Heat dissipation grease
The thermal grease composition, with a silicone-based matrix and optimized filler components, addresses the trade-off between viscosity and bleed resistance, providing excellent bleed resistance and heat dissipation performance.
Patent Information
- Application Number
- PCT/JP2024/018939
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2024-05-23
- Publication Date
- 2024-11-28
AI Technical Summary
Thermal greases face a trade-off between low viscosity for handling and bleed resistance, with low viscosity compositions prone to bleeding, which can contaminate surrounding areas and alter their characteristics over time.
A thermal grease composition featuring a matrix component with silicone and surfactant, along with a filler component including polyhedral spherical and spherical fillers, optimized for shear rates and particle sizes to achieve reduced viscosity and enhanced bleed resistance, with specific ratios and content percentages to suppress bleeding.
The thermal grease achieves excellent bleed resistance while maintaining reduced viscosity, ensuring effective heat dissipation and long-term stability without contaminating surrounding areas.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure 00000026_0000
Abstract
Description
thermal grease
[0001] The present invention relates to a thermal grease.
[0002] As heat-generating electronic components such as central processing units (CPUs) in personal computers become smaller and more powerful, the amount of heat generated per unit area by these electronic components has become extremely large. This amount of heat can reach approximately 20 times that of an iron. To prevent these heat-generating electronic components from breaking down over the long term, cooling of the heat-generating electronic components is necessary.
[0003] Metallic heat sinks and housings are used for cooling, and thermally conductive materials are also used to efficiently transfer heat from heat-generating electronic components to cooling parts such as heat sinks and housings. When a heat-generating electronic component comes into contact with a heat sink or other device without a thermally conductive material, air is present at the interface, microscopically, and acts as an obstacle to heat conduction. Therefore, heat can be efficiently transferred by placing a thermally conductive material between the heat-generating electronic component and the heat sink, replacing the air at the interface.
[0004] Thermally conductive materials include thermally conductive pads and sheets made by filling thermosetting resin with a thermally conductive filler and molding it into a sheet; thermal grease made by filling a fluid resin with a thermally conductive filler and making it possible to spread it or make it into a thin film; and phase-change thermally conductive materials that soften or flow at the operating temperature of heat-generating electronic components.
[0005] Sheet-type heat-dissipating materials are easy to handle and have excellent long-term shape retention, but they have high contact thermal resistance and are inferior to grease-type materials in terms of automated mounting. Therefore, in recent years, the use of heat-dissipating grease in the thicknesses that were previously used for sheets has been increasing.
[0006] Such thermal greases generally contain an inorganic filler in a resin that has been surface-treated with a silane coupling agent or the like. Known surface treatment agents other than silane coupling agents include, for example, copolymers containing polybutadiene structural units, structural units having hydrolyzable silyl groups, and structural units having a polysiloxane skeleton (see, for example, Patent Document 1).
[0007] Japanese Patent Application Laid-Open No. 2018-062552
[0008] Thermal grease is required to have low viscosity from the viewpoint of handling, such as ease of discharge and application. However, formulating a material to achieve low viscosity can actually lead to the problem of the components in the thermal grease being more susceptible to bleeding. In other words, there is a trade-off between low viscosity and improved bleeding resistance. If bleeding occurs, the properties of the thermal grease may change over time, and the bleed-out components may contaminate the surrounding area.
[0009] The present invention has been made in view of the above problems, and has an object to provide a thermal grease that has excellent bleeding resistance.
[0010] That is, the present invention is as follows: [1] A composition comprising a matrix component and a filler component, wherein the matrix component contains silicone A and surfactant B, and the composition is heated at a shear rate of 10 s -1 Shear rate 1s for viscosity η1 -1 A thermally conductive grease, wherein the ratio (η2 / η1) of the viscosity η2 of the filler C11 to the viscosity η2 of the filler C12 is 4.0 to 9.0, and the viscosity η1 is 800 mPa·s or less. [2] The thermally conductive grease according to [1], wherein the filler component includes filler C1 having an average particle size of 0.10 to 2.0 μm, and the filler C1 includes polyhedral spherical filler C11 and spherical filler C12. [3] The thermally conductive grease according to [2], wherein the content of the filler C11 is 3.0 to 15 mass% with respect to the total amount of the filler component, and spherical filler C12. [4] The thermally conductive grease according to [2] or [3], wherein the ratio of the content of the filler C11 to the content of the filler C12 is 0.5 to 5.0. [5] The thermal grease according to any one of [1] to [4], wherein the total content of the filler C1 is 5.0 to 25 mass% with respect to the total amount of the filler components.
[0011] According to the present invention, a thermal grease having excellent bleeding resistance can be provided.
[0012] FIG. 1 is a schematic diagram showing an image of bleed-out measurement.
[0013] The following describes in detail an embodiment of the present invention (hereinafter referred to as "the present embodiment"); however, the present invention is not limited to this embodiment, and various modifications are possible without departing from the spirit of the present invention.
[0014] 1. Thermal Grease The thermal grease of this embodiment contains a matrix component and a filler component. The matrix component contains silicone A and surfactant B. The thermal grease is heated at a shear rate of 10 s -1 Shear rate 1s for viscosity η1 -1 The ratio (η2 / η1) of the viscosity η2 of the ink is 4.0 to 9.0, and the viscosity η1 is 800 mPa·s or less.
[0015] 1.1 Viscosity of thermal grease at a shear rate of 10 s -1 The viscosity η1 of the ink composition is 800 mPa s or less, and may be preferably 100 to 750 mPa s, 150 to 700 mPa s, 200 to 650 mPa s, 250 to 600 mPa s, 300 to 550 mPa s, or 350 to 500 mPa s. When the viscosity η1 is 800 mPa s or less, the viscosity is further reduced, and bleeding tends to be further suppressed.
[0016] Shear rate of thermal grease: 1 s -1 The viscosity η2 of the ink composition may be preferably 1250 to 3900 mPa·s, 1500 to 3800 mPa·s, 1750 to 3700 mPa·s, 2000 to 3600 mPa·s, or 2250 to 3500 mPa·s. When the viscosity η2 is within the above range, the viscosity is further reduced, and bleeding tends to be further suppressed.
[0017] The ratio of viscosity η2 to viscosity η1 (η2 / η1) is 4.0 to 9.0, preferably 4.5 to 8.5, 5.0 to 8.0, 5.5 to 7.5, or even 6.0 to 7.0. When the ratio (η2 / η1) is within the above range, the viscosity tends to be further reduced, and bleeding tends to be further suppressed.
[0018] The viscosity η1, viscosity η2, and ratio (η2 / η1) can be adjusted by the type and amount of the matrix component and filler component of the thermal grease. More specifically, they can be adjusted by the combination of silicones with different kinematic viscosities that can be used in the matrix component, or by the particle size and amount of the filler.
[0019] The viscosities η1 and η2 in this embodiment can be measured under predetermined shear rate conditions in accordance with JIS Z 8803. The viscosity measurement temperature is 25° C. unless otherwise specified.
[0020] 1.2. Matrix Component The matrix component contains a silicone A and a surfactant B, and a silane coupling agent D may be used as needed.
[0021] 1.2.1. Silicone A The shape of silicone A is not particularly limited, but examples thereof include non-crosslinked silicones such as linear silicones, branched silicones, and cyclic silicones; and crosslinked silicones that are three-dimensionally crosslinked within the molecule. Among these, non-crosslinked silicones are preferred, and linear silicones are more preferred. By using such silicone A, viscosity tends to decrease and dripping tends to be more suppressed.
[0022] Generally, silicones contain monofunctional units (R 1 SiO 1/2 ), bifunctional units (R 2 SiO 2/2 ), trifunctional unit (R 3 SiO 3/2 ), and a tetrafunctional unit (SiO 4/2 For example, a linear silicone can be represented by a monofunctional unit (R 1 SiO 1/2 ) and a bifunctional unit (R 2 SiO 2/2 ) (n3, n4 = 0 in the following formula), and cyclic silicones can be expressed as having a bifunctional unit (RSiO 2/2 ) (n1, n3, n4 = 0 in the following formula). In addition, branched silicones and three-dimensionally crosslinked silicones have a trifunctional unit (R3 SiO 3/2 ) and / or tetrafunctional units (SiO 4/2 ), and further comprising a monofunctional unit (R 1 SiO 1/2 ), a bifunctional unit (R 2 SiO 2/2 ) can be expressed as having
[0023] A composition formula using such units can be expressed as follows: In the following formula, n1 to n4 indicate the composition ratio of each unit, and can be expressed as a ratio such that the sum of n1 to n4 is 1. Whether or not these units are contained can be measured by a known method such as Si-NMR. 1 ~R 3 Each of R can independently represent any group. 1 SiO 1/2 ) n1 (R 2 SiO 2/2 ) n2 (R 3 SiO 3/2 ) n3 (SiO 4/2 ) n4
[0024] Silicone A is not particularly limited, but examples thereof include non-curable silicone and curable silicone.Non-curable silicone resin is not particularly limited as long as it does not have the functional group that contributes to curing that curable silicone resin has, or is not used in combination with a catalyst.In addition, curable silicone is not particularly limited, but examples thereof include a combination of two types of silicone having functional groups that react with each other.Such curable silicone is not particularly limited, but examples thereof include addition curable silicone, condensation curable silicone, and peroxide curable silicone.
[0025] Among these, it is preferable that the silicone A is a non-curing type silicone. By using such a silicone A, a one-component type thermal grease can be obtained, which tends to further improve the ease of handling.
[0026] Silicone A is not particularly limited, but examples thereof include dimethyl silicone, diphenyl silicone, and methylphenyl silicone. These silicones may have an organic group introduced into their side chains and / or terminals. Examples of such silicones are not particularly limited, but examples thereof include non-reactive silicones such as long-chain alkyl-modified silicone, polyether-modified silicone, aralkyl-modified silicone, fatty acid ester-modified silicone, and fatty acid amide-modified silicone; and reactive silicones such as amine-modified silicone, epoxy-modified silicone, mercapto-modified silicone, carboxyl-modified silicone, carbinol-modified silicone, and hydrogen-modified silicone.
[0027] Among these, dimethyl silicone, diphenyl silicone, methylphenyl silicone, and non-reactive silicone are preferred, and dimethyl silicone is more preferred. By using such silicone A, viscosity tends to decrease and dripping tends to be further suppressed.
[0028] The content of silicone A is preferably 60% by mass or more, 65% by mass or more, 70% by mass or more, or even 75% by mass or more, relative to the total amount of the matrix components. Furthermore, the content of silicone A is preferably 90% by mass or less, 85% by mass or less, or even 80% by mass or less, relative to the total amount of the matrix components. When the content of silicone A relative to the total amount of the matrix components is within the above range, the viscosity tends to decrease, and dripping tends to be further suppressed.
[0029] In this embodiment, the silicone A may contain at least one of a first silicone A1 having a kinematic viscosity of 150 cs or more but less than 400 cs and a second silicone A2 having a kinematic viscosity of 400 cs or more but less than 800 cs, or may contain both. Among these, it is preferable to contain both the first silicone A1 and the second silicone A2. By containing both the first silicone A1 and the second silicone A2, the viscosity tends to be further reduced and bleeding suppression tends to be further improved.
[0030] The kinematic viscosity in this embodiment can be measured in accordance with JIS K 2283. The kinematic viscosity is measured at 25° C. unless otherwise specified.
[0031] The kinematic viscosity of the first silicone A1 is 150 cs or more and less than 400 cs, preferably 200 to 375 cs, 225 to 350 cs, or 250 to 350 cs. Use of such a first silicone A1 tends to further reduce the viscosity.
[0032] The content of the first silicone A1 is preferably 5 to 60 mass%, 10 to 50 mass%, 15 to 40 mass%, or 20 to 35 mass%, relative to the total amount of the matrix components. When the content of the first silicone A1 is within the above range, the viscosity tends to be further reduced.
[0033] The kinematic viscosity of the second silicone A2 is 400 cs or more and 800 cs or less, preferably 425 to 750 cs, 450 to 600 cs, 475 to 650 cs, 475 to 600 cs, or 475 to 550 cs. By using such a second silicone A2, bleeding tends to be further suppressed.
[0034] The content of the second silicone A2 is preferably 15 to 60 mass%, 20 to 55 mass%, 25 to 50 mass%, or 30 to 45 mass%, relative to the total amount of the matrix components. By keeping the content of the second silicone A2 within the above range, bleeding tends to be further suppressed.
[0035] The ratio (A1 / A2) of the content of the first silicone A1 to the content of the second silicone A2 is preferably 0.10 to 2.0, 0.25 to 1.5, 0.40 to 1.2, or 0.60 to 1.0. When the ratio (A1 / A2) is within the above range, the viscosity decreases and bleeding tends to be further suppressed.
[0036] 1.2.2. Surfactant B The surfactant B is not particularly limited. Among these, a polymer having a silicone (meth)acrylic monomer unit γ is preferred as the surfactant B, and a copolymer having a (meth)acrylic monomer unit α having an anionic group, a (meth)acrylic monomer unit β having a cationic group, and a silicone (meth)acrylic monomer unit γ is more preferred. By using such a surfactant B, the dispersibility of the filler component can be maintained. Therefore, even if the filler component is highly filled from the viewpoint of thermal conductivity, the viscosity tends to be further reduced and changes in hardness tend to be further suppressed. In addition, bleeding also tends to be further suppressed.
[0037] The content of surfactant B is preferably 10 to 60 wt %, 15 to 55 wt %, 20 to 50 wt %, or 25 to 45 wt %, relative to the total amount of the matrix components. When the content of surfactant B is within the above range, viscosity, hardness changes, and bleeding tend to be further suppressed.
[0038] Surfactant B will be described in more detail below. In this embodiment, "monomer" refers to a monomer having a polymerizable unsaturated bond before polymerization, and "monomer unit" refers to a repeating unit that constitutes part of surfactant B after polymerization and is derived from a specific monomer. Furthermore, (meth)acrylic includes acrylic and methacrylic, and (meth)acrylic monomers include (meth)acrylate and (meth)acrylamide. Furthermore, hereinafter, "(meth)acrylic monomer unit α" and the like will also be simply referred to as "unit α" and the like.
[0039] 1.2.2.1. (Meth)acrylic Monomer Unit α The (meth)acrylic monomer unit α is a repeating unit having an anionic group. The anionic group is not particularly limited, but examples thereof include a carboxy group, a phosphate group, a phenolic hydroxy group, and a sulfonic acid group. Among these, one or more groups selected from the group consisting of a carboxy group, a phosphate group, and a phenolic hydroxy group are preferred. The presence of such a group tends to further improve the dispersibility of the filler component.
[0040] Furthermore, it is preferable that the unit α further has an electron-withdrawing group bonded to the anionic group. Such an electron-withdrawing group is not particularly limited as long as it has the effect of stabilizing the anion of the anionic group. For example, an acrylic monomer containing an electron-withdrawing substituent such as a halogen element on the carbon atom at the α-position of the carboxy group may be used. The presence of such a group tends to further improve the dispersibility of the filler component.
[0041] The unit α preferably does not have an electron-donating group bonded to the anionic group or has a group with low electron-donating properties. Such electron-donating groups are not particularly limited as long as they have the effect of destabilizing the anion of the anionic group. For example, an acrylic monomer that does not contain a substituent of an electron-donating group such as a methyl group on the carbon atom at the α-position of the carboxyl group may be used. By using such a structure, the dispersibility of the filler component tends to be further improved.
[0042] Such a (meth)acrylic monomer is not particularly limited, but examples thereof include acrylic acid, methacrylic acid, acid phosphooxypropyl methacrylate, acid phosphooxypolyoxyethylene glycol monomethacrylate, acid phosphooxypolyoxypropylene glycol monomethacrylate, phosphoric acid-modified epoxy acrylate, 2-acryloyloxyethyl acid phosphate, 2-methacryloyloxyethyl acid phosphate, 4-hydroxyphenyl acrylate, 4-hydroxyphenyl methacrylate, 2-methacryloyloxyethyl succinic acid, and 2-acrylamido-2-methylpropanesulfonic acid.
[0043] Among these, acrylic acid, 2-methacryloyloxyethyl acid phosphate, 4-hydroxyphenyl methacrylate, and 2-acrylamido-2-methylpropanesulfonic acid are preferred, with acrylic acid being more preferred. By including units derived from such monomers, viscosity tends to be further reduced and hardness changes tend to be further suppressed. In addition, dripping tends to be further suppressed. The unit α may be used alone or in combination of two or more types.
[0044] The content of the units α is preferably 1.0 mol% or more, 5.0 mol% or more, 10 mol% or more, 20 mol% or more, 30 mol% or more, 40 mol% or more, or even 45 mol% or more, relative to 100 mol% of the total of the units α, units β, and units γ. Furthermore, the content of the units α is preferably 85 mol% or less, 80 mol% or less, 75 mol% or less, or even 70 mol% or less, relative to 100 mol% of the total of the units α, units β, and units γ. When the content of the units α is within the above range, the viscosity tends to be further reduced, and the change in hardness tends to be further suppressed.
[0045] The molar ratio of units α to units β is preferably 0.5 or more, 1.0 or more, 2.5 or more, 5.0 or more, 10 or more, 15 or more, 20 or more, or even 25 or more. The molar ratio of units α to units β is preferably 150 or less, 100 or less, 75 or less, 50 or less, or even 40 or less. When the molar ratio of units α to units β is within the above range, the viscosity tends to be further reduced and the change in hardness tends to be further suppressed.
[0046] 1.2.2.2. (Meth)acrylic Monomer Unit β The (meth)acrylic monomer unit β is a repeating unit having a cationic group. The cationic group is not particularly limited, but is preferably, for example, one or more selected from the group consisting of a primary amino group, a secondary amino group, a tertiary amino group, and a quaternary ammonium salt. Of these, a tertiary amino group is more preferred. The presence of such a group tends to further improve the dispersibility of the filler component.
[0047] Furthermore, it is preferable that the unit β further has an electron-donating group bonded to the cationic group. Such an electron-donating group is not particularly limited as long as it has the effect of stabilizing the cation of the cationic group. For example, an acrylic monomer containing an electron-donating substituent such as a methyl group on the carbon atom at the α-position of the amino group may be used. The presence of such a group tends to further improve the dispersibility of the filler component.
[0048] Preferably, the β unit does not have an electron-withdrawing group bonded to a cationic group or has a group with low electron-withdrawing properties. Such electron-withdrawing groups are not particularly limited as long as they have the effect of destabilizing the cation of the cationic group. For example, an acrylic monomer that does not contain a substituent of an electron-withdrawing group such as a carboxyl group on the carbon atom at the α-position of the amino group may be used. This structure tends to further improve the dispersibility of the filler component.
[0049] Such (meth)acrylic monomers are not particularly limited, and examples thereof include 1-aminoethyl acrylate, 1-aminopropyl acrylate, 1-aminoethyl methacrylate, 1-aminopropyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, t-butylaminoethyl (meth)acrylate, dimethylaminoethyl methacrylate quaternary salt, 1,2,2,6,6-pentamethyl-4-piperidyl acrylate, 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate, 2,2,6,6-tetramethyl-4-piperidyl methacrylate, and dimethylaminoethyl acrylate benzyl chloride quaternary salt.
[0050] Among these, 1,2,2,6,6-pentamethyl-4-piperidyl acrylate, 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate, and 1-aminoethyl methacrylate are preferred, and 1,2,2,6,6-pentamethyl-4-piperidyl acrylate and 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate are more preferred. By containing units derived from such monomers, the viscosity tends to be further reduced and the change in hardness tends to be further suppressed. The unit β may be used alone or in combination of two or more types.
[0051] The content of the units β is preferably 0.05 mol% or more, 0.10 mol% or more, 0.50 mol% or more, 1.00 mol% or more, or even 1.50 mol% or more, relative to 100 mol% of the total of the units α, β, and γ. Furthermore, the content of the units β is preferably 10 mol% or less, 8.0 mol% or less, 6.0 mol% or less, 3.0 mol% or less, or even 2.0 mol% or less, relative to 100 mol% of the total of the units α, β, and γ. When the content of the units β is within the above range, the viscosity tends to be further reduced, and the change in hardness tends to be further suppressed.
[0052] 1.2.2.3. (Meth)acrylic Monomer Unit γ The (meth)acrylic monomer unit γ is a silicone (meth)acrylic monomer unit, which is a (meth)acrylic monomer that does not contain a cationic group or an anionic group in the molecule but has a silicone group.
[0053] The (meth)acrylic monomer γ preferably has a skeleton that has high affinity or compatibility with other matrix components. The (meth)acrylic monomer γ has such a skeleton as a silicone skeleton such as dimethylsiloxane, methylphenylsiloxane, or diphenylsiloxane. By having such a skeleton, compatibility with other matrix components is improved, and the dispersibility of the filler component in the thermal grease tends to be improved.
[0054] Such a (meth)acrylic monomer is not particularly limited, but examples thereof include (meth)acrylic monomers having a siloxane skeleton, such as α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane, etc. The unit γ may be used alone or in combination of two or more.
[0055] The weight average molecular weight of the (meth)acrylic monomer γ is preferably 300 or more, 1000 or more, 2000 or more, 3000 or more, or may be 4000 or more. The weight average molecular weight of the (meth)acrylic monomer γ is preferably 20000 or less, 17500 or less, 15000 or less, 12500 or less, 10000 or less, or 7500 or less. When the weight average molecular weight of the (meth)acrylic monomer γ is within the above range, the viscosity tends to be further reduced, and changes in hardness tend to be further suppressed.
[0056] The content of the unit γ is preferably 10 mol% or more, 15 mol% or more, 20 mol% or more, 25 mol% or more, 30 mol% or more, 35 mol% or more, or even 40 mol% or more, relative to 100 mol% of the total of the units α, β, and γ. Furthermore, the content of the unit γ is preferably 90 mol% or less, 80 mol% or less, 70 mol% or less, 60 mol% or less, or even 50 mol% or less, relative to 100 mol% of the total of the units α, β, and γ. When the content of the unit γ is within the above range, the viscosity tends to be further reduced, and the change in hardness tends to be further suppressed.
[0057] 1.2.2.4 Weight Average Molecular Weight The weight average molecular weight of surfactant B is preferably 5,000 or more, 7,500 or more, 10,000 or more, 20,000 or more, 30,000 or more, 40,000 or more, or may be 50,000 or more. When surfactant B has a weight average molecular weight of 5,000 or more, dispersibility can be maintained even when the thermal grease is kept at high temperatures for a long period of time, and an increase in hardness of the thermal grease can be suppressed.
[0058] The weight average molecular weight of surfactant B may be preferably 500,000 or less, 250,000 or less, 150,000 or less, 125,000 or less, 100,000 or less, or 75,000 or less. When the weight average molecular weight of surfactant B is 500,000 or less, the viscosity of the thermal grease tends to be further reduced, and the handleability tends to be further improved.
[0059] In this embodiment, each weight average molecular weight can be determined by GPC (gel permeation chromatography).
[0060] 1.2.2.5 Surfactant B1 The surfactant B may contain at least one or both of a surfactant B1 having a silicone (meth)acrylic monomer unit γ1 with a weight-average molecular weight of 1,000 or more and less than 8,000, and a surfactant B2 having a silicone (meth)acrylic monomer unit γ2 with a weight-average molecular weight of 8,000 or more and 50,000 or less. It is preferable to contain at least surfactant B2, and it is preferable to contain both surfactant B1 and surfactant B2. This tends to further reduce viscosity and further suppress changes in hardness.
[0061] The surfactant B1 has a silicone (meth)acrylic monomer unit γ1 having a weight average molecular weight of 1000 or more and less than 8000, and may also have any unit α and unit β. Use of the surfactant B1 tends to further reduce the viscosity.
[0062] The content of surfactant B1 is preferably 5 to 50 mass %, or may be 10 to 45 mass %, 15 to 40 mass %, or 20 to 35 mass %, relative to the total amount of the matrix components. When the content of surfactant B1 is within the above range, the viscosity tends to be further reduced.
[0063] Surfactant B2 has a silicone (meth)acrylic monomer unit γ2 having a weight-average molecular weight of 8,000 to 50,000, and may also have any unit α and unit β. Use of such a surfactant B2 tends to further suppress changes in hardness.
[0064] The content of surfactant B2 is preferably 3.5 to 30 mass %, 5 to 25 mass %, 7.5 to 20 mass %, or 10 to 15 mass %, relative to the total amount of the matrix components. When the content of surfactant B2 is within the above range, changes in hardness tend to be further suppressed.
[0065] 1.2.2.7 Viscosity The viscosity of surfactant B at 25°C is preferably 10 mPa·s or more, 50 mPa·s or more, 75 mPa·s or more, or may be 100 mPa·s or more. The viscosity of surfactant B at 25°C is preferably 2000 mPa·s or less, 1500 mPa·s or less, 1000 mPa·s or less, or may be 750 mPa·s or less. When the viscosity of surfactant B is within the above range, changes in hardness and dripping tend to be further suppressed.
[0066] 1.2.2.8. Method for Producing Surfactant B The method for producing surfactant B is not particularly limited, and any known polymerization method for (meth)acrylic monomers can be used. Examples of the polymerization method include radical polymerization and anionic polymerization. Among these, radical polymerization is preferred.
[0067] The thermal polymerization initiator used in the radical polymerization is not particularly limited, but examples thereof include azo compounds such as azobisisobutyronitrile; and organic peroxides such as benzoyl peroxide, tert-butyl hydroperoxide, and di-tert-butyl peroxide. Furthermore, the photopolymerization initiator used in the radical polymerization is not particularly limited, but examples thereof include benzoin derivatives. Furthermore, known polymerization initiators used in living radical polymerization such as ATRP and RAFT can also be used.
[0068] The polymerization conditions are not particularly limited and can be appropriately adjusted depending on the initiator and boiling point of the solvent used, as well as the types of other monomers.
[0069] The order of addition of the monomers is not particularly limited. For example, from the viewpoint of synthesizing a random copolymer, the monomers may be mixed to initiate polymerization, or from the viewpoint of synthesizing a block copolymer, the monomers may be added sequentially to the polymerization system.
[0070] 1.2.3 Silane Coupling Agent D The matrix component may further contain a silane coupling agent D. By including the silane coupling agent D, the viscosity tends to be further reduced, and changes in hardness and bleeding tend to be further suppressed. In addition, dripping also tends to be further suppressed.
[0071] The silane coupling agent D is not particularly limited, but examples thereof include epoxy silanes such as γ-glycidoxypropyltrimethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino silanes such as aminopropyltriethoxysilane, ureidopropyltriethoxysilane and N-phenylaminopropyltrimethoxysilane; and hydrophobic silane compounds such as phenyltrimethoxysilane, methyltrimethoxysilane, octadecyltrimethoxysilane and n-decyltrimethoxysilane.
[0072] Among these, hydrophobic silane compounds are more preferred. By using such a silane coupling agent D, the viscosity tends to be further reduced, the hardness change tends to be further suppressed, and dripping tends to be further suppressed.
[0073] The content of silane coupling agent D is preferably 2.0 to 10% by mass, or may be 4.0 to 8.0% by mass, based on the total amount of the matrix components. When the content of silane coupling agent D is within the above range, the viscosity tends to be further reduced, and changes in hardness and bleeding tend to be further suppressed.
[0074] 1.3. Filler Component The filler component is not particularly limited, but examples thereof include aluminum oxide (hereinafter also referred to as "alumina"), aluminum nitride, boron nitride, silicon nitride, zinc oxide, aluminum hydroxide, metallic aluminum, magnesium oxide, diamond, carbon, indium, gallium, copper, silver, iron, nickel, gold, tin, metallic silicon, and the like.
[0075] Among these, it is preferable to include at least one selected from the group consisting of aluminum oxide, aluminum nitride, boron nitride, silicon nitride, zinc oxide, aluminum hydroxide, metallic aluminum, magnesium oxide, copper, silver, and diamond, and alumina and magnesium oxide are more preferable. The use of such filler components tends to improve the filling property and further improve the thermal conductivity of the thermal grease. These fillers may be used alone or in combination of two or more.
[0076] The content of the filler component is preferably 65 to 95 volume %, 70 to 93 volume %, 75 to 90 volume %, or 80 to 87 volume % of the total amount of the thermal dissipation grease. When the content of the filler component is within the above range, thermal conductivity is further improved, viscosity is further reduced, and changes in hardness and bleeding are further suppressed.
[0077] Each filler component may be surface-treated with a surface treatment agent by a known wet or dry treatment method. The surface treatment agent is not particularly limited, but an example thereof is the above-mentioned silane coupling agent D, but the silane coupling agent D may be added separately regardless of the surface treatment.
[0078] 1.3.1 Filler C1 The filler component preferably contains filler C1 as small particles having an average particle size of 0.10 to 2.0 μm. Filler C1 may also contain polyhedral spherical filler C11 and spherical filler C12. Here, the term "polyhedral spherical" does not necessarily have to be interpreted in the strict sense, and the edges connecting the surfaces may be rounded. Using polyhedral spherical filler C11 tends to further reduce viscosity and further suppress hardness changes and bleeding.
[0079] The content of filler C1 is preferably 5 to 25 mass%, 7.5 to 22.5 mass%, 10 to 20 mass%, or 12.5 to 17.5 mass%, relative to the total amount of filler components. When the content of filler C1 is within the above range, thermal conductivity is further improved, viscosity is further reduced, and changes in hardness and bleeding tend to be further suppressed.
[0080] The content of filler C11 is preferably 3.0 to 15 mass%, or may be 5.0 to 13 mass%, or 7.0 to 11 mass%, relative to the total amount of filler components. When the content of filler C11 is within the above range, thermal conductivity tends to be further improved, viscosity tends to be further reduced, and changes in hardness and bleeding tend to be further suppressed.
[0081] The content of filler C12 is preferably 3.0 to 15 mass%, or may be 5.0 to 13 mass%, or 7.0 to 11 mass%, relative to the total amount of filler components. When the content of filler C12 is within the above range, thermal conductivity tends to be further improved, viscosity tends to be further reduced, and changes in hardness and bleeding tend to be further suppressed.
[0082] The ratio of the content of filler C11 to the content of filler C12 is preferably 0.5 to 5.0, or may be 0.75 to 4.0, or 1.0 to 3.0. When the ratio of the content of filler C11 to the content of filler C12 is within the above range, thermal conductivity tends to be further improved, viscosity tends to be further reduced, and changes in hardness and bleeding tend to be further suppressed.
[0083] 1.3.2 Filler C2 The filler component may contain filler C2 as medium-sized particles having an average particle size of 2.5 to 25 μm. The content of filler C2 is preferably 10 to 45 mass%, 15 to 40 mass%, or even 20 to 35 mass% relative to the total amount of the filler component. When the content of filler C2 is within the above range, thermal conductivity is further improved, viscosity is further reduced, and changes in hardness and bleeding tend to be further suppressed.
[0084] 1.3.3 Filler C3 The filler component may contain filler C3 as large particles having an average particle size of 30 to 200 μm. The content of filler C3 is preferably 40 to 75 mass%, 45 to 70 mass%, or even 50 to 65 mass%, relative to the total amount of the filler components. When the content of filler C2 is within the above range, thermal conductivity is further improved, viscosity is further reduced, and changes in hardness and bleeding tend to be further suppressed.
[0085] 2. Electronic Device The electronic device of this embodiment includes a heat generating element, a heat sink, and the above-described thermal dissipation grease, with the thermal dissipation grease disposed between the heat generating element and the heat sink. In this electronic device, the heat generating element and the heat sink are thermally coupled via the thermal dissipation grease.
[0086] Here, the heat generating body is not particularly limited, but examples thereof include heat generating electronic components such as motors, battery packs, circuit boards used in on-board power supply systems, power transistors, microprocessors, etc. Among these, electronic components used in on-board power supply systems for vehicles are preferred. Furthermore, the heat sink is not particularly limited as long as it is a component configured for the purpose of heat dissipation or heat absorption.
[0087] The method for bonding a heat generating element and a heat sink via the thermal grease is not particularly limited. For example, an electronic device may be obtained by bonding a heat generating element and a heat sink using the thermal grease.
[0088] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples.
[0089] 1. Preparation of Thermal Grease (Examples 1 to 12 and Comparative Example 1) Thermal grease was prepared by mixing silicone A, surfactant B, and filler C according to the composition shown in Table 1. In Table 1, the composition of each component is shown so that the matrix component and filler component each total 100 parts by weight. The mixing ratio of the matrix component and filler component is expressed as the total filling amount of the filler component. The following evaluations were carried out using each of the obtained thermal greases. The results are shown in Table 1.
[0090] 1.1. Raw Materials (Silicone A) Silicone A1: "KF-96-300CS" manufactured by Shin-Etsu Silicone Co., Ltd. Silicone A2: "KF-96-500CS" manufactured by Shin-Etsu Silicone Co., Ltd. Silicone A3: "KF-96-100CS" manufactured by Shin-Etsu Silicone Co., Ltd. Silicone A4: "SRH-32" manufactured by Momentive (viscosity >500CS) (Surfactant B) Surfactant B1: Surfactant obtained by Preparation Example 1 below Surfactant B2: Surfactant obtained by Preparation Example 2 below "Silane 10" (Filler C) Magnesium oxide: "DMG120" manufactured by Denka Company Limited, particle size 120 μm Aluminum oxide: "DAW45S" manufactured by Denka Company Limited, average particle size: 45 μm, thermal conductivity 35 W / mK Aluminum oxide: "DAW10" manufactured by Denka Company Limited, average particle size: 10 μm, thermal conductivity 35 W / mK Aluminum oxide: "DAW05" manufactured by Denka Company Limited, average particle size: 5 μm, thermal conductivity 35 W / mK Aluminum oxide: "AA05" manufactured by Denka Company Limited, average particle size: 0.5 μm, thermal conductivity 35 W / mK, polyhedral spherical Aluminum oxide: "ASFP40" manufactured by Denka Company Limited, average particle size: 0.4 μm, thermal conductivity 35 W / mK
[0091] The average particle size of each filler component was measured using a laser diffraction particle size distribution analyzer, SALD-20, manufactured by Shimadzu Corporation. To prepare the evaluation sample, 50 ml of pure water and 5 g of each filler component to be measured were added to a glass beaker, stirred with a spatula, and then dispersed in an ultrasonic cleaner for 10 minutes. The dispersion of each dispersed filler component was added drop by drop to the sampler section of the analyzer using a dropper, and measurement was performed once the absorbance had stabilized. D50 (median diameter) was used as the average particle size.
[0092] 1.2. Preparation Example 1 (Surfactant B1) Acrylic acid (manufactured by Toagosei Co., Ltd.) which constitutes the units α, 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate ("ADK STAB LA-82" manufactured by ADEKA Corporation) which constitutes the units β, and α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane ("Silaplane FM-0725" manufactured by JNC Corporation, number average molecular weight 5000) which constitutes the units γ were added to an autoclave equipped with a stirrer. Next, azobisisobutyronitrile (manufactured by Tokyo Chemical Industry Co., Ltd.) was added as an initiator, and a mixed solution of toluene and 2-propanol was added as a solvent, and the atmosphere inside the autoclave was replaced with nitrogen. Thereafter, the autoclave was heated in an oil bath at 65°C for 20 hours to carry out radical polymerization. After completion of polymerization, the mixture was degassed under reduced pressure at 120°C for 1 hour to obtain surfactant B1.
[0093] The polymerization rate relative to 100% of the monomer charge was analyzed by gas chromatography and found to be 98% or more. From this, it was estimated that the ratio of each monomer unit contained in surfactant B1 was approximately the same as the monomer charge ratio. In other words, surfactant B1 was a copolymer containing 48.4 mol% of units α, 1.6 mol% of units β, and 50 mol% of units γ.
[0094] The weight-average molecular weight of the obtained surfactant B1 was determined as a weight-average molecular weight converted into standard polystyrene using a GPC (gel permeation chromatography) method, and was found to be 65,000. The measurement conditions were as follows. High-speed GPC apparatus: "HLC-8020" manufactured by Tosoh Corporation Columns: one "TSK guard column MP (xL)" manufactured by Tosoh Corporation, 6.0 mm ID x 4.0 cm, and two "TSK-GELMULTIPORE HXL-M" manufactured by Tosoh Corporation, 7.8 mm ID x 30.0 cm (theoretical plate number: 16,000), for a total of three (total theoretical plate number: 32,000) Developing solvent: tetrahydrofuran Detector: RI (differential refractometer)
[0095] 1.3. Preparation Example 2 (Surfactant B2) Acrylic acid (manufactured by Toagosei Co., Ltd.) which constitutes the units α, 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate ("ADK STAB LA-82" manufactured by ADEKA Corporation) which constitutes the units β, and α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane ("Silaplane FM-0725" manufactured by JNC Corporation, number average molecular weight 10,000) which constitutes the units γ were added to an autoclave equipped with a stirrer. Next, azobisisobutyronitrile (manufactured by Tokyo Chemical Industry Co., Ltd.) was added as an initiator, and a mixed solution of toluene and 2-propanol was added as a solvent, and the atmosphere inside the autoclave was replaced with nitrogen. Thereafter, the autoclave was heated in an oil bath at 65°C for 20 hours to carry out radical polymerization. After completion of polymerization, the mixture was degassed under reduced pressure at 120°C for 1 hour to obtain surfactant B2.
[0096] The polymerization rate relative to 100% of the monomer charge was analyzed by gas chromatography and found to be 98% or more. From this, it was estimated that the ratio of each monomer unit contained in surfactant B2 was approximately the same as the monomer charge ratio. In other words, surfactant B2 was a copolymer containing 67.7 mol% of units α, 2.3 mol% of units β, and 30 mol% of units γ.
[0097] The weight-average molecular weight of the resulting surfactant B2 was determined as a weight-average molecular weight converted into standard polystyrene using GPC (gel permeation chromatography) and found to be 85,000. The measurement conditions were the same as in Preparation Example 1.
[0098] 2. Evaluation 2.1. Viscosity Using a rotational rheometer MARS III manufactured by Thermo Scientific, a 35 mm diameter parallel plate was used as the upper jig, and the thermal grease was placed on a 35 mm diameter lower plate whose temperature could be controlled by a Peltier element. The grease was compressed to a thickness of 1 mm with the upper jig, and the excess was scraped off. Measurement was performed at 25°C. Shear rate: 10 s -1 Viscosity η1 and shear rate 1s -1 The viscosities η2 and η1 were measured, and the ratio (η2 / η1) was also calculated.
[0099] 2.2. Thermal conductivity A rectangular copper jig with an embedded heater and a tip of 100 mm 2 (10mm x 10mm) and a rectangular copper jig with a cooling fin attached, the tip of which is 100mm 2 The thermal resistance was measured with a thermal grease sandwiched between the copper jigs (10 mm x 10 mm) and the thickness of the gap was set in the range of 0.05 mm to 0.30 mm. The thermal conductivity (W / m·k) was calculated from the gradient of the thermal resistance and thickness. The thermal resistance was evaluated by applying 10 W of power to the heater and holding it for 30 minutes, measuring the temperature difference (°C) between the copper jigs, and calculating it using the following formula: Thermal resistance (°C / W) = {Temperature difference (°C) / Power (W)}
[0100] 2.3. Change in Asker C Hardness The Asker C hardness of the thermal grease was measured using an Asker Rubber Hardness Tester Type C manufactured by Kobunshi Keiki Co., Ltd. Table 1 shows the Asker C hardness values after storage for a specified time of 0 to 1000 hours in a 150°C environment, with the initial hardness measured immediately after preparation of the thermal grease as the reference (0).
[0101] 2.4 Bleed-out Using a dispenser, 0.85 g (8-9 mm diameter) of thermal grease 1 was applied to a ground glass 2 (AGC, 2 mm thick) in a hemispherical shape. After storing the glass at 150°C for 24 hours, the distance L from the edge E1 of the thermal grease 1 to the edge E2 of the bleed mark 3 was measured. An image of the bleed-out measurement is shown in Figure 1.
[0102] (-: Not measured)
[0103] The thermal grease of the present invention has industrial applicability as a thermal grease for thermally connecting a heat generating element and a heat sink in an electronic device.
Claims
1. A matrix component and a filler component are included, the matrix component includes silicone A and surfactant B, and the shear rate is 10 s -1 Viscosity η1 vs shear rate 1s -1 a ratio (η2 / η1) of viscosity η2 of said grease to viscosity η1 of said grease is 4.0 to 9.0, and said viscosity η1 is 800 mPa·s or less.
2. The thermal grease according to claim 1, wherein the filler component includes filler C1 having an average particle size of 0.10 to 2.0 μm, and the filler C1 includes polyhedral spherical filler C11 and spherical filler C12.
3. The thermal grease according to claim 2, comprising: a content of said filler C11 of 3.0 to 15 mass% relative to the total amount of said filler components; and spherical filler C12.
4. The thermal grease according to claim 2, wherein the ratio of the content of said filler C11 to the content of said filler C12 is 0.5 to 5.
0.
5. The thermal grease according to claim 2, wherein the total content of the filler C1 is 5.0 to 25 mass % based on the total amount of the filler components.
Citation Information
Patent Citations
thermal grease
JP2009503236A
Thermal grease based on hyperbranched olefin fluid
JP2017530220A
Thermal conductive grease
JP2020002204A
Dispensable chemical compositions with high filler material content and low thixotropic index levels
JP2021515814A
thermal grease
JP7262699B1