 1 mol / L of propyl propionate, the peel strength between the metal layer and the heat-sealable resin layer at room temperature is 7 N / 15 mm or more, and after immersion for 7 days in propyl propionate at 85°C, the peel strength between the metal layer and the heat-sealable resin layer at room temperature is 5 N / 15 mm or more. <10> The packaging material for an electricity storage device according to any one of <1> to <9>, wherein the peel strength between the metal layer and the heat-sealable resin layer at 80°C is 6 N / 15 mm or more.
[0008] According to the present disclosure, a packaging material for an electricity storage device having excellent durability against an electrolyte solution can be obtained.
[0009] Fig. 1 is a schematic perspective view showing an example of a packaging material for an electricity storage device, and Fig. 2 is a schematic perspective view showing another example of a packaging material for an electricity storage device.
[0010] The following description of the constituent elements may be based on a representative embodiment of the present disclosure, but the present disclosure is not limited to such an embodiment. In this specification, the word "to" is used to mean that the numerical values before and after it are included as the lower and upper limits.
[0011] In the present specification, in which numerical ranges are described in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. Furthermore, in the present specification, in which numerical ranges are described in stages, the upper or lower limit value of that numerical range may be replaced with a value shown in the examples. In the present specification, "mass %" and "wt %" are synonymous, and "parts by mass" and "parts by weight" are synonymous.
[0012] [Packaging Material for Electricity Storage Device] The packaging material for an electricity storage device of the present disclosure includes an adhesive layer, a metal layer bonded to one side of the adhesive layer, and a heat-sealable resin layer bonded to the other side of the adhesive layer, wherein the adhesive layer is a cured product of an adhesive composition containing an acid-modified polyolefin and a polyfunctional isocyanate compound and / or a derivative thereof, and the acid-modified polyolefin has an acid value of 5 mgKOH / g to 16 mgKOH / g, a weight-average molecular weight of 70,000 to 120,000, and a melting point of 60°C to 85°C.
[0013] As described above, conventional packaging materials for electricity storage devices lack sufficient durability against electrolyte solutions. As a result of extensive research, the present inventors have found that by using an adhesive composition having the above-described configuration, it is possible to provide a packaging material for electricity storage devices that, when cured, exhibits excellent durability against electrolyte solutions. The adhesive layer is a cured product of an adhesive composition containing an acid-modified polyolefin and a polyfunctional isocyanate compound, and the acid-modified polyolefin has an acid value of 5 mg KOH / g to 16 mg KOH / g, a weight-average molecular weight of 70,000 to 120,000, and a melting point of 60°C to 85°C. This allows a moderate crosslinked structure to be obtained in the cured product of the adhesive composition. Furthermore, it is estimated that a packaging material for electricity storage devices that exhibits excellent durability against organic solvents and excellent durability against electrolyte solutions can be obtained.
[0014] Furthermore, the packaging material for an electricity storage device according to the present disclosure has high durability even at high temperatures.
[0015] Hereinafter, the adhesive composition used in the packaging material for an electricity storage device will be described in detail for each of its constituent components.
[0016] <Acid-Modified Polyolefin> The adhesive layer is a cured product of an adhesive composition containing an acid-modified polyolefin and a polyfunctional isocyanate compound. The acid-modified polyolefin is a polyolefin having a carboxy group and / or a carboxylic anhydride group. The acid-modified polyolefin is preferably a polyolefin modified with a carboxy group-containing monomer and / or a carboxylic anhydride group-containing monomer.
[0017] The modification may be carried out by a known method, such as graft modification in which a carboxyl group-containing monomer and / or a carboxylic anhydride group-containing monomer is added to a polyolefin in the presence of a known radical polymerization initiator, such as an organic peroxide or an aliphatic azo compound, in melt kneading or in an organic solvent, and copolymerization of a carboxyl group-containing monomer and / or a carboxylic anhydride group-containing monomer with an olefin.
[0018] Among these methods, acid-modified polyolefins are preferably produced by acid-modifying a radically graft-reactive polyolefin with an unsaturated carboxylic acid anhydride. Radical-graft-reactive polyolefins are polyolefins containing monomer units having hydrogen atoms that can be abstracted by radicals. Radical-graft-reactive polyolefins may be non-acid-modified polyolefins (i.e., polyolefins that do not contain carboxy groups or acid anhydride structures), or may be polyolefins that have been acid-modified in part, such as at the terminal portions. For convenience, this radical-graft-reactive polyolefin may be referred to herein as "polyolefin before acid modification." Radical-graft-reactive polyolefins may be used singly or in combination of two or more.
[0019] Specific examples of polyolefins capable of undergoing radical grafting reactions include those obtained by homopolymerizing or copolymerizing at least one polymerizable monomer selected from the group consisting of olefins (preferably having 2 to 6 carbon atoms, more preferably having 2 to 4 carbon atoms), styrene, cycloolefins (preferably having 3 to 10 carbon atoms, more preferably having 5 to 8 carbon atoms), and combinations thereof. In particular, polyolefins capable of undergoing radical grafting reactions are preferably polyolefins obtained from polymerizable monomers that generate relatively stable tertiary carbon radicals. Among these, copolymers of propylene and 1-butene have good solubility in solvents such as toluene and cyclohexane, and also have high adhesive performance, making them more suitable for use as solution-type adhesives.
[0020] In the copolymer of propylene and 1-butene, the copolymerization ratio of 1-butene [1-butene / (propylene+1-butene)] is preferably 5 mol % to 40 mol %, more preferably 10 mol % to 30 mol %. When the copolymerization ratio of 1-butene is within the above range, the solubility in solvents is sufficient, and the adhesive has excellent coatability and hot adhesion properties.
[0021] The melting point of the radically graftable polyolefin is preferably 44°C or higher, more preferably 54°C or higher, particularly preferably 64°C or higher, and may be 74°C or higher. Within this range, the adhesive composition can obtain sufficient peel strength. The melting point of the radically graftable polyolefin is preferably 125°C or lower, more preferably 120°C or lower, particularly preferably 105°C or lower, and may be 95°C or lower. Within this range, sufficient storage stability at low temperatures can be obtained.
[0022] The unsaturated carboxylic acid anhydride is a carboxylic acid anhydride having at least one ethylenically unsaturated double bond. The number of carbon atoms in the unsaturated carboxylic acid anhydride is usually 4 or more, and may be, for example, 5 or more or 6 or more. There is no particular upper limit on the number of carbon atoms in the unsaturated carboxylic acid anhydride, but the number of carbon atoms in the unsaturated carboxylic acid anhydride may be, for example, 10 or less or 8 or less.
[0023] Examples of the unsaturated carboxylic acid anhydride include acid anhydrides of unsaturated dicarboxylic acid compounds such as maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, nadic anhydride, and endic anhydride; and acid anhydrides of unsaturated tricarboxylic acid compounds such as aconitic anhydride.
[0024] As the unsaturated carboxylic acid anhydride, unsaturated dicarboxylic acid anhydrides are preferred because they are easily modified and have excellent adhesive properties, and specifically, maleic anhydride and itaconic anhydride are preferred.
[0025] These unsaturated carboxylic acid anhydrides may be used alone or in combination of two or more.
[0026] In the acid-modified polyolefin, a portion of the acid anhydride structures derived from unsaturated carboxylic acid anhydrides (for example, more than 0 mol % to 30 mol %, or 5 mol % to 20 mol %, based on the total amount of acid anhydride structures derived from unsaturated carboxylic acid anhydrides) may be hydrolyzed to carboxylic acids. Furthermore, a portion of the unsaturated carboxylic acid anhydrides used in the radical grafting reaction (for example, more than 0 mol % to 30 mol %, or 5 mol % to 20 mol %, based on the total amount of unsaturated carboxylic acid anhydrides) may be hydrolyzed to carboxylic acids. The unsaturated carboxylic acid may be an unsaturated dicarboxylic acid formed by hydrolysis of the above-mentioned unsaturated dicarboxylic acid anhydride, but unsaturated monocarboxylic acids such as acrylic acid and methacrylic acid can also be preferably used.
[0027] The graft amount of unsaturated carboxylic acid anhydride in the acid-modified polyolefin can be confirmed by the amount of acid anhydride structure (—CO—O—CO—) present in the acid-modified polyolefin. The amount of acid anhydride structure is evaluated by its acid value. The acid value of the acid-modified polyolefin is 5 mg KOH / g to 16 mg KOH / g, preferably 7 mg KOH / g to 14 mg KOH / g, and more preferably 9 mg KOH / g to 13 mg KOH / g. When the acid value of the acid-modified polyolefin is within any of these ranges, the electrolyte resistance of the adhesive composition can be improved. The acid value can be measured in accordance with JIS K0070 (1992). Details will be described later in the Examples.
[0028] The acid anhydride structures of the unsaturated carboxylic acid anhydride grafted onto the acid-modified polyolefin may all be hydrolyzed to carboxylic acids.
[0029] The acid-modified polyolefin may be further graft-modified with a (meth)acrylic acid alkyl ester. However, in one embodiment of the present disclosure, it may be preferable that the acid-modified polyolefin is not graft-modified with a (meth)acrylic acid alkyl ester. The (meth)acrylic acid alkyl ester is preferably an ester compound of an alkyl alcohol having 8 to 18 carbon atoms and (meth)acrylic acid (hereinafter referred to as a "(meth)acrylic acid long-chain alkyl ester"). The order in which the unsaturated carboxylic acid anhydride and the (meth)acrylic acid alkyl ester are grafted onto the polyolefin before acid modification is not particularly limited, and they may be graft-modified simultaneously or separately.
[0030] The melting point of the acid-modified polyolefin is 60°C to 85°C, preferably 65°C to 80°C, more preferably 70°C to 75°C, and may be, for example, 72°C to 74°C. Within this range, the electrolyte resistance of the adhesive composition can be improved. The melting point can be measured in accordance with JIS K7121 (2012) using a differential scanning calorimeter (DSC) at a temperature rise rate of 10°C / min. Details will be described later in the examples.
[0031] The melt flow rate of the acid-modified polyolefin is preferably 21 g / 10 min to 31 g / 10 min. The melt flow rate of the acid-modified polyolefin is more preferably 22 g / 10 min or more, and particularly preferably 23 g / 10 min or more. The melt flow rate of the acid-modified polyolefin is more preferably 30 g / 10 min or less, and particularly preferably 29 g / 10 min or less. By setting the melt flow rate to 21 g / 10 min or more, the solution viscosity of the adhesive composition can be reduced, and the coating speed can be improved. On the other hand, by setting the melt flow rate to 31 g / 10 min or less, the hot peel strength can be further improved. The melt flow rate can be measured in accordance with JIS K7210-1 (2014) at a test temperature of 130°C and a test load of 2.16 kg. Details will be described later in the examples.
[0032] The weight average molecular weight of the acid-modified polyolefin is within the range of 70,000 to 120,000. From the viewpoint of improving peel strength and electrolyte resistance, the weight average molecular weight of the acid-modified polyolefin is preferably 70,000 or more. Furthermore, from the viewpoint of improving solubility in organic solvents, the weight average molecular weight of the acid-modified polyolefin is preferably 120,000 or less. The weight average molecular weight of the acid-modified polyolefin is preferably 75,000 to 110,000, more preferably 80,000 to 95,000. The weight average molecular weight (Mw) of the resin in this disclosure refers to the value obtained by converting the molecular weight measured by gel permeation chromatography (hereinafter also referred to as "GPC") into polystyrene equivalents. Details will be described later in the Examples.
[0033] The content of the acid-modified polyolefin in the adhesive composition is preferably 50 wt % to 95 wt %, and more preferably 60 wt % to 90 wt %, relative to 100 wt % of the solids content of the adhesive composition, in terms of excellent hot peel strength and electrolyte resistance.
[0034] The adhesive composition may contain a polymer component other than the acid-modified polyolefin. The polymer component may be a component having a molecular weight of 2,000 or more. In one embodiment of the present disclosure, the content of the acid-modified polyolefin in the polymer component is preferably 80 wt % or more, more preferably 85 wt % or more, particularly preferably more than 90 wt %, and may even be 100 wt %.
[0035] In the acid-modified polyolefin, it is preferable that the acid-modified moieties (i.e., graft chains) are dispersed relatively uniformly in the main chain. When the acid-modified polyolefin in which the acid-modified moieties are dispersed relatively uniformly in the main chain is crosslinked with a polyfunctional isocyanate compound, the distribution of crosslinking points is less likely to be uneven, and it is more likely to contribute to improving the crosslink density, compared with the acid-modified polyolefin in which the acid-modified moieties are unevenly distributed. Therefore, when the same amount of polyfunctional isocyanate compound is used for an acid-modified polyolefin with the same acid value, it is thought that the more uniform the acid-modified moieties are, the more the hot peel strength and electrolyte resistance are improved.
[0036] Radical graft reaction methods for acid-modified polyolefins are classified into two types. One is a method (thermal melting method) in which other reactive components are mixed into a thermally melted polyolefin capable of radical graft reaction and allowed to react. The other is a method (solution method) in which a solvent is used to mix and dissolve reactive components including a polyolefin capable of radical graft reaction in the solvent and allow to react. Of these two methods, acid-modified polyolefins produced by the solution method are preferred in the present disclosure. Compared to acid-modified polyolefins produced by the thermal melting method, acid-modified polyolefins produced by the solution method are more easily mixed uniformly with the radical initiator in the radical graft reaction system, allowing acid-modified moieties to be added to the polyolefin in a moderately uniform manner.
[0037] If a portion of the unsaturated carboxylic acid anhydride used for the acid modification remains unreacted, it may be removed by a known method such as distillation by heating or reprecipitation purification, if necessary.
[0038] <Polyfunctional Isocyanate Compound> The adhesive layer is a cured product of an adhesive composition containing an acid-modified polyolefin and a polyfunctional isocyanate compound and / or a derivative thereof. The polyfunctional isocyanate compound is a compound having two or more isocyanate groups (preferably a compound having two isocyanate groups). The polyfunctional isocyanate compound and its derivative can crosslink the acid-modified polyolefin. The polyfunctional isocyanate compound and its derivative may be used alone or in combination of two or more.
[0039] The polyfunctional isocyanate compound is not particularly limited, and various polyfunctional isocyanate compounds such as aromatic, aliphatic, and alicyclic polyfunctional isocyanate compounds can be used. Examples of the polyfunctional isocyanate compound include pentamethylene diisocyanate, hexamethylene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, and norbornane diisocyanate.
[0040] In this specification, the term "polyfunctional isocyanate compound" includes not only polyfunctional isocyanate compounds but also derivatives formed from polyfunctional isocyanate compounds, unless otherwise specified.
[0041] A derivative of a polyfunctional isocyanate compound (hereinafter simply referred to as "derivative") is a compound in which at least one isocyanate group in its molecular structure has been converted to an isocyanurate bond, a biuret bond, a urethane bond, an allophanate bond, a urea bond, or a uretdione bond through a chemical reaction. From the viewpoint of enhancing the effect of improving adhesion to an adherend and improving room-temperature peel strength and electrolyte resistance, the derivative is preferably a compound in which at least one isocyanate group in its structure has been converted to an isocyanurate bond. The derivative may be a derivative in which all isocyanate groups have been chemically converted, but is preferably a derivative in which one or more, more preferably two or more, isocyanate groups remain unreacted.
[0042] The derivative may be a multimer formed from two or more of the same or different multifunctional isocyanate compounds. The multimer may be formed by linking the multifunctional isocyanate compounds via the above-mentioned bonds, such as a uretdione bond, an isocyanurate bond, or an allophanate bond. The multimer may be a multimer formed from all the same type of multifunctional isocyanate compounds (i.e., a homomultimer), or a multimer formed from different types of multifunctional isocyanate compounds (i.e., a heteromultimer). For example, a homomultimer may be an isocyanurate in which two hexamethylene diisocyanate molecules are linked via an isocyanurate bond. For example, a heteromultimer may be an isocyanurate in which hexamethylene diisocyanate and isophorone diisocyanate are linked via an isocyanurate bond. The use of a multimer formed from different types of multifunctional isocyanate compounds may improve the peel strength of the adhesive composition. The number of polyfunctional isocyanate compounds constituting the polymer is not particularly limited, and may be a polymer of a general isocyanate compound. Specifically, the polymer may be a dimer, trimer, tetramer, or the like.
[0043] In this specification, when a derivative of a polyfunctional isocyanate compound is a multimer formed from different types of polyfunctional isocyanate compounds (i.e., a heteromultimer), the multimer is described as a derivative of any of the polyfunctional isocyanate compounds contained in the multimer. For example, a multimer formed from a polyfunctional isocyanate compound (A) and a polyfunctional isocyanate compound (B) is a derivative of both the polyfunctional isocyanate compound (A) and the polyfunctional isocyanate compound (B).
[0044] In one embodiment of the present disclosure, the adhesive composition may contain at least one of a polyfunctional isocyanate compound and a derivative thereof, but preferably contains two or more of them, and more preferably contains two of at least one of a polyfunctional isocyanate compound and a derivative thereof. By containing two or more of a polyfunctional isocyanate compound and a derivative thereof, hot peel strength and electrolyte resistance can be improved.
[0045] From the viewpoint of providing a cured product with excellent durability to an electrolyte solution, the adhesive composition preferably contains at least two types of polyfunctional isocyanate compounds and / or derivatives thereof. Here, as an example, the two types of polyfunctional isocyanate compounds are referred to as polyfunctional isocyanate compound (1) and polyfunctional isocyanate compound (2). The polyfunctional isocyanate compound (1) and the polyfunctional isocyanate compound (2) are compounds with different molecular structures. One or both of the polyfunctional isocyanate compound (1) and the polyfunctional isocyanate compound (2) may be derivatives. When the adhesive composition contains a derivative of a polyfunctional isocyanate compound, the polyfunctional isocyanate compound (1) and the polyfunctional isocyanate compound (2) may form a single derivative, or the polyfunctional isocyanate compound (1) and the polyfunctional isocyanate compound (2) may form different derivatives.
[0046] In one embodiment of the present disclosure, the polyfunctional isocyanate compound (1) may be a polyfunctional isocyanate compound having a hydrocarbon group having 4 to 7 carbon atoms, particularly a diisocyanate compound, and the polyfunctional isocyanate compound (2) may be a polyfunctional isocyanate compound having a hydrocarbon group having 8 to 14 carbon atoms, particularly a diisocyanate compound.
[0047] Specific examples of polyfunctional isocyanate compounds having a hydrocarbon group having 4 to 7 carbon atoms include hexamethylene diisocyanate, pentamethylene diisocyanate, and tetramethylene diisocyanate.
[0048] Commercially available products can be used as derivatives of polyfunctional isocyanate compounds having hydrocarbon groups with 4 to 7 carbon atoms. Commercially available compounds having an isocyanurate bond include Duranate TPA-100 (manufactured by Asahi Kasei Corporation), Duranate MFA-75B (manufactured by Asahi Kasei Corporation), Duranate TUL-100 (manufactured by Asahi Kasei Corporation), Duranate TSA-100 (manufactured by Asahi Kasei Corporation), Coronate HX (manufactured by Tosoh Corporation), and Takenate D-170N (manufactured by Mitsui Chemicals, Inc.). Commercially available compounds having a buret bond include Duranate 24A-100 (manufactured by Asahi Kasei Corporation), Duranate 21S-75E (manufactured by Asahi Kasei Corporation), Takenate D-165NN (manufactured by Mitsui Chemicals, Inc.), and Desmodur N3200 (manufactured by Sumika Covestro Urethane Co., Ltd.). Commercially available compounds having a urethane bond include Duranate P301-75E (manufactured by Asahi Kasei Corporation), which is an adduct of hexamethylene diisocyanate and trimethylolpropane, and Sumidur HT (manufactured by Sumika Covestro Urethane Co., Ltd.). Commercially available compounds having an allophanate bond include Desmodur XP2580 (manufactured by Sumika Covestro Urethane Co., Ltd.).
[0049] Specific examples of polyfunctional isocyanate compounds having a hydrocarbon group having 8 to 14 carbon atoms include polyfunctional isocyanate compounds having one secondary isocyanate group such as isophorone diisocyanate and norbornane diisocyanate, polyfunctional isocyanate compounds having two secondary isocyanate groups such as 4,4'-methylenebis(cyclohexyl isocyanate), and polyfunctional isocyanate compounds having no secondary isocyanate group such as dodecane diisocyanate and 1,3-bis(isocyanatomethyl)cyclohexane.
[0050] Commercially available products can be used as derivatives of polyfunctional isocyanate compounds having a hydrocarbon group having 8 to 14 carbon atoms. Commercially available products of compounds having an isocyanurate bond include Desmodur Z4470 BA (manufactured by Sumika Covestro Urethane Co., Ltd.) and Duranate T4900-70B (manufactured by Asahi Kasei Corporation). Commercially available products of compounds having an allophanate bond include Desmodur XP2565 (manufactured by Sumika Covestro Urethane Co., Ltd.). Commercially available products of compounds having a urethane bond include Takenate D-140N (manufactured by Mitsui Chemicals, Inc.), which is an adduct of isophorone diisocyanate and trimethylolpropane, and VESTANAT EP-DC1241 (manufactured by Evonik Japan Co., Ltd.), which is a monoadduct of isophorone diisocyanate and hydroxyethyl acrylate.
[0051] In the adhesive composition, for example, from the viewpoint of improving the durability of the cured product against an electrolyte solution, the polyfunctional isocyanate compound preferably includes an alicyclic polyfunctional isocyanate compound and an aliphatic polyfunctional isocyanate compound. In one embodiment of the present disclosure, the polyfunctional isocyanate compound (1) may be a polyfunctional isocyanate compound having an aliphatic hydrocarbon group, particularly a diisocyanate compound, and the polyfunctional isocyanate compound (2) may be a polyfunctional isocyanate compound having an alicyclic hydrocarbon group, particularly a diisocyanate compound. The number of carbon atoms in the aliphatic hydrocarbon group may be, for example, 1 to 10. The alicyclic hydrocarbon group is a hydrocarbon group containing an aliphatic ring, and the aliphatic ring may be linked to an aliphatic hydrocarbon group having, for example, 1 to 3 carbon atoms. As the aliphatic ring, a cyclohexane ring, a cyclopentane ring, or the like can be preferably used. The number of carbon atoms in the aliphatic ring may be, for example, 4 to 10. From the viewpoints of electrolyte resistance and adhesion durability at high temperatures, the aliphatic polyfunctional isocyanate compound is preferably selected from the group consisting of pentamethylene diisocyanate, hexamethylene diisocyanate, and combinations thereof. From the viewpoints of electrolyte resistance and adhesion durability at high temperatures, the alicyclic polyfunctional isocyanate compound is preferably selected from the group consisting of hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, norbornane diisocyanate, and combinations thereof.
[0052] From the viewpoint of electrolyte resistance of a cured product of the adhesive composition and adhesion durability at high temperatures, the adhesive composition is preferably such that the alicyclic polyfunctional isocyanate compound is selected from the group consisting of hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, norbornane diisocyanate, and combinations thereof, and the aliphatic polyfunctional isocyanate compound is selected from the group consisting of pentamethylene diisocyanate, hexamethylene diisocyanate, and combinations thereof.
[0053] The weight ratio of the polyfunctional isocyanate compound (1) to the polyfunctional isocyanate compound (2) (polyfunctional isocyanate compound (1) / polyfunctional isocyanate compound (2)) is not particularly limited. In one embodiment, the weight ratio of the polyfunctional isocyanate compound (1) to the polyfunctional isocyanate compound (2) (polyfunctional isocyanate compound (1) / polyfunctional isocyanate compound (2)) is preferably in the range of 1 / 3 to 3 / 1, more preferably in the range of 1 / 2 to 2 / 1, and the weight of the polyfunctional isocyanate compound (1) and the weight of the polyfunctional isocyanate compound (2) may be the same.
[0054] The amount of polyfunctional isocyanate compound in the adhesive composition can be determined from the ratio of the number of moles of isocyanate groups in the polyfunctional isocyanate compound to the number of moles of carboxy groups in the acid-modified polyolefin (number of moles of isocyanate groups / number of moles of carboxy groups). However, when the acid-modified polyolefin contains an acid anhydride structure (-CO-O-CO-), the "number of moles of carboxy groups in the acid-modified polyolefin" refers to 2 moles of carboxy groups per mole of the acid anhydride structure.
[0055] In terms of the electrolyte resistance of the cured product of the adhesive composition and the adhesive durability at high temperatures, the ratio of the number of moles of isocyanate groups in the polyfunctional isocyanate compound to the number of moles of carboxy groups in the acid-modified polyolefin (number of moles of isocyanate groups / number of moles of carboxy groups) is preferably 1.5 to 10. In order to improve the hot peel strength of the adhesive composition, the ratio of the number of moles of isocyanate groups in the polyfunctional isocyanate compound to the number of moles of carboxy groups in the acid-modified polyolefin (number of moles of isocyanate groups / number of moles of carboxy groups) is preferably 1.5 or more, more preferably 2 or more. In order to improve the adhesive strength with metals such as aluminum, particularly the hot peel strength, the ratio of the number of moles of isocyanate groups in the polyfunctional isocyanate compound to the number of moles of carboxy groups in the acid-modified polyolefin is preferably 10 or less, more preferably 9 or less. The number of moles of carboxy groups can be calculated from the acid value.
[0056] The amount of the polyfunctional isocyanate compound in the adhesive composition can also be determined by the weight ratio of the polyfunctional isocyanate compound to the total weight of the acid-modified polyolefin and the polyfunctional isocyanate compound (hereinafter also referred to as the polyfunctional isocyanate compound content). The polyfunctional isocyanate compound content is preferably 5 wt% or more, more preferably 10 wt% or more, and particularly preferably 20 wt% or more. The polyfunctional isocyanate compound content is preferably 60 wt% or less, more preferably 40 wt% or less.
[0057] <Solvent> The adhesive composition may further contain a solvent that dissolves the acid-modified polyolefin, from the viewpoint of further improving the hot peel strength of a cured product of the adhesive composition. Specific examples of the solvent include aromatic organic solvents such as toluene and xylene; aliphatic organic solvents such as n-hexane; alicyclic organic solvents such as cyclohexane, methylcyclohexane, and ethylcyclohexane; ketone organic solvents such as acetone and methyl ethyl ketone; alcohol organic solvents such as methanol and ethanol; ester organic solvents such as ethyl acetate and butyl acetate; and propylene glycol ether organic solvents such as propylene glycol methyl ether, propylene glycol ethyl ether, and propylene glycol t-butyl ether.
[0058] In the adhesive composition, the solvent may be used alone or in combination of two or more kinds.
[0059] Among these, the solvent is preferably a mixed solvent containing an alicyclic organic solvent and a ketone organic solvent. A mixed solvent of an alicyclic organic solvent and a ketone organic solvent can adequately dissolve a polyfunctional isocyanate compound and improve the hot peel strength of a cured product of the adhesive composition. The total content of the alicyclic organic solvent and the ketone organic solvent in the mixed solvent is preferably 80% by weight or more, more preferably 90% by weight or more, and may even be 100% by weight. The weight ratio of the alicyclic organic solvent to the ketone organic solvent in the mixed solvent (weight of the alicyclic organic solvent / weight of the ketone organic solvent) is preferably 2 / 8 to 8 / 2. The weight ratio of the alicyclic organic solvent to the ketone organic solvent in the mixed solvent (weight of the alicyclic organic solvent / weight of the ketone organic solvent) is preferably 8 / 2 or less, more preferably 7 / 3 or less, and particularly preferably 6 / 4 or less. The weight ratio of the alicyclic organic solvent to the ketone organic solvent in the mixed solvent (weight of the alicyclic organic solvent / weight of the ketone organic solvent) is preferably at least 2 / 8, more preferably at least 3 / 7, and particularly preferably at least 4 / 6. By adjusting the weight ratio of the alicyclic organic solvent to the ketone organic solvent within the above preferred range, the hot peel strength can be improved.
[0060] The amount of solvent in the adhesive composition is not particularly limited and may be determined appropriately depending on the type of acid-modified polyolefin. When the total amount of the acid-modified polyolefin and solvent contained in the adhesive composition is taken as 100 wt%, the amount of the acid-modified polyolefin is preferably 5 wt% to 25 wt%, more preferably 10 wt% to 20 wt%. When the solvent is present in the adhesive composition in such an amount, the adhesive composition can be easily applied to an adherend and has excellent workability.
[0061] <Additional Components> The adhesive composition may further contain additional components depending on the purpose. Specific examples of the additional components include a curing catalyst, a styrene-based thermoplastic elastomer, a tackifier, an antioxidant, a hindered amine-based light stabilizer, an ultraviolet absorber, an antistatic agent, a flame retardant, a colorant, a dispersant, an adhesion promoter, an antifoaming agent, a leveling agent, a plasticizer, a lubricant, a crystal nucleating agent, and a filler.
[0062] These components are described below. The additional components are optional components, and may not be used, or only one type may be used, or two or more types may be used in combination.
[0063] The curing catalyst can be blended to promote the crosslinking reaction between the acid-modified polyolefin and the polyfunctional isocyanate compound and to obtain excellent adhesive properties. Preferred curing catalysts include tertiary amines, metal carboxylates and complex salts, and organometallic compounds.
[0064] Specific examples of tertiary amines include tetraalkylethylenediamines such as tetramethylethylenediamine; N,N'-dialkylbenzylamines such as dimethylbenzylamine; triethylenediamine, pentamethyldiethylenetriamine, N-ethylmorpholine, N-methylmorpholine, 1-methyl-4-dimethylamineethylpiperazine, and 1,8-diazabicyclo[5.4.0]undecene-7, and the like.
[0065] Examples of metal carboxylates and complex salts include metal octanoates such as metal acetates, metal hexanoates, and metal 2-ethylhexanoates; metal carboxylates such as metal neodecanoates, metal laurates, metal stearates, and metal oleates; and metal complex salts such as metal acetylacetonates. The organometallic compound is not particularly limited as long as it is a metal compound having a bond with carbon, and examples include organometallic oxides. The metal is preferably one or more metals selected from the group consisting of metals in Groups 7, 12, and 14 of the periodic table. These metals may be used alone or in combination of two or more. Of these, carboxylates, acetylacetonates, and organometallic compounds of tin, zinc, and manganese are more preferred from the viewpoint of adhesiveness when an adhesive layer formed from the adhesive composition comes into contact with an electrolyte. Specific examples include zinc neodecanoate, dibutyltin dilaurate, dioctyltin dilaurate, dioctyltin diacetate, dibutyltin maleate, dibutyltin oxide, dioctyltin oxide, zinc bis(neodecanoate), zinc bis(2-ethylhexanoate), zinc distearate, zinc(II) acetylacetonate, manganese bis(2-ethylhexanoate), etc. Among these, from the viewpoint of the balance of adhesive properties, electrolyte resistance, and heat resistance of the adhesive layer, dibutyltin dilaurate, dioctyltin dilaurate, or dioctyltin oxide is more preferred.
[0066] Furthermore, an organotin compound and a tertiary amine can be used in combination as a curing catalyst.
[0067] The content of the curing catalyst is preferably 0.001 to 5 parts by weight per 100 parts by weight of the total amount of the acid-modified polyolefin and the polyfunctional isocyanate compound. By setting the content of the curing catalyst to 0.001 part by weight or more, it becomes easier to obtain a sufficient catalytic effect, and by setting the content of the curing catalyst to 5 parts by weight or less, the storage stability of the adhesive composition can be ensured.
[0068] A styrene-based thermoplastic elastomer can be blended into the adhesive composition for the purpose of improving adhesive strength.
[0069] Specific examples of styrene-based thermoplastic elastomers include styrene-based resins such as styrene-butadiene copolymer, epoxy-modified styrene-butadiene copolymer, styrene-butadiene-styrene block copolymer, styrene-ethylene / propylene-styrene block copolymer (hereinafter referred to as "SEPS"), styrene-ethylene / butylene-styrene block copolymer (hereinafter referred to as "SEBS"), styrene-isoprene / butadiene-styrene block copolymer, and styrene-isoprene-styrene block copolymer, and these may be those which do not have acidic groups and acid anhydride groups, or those which have acidic groups and / or acid anhydride groups, or those which have amino groups.
[0070] As the tackifier, known ones can be used, and examples thereof include polyterpene resins, rosin resins, aliphatic petroleum resins, alicyclic petroleum resins, copolymer petroleum resins, and hydrogenated petroleum resins.
[0071] The content of the tackifier is preferably 1 to 20% by weight, and more preferably 1 to 10% by weight, relative to 100% by weight of the adhesive composition, in order to provide excellent hot water resistance.
[0072] <Adhesive Composition> The viscosity of the adhesive composition at 25°C is preferably 10 mPa·s to 5,000 mPa·s. From the viewpoint of excellent coatability, the viscosity is preferably 10 mPa·s or more. Furthermore, from the viewpoint of excellent leveling property, the viscosity is preferably 5,000 mPa·s or less, and more preferably 1,000 mPa·s or less.
[0073] The adhesive composition is suitable for bonding polyolefin resin molded articles to other members (metal members, resin members, etc.), and can be used not only to bond polyolefin resin molded articles such as polyolefin resin films to each other, but also to bond a polyolefin resin film to a metal foil made of aluminum or the like, or to bond a polyolefin resin film to a metal layer in a composite film comprising a resin layer and a metal layer, etc. The adhesive layer obtained from the adhesive composition has high room-temperature peel strength and hot peel strength, excellent adhesion, and also has high electrolyte resistance.
[0074] The cured adhesive composition is in a state in which the acid-modified polyolefin and the polyfunctional isocyanate compound and / or its derivative have reacted to form crosslinks. The cured product is formed as long as some of the polyfunctional isocyanate compound or its derivative has formed crosslinks, and the degree of curing of the cured product is not particularly limited. Curing can also be confirmed by observing a rubbery flat area in dynamic viscoelasticity measurement.
[0075] For adhesive compositions containing an acid-modified polyolefin, a polyfunctional isocyanate compound and / or a derivative thereof, and optionally a curing catalyst, the curing temperature may be appropriately determined depending on the type of polyfunctional isocyanate compound, etc. The polyfunctional isocyanate compound can form crosslinks even at room temperature. As described above, the adhesive composition may contain a solvent, but unless otherwise specified, the cured product is one in which the solvent has been dried and removed.
[0076] <Method for producing adhesive composition> The adhesive composition can be produced by a known method. Specifically, this method involves mixing a solution obtained by dissolving an acid-modified polyolefin in a solvent with other components excluding the polyfunctional isocyanate compound and its derivatives, and then mixing the resulting mixture with the polyfunctional isocyanate compound. The temperature during mixing is preferably 40°C or less, more preferably 10°C to 30°C.
[0077] The adhesive composition can be used to produce a packaging material for an electricity storage device. The packaging material for an electricity storage device of the present disclosure includes an adhesive layer formed by curing the adhesive composition, a metal layer bonded to one side of the adhesive layer, and a heat-sealable resin layer bonded to the other side of the adhesive layer.
[0078] Schematic diagrams of packaging materials for electricity storage devices are shown in Figures 1 and 2. That is, the packaging material for electricity storage devices 1 in Figure 1 sequentially comprises a heat-sealable resin layer 11, an adhesive layer 12, and a metal layer 13. Also, the packaging material for electricity storage devices 1 in Figure 2 sequentially comprises a heat-sealable resin layer 11, an adhesive layer 12, a metal layer 13, and another layer 14.
[0079] The shape of the packaging material for an electricity storage device may be appropriately determined depending on the application, etc., and is not particularly limited, but examples include a film, sheet, plate, bag, cylinder, package, etc.
[0080] The heat-sealable resin layer is a layer containing a resin that melts with heat and can fuse the material constituting one layer with the material constituting the other layer. This heat-sealable resin layer is preferably a layer containing a resin that melts at a temperature of 50°C to 200°C. Examples of resins having such properties include polyolefin resins, polyamide resins, and polyester resins. Among these, polyolefin resins are preferred because they can achieve heat fusion with sufficient strength. Furthermore, polypropylene is preferred as the polyolefin resin. In particular, unstretched polypropylene is more preferred as the heat-sealable resin because it exhibits minimal dimensional change (shrinkage).
[0081] The above-mentioned heat-fusible resin layer may be a layer containing additives such as a lubricant, a filler, a heat stabilizer, an antioxidant, an ultraviolet absorber, an antistatic agent, a flame retardant, a colorant, a dispersant, and an adhesion imparting agent, as necessary.
[0082] The thickness of the heat-sealable resin layer is not particularly limited and depends on the resin material, etc., but for example, when the layer contains unstretched polypropylene, it is preferably 10 μm to 200 μm, more preferably 20 μm to 100 μm. If the thickness of the layer containing unstretched polypropylene is 10 μm to 200 μm, it is possible to obtain a packaging material for an electricity storage device that is not easily broken and has high durability.
[0083] The adhesive layer is a layer formed by curing the adhesive composition. The thickness of the adhesive layer is not particularly limited, but is preferably 1 μm to 20 μm, and particularly preferably 2 μm to 10 μm. If the thickness of the adhesive layer is 1 μm to 20 μm, the packaging material for an electricity storage device can be easily processed, for example, by folding, when it is in a sheet form.
[0084] The metal layer is a layer containing a metal or an alloy. Examples of metals or alloys include aluminum, iron, titanium, magnesium, copper, nickel, chromium, and other metals, as well as alloys thereof. Among these, aluminum is preferred due to its excellent workability. The thickness of the metal layer is not particularly limited, depending on the material and other factors. When the metal layer is made of aluminum, for example, the thickness is preferably 20 μm to 100 μm, more preferably 20 μm to 80 μm, and particularly preferably 30 μm to 60 μm.
[0085] As shown in FIG. 2 , the packaging material for an electricity storage device may include another layer 14 on the surface of the metal layer 13. The material constituting the other layer preferably contains a resin from the viewpoint of protecting the metal layer. That is, the other layer is preferably a resin layer. This resin is not particularly limited and can be a polyamide resin, a polyester resin, or the like. The transparency of the resin layer is not particularly limited, but when this resin layer is transparent or translucent, an excellent appearance can be obtained when the packaging material for an electricity storage device is used. The other layer may have a multilayer structure and, for example, may include an adhesive layer for bonding the resin layer and the metal layer. The adhesive layer in the other layer may be the same as or different from the adhesive layer provided between the heat-sealable resin layer and the metal layer. The thickness of the other layer is not particularly limited and is preferably 30 μm to 60 μm, particularly preferably 30 μm to 50 μm.
[0086] The packaging material for an electricity storage device disclosed herein has high hot peel strength and excellent adhesiveness, and also has excellent resistance to solvents such as electrolyte solutions, so it can prevent deterioration of the contents while maintaining its structure.
[0087] The packaging material for the power storage device was prepared by dissolving LiPF in a mixed solvent of ethylene carbonate (EC) and diethylene carbonate (DEC) (volume ratio 1 / 1). 6 The peel strength between the metal layer and the heat-fusible resin layer at room temperature after immersion in an electrolytic solution containing 1 mol / L of hydroxybenzoate at 85°C for 7 days is preferably 7 N / 15 mm or more, and more preferably 9 N / 15 mm or more.
[0088] The peel strength between the metal layer and the heat-sealable resin layer at room temperature after the packaging material for an electricity storage device is immersed in propyl propionate at 85°C for 7 days is preferably 5 N / 15 mm or more, and more preferably 9 N / 15 mm or more.
[0089] The peel strength between the metal layer and the heat-fusible resin layer at 80° C. is preferably 6 N / 15 mm or more, and more preferably 9 N / 15 mm or more. The peel strength is preferably measured by the method described in the Examples below.
[0090] When the packaging material for an electricity storage device is used as a packaging material for a lithium-ion battery, adhesive performance can be maintained even if there are temperature changes in the battery storage or usage environment, and adhesive performance can be maintained in particular in a temperature range higher than normal temperature in summer or inside a car, and a temperature range lower than the ambient temperature in cold regions, due to the chemical temperature increase in the battery constituent materials that accompanies charging or discharging.
[0091] <Method for producing packaging material for electricity storage device> Examples of methods for producing the packaging material for electricity storage device shown in Fig. 1 include the following methods. (1) A method in which an adhesive composition is applied to the surface of a metal foil or the like for forming metal layer 13, and then the organic solvent in the composition is removed to form adhesive layer 12, and then a resin film for forming heat-sealable resin layer 11 (hereinafter referred to as "heat-sealable resin film") is brought into contact with the surface on which adhesive layer 12 has been formed, and pressure-bonded while heating. (2) A method in which an adhesive composition is applied to the surface of a heat-sealable resin film, and then the organic solvent in the composition is removed to form adhesive layer 12, and then a metal foil or the like for forming metal layer 13 is brought into contact with the surface on which adhesive layer 12 has been formed, and pressure-bonded while heating.
[0092] Also, as a method for manufacturing the packaging material for the power storage device shown in FIG. 2, the following methods can be mentioned. (3) The adhesive composition is applied to the surface of the metal layer 13 in a composite film having a resin layer constituting the other layer 14 and a metal layer 13 formed by laminating or vapor-depositing on one side of this resin layer. Then, the organic solvent in the composition is removed to form the adhesive layer 12. Next, the surface on which the adhesive layer 12 is formed is brought into contact with the heat-sealable resin film, and pressure bonding is performed while heating. (4) The adhesive composition is applied to the surface of the heat-sealable resin film. Then, the organic solvent in the composition is removed to form the adhesive layer 12. Next, the surface on which the adhesive layer 12 is formed is brought into contact with the surface on which the metal layer 13 is formed in a composite film having a resin layer constituting the other layer 14 and a metal layer 13 formed by laminating or vapor-depositing on one side of this resin layer, and pressure bonding is performed while heating. (5) A method of extrusion molding a film for forming the other layer 14 on the surface of the metal layer 13 in the laminate obtained by the method (1) or (2) above.
[0093] The adhesive composition is often applied to a material for forming a metal layer such as a metal foil, or to the surface of the metal layer in a composite film having a metal layer and other layers (resin layers), but is not particularly limited. When using a metal foil, it is preferable to use an aluminum foil with a thickness of 20 μm to 100 μm. Thereby, a packaging material for a power storage device with suppressed damage can be easily formed. Also, when using a composite film, it is preferable that the metal layer contains aluminum and the other layer (resin layer) contains a polyamide resin, a polyester resin, etc. Further, when manufacturing the packaging material for the power storage device shown in FIG. 2 without using a composite film, that is, when adopting the method (5) above, it is preferable to use a film containing a polyamide resin, a polyester resin, etc. as the film for forming the other layer 14.
[0094] Examples of heat-sealable resin films that can be used include polyolefin resin films, polyamide resin films, and polyester resin films. These resin films can be obtained by film-forming methods such as extrusion, cast molding, T-die molding, and inflation molding. The thickness of the heat-sealable resin film is typically 10 to 200 μm. In the present disclosure, polyolefin resin films are preferred because they facilitate heat fusion of packaging materials for electricity storage devices. Unstretched polypropylene films are particularly preferred because they allow for the production of packaging materials for electricity storage devices that are resistant to breakage and have excellent durability. When using this unstretched polypropylene film, the preferred thickness is 10 μm to 200 μm, and more preferably 20 μm to 100 μm.
[0095] The adhesive composition can be applied by a conventionally known method, for example, using a bar coater, a gravure coater, or the like. The thickness of the coating film and the drying temperature thereof are not particularly limited. The drying temperature of the coating film is not particularly limited, but is preferably 30°C to 150°C from the viewpoint of workability.
[0096] As described above, the dried coating film generally has tackiness and adhesiveness, and therefore can bond two members together without heating, but when bonding, a method of heating to an appropriate temperature while pressing can be applied, taking into consideration the melting point and melt viscosity of the acid-modified polyolefin, etc. Heating and pressing conditions are, for example, a temperature of 60°C to 100°C, a pressure of 0.3 MPa, and a pressing time of 2 seconds.
[0097] Furthermore, the conditions for accelerating the crosslinking reaction between the acid-modified polyolefin and the polyfunctional isocyanate compound and / or its derivative to complete the packaging material for an electricity storage device (hereinafter referred to as "aging conditions") are not particularly limited, and are preferably set depending on the material of the metal foil, the material of the heat-fusible resin film, the melting temperature, the composition of the adhesive layer, etc. Examples of aging conditions include heating at 25°C to 80°C, for example 40°C, for about 3 to 7 days.
[0098] Examples of electricity storage devices for which the packaging material for electricity storage devices can be used include secondary batteries such as lithium ion batteries and lithium ion polymer batteries.
[0099] In the tables shown below, the raw materials of the adhesive compositions may be indicated by abbreviations, and the abbreviations have the following meanings.
[0100] (Acid-modified polyolefin) Acid-modified polyolefin A: Acid-modified polyolefin produced as follows: In a 1 L autoclave, 100 parts by weight of propylene-butene copolymer (Mitsui Chemicals, Inc. "TAFMER (registered trademark) XM7070"), 150 parts by weight of toluene, 6 parts by weight of maleic anhydride, and 1 part by weight of di-tert-butyl peroxide were added, and the mixture was heated to 140 ° C. and stirred for 3 hours. The resulting reaction solution was cooled to 100 ° C. and poured into a container containing 717 parts by weight of toluene and 950 parts by weight of methyl ethyl ketone preheated to 40 ° C. with stirring, cooled to 40 ° C., further stirred for 30 minutes, and further cooled to 25 ° C. to precipitate a resin. Thereafter, the slurry containing the resin was centrifuged to separate the acid-modified propylene-butene copolymer, maleic anhydride, and low molecular weight substances. Furthermore, the acid-modified propylene-butene copolymer removed by centrifugation was poured into a container containing 2,000 parts by weight of methyl ethyl ketone, which had been previously kept at 25°C, while stirring, and the stirring was continued for 1 hour. The slurry was then centrifuged to further separate the acid-modified propylene-butene copolymer from maleic anhydride and low-molecular-weight substances. This operation was repeated twice for purification. After purification, the mixture was dried under reduced pressure at 40°C for 5 hours to obtain acid-modified polyolefin A. The obtained acid-modified polyolefin A had a weight-average molecular weight of 82,000, a melting point of 72°C, a melt flow rate of 24 g / 10 min, and an acid value of 13 mgKOH / g.
[0101] Acid-modified polyolefin B: Acid-modified polyolefin produced as follows: Acid-modified polyolefin B was obtained in the same manner as Acid-modified polyolefin A, except that the raw polyolefin was changed to a propylene-butene copolymer ("TAFMER (registered trademark) XM7080" manufactured by Mitsui Chemicals, Inc.), the amount of maleic anhydride was changed to 11 parts by weight, and the amount of di-tert-butyl peroxide was changed to 2 parts by weight. The obtained Acid-modified polyolefin B had a weight average molecular weight of 68,000, a melting point of 76°C, a melt flow rate of 36 g / 10 min, and an acid value of 24 mgKOH / g.
[0102] Acid-modified polyolefin C: An acid-modified polyolefin produced as follows: 1,000 parts by weight of a propylene-butene copolymer (Tafmer XM7070 manufactured by Mitsui Chemicals, Inc.), 15 parts by weight of maleic anhydride, 40 parts by weight of lauryl methacrylate, and 15 parts by weight of 2,5-dimethyl-2,5-di(t-butylperoxy)hexane were added to a twin-screw extruder with an L / D ratio of 42 and a diameter of 58 mm. The mixture was allowed to react for 10 minutes at a barrel temperature of 180°C (barrels 1 to 7). Degassing was performed in the seventh barrel, and residual unreacted material was removed to obtain acid-modified polyolefin C. The resulting acid-modified polyolefin C had a weight-average molecular weight of 138,000, a melting point of 74°C, a melt flow rate of 14 g / 10 min, and an acid value of 13 mgKOH / g. The graft weight of lauryl methacrylate in the acid-modified polyolefin C was 3.6% by weight, and the graft weight of maleic anhydride was 1.1% by weight. The graft weight of maleic anhydride was measured by alkali titration, and the graft weight of lauryl methacrylate was measured by 1H-NMR.
[0103] Acid-modified polyolefin D: Acid-modified polyolefin produced as follows: Acid-modified polyolefin D was obtained in the same manner as Acid-modified polyolefin C, except that the propylene and 1-butene copolymer was changed to Tafmer XM7080 manufactured by Mitsui Chemicals, Inc. The obtained Acid-modified polyolefin D had a weight-average molecular weight of 146,000, a melting point of 85°C, a melt flow rate of 11 g / 10 min, and an acid value of 15 mgKOH / g. The graft weight of lauryl methacrylate in Acid-modified polyolefin D was 3.8 wt% and the graft weight of maleic anhydride was 1.3 wt%.
[0104] The acid values, melting points, weight average molecular weights, and melt flow rates of the acid-modified polyolefins A to D are summarized in Table 1 below.
[0105]
[0106] (Polyfunctional isocyanate compounds) Polyfunctional isocyanate compound A: isocyanurate of hexamethylene diisocyanate, NCO content 23% Polyfunctional isocyanate compound B: solution of isocyanurate of hexamethylene diisocyanate and isophorone diisocyanate, NCO content 12%
[0107] (Curing catalyst) DOTL: dioctyltin dilaurate
[0108] The acid value, melting point, weight-average molecular weight, and melt flow rate of acid-modified polyolefins A to D were measured according to the method described below. (Acid Value Measurement) (1) 35 g of non-acid-modified resin (propylene butene copolymer) and octadecyl succinic anhydride (no additives, 1 g, 2 g, 4 g) were weighed and placed in a Laboplastomill (manufactured by Toyo Seiki Seisaku-sho, Ltd.) heated to 170°C. The mixture was heated and stirred to produce four samples with different octadecyl succinic anhydride contents. (2) A small amount of each sample was cut out, sandwiched between two 1 mm-thick fluororesin sheets, and pressed in a hot press at 110°C to form a film. This film was vacuum-dried at 130°C for 5 hours to close the acid anhydride ring 100%. After cooling to room temperature, it was placed in a moisture-proof bag with a desiccant and sealed. It was then left at room temperature for at least one day, and its infrared absorption spectrum was measured by a transmission method. (3) From the transmission IR spectra of the four samples, approximately 1165 cm -1 Absorption (resin-derived peak) at about 1799 cm -1 A calibration curve was created by plotting the absorbance ratio of the absorption (peak derived from the acid anhydride) and the octadecyl succinic anhydride content. (4) Acid-modified polyolefins A to D were each vacuum dried at 130°C for 5 hours to close the acid anhydride ring 100%, cooled to room temperature, and then left in a dry state for at least one day before measuring the infrared absorption spectrum by a transmission method. (5) From the spectrum measured in (4), the peak at 1165 cm -1 Absorption at 1799 cm -1 The absorbance ratio was calculated and compared with the calibration curve prepared in (3) to determine the acid value.
[0109] (Measurement of Melting Point) The melting point was measured in accordance with JIS K7121 (2012). Specifically, the melting point was determined from the temperature at which the secondary temperature rise in the heat flux curve obtained using a differential scanning calorimeter becomes minimal. The heat flux curve was obtained by cooling approximately 10 mg of a sample to -50°C and holding it for 5 minutes, heating it to 150°C at 10°C / min and holding it for 5 minutes, cooling it to -50°C at 10°C / min and holding it for 5 minutes, then heating it to 150°C at 10°C / min and holding it for 5 minutes, and cooling it to -50°C at 10°C / min. Apparatus: DSC6220 manufactured by SII Nanotechnology Inc. Measurement atmosphere: Nitrogen atmosphere
[0110] (Measurement of Weight-Average Molecular Weight) The weight-average molecular weight of the acid-modified polyolefin was determined in terms of polystyrene using gel permeation chromatography (GPC). The apparatus and conditions used for the measurement were as follows: Apparatus: Model "HLC-8320" manufactured by Tosoh Corporation Column: TSKgel-SuperMultipore HZ-M (4.6 mm ID x 15 cm) x 3 manufactured by Tosoh Corporation Solvent: Tetrahydrofuran Column temperature: 40°C Detector: RI (differential refractive index detector) Flow rate: 350 μL / min
[0111] (Melt flow rate measurement) The melt flow rate was measured in accordance with JIS K7210-1 (2014). Specifically, the measurement was performed in automatic measurement mode using a melt indexer G-02 manufactured by Toyo Seiki Seisakusho, Ltd., at a furnace temperature of 130 ° C. and a load of 2.16 kg.
[0112] Example 1 (Preparation of Adhesive Solution) 15 g of acid-modified polyolefin A and 85 g of a mixed solvent of methylcyclohexane:methyl ethyl ketone = 51:34 (weight ratio) were weighed into a four-neck flask equipped with a condenser and a stirring motor, and the flask was immersed in an oil bath under a dry nitrogen stream and heated to 70 °C while stirring until the acid-modified polyolefin A was completely dissolved. The mixture was then cooled to room temperature. A solution containing 3.5 g of polyfunctional isocyanate compound A, 3.5 g of polyfunctional isocyanate compound B, 3.0 g of methyl ethyl ketone, and 0.13 g of dioctyltin dilaurate as a catalyst was added and stirred to prepare an adhesive solution. In the adhesive solution, the ratio (NCO / COOH) of the number of moles of isocyanate groups to the number of moles of carboxyl groups in the acid-modified polyolefin was 8.4.
[0113] (Preparation of Test Pieces for Peel Strength Evaluation) The adhesive solution was applied to a 40 μm thick aluminum foil that had been chemically treated on the adhesive-coated surface using a bar coater. The gap of the bar coater was adjusted in advance so that the average adhesive thickness after drying would be 2 μm to 4 μm. Furthermore, when measuring the peel strength to be performed later, the adhesive was not applied to the portion that would be clamped by the gripping tools of the tensile tester. This aluminum foil was dried for 1 minute in an oven heated to 80°C, and an 80 μm thick CPP (cast polypropylene) film that had been corona discharge-treated was placed on the surface that contacted the adhesive, and the film was sandwiched and bonded between a roll laminator at a roll temperature of 80°C. This was cured in a 40°C oven for 1 week to allow the curing reaction to proceed, and then cut into 15 mm wide strips to prepare test pieces for peel strength evaluation.
[0114] (Measurement of Peel Strength) Using a thermostatically-equipped tensile tester (Autograph AGS-X manufactured by Shimadzu Corporation), a T-peel test was performed at a pulling rate of 100 mm / min until the gripper had moved 100 mm, and the peel strength (N / 15 mm) was calculated by averaging the peel strengths from a moving distance of 40 mm to 100 mm. The peel test was performed at three temperatures: room temperature (rt, 23°C; the same applies below), 80°C, and 120°C.
[0115] (Measurement of peel strength after solvent immersion) A test piece for evaluating peel strength was placed in a pressure-resistant container with a liquid-contacting portion made of fluororesin, and solvent was poured in until the test piece was completely immersed, and the container was sealed. The solvent for immersion was a mixed solvent of ethylene carbonate (EC) and diethylene carbonate (DEC) (volume ratio 1 / 1) in which LiPF 6 Two types of electrolytes were evaluated: an electrolyte solution containing 1 mol / L of propyl propionate (PrP). The container was placed in an oven set at 85°C and left for 7 days. The test piece for peel strength evaluation was removed and immersed in water at room temperature for 2 hours. After wiping off the surface water, a T-peel test was performed at room temperature (rt) using a tensile tester (Shimadzu Corporation, Autograph AGS-X) at a pulling rate of 100 mm / min until the gripper moved 100 mm. The peel strength (N / 15 mm) was averaged from a moving distance of 40 mm to 100 mm.
[0116] Examples 2 to 4 and Comparative Examples 1 to 5 Examples 2 to 4 and Comparative Examples 1 to 5 (acid-modified polyolefin, polyfunctional isocyanate compound, curing catalyst) were as shown in Table 2, and adhesive solutions were prepared in the same manner as in Example 1. Test pieces for evaluating peel strength were prepared in the same manner as in Example 1, and evaluated in the same manner as in Example 1.
[0117] The results of measuring the peel strength of Examples 1 to 4 and Comparative Examples 1 to 5 are also summarized in Table 2 along with the compositions.
[0118]
[0119] As shown in Table 2, the packaging materials for electricity storage devices of the Examples were superior in durability to electrolyte solution compared to the packaging materials for electricity storage devices of the Comparative Examples. Furthermore, among the Examples, the packaging materials for electricity storage devices having an adhesive layer containing polyfunctional isocyanate compound B in addition to polyfunctional isocyanate compound A were particularly superior in durability to electrolyte solution. Furthermore, as shown in Table 2, the packaging materials for electricity storage devices of the Examples were also superior in adhesion durability at high temperatures.
[0120] The disclosure of Japanese Patent Application No. 2023-083431, filed on May 19, 2023, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards mentioned herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. A packaging material for an electricity storage device comprising: an adhesive layer, a metal layer bonded to one side of the adhesive layer, and a heat-sealable resin layer bonded to the other side of the adhesive layer, wherein the adhesive layer is a cured product of an adhesive composition containing an acid-modified polyolefin and a polyfunctional isocyanate compound and / or a derivative thereof, and wherein the acid-modified polyolefin has an acid value of 5 mg KOH / g to 16 mg KOH / g, a weight average molecular weight of 70,000 to 120,000, and a melting point of 60°C to 85°C.
2. A packaging material for an electricity storage device according to claim 1, wherein the polyfunctional isocyanate compound and / or derivative thereof comprises at least two types of polyfunctional isocyanate compounds and / or derivatives thereof.
3. The packaging material for an electricity storage device according to claim 2, wherein the polyfunctional isocyanate compound includes an alicyclic polyfunctional isocyanate compound and an aliphatic polyfunctional isocyanate compound.
4. The packaging material for an electricity storage device according to claim 3, wherein the alicyclic polyfunctional isocyanate compound is selected from the group consisting of hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, norbornane diisocyanate, and combinations thereof, and the aliphatic polyfunctional isocyanate compound is selected from the group consisting of pentamethylene diisocyanate, hexamethylene diisocyanate, and combinations thereof.
5. A packaging material for an electricity storage device according to claim 1 or 2, wherein a ratio of the number of moles of isocyanate groups in the polyfunctional isocyanate compound to the number of moles of carboxy groups in the acid-modified polyolefin (number of moles of isocyanate groups / number of moles of carboxy groups) is 1.5 to 10, and an acid anhydride structure (-CO-O-CO-) is contained in the carboxy groups as 2 moles of carboxy groups per mole of the acid anhydride structure.
6. A packaging material for an electricity storage device according to claim 1 or 2, wherein the adhesive composition further contains a solvent, and the solvent is a mixed solvent containing an alicyclic organic solvent and a ketone organic solvent.
7. A packaging material for an electricity storage device according to claim 6, wherein the weight ratio of the alicyclic organic solvent to the ketone organic solvent (weight of alicyclic organic solvent / weight of ketone organic solvent) is 2 / 8 to 8 / 2.
8. A packaging material for an electricity storage device according to claim 1 or 2, wherein the acid-modified polyolefin has a melt flow rate of 21 g / 10 min to 31 g / 10 min at 130° C. under a load of 2.16 kg.
9. LiPF in a mixed solvent of ethylene carbonate (EC) and diethylene carbonate (DEC) (volume ratio 1 / 1) 6 3. The packaging material for an electricity storage device according to claim 1, wherein after immersion for 7 days at 85° C. in an electrolyte solution containing 1 mol / L of propyl propionate, the peel strength between the metal layer and the heat-sealable resin layer at room temperature is 7 N / 15 mm or more, and after immersion for 7 days in propyl propionate at 85° C., the peel strength between the metal layer and the heat-sealable resin layer at room temperature is 5 N / 15 mm or more.
10. A packaging material for an electricity storage device according to claim 1 or 2, wherein the peel strength between the metal layer and the heat-sealable resin layer at 80°C is 6 N / 15 mm or more.
Citation Information
Patent Citations
Adhesive composition, laminate, and packaging material for lithium ion battery