Absorbent article and packaging
The use of polyolefin resin with biodegradation additives in absorbent articles and controlled packaging addresses the challenges of material strength and biodegradation in conventional absorbent articles, ensuring effective and cost-efficient decomposition and extended product life.
Patent Information
- Application Number
- PCT/JP2024/018862
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2024-05-22
- Publication Date
- 2024-11-28
AI Technical Summary
Conventional absorbent articles with biodegradable outer sheet members are expensive and have insufficient material strength, making it difficult to ensure necessary strength while promoting biodegradation after disposal, and there is a risk of delayed decomposition due to microorganisms' inability to penetrate effectively.
Incorporating a polyolefin resin nonwoven fabric as the outer exposed portion with additives that promote biodegradation using oxygen, water, and ultraviolet light, ensuring the carbonyl index is 1 or more within 28 days, while maintaining material strength and cost-effectiveness, and using a packaging sheet with lower oxygen permeability and ultraviolet transmittance to control biodegradation.
The absorbent article achieves necessary material strength while reducing costs and promoting quick biodegradation after disposal, with controlled biodegradation initiation, and the packaging ensures the absorbent articles remain effective for their intended period.
Smart Images

Figure JP2024018862_28112024_PF_FP_ABST
Abstract
Description
Absorbent articles and packaging
[0001] The present disclosure relates to absorbent articles and packages.
[0002] Conventionally, there has been known an absorbent article comprising an inner sheet member that faces the skin of the wearer, an outer sheet member that is positioned on the opposite side of the inner sheet member from the skin side, and an absorbent body that is positioned between the inner sheet member and the outer sheet member and absorbs the wearer's excrement (see, for example, Patent Document 1).
[0003] Japanese Patent Application Laid-Open No. 2020-195428
[0004] The absorbent articles described above generally have a structure in which multiple sheet materials are stacked, and when discarded, they are rolled up and folded to trap excrement inside. Therefore, for example, when used absorbent articles (e.g., absorbent articles discarded in the folded state described above) are disposed of in soil, microorganisms in the soil may have difficulty penetrating into the absorbent article, potentially resulting in a long decomposition process. Therefore, to accelerate the decomposition process of the absorbent article (i.e., to promote the introduction of microorganisms into the absorbent article), it is conceivable to construct the outer sheet members of the absorbent article from a biodegradable resin such as polylactic acid resin. However, such biodegradable resins generally have problems such as high cost and insufficient material strength.
[0005] Therefore, the present disclosure aims to provide an absorbent article that can ensure the necessary material strength while suppressing increases in costs, and that can promote the biodegradation of the absorbent article after disposal, and a packaging body that can suitably package the absorbent article.
[0006] an absorbent article according to one aspect of the present disclosure, which is an absorbent article that absorbs excrement discharged by a wearer, comprising: an inner sheet member including one or more sheets that face the wearer's skin; an outer sheet member including one or more sheets that are arranged on the opposite side of the inner sheet member from the skin side; an absorbent body that is arranged between the inner sheet member and the outer sheet member and absorbs the wearer's excrement; and a fixing member for fixing the shape of the absorbent article so that the absorbent article maintains a folded state in which the inner sheet member is surrounded on the inside; at least one of the outer sheet member and the fixing member has an outer exposed portion that is exposed to the outside in the folded state, and a first portion that is at least a part of the outer exposed portion is comprised of a polyolefin resin that is not biodegradable by itself, and the first portion contains an additive that biodegrades the polyolefin resin using at least one of oxygen, water, and ultraviolet rays as an accelerating factor, thereby satisfying the biodegradation condition that the first portion exhibits a carbonyl index of 1 or more within 28 days from the start of a biodegradability evaluation test specified in PAS9017:2020.
[0007] The packaging body according to the first aspect of the present disclosure is a packaging body for packaging a plurality of the above-mentioned absorbent articles together, and includes a packaging sheet for packaging the plurality of absorbent articles, and the oxygen permeability of the packaging sheet is lower than the oxygen permeability of the first part.
[0008] The packaging body relating to the second aspect of the present disclosure is a packaging body for packaging multiple absorbent articles together, and includes a packaging sheet for packaging the multiple absorbent articles, and the ultraviolet transmittance of the packaging sheet is lower than the ultraviolet transmittance of the first portion.
[0009] The packaging body relating to the third aspect of the present disclosure is a packaging body for packaging a plurality of the above-mentioned absorbent articles together, and includes a packaging sheet for packaging the plurality of absorbent articles, the packaging sheet sealing the internal space in which the absorbent articles are contained.
[0010] According to the present disclosure, it is possible to provide an absorbent article that can ensure the necessary material strength while suppressing increases in costs, and that can promote the biodegradation of the absorbent article after disposal, and a packaging body that can suitably package the absorbent article.
[0011] Fig. 7 is a plan view of an absorbent article according to one embodiment, as seen from the non-skin facing side. Fig. 1 is a plan view of the absorbent article of Fig. 1, as seen from the skin facing side. Fig. 2 is a cross-sectional view of the absorbent article taken along line III-III of Fig. 2. Fig. 3 is a diagram showing an example of a folded state of the absorbent article of Fig. 1. Fig. 4 is a perspective view of an absorbent article according to a modified example. Fig. 5 is a diagram showing an example of a folded state of the absorbent article of Fig. 5. Fig. 6 is a perspective view of a package according to one embodiment. Fig. 7 is a side view of the package of Fig. 7.
[0012] The present disclosure includes the following aspects 1 to 27.
[0013] (Aspect 1) An absorbent article for absorbing body waste discharged by a wearer, comprising: an inner sheet member including one or more sheets facing the skin of the wearer; an outer sheet member including one or more sheets arranged on the opposite side of the inner sheet member from the skin side; an absorbent body arranged between the inner sheet member and the outer sheet member for absorbing the body waste of the wearer; and a fixing member for fixing the shape of the absorbent article so as to maintain a folded state in which the absorbent article is folded so that the inner sheet member is surrounded on the inside, wherein at least one of the outer sheet member and the fixing member has an outer exposed portion that is exposed to the outside in the folded state, and a first portion that is at least a part of the outer exposed portion is composed of a polyolefin resin that is not biodegradable by itself, The first part contains an additive that causes the polyolefin resin to biodegrade using at least one of oxygen, water, and ultraviolet light as an accelerating factor, thereby satisfying the biodegradation condition that the carbonyl index of the first part is 1 or more within 28 days from the start of the biodegradability evaluation test specified in PAS9017:2020. An absorbent article.
[0014] In the above-mentioned absorbent article, by constructing the first portion, which is at least a part of the outer exposed portion, from a polyolefin resin that is not biodegradable by itself, the cost of the absorbent article can be reduced while ensuring the material strength of the first portion compared to when the first portion is constructed from a biodegradable resin such as polylactic acid resin. Furthermore, after use, absorbent articles are typically discarded with the outer exposed portion exposed to the outside and the inner sheet member and absorber rolled up inside. In the above-mentioned absorbent article, the first portion contains an additive that promotes biodegradation so as to satisfy the above-mentioned biodegradation conditions, allowing the first portion of the absorbent article to decompose quickly after disposal. As a result, microorganisms can penetrate quickly into the interior of the discarded absorbent article, thereby promoting the biodegradation of the entire absorbent article. Therefore, the above-mentioned absorbent article can ensure the necessary material strength while suppressing increases in cost and promoting the biodegradation of the absorbent article after disposal.
[0015] (Aspect 2) The absorbent article of Aspect 1, wherein the additive contains a phenolic antioxidant stabilizer. (Aspect 3) The absorbent article of Aspect 2, wherein the content of the phenolic antioxidant stabilizer in the additive is 0.02 to 0.15 wt % based on the total weight of the polyolefin resin and the additive. According to Aspects 2 and 3, the start time of biodegradation can be appropriately adjusted so that decomposition begins after an expected certain product storage period has elapsed.
[0016] (Aspect 4) The absorbent article of Aspect 2 or 3, wherein the outer sheet member includes a plurality of sheets, the additive is added to at least two of the plurality of sheets, and the content of the phenolic antioxidant stabilizer in each of the two or more sheets increases toward the outermost sheet. According to Aspect 4, by increasing the degree of biodegradation inhibition in the portion (outer portion) that is more likely to be exposed to outside air under normal circumstances (during storage or use), it is possible to appropriately prevent unexpected acceleration of biodegradation in the outer portion of the outer sheet member.
[0017] (Aspect 5) The tensile strength of the first portion is MD: 0.3 N / mm 2 or more and CD: 0.07 N / mm2 The absorbent article of any one of Aspects 1 to 4. (Aspect 6) The absorbent article of any one of Aspects 1 to 5, wherein the first portion has durability such that no pilling occurs after 50 reciprocating rubs under a 200 g load in a surface rub fastness test specified in JIS L0849. According to Aspects 5 and 6, the material strength of the first portion can be suitably ensured, thereby improving the stability of the absorbent article against deformation, breakage, and the like under normal conditions (during storage or use).
[0018] (Aspect 7) The absorbent article of any one of Aspects 1 to 6, wherein the first portion has a thickness of 0.1 mm or more and 2.0 mm or less. If the thickness of the first portion (outer exposed member) is less than 0.1 mm, the feel of the first portion is likely to be poor. Furthermore, if the thickness of the first portion is greater than 2.0 mm, the large thickness reduces the decomposition rate of the first portion. Therefore, according to Aspect 7, by setting the thickness of the first portion in the range of 0.1 mm or more and 2.0 mm or less, it is possible to suppress a decrease in the decomposition rate while maintaining a good feel of the first portion.
[0019] (Aspect 8) The absorbent article of any one of Aspects 1 to 7, wherein the ultraviolet transmittance of the first portion is 15% or more. According to Aspect 8, ultraviolet light, which may be a factor in promoting biodegradation of components of the absorbent article that are located inside the first portion, can be transmitted through the first portion and suitably guided to the inner components. As a result, the start of biodegradation inside the absorbent article can be accelerated, and the decomposition rate of the entire absorbent article can be improved.
[0020] (Aspect 9) The absorbent article of any one of Aspects 1 to 8, wherein the outer sheet member has a biodegradable intermediate sheet disposed between the first portion and the absorbent body, and the air permeability of the first portion measured by the Frazier test is higher than the air permeability of the intermediate sheet measured by the Frazier test. (Aspect 10) The absorbent article of any one of Aspects 1 to 9, wherein the outer sheet member has a biodegradable intermediate sheet disposed between the first portion and the absorbent body, and the density of the first portion is lower than the density of the intermediate sheet. According to Aspects 9 and 10, water, oxygen, etc., which may promote the biodegradation of the intermediate sheet, can be permeated through the first portion and suitably guided to the intermediate sheet. As a result, the start of biodegradation of the interior (intermediate sheet) of the absorbent article can be accelerated, and the decomposition rate of the entire absorbent article can be improved.
[0021] (Aspect 11) The air permeability of the first part measured by a Frazier test is 100 cm 3 / (cm 2 ・s) or more 700cm 3 / (cm 2 According to an eleventh aspect, the absorbent article of any one of the first to tenth aspects has an air permeability of 700 cm or less. 3 / (cm 2 s) or less, preventing the loss of the function of the absorbent article (for example, preventing leakage of excrement, etc.) while maintaining the air permeability to 100 cm 3 / (cm 2 By setting the first portion to be equal to or greater than s, water, oxygen, and the like, which may be factors that promote biodegradation, can be properly guided through the first portion to the inside of the absorbent article, thereby hastening the start of biodegradation inside the absorbent article and improving the decomposition rate of the entire absorbent article.
[0022] (Aspect 12) The density of the first portion is 0.02 g / m 3 0.1g / m or more 3 According to aspect 12, the absorbent article of any one of aspects 1 to 11 has a density of 0.1 g / m or less. 3 By suppressing the density to 0.02 g / m or less, the function of the absorbent article (for example, prevention of leakage of excrement) is prevented from being impaired, and the density is 0.02 g / m or less.3 By doing so, water, oxygen, and the like, which may be factors that promote biodegradation, can be properly guided through the first portion to the inside of the absorbent article, thereby hastening the start of biodegradation inside the absorbent article and improving the decomposition rate of the entire absorbent article.
[0023] (Aspect 13) The absorbent article of any one of Aspects 1 to 12, wherein the absorbent body comprises a biodegradable superabsorbent polymer. According to Aspect 13, the first portion of the absorbent article is biodegraded to allow microorganisms to reach the absorbent body, thereby allowing the absorbent body to be properly biodegraded.
[0024] (Aspect 14) The absorbent article of Aspect 13, wherein the biodegradation promoter of the superabsorbent polymer is the same as the biodegradation promoter of the first portion. According to Aspect 14, it is possible to prevent a situation in which only one of the first portion and the superabsorbent polymer remains without being decomposed in the same environment.
[0025] (Aspect 15) The absorbent article of Aspect 13, wherein the factor promoting the biodegradation of the superabsorbent polymer includes a substance derived from the excrement, and the factor promoting the biodegradation of the first portion does not include a substance derived from the excrement. According to Aspect 15, the decomposition of the absorbent body (the superabsorbent polymer) can be initiated from the time the wearer excretes excrement in the absorbent article, thereby shortening the time until the biodegradation of the absorbent body is complete. Meanwhile, because the factor promoting the biodegradation of the first portion does not include a substance derived from the excrement, it is possible to prevent the first portion from starting to decompose before the appropriate time for decomposition to begin (i.e., the time after the absorbent article has been disposed of) triggered by excretion processing.
[0026] (Aspect 16) The absorbent article of any one of Aspects 1 to 15, wherein the first portion is rendered biodegradable by the additive, such that a portion accounting for 90% or more of the total weight of the absorbent article is biodegradable. According to Aspect 16, it is possible to more effectively promote the biodegradation of the absorbent article after disposal.
[0027] (Aspect 17) The absorbent article of any one of Aspects 1 to 16, wherein the outer sheet member has a biodegradable intermediate sheet disposed between the first portion and the absorbent, and the degree of deterioration of the intermediate sheet measured by the evaluation test is higher than the degree of deterioration of the first portion measured by the evaluation test. (Aspect 18) The absorbent article of Aspect 17, wherein the intermediate sheet also contains the additive, and the content of the additive in the intermediate sheet is higher than the content of the additive in the first portion. From the perspective of preventing leakage of excrement, intermediate sheets generally have a structure that is difficult to decompose. According to Aspects 17 and 18, such intermediate sheets can be made to be easily biodegradable. As a result, the decomposition rate of the entire absorbent article can be improved.
[0028] (Aspect 19) The absorbent article of any one of Aspects 1 to 18, wherein the fixing member includes a base sheet and an engaging portion provided on the surface of the base sheet, the first portion includes the base sheet, and the engaging portion is configured to be engageable with the outer surface of the outer sheet member or the fixing member so as to maintain the folded state. According to Aspect 19, in the absorbent article after disposal, the folded state can be released to expose the interior of the absorbent article to the outside by promoting biodegradation of the base sheet of the engaging member. As a result, microorganisms can easily come into contact with the inner members of the absorbent article, thereby improving the decomposition rate of the entire absorbent article.
[0029] (Aspect 20) The absorbent article of Aspect 19, wherein the engagement strength between the engaging portion and the outer surface after a predetermined period of time has elapsed since the start of the evaluation test of the first portion is lower than the engagement strength between the engaging portion and the outer surface before the evaluation test was started. The engagement strength acts to maintain the folded state. In Aspect 20, the biodegradability of at least a portion of the first portion (e.g., the amount of additive added) is adjusted so that the engagement strength between the engaging portion and the outer surface after a predetermined period of time from the start of the evaluation test of the first portion (i.e., the start of the promotion of biodegradation) is lower than the engagement strength before the evaluation test was started. This makes it easier for the engagement portion and the outer surface to disengage after a predetermined period of time from the start of the promotion of biodegradation, thereby increasing the likelihood that the folded state will be released.
[0030] (Aspect 21) The absorbent article of any one of Aspects 1 to 20, wherein the biodegradation conditions further include the condition that, within 14 days from the start of the evaluation test, the number average molecular weight of the first portion becomes 5,000 or less, the z-average molecular weight of the first portion becomes 30,000 or less, and the loss of the weight average molecular weight of the first portion becomes 90% or more. According to Aspect 21, the biodegradation of the first portion can be promoted more effectively.
[0031] (Aspect 22) A packaging body for packaging a plurality of absorbent articles according to any one of Aspects 1 to 21, comprising a packaging sheet for packaging the plurality of absorbent articles, wherein the packaging sheet has an oxygen permeability lower than that of the first portion. (Aspect 23) The packaging body of Aspect 22, wherein the outer sheet member of the absorbent article has an intermediate sheet disposed between the first portion and the absorbent body, wherein the oxygen permeability of the packaging sheet is lower than that of the intermediate sheet. (Aspect 24) A packaging body for packaging a plurality of absorbent articles according to any one of Aspects 1 to 21, comprising a packaging sheet for packaging the plurality of absorbent articles, wherein the ultraviolet transmittance of the packaging sheet is lower than that of the first portion. (Aspect 25) The packaging body of Aspect 24, wherein the outer sheet member of the absorbent article has an intermediate sheet disposed between the first portion and the absorbent body, wherein the ultraviolet transmittance of the packaging sheet is lower than that of the intermediate sheet. (Aspect 26) A package for packaging a plurality of absorbent articles according to any one of Aspects 1 to 21, comprising a packaging sheet for packaging the plurality of absorbent articles, the packaging sheet sealing an internal space in which the absorbent articles are housed. According to the packages of Aspects 22 to 26, when the absorbent articles are housed and stored in the packaging sheet before use (in a packaged state), it is possible to prevent oxygen, ultraviolet rays, and the like, which may be factors that promote biodegradation, from entering the interior of the package. This prevents the start of biodegradation of the absorbent article (first part) from being accelerated, i.e., the product life of the absorbent article from being shorter than expected. Therefore, the above-mentioned package can suitably package the absorbent articles described above.
[0032] [Embodiments] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings. In the following description, the same or equivalent elements will be designated by the same reference numerals, and redundant description will be omitted.
[0033] (Absorbent article) Fig. 1 is a plan view of an absorbent article 1 according to one embodiment, as viewed from the non-skin-facing side. Fig. 2 is a plan view of the absorbent article 1 as viewed from the skin-facing side. Fig. 3 is a cross-sectional view taken along line III-III in Fig. 2. The plan views of Figs. 1 and 2 show the absorbent article 1 in a stretched state in which it has been stretched to a state in which no wrinkles are formed. In this embodiment, the "skin-facing side" refers to the side that faces the skin of the wearer when the absorbent article 1 is in use (worn), and the "non-skin-facing side" refers to the side that faces away from the skin of the wearer when the absorbent article 1 is in use (worn). In this embodiment, the "wearer" refers to a person who wears the absorbent article 1, and the "wearer" refers to a person who puts the absorbent article 1 on the wearer.
[0034] In the following description, the longitudinal direction (MD: machine direction) of the absorbent article 1 in a stretched state (see FIGS. 1 and 2 ) is referred to as the front-to-back direction L, and the width direction (CD: cross direction) of the absorbent article 1 in a stretched state, which is perpendicular to the front-to-back direction L, is referred to as the width direction W. The front-to-back direction L is the direction extending from the front to the back of the wearer's body when the absorbent article 1 is in use. The width direction W is the direction that corresponds to the left-to-right direction of the wearer when the absorbent article 1 is in use.
[0035] The absorbent article 1 is an article that absorbs excrement such as urine excreted by a wearer, and is, for example, a disposable diaper. The absorbent article 1 may be a disposable diaper for children or a disposable diaper for adults. As an example, the absorbent article 1 is configured as a so-called tape-type disposable diaper.
[0036] The absorbent article 1 comprises an absorbent main body 10, a pair of fastening tapes 21A, 21B (fixing members), and a target tape 30. In the absorbent article 1, the absorbent main body 10 is a part that has the function of absorbing bodily waste, and the pair of fastening tapes 21A, 21B and the target tape 30 are parts that have the function of attaching and fixing the absorbent main body 10 to a wearer. The fastening tapes 21A, 21B also have the function of fixing the shape of the absorbent article 1 so that the absorbent article 1 is maintained in a folded state, which will be described later, after use of the absorbent article 1, etc.
[0037] The absorbent main body 10 is divided into a front waist region 101, a rear waist region 102, and a crotch region 103. The front waist region 101 is a region that is located on the front waist side of the wearer when in use (when worn). The rear waist region 102 is a region that is located on the rear waist side of the wearer when in use. The crotch region 103 is a region that is located between the front waist region 101 and the rear waist region 102 in the front-to-back direction L, and is a region that is located under the crotch of the wearer when in use.
[0038] As shown in FIG. 3, the absorbent body 10 is configured to include an inner sheet member 11, an outer sheet member 12, and an absorbent body 13.
[0039] The absorbent body 13 is disposed between the inner sheet member 11 and the outer sheet member 12 and is responsible for absorbing the wearer's excrement. The absorbent body 13 includes an absorbent core 13a and a core wrap 13b. As an example, the absorbent core 13a is a laminate of absorbent materials including pulp (crushed pulp) and superabsorbent polymer (SAP). The core wrap 13b is formed of, for example, tissue or a nonwoven fabric sheet and is disposed so as to cover the skin-facing and non-skin-facing sides of the absorbent core 13a. The absorbent body 13 is disposed in the central portion of the absorbent body 10 in the width direction W, extending over substantially the entire area in the front-to-back direction L, except for both ends in the front-to-back direction L.
[0040] The SAP contained in the absorbent core 13a is biodegradable. Examples of biodegradable SAP materials include cellulose, cellulose nanofiber, carboxymethyl cellulose, starch, polyaspartic acid, and polyglutamic acid. The pulp contained in the absorbent core 13a is also derived from biomass and is therefore biodegradable. The core wrap 13b is also made of a biodegradable material, such as tissue made of cellulose. As a result, the absorbent body 13 as a whole is biodegradable.
[0041] The inner sheet member 11 is a member including one or more sheets that face the wearer's skin. In this embodiment, the inner sheet member 11 includes a top sheet 11a and a side sheet 11b. The top sheet 11a is a liquid-permeable sheet that is arranged on the skin-facing side so as to cover the absorbent body 13, and allows excrement such as urine to pass through to the absorbent body 13. The top sheet 11a is made of, for example, a liquid-permeable nonwoven fabric. The side sheets 11b are liquid-impermeable sheets that are arranged over the entire front-to-rear direction L outside the central portion of the absorbent body 13 in the width direction W so as to cover both side edges of the top sheet 11a in the width direction W. The side sheets 11b are made of, for example, a hydrophobic nonwoven fabric.
[0042] The top sheet 11a and the side sheets 11b are both biodegradable. They may be configured to be biodegradable by incorporating an additive (an additive for promoting biodegradation that is incorporated into the outer nonwoven fabric 12b) described below, or by being made of a biodegradable material such as cotton, regenerated cellulose such as rayon or lyocell, PBAT, PLA, PBS, PHA, PVA, PBSA, PGA, PETS, cellulose acetate, or a mixture of these in any ratio.
[0043] An elastic member 116a (see FIG. 2 ), such as rubber thread, is provided at the inner end of the side sheet 11b in the width direction W along the front-to-back direction L. The front end of the elastic member 116a reaches the front waist region 101, and its rear end reaches the rear waist region 102. Both ends of the side sheet 11b in the front-to-back direction L are attached (fixed) to the top sheet 11a with an adhesive or the like. The method of fixing the side sheet 11b to the top sheet 11a is not limited to adhesion, and may be ultrasonic bonding or heat fusion bonding using an embossing roll. An elastic member 115a, such as a stretchable sheet, is provided at the outer end of the side sheet 11b in the width direction W along the front-to-back direction L between the side sheet 11b and the outer nonwoven fabric 12b (described later). The front end of the elastic member 115a reaches the front waist region 101, and its rear end reaches the rear waist region 102.
[0044] The outer sheet member 12 is a member including one or more sheets disposed on the opposite side of the inner sheet member 11 from the skin side. Specifically, the outer sheet member 12 is disposed on the opposite side of the inner sheet member 11 across the absorbent body 13. The outer sheet member 12 includes a leak-proof sheet 12a (intermediate sheet) and an outer nonwoven fabric 12b. The leak-proof sheet 12a is a liquid-impermeable sheet disposed on the non-skin-facing side so as to cover the absorbent body 13, and functions to prevent leakage of bodily waste to the outside. Specifically, the leak-proof sheet 12a is disposed between the outer nonwoven fabric 12b and the absorbent body 13. The leak-proof sheet 12a is formed, for example, of a film. The outer nonwoven fabric 12b is a liquid-impermeable sheet disposed on the non-skin-facing side of the leak-proof sheet 12a. The outer nonwoven fabric 12b is formed, for example, of a hydrophobic nonwoven fabric. The outer nonwoven fabric 12b is an outer surface sheet that forms the outer surface of the outer sheet member 12 (i.e., the outermost surface facing away from the skin).
[0045] Both the leak-barrier sheet 12a and the outer nonwoven fabric 12b are biodegradable. The outer nonwoven fabric 12b is made of a degradable polymer composition that has been adjusted to have biodegradability (for example, the degradable polymer composition described in JP-A-2020-500254).
[0046] The outer nonwoven fabric 12b contains, as a main material (for example, a material constituting 50% by weight or more of the entire outer nonwoven fabric 12b), a polyolefin resin derived from petroleum or biomass, which is not biodegradable by itself. 2CRR']- repeating units. Preferably, R and R' are individually selected from the list including hydrogen, methyl, ethyl, acetate, vinyl acetate, methyl methacrylate, vinyl alcohol, and acrylic acid. The polyolefin resin constituting the outer nonwoven fabric 12b may, for example, contain ethylene and / or propylene monomers and may optionally further contain a monomer selected from the list including acetate, vinyl acetate, methyl methacrylate, vinyl alcohol, and acrylic acid. Alternatively, the polyolefin resin constituting the outer nonwoven fabric 12b may be selected from LDPE, LLDPE, HDPE, MDPE, VLDPE, EVA, EVOH, EMMA, and EAA.
[0047] Here, "not biodegradable" means that when left in a natural environment such as the air, soil, or sea, the material will not be decomposed into inorganic substances (water, carbon dioxide, methane, etc.) over a long period of time (e.g., two years) due to the absence of microbial action (i.e., not being decomposed by microorganisms), in other words, microplastics will remain without being decomposed. In other words, the polyolefin resin constituting the outer nonwoven fabric 12b itself is not biodegradable like, for example, polylactic acid resin. More specifically, the polyolefin resin constituting the outer nonwoven fabric 12b has a density of 1.0 g / m 3 The outer nonwoven fabric 12b has a density of 0.1 to 1.0 mm and is stronger than common biodegradable resins (e.g., polylactic acid resins). The outer nonwoven fabric 12b contains such a polyolefin resin as a primary material and is configured as a nonwoven fabric sheet having heat-sealed points or fused joints between fibers. The heat-sealed points are fused joints formed by heat-sealing (point bonding) using a thermal embossing process or the like. The fused joints are joints formed by joining the surfaces of resin fibers that have been melted by heat. This allows the outer nonwoven fabric 12b to have higher material strength (e.g., tensile strength) than when a biodegradable resin such as polylactic acid resin, which is biodegradable alone, is used.
[0048] As described above, the polyolefin resin constituting the outer nonwoven fabric 12b is not biodegradable by itself. For this reason, in this embodiment, an additive is added to the polyolefin resin constituting the outer nonwoven fabric 12b to modify the entire outer nonwoven fabric 12b to make it biodegradable. The additive is configured to promote biodegradation using at least one of oxygen, water, and ultraviolet light as a promoting factor. In the additive of this embodiment (i.e., the additive exemplified below), oxygen, water, and ultraviolet light all function as promoting factors for the decomposition reaction (breaking of C-C bonds).
[0049] As an example, the additives contained in the outer nonwoven fabric 12b may include, relative to the total weight of the polyolefin resin and additives constituting the outer nonwoven fabric 12b, (a) a total amount of 0.15 to 0.6 wt % of two or more transition metal compounds, and (b) a mono- or polyunsaturated C olefin copolymer in an amount of 0.04 to 0.08 wt %. 14 -C 24 (c) a carboxylic acid, or an ester, anhydride, or amide thereof, and a synthetic rubber in an amount of 0.04 to 0.2 wt %, and optionally, (d) dry starch in an amount of 0 to 20 wt %, and / or (e) calcium oxide in an amount of 0 to 1 wt %, and / or (f) a phenolic antioxidant stabilizer in an amount of 0 to 0.2 wt %, wherein the two or more transition metal compounds in (a) are selected from iron compounds, manganese compounds, copper compounds, cobalt compounds, and cerium compounds, and the transition metals in the two or more transition metal compounds are different.
[0050] The leakproof sheet 12a is a resin film that, like the outer nonwoven fabric 12b, contains a polyolefin resin, which is not biodegradable by itself, as its main material (e.g., a material that constitutes 50% by weight or more of the entire leakproof sheet 12a). In other words, the leakproof sheet 12a is a film member formed by melting a polyolefin resin and forming it into a sheet. Like the outer nonwoven fabric 12b, the polyolefin resin that constitutes the leakproof sheet 12a also contains the above-mentioned additives blended therein.
[0051] As shown in FIG. 2, the absorbent main body 10 has, as its functional configuration, leg stretchable sections 115 and leg side gathers 116.
[0052] The leg stretchable sections 115 are configured to have elastic members 115a, which are stretchable sections that are stretchable in the front-to-rear direction L, on both sides (both ends in the width direction W) of the absorbent main body 10. In the leg stretchable sections 115, the elastic members 115a contract to form leg gathers that improve the fit around the legs of the wearer in the crotch region 103 when in use.
[0053] The leg side gathers 116 are located more inward in the width direction W than the leg stretchable portions 115, have both ends in the front-to-back direction L fixed, and are configured to stand up by contracting in the front-to-back direction L. The leg side gathers 116 include the above-mentioned side sheets 11b. In the leg side gathers 116, both ends in the front-to-back direction L of the side sheets 11b are fixed to the top sheet 11a, and the elastic members 116a contract, thereby forming a pair of leakage-proof cuffs in the crotch region 103 in the used state that stand up toward the wearer's skin and prevent body waste from leaking along the surface of the top sheet 11a.
[0054] The fastening tapes 21A, 21B are configured to attach and secure the absorbent main body 10 to the wearer by being fastened to the target tape 30 when worn. As shown in FIGS. 1 and 2 , the fastening tapes 21A, 21B are provided at both ends in the width direction W of the rear waist region 102 of the absorbent main body 10 and are members that extend outward in the width direction W. The fastening tapes 21A, 21B are sandwiched and fixed between the side sheets 11b and the outer nonwoven fabric 12b of the absorbent main body 10, and are provided rearward of the rear end of the elastic member 115a. The fastening tapes 21A, 21B are provided symmetrically with respect to each other with respect to the central portion of the absorbent main body 10 in the width direction W and are provided at the same position in the front-to-rear direction. The fastening tapes 21A, 21B have similar shapes and structures. Each of the fastening tapes 21A, 21B has a base sheet 211, which is a main body, and an engaging portion 212 provided on the skin-facing surface of the base sheet 211. The engaging portion 212 is a portion that is fastened to the target tape 30. The engaging portion 212 is, for example, a hook sheet provided with a plurality of engaging hooks.
[0055] 1, the target tape 30 is provided in the front waist region 101 of the absorbent main body 10, and is a target portion to which the fastening portions 210 of the fastening tapes 21A, 21B are fastened. The target tape 30 is attached to the outer nonwoven fabric 12b in the front waist region 101.
[0056] As shown in Fig. 4 , the fastening tapes 21A, 21B also function as fixing members for fixing the shape of the absorbent article 1 so that the absorbent article 1 is maintained in a folded (rolled) state with the inner sheet member 11 enclosed inside. For example, after using the absorbent article 1, as shown in Fig. 4(A), the fastening tapes 21A, 21B are removed from the target tape 30 to unfold the absorbent article 1, and then the absorbent article 1 is rolled up from the front side (the front waist region 101 side) so that the inner sheet member 11 is on the inside. Thereafter, as shown in Fig. 4(B), the fastening tapes 21A, 21B are engaged with the outer surface of the outer nonwoven fabric 12b. This maintains the absorbent article 1 in a folded state. As such, in this embodiment, the engaging portions 212 of the fastening tapes 21A, 21B are configured to be engageable with the outer surface of the opposing outer nonwoven fabric 12b in the folded state. The engaging portions 212 of each fastening tape 21A, 21B may be configured to be engageable with the outer surface of the fastening tapes 21A, 21B (base sheet 211). In this case, the folded state can also be achieved by engaging the engaging portion 212 of one fastening tape with the outer surface of the base sheet 211 of the other fastening tape (the surface opposite to the side on which the engaging portion 212 is provided). In either case, the absorbent article 1 is maintained in the folded state by the engaging portions 212 of the fastening tapes 21A, 21B engaging with the outer surface of the base sheet 211 or the outer surface of the outer nonwoven fabric 12b.
[0057] The outer sheet member 12 and the fastening tapes 21A, 21B have outer exposed portions that are exposed to the outside in the folded state described above (see FIG. 4B). In this embodiment, the outer nonwoven fabric 12b of the outer sheet member 12 and the base sheet 211 of the fastening tapes 21A, 21B constitute the outer exposed portions.
[0058] Furthermore, the first portion, which is at least a part of the exposed outer portion, is composed of a polyolefin resin that is not biodegradable by itself and is configured to be biodegradable by blending the above-mentioned additive. As described above, in this embodiment, the entire outer nonwoven fabric 12b constitutes the first portion. Due to the addition of the above-mentioned additive, the first portion is configured to satisfy the biodegradation condition that the carbonyl index of the first portion is 1 or greater within 28 days from the start of the biodegradability evaluation test (ultraviolet accelerated weathering test) specified in PAS9017:2020.
[0059] In addition to the above-mentioned condition (the condition that the first portion has a carbonyl index of 1 or more), the biodegradation conditions may further include the condition that, within 14 days from the start of the evaluation test, the number-average molecular weight of the first portion becomes 5,000 or less, the z-average molecular weight of the first portion becomes 30,000 or less, and the loss of the weight-average molecular weight of the first portion becomes 90% or more. In this case, the biodegradation of the first portion can be promoted even more effectively.
[0060] Whether the first part satisfies the biodegradation conditions described above can be confirmed by the test method described below in accordance with PAS9017:2020. Note that this test method also includes a section that complies with the laboratory weathering standards of ASTM D4329-13 or BS EN ISO 4892-1. The sample (first part) is mounted on a jig. An ultraviolet accelerated weathering device capable of irradiating a combination of air, heat, and ultraviolet light is used. The calibration and test procedures for the device are as described in BS EN ISO 4892-3 or ASTM D4329-13. <For sample thicknesses less than 0.25 mm> The cycle of the ultraviolet accelerated weathering device is set to the following test conditions: (1) Irradiance: 0.8 W / m 2 ±0.02W / m 2(2) UV cycle time: 1 hour (3) Dark cycle time: 23 hours (4) Air chamber temperature: Set to 60°C ± 2°C, ensure test days are within 14 consecutive days, and ensure N3 for each sample. <For samples with a thickness of 0.25 mm or more> The above test conditions are adjusted as follows in accordance with the laboratory weathering standards of ASTM D2565-16 or BS EN ISO 4892-1. (1) Irradiance: 0.35 W / m 2 ±0.02W / m 2 (1) UV cycle time: 8 hours (2) Dark cycle time: 16 hours (3) Air chamber temperature: 60°C ± 2°C (4) Non-insulated black panel temperature: 70°C ± 2°C, and the test period must be within 28 consecutive days. The carbonyl index is determined using infrared spectroscopy and the resulting IR spectrum. The spectrum is measured from 500 to 3000 cm. -1 in the region of 1420 to 1500 cm -1 and 1650-1850 cm -1 The area of the carbonyl index is the focus. The resolution is set to 4 cm or less, and the number of scans is set to 32 or more. During the measurement, software capable of removing background noise and calculating the integral of the peak area is used. The carbonyl index is measured at least three times. The carbonyl index is calculated from the 1850-1650 cm -1 and 1500-1420 cm -1 The average carbonyl index for each sample is determined from the integrated peak areas of the three spectra collected. The molecular weight (number average, z-average, and weight average) of the sample is measured by gel permeation chromatography (GPC) or size exclusion chromatography (GPC-SEC). The measurements are performed with preparations according to BS ISO 16014-4 or ASTM D6474-20. The analysis of each sample is reported as the average of three runs. The collected samples should cover one-third of the total polyolefin material tested. The sample should be completely dissolved in the solvent used for molecular weight analysis.
[0061] Furthermore, the biodegradability evaluation described below may be performed using the entire absorbent article 1 in accordance with ASTM D 5988-18 and BS EN ISO 17556:2019. In this case, the evaluation may be performed using a sample prepared by adding the following additional conditions to the conditions of the test method described above. It is preferable that the sample meets N3 or higher, and if an invasive test is performed, it is preferable to meet even higher standards. <Additional Conditions> The water-absorbing material (absorbent core 13) contained in the sample (absorbent article 1) is 100% hydrated with physiological saline. The sample is placed in a state simulating disposal. For example, the sample is placed in the folded state shown in FIG. 4(B). The sheet materials constituting the sample (in this embodiment, the inner sheet member 11, outer sheet member 12, leak-proof sheet 12a, outer nonwoven fabric 12b, etc.) are maintained in a stacked state (this condition is met when an actual absorbent article 1 is used as the sample and folded as described above).
[0062] In the above additional conditions, "saline" refers to a 0.9% aqueous NaCl solution (aq) prepared using distilled water. Furthermore, "100% water-retained state" refers to the state after a sample is immersed in the saline solution for 30 minutes, placed on a mesh with the water-absorbent surface (i.e., the inner sheet member 11 on the absorbent body 13) facing downward, an acrylic plate (weight) is placed on the sample, a 10 kg load is applied for 20 minutes, and then dehydrated for 90 seconds at a rotation speed of 540 rpm using a centrifugal dehydrator (e.g., the top-discharge centrifuge H-130E manufactured by Kokusan Co., Ltd.).
[0063] Such evaluation of the biodegradation of the entire absorbent article 1 is carried out by placing the sample in an evaluation device having a space large enough to fit the entire sample (absorbent article 1) in, and irradiating the sample with ultraviolet light under test conditions similar to those of the ultraviolet accelerated weathering device described above. Note that, in order to ensure uniformity of the ultraviolet light irradiation on the sample, the sample may be rotated every predetermined period (for example, every three days).
[0064] (Effects) In the absorbent article 1, the first portion, which is at least a part of the outer exposed portion (in this embodiment, the entire outer nonwoven fabric 12b), is made of a polyolefin resin that is not biodegradable by itself. This reduces the cost of the absorbent article 1 and ensures the material strength of the first portion compared to when the first portion is made of a biodegradable resin such as polylactic acid resin. Furthermore, after use, the absorbent article 1 is typically discarded with the outer exposed portion exposed to the outside and the inner sheet member 11 and absorber 13 rolled up inward (i.e., in a folded state as shown in FIG. 4(B)). In the absorbent article 1, the first portion contains an additive that promotes biodegradation so as to satisfy the above-mentioned biodegradation conditions, thereby allowing the first portion of the absorbent article 1 to decompose quickly after disposal. As a result, microorganisms can penetrate quickly into the interior of the discarded absorbent article 1, thereby promoting the biodegradation of the entire absorbent article 1. Therefore, the absorbent article 1 can ensure the necessary material strength while suppressing increases in cost and promoting the biodegradation of the absorbent article 1 after disposal.
[0065] The additive blended in the first portion preferably contains the above-mentioned (f) phenolic antioxidant stabilizer. Known antioxidant stabilizers (e.g., Irganox 1076, Irganox 1010, etc.) can be used as the phenolic antioxidant stabilizer. Such phenolic antioxidant stabilizers suppress the biodegradation-promoting function of the additive for a certain period of time, delaying the onset of decomposition and extending the shelf life of the product. Therefore, with the above configuration, the start time of biodegradation can be appropriately adjusted so that decomposition begins after the expected shelf life of the product has elapsed. Note that, from the viewpoint of optimally exhibiting the biodegradation-suppressing function described above, the content of the phenolic antioxidant stabilizer in the additive is preferably set to 0.02 to 0.15 wt % relative to the total weight of the polyolefin resin and the additive.
[0066] As described above, in this embodiment, the additive for promoting biodegradation is added to two sheets (the outer nonwoven fabric 12b and the leakproof sheet 12a). The content (wt %) of the phenolic antioxidant stabilizer in each sheet may be greater in the outermost sheet. That is, in this embodiment, the content (wt %) of the phenolic antioxidant stabilizer in the outer nonwoven fabric 12b may be greater than the content (wt %) of the phenolic antioxidant stabilizer in the leakproof sheet 12a. In this way, by increasing the content of the phenolic antioxidant stabilizer in the outer portion (outer portion) that is more likely to be exposed to the outside air under normal conditions (during storage or use), thereby increasing the degree of inhibition of biodegradation, it is possible to appropriately prevent unexpected acceleration of biodegradation in the outer portion (outer nonwoven fabric 12b) of the outer sheet member 12. More specifically, the biodegradation of the outer nonwoven fabric 12b can be prevented from proceeding extremely faster than the biodegradation of the leak-barrier sheet 12a, and the biodegradation of the outer nonwoven fabric 12b and the leak-barrier sheet 12a can be adjusted so that they proceed in a balanced manner.
[0067] The tensile strength of the first portion (outer nonwoven fabric 12b) is preferably 0.3 N / mm in MD (tensile strength in the front-rear direction L). 2 and CD (tensile strength in the width direction W): 0.07 N / mm 2That's all. The tensile strength is measured by the following method. That is, a test piece having a length (length in the front-to-back direction L) of approximately 160 mm and a width (length in the width direction W) of 25 mm is taken, and the test piece is pulled in the vertical direction using a tensile tester (e.g., a constant-rate extension tensile tester) at a pulling rate of 100 mm / min and a chuck distance of 100 mm until the test piece breaks. The maximum force applied to the test piece when the test piece breaks is recorded as the tensile strength value. Note that if a sufficient length or width of the test piece cannot be ensured, the length and width of the test piece and the chuck distance can be changed as desired. Furthermore, the first portion has durability such that no pilling occurs after 50 reciprocating rubs under a 200 g load in a surface rub fastness test. The abrasion resistance of such a first portion is measured using a dyed fabric rub fastness tester based on JIS L0849. That is, a test specimen cut to a width (length in the width direction W) of 300 mm and a length (length in the front-rear direction L) of 150 mm is taken and attached to the stage of the testing machine with cellophane tape. Cloth tape is attached to the friction surface of the friction element, and the friction element is placed on the center surface of the test specimen. The number of reciprocating movements is set to 50, and the evaluation begins. After completion, the test specimen is removed from the stage, and the surface condition is observed. With the above configuration, the material strength of the first part can be suitably ensured, thereby improving the stability of the absorbent article 1 against deformation, breakage, etc. under normal conditions (storage or use).
[0068] The first portion (outer nonwoven fabric 12b) preferably has a thickness of 0.1 mm or more and 2.0 mm or less. If the thickness of the first portion is thinner than 0.1 mm, the feel on the skin is likely to be poor. Furthermore, if the thickness of the first portion is thicker than 2.0 mm, the large thickness reduces the decomposition rate of the first portion. Therefore, by setting the thickness of the first portion in the range of 0.1 mm or more and 2.0 mm or less, it is possible to suppress a decrease in the decomposition rate while maintaining a good feel on the skin. Note that, from the viewpoint of improving the decomposition rate of the first portion, the thickness of the first portion is preferably set to 0.25 mm or less.
[0069] The UV transmittance of the first portion (outer nonwoven fabric 12b) is preferably 15% or more. Whether or not the above condition is satisfied can be confirmed, for example, as follows. For example, a sample is irradiated with UV light of several wavelengths within the wavelength range of 280 to 400 nm, and the UV transmittance at each wavelength is measured using a spectrophotometer. The minimum UV transmittance at each wavelength must be 15% or more. This configuration allows UV light, which may promote biodegradation of components of the absorbent article 1 that are located inside the first portion (in this embodiment, the leak-barrier sheet 12a, absorber 13, and inner sheet member 11, etc.), to be transmitted through the first portion and effectively guided to the inner components. As a result, the onset of biodegradation within the absorbent article 1 can be accelerated, thereby improving the decomposition rate of the entire absorbent article 1.
[0070] The first part (outer nonwoven fabric 12b) and the leak-barrier sheet 12a are preferably configured so that the air permeability of the first part measured by a Frazier test is higher than the air permeability of the leak-barrier sheet 12a measured by a Frazier test. The Frazier test is a test to determine the air permeability (1 cm) based on the test method (Fragile method) specified in the air permeability test (JIS L 1096). 2 This test measures the density (a numerical value indicating how much air passes through an area of the first portion in one second). Furthermore, the first portion and the leak-barrier sheet 12a are preferably configured so that the density of the first portion is lower than the density of the leak-barrier sheet 12a. The density is measured, for example, as follows: The thickness of the first portion is measured using a thickness gauge, the dimensions (area) of the first portion are measured using a ruler, and the mass of the first portion is measured using an electronic balance. Finally, the "mass / volume (= thickness x area)" of the first portion is calculated as the density. This configuration allows water, oxygen, and other factors that can promote the biodegradation of the leak-barrier sheet 12a to permeate the first portion and be effectively guided to the leak-barrier sheet 12a. As a result, the onset of biodegradation of the interior of the absorbent article 1 (the leak-barrier sheet 12a) can be accelerated, thereby improving the decomposition rate of the entire absorbent article 1.
[0071] The air permeability of the first portion (outer nonwoven fabric 12b) measured by the Frazier test is preferably 100 cm3 / (cm 2 ・s) or more 700cm 3 / (cm 2 The air permeability is 700 cm 3 / (cm 2 s) or less, the function of the absorbent article 1 (for example, preventing leakage of body exudates from the first portion) is not impaired, while the air permeability is maintained at 100 cm 3 / (cm 2 By making the first portion s or more, water, oxygen, etc., which may be factors that promote biodegradation, can be properly guided through the first portion to the inside of the absorbent article 1. As a result, the start of biodegradation inside the absorbent article 1 can be accelerated, and the decomposition rate of the entire absorbent article 1 can be improved.
[0072] The density of the first portion (outer nonwoven fabric 12b) is preferably 0.02 g / m 3 0.1g / m or more 3 The density is 0.1 g / m or less. 3 By suppressing the density to 0.02 g / m or less, it is possible to prevent the loss of the functions of the absorbent article 1 (for example, prevention of leakage of excrement from the first portion, etc.) and to keep the density to 0.02 g / m or less. 3 By doing so, water, oxygen, and the like, which may be factors that promote biodegradation, can be properly guided through the first portion to the inside of the absorbent article 1. As a result, the start of biodegradation inside the absorbent article 1 can be accelerated, and the decomposition rate of the entire absorbent article 1 can be improved.
[0073] Since the absorbent body 13 (absorbent core 13a) contains a biodegradable superabsorbent polymer (SAP), the first part (outer nonwoven fabric 12b) of the absorbent article 1 can be biodegraded to allow microorganisms to reach the absorbent body 13, thereby allowing the absorbent body 13 to be properly biodegraded.
[0074] The factor promoting the biodegradation of the SAP contained in the absorbent 13 may be the same as the factor promoting the biodegradation of the first portion. In this embodiment, the first portion contains the additive described above, and decomposition (i.e., cleavage of carbon bonds, etc.) is initiated by each of water, oxygen, and ultraviolet light as promoting factors. In this case, the SAP may be configured to initiate decomposition by the same promoting factor as that of the first portion (in this embodiment, water, oxygen, and ultraviolet light). This configuration can prevent a situation in which only one of the first portion and the absorbent 13 (SAP) remains undecomposed in the same environment.
[0075] Alternatively, the factor promoting the biodegradation of the SAP contained in the absorbent body 13 may be different from the factor promoting the biodegradation of the first portion. More specifically, the factor promoting the biodegradation of the SAP contained in the absorbent body 13 may be configured to include a substance derived from excrement (e.g., urea), while the factor promoting the biodegradation of the first portion may be configured to not include a substance derived from excrement. With this configuration, the decomposition of the absorbent body 13 (superabsorbent polymer) can be initiated from the time the wearer excretes excrement on the absorbent article 1, thereby shortening the time until the biodegradation of the absorbent body 13 is complete. On the other hand, since the factor promoting the biodegradation of the first portion does not include a substance derived from excrement, it is possible to prevent the first portion from starting to decompose before the appropriate time for decomposition to begin (i.e., the time after the absorbent article 1 is discarded) triggered by excretion processing.
[0076] In the absorbent article 1, the first portion is configured to be biodegradable by the additive, so that a portion accounting for 90% or more of the total weight of the absorbent article 1 is configured to be biodegradable. As described above, the first portion is modified to be biodegradable by blending the additive. However, portions of the absorbent article 1 other than the first portion may be modified to be biodegradable by blending the additive, as with the first portion, or may be configured to be biodegradable by being formed of a biodegradable material other than the additive. An example of a non-biodegradable portion of the absorbent article 1 is the elastic member 116a, such as the rubber thread described above. This configuration can more effectively promote the biodegradation of the absorbent article 1 after disposal.
[0077] The degree of deterioration of the leakbarrier sheet 12a measured by the above-mentioned evaluation test (ultraviolet accelerated weathering test) is preferably higher than the degree of deterioration of the first portion measured by the above-mentioned evaluation test. Specifically, the degrees of deterioration of the leakbarrier sheet 12a and the first portion are compared based on the carbonyl index values after the above-mentioned evaluation test. The higher the carbonyl index value, the higher the degree of deterioration. More preferably, the content (wt %) of the additive in the leakbarrier sheet 12a is higher than the content (wt %) of the additive in the first portion. From the perspective of preventing leakage of excrement, the leakbarrier sheet 12a generally has a structure that is difficult to decompose. With the above-mentioned configuration, the leakbarrier sheet 12a can be made to be easily biodegradable. As a result, the decomposition rate of the entire absorbent article 1 can be improved.
[0078] Furthermore, the base sheet 211 of the fastening tapes 21A, 21B may contain, as a primary material, a polyolefin resin that is not biodegradable by itself, similar to the outer nonwoven fabric 12b. Furthermore, the fastening tapes 21A, 21B may be configured to have biodegradability that satisfies the above-mentioned biodegradation conditions by incorporating the same additives as the outer nonwoven fabric 12b. In other words, the first portion described above may include the base sheet 211 of the fastening tapes 21A, 21B. According to the above configuration, by promoting the biodegradation of the base sheet 211 of the fastening tapes 21A, 21B, which functions as a fixing member for fixing the shape of the absorbent article 1 so as to maintain the folded state in the discarded absorbent article 1, it is possible to cause the base sheet 211 to break, thereby releasing the folded state (see FIG. 4B ), and exposing the interior of the absorbent article 1 to the outside. As a result, microorganisms can easily come into contact with the inner components of the absorbent article 1, thereby improving the decomposition rate of the entire absorbent article 1.
[0079] The engagement strength between the engaging portion 212 and the outer surface (the outer surface of the outer nonwoven fabric 12b or the surface of the base sheet 211 of the other fastening tape) engaged with the engaging portion 212 after a predetermined period of time has elapsed since the start of the evaluation test (ultraviolet accelerated weathering test) of the first portion (here, the outer nonwoven fabric 12b or the base sheet 211 of the fastening tapes 21A, 21B) was initiated is preferably lower than the engagement strength between the engaging portion 212 and the outer surface before the evaluation test was initiated. The "predetermined period" is, for example, a period determined by the biodegradation conditions described above (i.e., 28 days from the start of biodegradation). The "engagement strength between the engaging portion 212 and the outer surface" is a value indicating the degree of engagement (difficulty in separating) between the engaging portion 212 and the outer surface of the outer nonwoven fabric 12b or the base sheet 211 with which the engaging portion 212 is engaged. The engagement strength is evaluated, for example, in an incubator at 40 degrees. For example, the value is measured by cutting the engaging portion 212 and the outer nonwoven fabric 12b, or the engaging portion 212 and the base sheet 211, into 50 mm square pieces, engaging them together, hanging an 800 g weight on the side of the engaging portion 212, and measuring the durability time until the weight falls.
[0080] The engagement strength acts to maintain the folded state (see FIG. 4B ). Furthermore, the biodegradability of at least a portion of the first portion (e.g., the amount of additive added) is adjusted so that the engagement strength between the engaging portion 212 and the outer surface engaged with the engaging portion 212 after a predetermined period of time has passed since the start of the biodegradation promotion of the first portion is lower than the engagement strength before the evaluation test was started. That is, the material strength of the first portion (including at least one of the outer nonwoven fabric 12b and the base sheet 211 of each fastening tape 21A, 21B) is reduced by biodegradation, resulting in a lower engagement strength than before the biodegradation of the first portion. This makes it easier for the engagement portion 212 to disengage from the outer surface after a predetermined period of time has passed since the start of the biodegradation promotion, thereby increasing the likelihood that the folded state will be released.
[0081] (Modifications of Absorbent Articles) While the embodiments of the absorbent article of the present disclosure have been described above, the materials and shapes of the components of the absorbent article are not limited to those described above, and various materials and shapes can be used. Furthermore, some of the components included in the configurations of the above-described embodiments may be modified or omitted, or other components may be added.
[0082] For example, in the above embodiment, a configuration in which both the outer nonwoven fabric 12b and the base sheet 211 correspond to the first part is exemplified, but it is also possible to configure the outer nonwoven fabric 12b and the base sheet 211 so that only one of them corresponds to the first part.
[0083] Furthermore, the type of absorbent article is not limited to the tape-type disposable diaper exemplified in the above embodiment. Fig. 5 is a perspective view of an absorbent article 1A according to a modified example. As shown in Fig. 5, the absorbent article 1A may be a pants-type disposable diaper. The absorbent main body 10A of the absorbent article 1A differs from the absorbent main body 10 of the absorbent article 1 mainly in that it is provided with a waist-opening H1 and a pair of left and right leg-openings H2. The waist-opening H1 is a portion through which the wearer's torso is inserted, and the pair of leg-openings H2 are portions through which the wearer's left and right legs are inserted. When the absorbent article 1A is worn by a wearer, engaging portions E extending in the vertical direction are provided at portions located on both the left and right sides of the wearer's torso. After use, the absorbent article 1A can be unfolded like the above-mentioned tape-type absorbent article 1 (see Figs. 1 and 2) by tearing the engaging portions E.
[0084] The absorbent article 1A does not include the fastening tapes 21A, 21B and the target tape 30 that are included in the absorbent article 1. On the other hand, as shown in Fig. 6 , a fastening tape 22 is provided in the widthwise center of the back side of the outer nonwoven fabric 12b of the absorbent article 1A to maintain the absorbent article 1A in a compactly rolled, folded state. In the absorbent article 1A, this fastening tape 22 functions as a fixing member for fixing the shape of the absorbent article 1A so as to maintain the folded state. For example, as shown in Fig. 6(A), the absorbent article 1A is rolled up so that the inner sheet member 11 is on the inside and the back side portion of the outer nonwoven fabric 12b on which the fastening tape 22 is provided is exposed on the outside, and then, as shown in Fig. 6(B), the adhesive surface of the fastening tape 22 is adhered to the outer surface of the outer nonwoven fabric 12b. This maintains the absorbent article 1A in a folded state. Note that Figure 6 (A) shows an example of rolling up the absorbent article 1A without tearing the engaging portion E, but the absorbent article 1A may also be rolled up in the same manner as the absorbent article 1 (see Figure 4 (A)) after tearing the engaging portion E.
[0085] The absorbent article may be a disposable absorbent pad to be worn inside a worn article such as cloth underwear, or a sanitary napkin for women. When the absorbent article is a sanitary napkin, the sheet member corresponding to the outer nonwoven fabric 12b may be omitted, and a sheet member (film) corresponding to the leak-barrier sheet 12a may constitute the outermost layer of the absorbent article. In this case, the sheet member corresponding to the leak-barrier sheet 12a may correspond to the first portion described above.
[0086] (Package) Figures 7 and 8 are diagrams showing an example of a package 50 in which a plurality of absorbent articles 1 (for example, 26) are housed together. The package 50 includes a package sheet 51 for packaging the plurality of absorbent articles 1. The package sheet 51 is formed, for example, in the shape of a bag having a substantially rectangular parallelepiped shape when the plurality of absorbent articles 1 are housed inside. The package sheet 51 is made of a synthetic resin such as polyethylene, polypropylene, or polyethylene terephthalate. As an example, the package 50 can house a plurality of absorbent articles 1 in two tiers as shown in Figure 8. The housed absorbent articles 1 are folded in half so that the inner sheet member 11 is on the inside. In each tier, the plurality of absorbent articles 1 are arranged so that the outer surfaces of the outer nonwoven fabrics 12b of adjacent absorbent articles 1 are in surface contact with each other.
[0087] The oxygen permeability of the packaging sheet 51 is preferably lower than that of the first portion (e.g., the outer nonwoven fabric 12b) of the absorbent article 1. More preferably, the oxygen permeability of the packaging sheet 51 is lower than that of the leakproof sheet 12a of the absorbent article 1. The oxygen permeability is measured by gas chromatography or electrolytic sensor method in accordance with JIS K 7126-2 or ISO 15105-2.
[0088] The UV transmittance of the packaging sheet 51 is preferably lower than that of the first portion (e.g., the outer nonwoven fabric 12b) of the absorbent article 1. More preferably, the UV transmittance of the packaging sheet 51 is lower than that of the leakproof sheet 12a of the absorbent article 1. The UV transmittance for the above comparison can be obtained, for example, as follows. For example, a sample is irradiated with UV light of several wavelengths in the wavelength range of 280 to 400 nm, and the UV transmittance of each wavelength is measured using a spectrophotometer. The minimum UV transmittance of each wavelength can then be used as the comparison target.
[0089] The packaging sheet 51 preferably seals the internal space (i.e., the space inside the packaging sheet 51) in which the absorbent article 1 is housed. More specifically, the packaging sheet 51 does not have perforated through holes that are generally provided for opening.
[0090] The packaging body 50 can prevent oxygen, ultraviolet rays, and the like, which may accelerate biodegradation, from entering the packaging body 50 when the absorbent article 1 is contained and stored in the packaging sheet 51 before use (packaged state). This prevents the start of biodegradation of the absorbent article 1 (first part) from being accelerated, i.e., prevents the product life of the absorbent article 1 from being shorter than expected. Therefore, the packaging body 50 can suitably package the absorbent article 1 described above. The absorbent article contained in the packaging body 50 may be a pants-type absorbent article 1A, or may be an absorbent article other than a disposable diaper (e.g., an absorbent pad, a sanitary napkin, etc.). The shape of the packaging sheet 51 may be changed depending on the type and quantity of absorbent articles to be contained.
[0091] DESCRIPTION OF SYMBOLS 1, 1A...absorbent article, 11...inner sheet member, 12...outer sheet member, 12a...leak-proof sheet (intermediate sheet), 12b...outer nonwoven fabric (exposed outer portion, first portion), 13...absorbent body, 21A, 21B...fastening tape (fixing member, exposed outer portion, first portion), 22...fastening tape (fixing member, exposed outer portion, first portion), 50...packaging body, 51...packaging sheet, 211...base material sheet, 212...engaging portion.
Claims
1. An absorbent article for absorbing excrement discharged by a wearer, comprising: an inner sheet member including one or more sheets facing the skin of the wearer; an outer sheet member including one or more sheets arranged on the opposite side of the inner sheet member from the skin side; an absorbent body arranged between the inner sheet member and the outer sheet member for absorbing excrement of the wearer; and a fixing member for fixing the shape of the absorbent article so as to maintain a folded state in which the absorbent article is folded so that the inner sheet member is surrounded on the inside; at least one of the outer sheet member and the fixing member has an outer exposed portion exposed to the outside in the folded state; a first portion which is at least a part of the outer exposed portion is composed of a polyolefin resin which does not have biodegradability by itself; and the first portion is configured to satisfy the biodegradation condition that the carbonyl index of the first portion is 1 or more within 28 days from the start of an evaluation test specified in PAS9017:2020 by containing an additive which causes the polyolefin resin to biodegrade using at least one of oxygen, water, and ultraviolet light as an accelerating factor. Absorbent articles.
2. The absorbent article according to claim 1, wherein the additive comprises a phenolic antioxidant stabilizer.
3. The absorbent article according to claim 2, wherein the content of said phenol-based antioxidant stabilizer in said additive is 0.02 to 0.15% by weight based on the total weight of said polyolefin resin and said additive.
4. The absorbent article according to claim 2 or 3, wherein the outer sheet member comprises a plurality of sheets, the additive is added to at least two or more of the plurality of sheets, and the content of the phenol-based antioxidant stabilizer in each of the two or more sheets is greater in the sheet disposed on the outside.
5. The tensile strength of the first portion is MD: 0.3 N / mm 2 or more and CD: 0.07 N / mm 2 The absorbent article according to claim 1 .
6. The absorbent article according to claim 1, wherein the first portion has durability such that no pilling occurs after 50 reciprocating rubs under a load of 200 g in the surface rub fastness test specified in JIS L0849.
7. The absorbent article according to claim 1, wherein the first portion has a thickness of 0.1 mm or more and 2.0 mm or less.
8. The absorbent article according to claim 1, wherein the ultraviolet transmittance of the first portion is 15% or more.
9. The absorbent article according to claim 1, wherein the outer sheet member has a biodegradable intermediate sheet disposed between the first portion and the absorbent body, and the air permeability of the first portion measured by a Frazier test is higher than the air permeability of the intermediate sheet measured by a Frazier test.
10. The absorbent article according to claim 1, wherein the outer sheet member has a biodegradable intermediate sheet disposed between the first portion and the absorbent body, and the density of the first portion is lower than the density of the intermediate sheet.
11. The air permeability of the first part measured by the Frazier test is 3 / (cm 2 ・s) or more 700cm 3 / (cm 2 The absorbent article of claim 1, wherein the thickness of the absorbent article is less than or equal to s.
12. The density of the first portion is 0.02 g / m 3 0.1g / m or more 3 2. The absorbent article of claim 1, wherein:
13. The absorbent article according to claim 1, wherein the absorbent body comprises a biodegradable highly absorbent polymer.
14. The absorbent article according to claim 13, wherein the biodegradation promotion factor of the superabsorbent polymer is the same as the biodegradation promotion factor of the first portion.
15. The absorbent article according to claim 13, wherein the biodegradation promoter of the superabsorbent polymer includes a substance derived from the excrement, and the biodegradation promoter of the first portion does not include a substance derived from the excrement.
16. The absorbent article according to claim 1, wherein the first portion is rendered biodegradable by the additive, so that a portion accounting for 90% or more of the total weight of the absorbent article is configured to be biodegradable.
17. The absorbent article described in claim 1, wherein the outer sheet member has a biodegradable intermediate sheet disposed between the first portion and the absorbent body, and the degree of deterioration of the intermediate sheet measured by the evaluation test is higher than the degree of deterioration of the first portion measured by the evaluation test.
18. The absorbent article according to claim 17, wherein the intermediate sheet also contains the additive, and the content of the additive in the intermediate sheet is greater than the content of the additive in the first portion.
19. The absorbent article described in claim 1, wherein the fixing member includes a base sheet and an engagement portion provided on a surface of the base sheet, the first portion includes the base sheet, and the engagement portion is configured to be engageable with the outer sheet member or the outer surface of the fixing member so as to maintain the folded state.
20. An absorbent article as described in claim 19, wherein the engagement strength between the engagement portion and the outer surface after a predetermined period of time has elapsed since the start of the evaluation test of the first part is lower than the engagement strength between the engagement portion and the outer surface before the evaluation test is started.
21. The absorbent article of claim 1, wherein the biodegradation conditions further include the conditions that, within 14 days from the start of the evaluation test, the number average molecular weight of the first portion is 5,000 or less, the z-average molecular weight of the first portion is 30,000 or less, and the loss of the weight average molecular weight of the first portion is 90% or more.
22. A packaging body for packaging a plurality of absorbent articles according to claim 1 together, comprising a packaging sheet for packaging the plurality of absorbent articles, the packaging sheet having an oxygen permeability lower than the oxygen permeability of the first portion.
23. The packaging body according to claim 22, wherein the outer sheet member of the absorbent article has an intermediate sheet disposed between the first portion and the absorbent body, and the oxygen permeability of the packaging sheet is lower than the oxygen permeability of the intermediate sheet.
24. A packaging body for packaging a plurality of absorbent articles according to claim 1 together, comprising a packaging sheet for packaging the plurality of absorbent articles, the packaging sheet having an ultraviolet transmittance lower than the ultraviolet transmittance of the first portion.
25. The packaging body according to claim 24, wherein the outer sheet member of the absorbent article has an intermediate sheet disposed between the first portion and the absorbent body, and the ultraviolet transmittance of the packaging sheet is lower than the ultraviolet transmittance of the intermediate sheet.
26. A packaging unit for packaging a plurality of absorbent articles according to claim 1 together, comprising a packaging sheet for packaging a plurality of said absorbent articles, said packaging sheet sealing an internal space in which said absorbent articles are contained.
Citation Information
Patent Citations
disposable diaper
JP1994061227U
Disintegrable polyolefin composition
JP1996188678A
Method for inhibiting microbial infections associated with hygiene products
JP2002540900A
Method and device for manufacturing composite of continuous sheets for absorptive article
JP2011083547A
Different-phase structured fibers, textile sheets, and their uses
JP2011514450A