Two-component adhesive composition

The two-component adhesive composition, featuring an acid-modified polyolefin and a controlled epoxy resin content, addresses the issue of viscosity increase and adhesive performance degradation at high temperatures, ensuring stable adhesion and coatability.

WO2024242186A1PCT designated stage expired Publication Date: 2024-11-28TOAGOSEI CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/019096
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-05-23
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional two-component adhesive compositions using acid group-containing resins, such as acid-modified olefins, suffer from viscosity thickening over time, especially at high temperatures, leading to deterioration of adhesive performance and coatability.

Method used

A two-component adhesive composition comprising a first part with an acid group-containing resin and an epoxy resin as a hardening agent, and a second part with a curing accelerator, where the acid group-containing resin is an acid-modified polyolefin, and the epoxy resin content is between 1 to 30 parts by mass based on 100 parts by mass of the resin, which suppresses the increase in viscosity over time.

Benefits of technology

The composition effectively prevents the deterioration of adhesive performance and coatability, maintaining stability and applicability even at elevated temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

A two-component adhesive composition comprising: a first agent including an acid radical-containing resin and an epoxy resin that serves as a curing agent; and a second agent including a curing accelerator.
Need to check novelty before this filing date? Find Prior Art

Description

Two-component adhesive composition

[0001] The present disclosure relates to two-part adhesive compositions.

[0002] BACKGROUND ART Adhesive compositions using acid group-containing resins, such as acid-modified olefins, have been known due to their high adhesive properties.

[0003] For example, Patent Document 1 discloses a composition comprising: "a modified olefin polymer (A) in which a polymer (a) of an α-olefin having 2 to 20 carbon atoms is modified with a monomer (b) having a functional group reactive to an epoxy group or an oxazoline group, the modified olefin polymer satisfying the following requirements (i) and (ii): a crosslinking agent (B) containing at least one of an epoxy compound or an oxazoline compound; and a catalyst (C) having a pKa of 11 or more. Requirement (i): the polymer (a) contains a structural unit derived from an α-olefin having 4 to 20 carbon atoms; and Requirement (ii): the modified olefin polymer (A) has a heat of fusion of 0 to 50 J / g as measured in accordance with JIS K7122."

[0004] Furthermore, Patent Document 2 discloses "an adhesive comprising a first agent and a second agent, wherein the first agent comprises a resin (A) containing an acid group-containing resin (A1), the second agent comprises an epoxy compound (B1) having a viscosity at 52°C of 0.05 Pa·s or more and 25 Pa·s or less, and further comprises an organic phosphorus compound (C) and an imidazole compound (D), wherein the blending amount of the organic phosphorus compound (C) is 0.01 parts by mass or more and 5 parts by mass or less per 100 parts by mass of the resin (A), and the blending amount of the imidazole compound (D) is 0.06 parts by mass or more and 0.35 parts by mass or less per 100 parts by mass of the resin (A)."

[0005] Furthermore, Patent Document 3 discloses "a battery packaging material comprising a barrier layer, an adhesive layer, and a sealant layer laminated in this order, wherein the adhesive layer contains a reaction product of an acid-modified polyolefin (A) having an acid value of 5 to 50 mg KOH / g-resin, a glycidylamine-type epoxy resin (B1), and a glycidyl ether-type epoxy resin (B2)."

[0006] Japanese Patent No. 6680804 Japanese Patent Publication No. 2020-169250 Japanese Patent No. 6733674

[0007] Conventionally, two-component adhesive compositions using acid group-containing resins, such as acid-modified olefins, generally combine a first component containing the acid group-containing resin and a curing accelerator with a second component containing an epoxy resin as a curing agent. However, the first component of conventional two-component adhesive compositions thickens over time during storage. Considering summer, in particular, storage in a high-temperature atmosphere of about 40°C is expected, resulting in a high rate of viscosity increase. As a result, the original adhesive performance cannot be achieved.

[0008] Therefore, an object of the present disclosure is to provide a two-component adhesive composition that suppresses deterioration of adhesive performance over time.

[0009] Means for solving the above problems include the following aspects. <1> A two-component adhesive composition comprising: a first part containing an acid group-containing resin and an epoxy resin as a curing agent; and a second part containing a curing accelerator. <2> The two-component adhesive composition according to <1>, wherein the acid group-containing resin is an acid-modified polyolefin. <3> The two-component adhesive composition according to <1> or <2>, wherein the content of the epoxy resin is 1 to 30 parts by mass per 100 parts by mass of the acid group-containing resin.

[0010] According to the present disclosure, it is possible to provide a two-component adhesive composition that suppresses deterioration of adhesive performance over time.

[0011] An embodiment of the present disclosure will be described below. These descriptions and examples are illustrative of the embodiments and do not limit the scope of the embodiments. In this disclosure, a numerical range indicated using "to" indicates a range that includes the numerical values ​​before and after "to" as the minimum and maximum values, respectively. In numerical ranges described in stages in this disclosure, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In numerical ranges described in this disclosure, the upper or lower limit value of that numerical range may be replaced with a value shown in the examples. In this disclosure, the term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the purpose of that process is achieved. When embodiments are described in this disclosure with reference to drawings, the configuration of the embodiment is not limited to the configuration shown in the drawings. Furthermore, the sizes of components in each drawing are conceptual, and the relative size relationships between components are not limited thereto. In this disclosure, each component may contain multiple corresponding substances. In this disclosure, when referring to the amount of each component in a composition, if the composition contains multiple substances corresponding to each component, the total amount of the multiple substances present in the composition is meant unless otherwise specified. In this disclosure, "(meth)acrylic" is an expression that includes both acrylic and methacrylic, and "(meth)acrylate" is an expression that includes both acrylate and methacrylate.

[0012] <Two-component adhesive composition> The two-component adhesive composition (hereinafter also referred to as "adhesive composition") of the present disclosure has a first part containing an acid group-containing resin and an epoxy resin as a curing agent, and a second part containing a curing accelerator.

[0013] The adhesive composition of the present disclosure contains an acid group-containing resin and an epoxy resin as a curing agent in the first part, and a curing accelerator in the second part, which prevents the first part from thickening over time and prevents deterioration of adhesive performance over time. Furthermore, because the first part does not thicken over time, deterioration of coatability is also prevented.

[0014] The adhesive composition of the present disclosure will be described in detail below.

[0015] <First Agent> The first agent contains an acid group-containing resin and an epoxy resin. The first agent may also contain a solvent and other components.

[0016] (Acid group-containing resin) Examples of the acid group-containing resin include well-known acid group-containing resins such as acid-modified polyolefin, acid-modified styrene-based elastomer, acid group-containing acrylic resin, acid group-containing urethane resin, etc. Among these, acid-modified polyolefin is preferred as the acid group-containing resin in terms of adhesiveness.

[0017] - Acid-modified polyolefin - An acid-modified polyolefin is a polyolefin (hereinafter also referred to as "unmodified polyolefin") that has been modified by adding acid groups. Specifically, the acid-modified polyolefin is obtained by modifying an unmodified polyolefin with an acid group-containing monomer.

[0018] Specific examples of unmodified polyolefins include polyethylene, polypropylene, random copolymers of propylene and ethylene, block copolymers of propylene and ethylene, random copolymers of ethylene and α-olefins, block copolymers of ethylene and α-olefins, random copolymers of propylene and α-olefins, block copolymers of propylene and α-olefins, etc. Here, examples of α-olefins include 1-butene, isobutylene, 1-hexene, and 1-octene.

[0019] Among these, from the viewpoint of improving adhesiveness, polypropylene-based polymers such as polypropylene, propylene-ethylene block copolymers, propylene-ethylene random copolymers, propylene and α-olefin random copolymers, and propylene and α-olefin block copolymers are preferred as unmodified polyolefins.

[0020] In the acid group-containing monomer for modifying the unmodified polyolefin, examples of the acid group include a carboxylic acid group, a carboxylic acid anhydride group, a sulfonic acid group, and a phosphoric acid group. Among these, a carboxylic acid group (or a carboxylic acid anhydride group) is preferred because it is easy to modify.

[0021] The carboxylic acid group (or carboxylic anhydride group)-containing monomer is a compound having an ethylenic double bond and a carboxylic acid group in the same molecule, and examples thereof include various unsaturated monocarboxylic acid compounds, unsaturated dicarboxylic acid compounds, and unsaturated tricarboxylic acid compounds. Specific examples of unsaturated monocarboxylic acid compounds include acrylic acid, methacrylic acid, crotonic acid, and isocrotonic acid. Examples of unsaturated dicarboxylic acid compounds include maleic acid, itaconic acid, citraconic acid, tetrahydrophthalic acid, nadic acid, and endic acid. Examples of unsaturated tricarboxylic acid compounds include aconitic acid. As the acid group-containing monomer, unsaturated dicarboxylic acid compounds and unsaturated tricarboxylic acid compounds are preferred, with itaconic acid, maleic acid, and aconitic acid being particularly preferred, due to their ease of modification and excellent adhesive properties. The acid group-containing monomer may be used alone or in combination of two or more types.

[0022] The acid-modified polyolefin may be modified (e.g., graft-modified) with a (meth)acrylic acid alkyl ester. The (meth)acrylic acid alkyl ester is preferably an ester of an alkyl alcohol having 8 to 18 carbon atoms with (meth)acrylic acid.

[0023] The acid value can be used as a measure of the amount of functional groups introduced into the acid-modified polyolefin. From the viewpoint of improving adhesiveness, the acid value is preferably 1.0 to 30.0 mgKOH / g, more preferably 5.0 to 25.0 mgKOH / g, and even more preferably 8.0 to 20.0 mgKOH / g. The acid value of the acid-modified polyolefin is measured as follows: Approximately 10 g of acid-modified polyolefin is accurately weighed and placed in a 200 mL tall beaker. 150 mL of a mixed solvent consisting of xylene and dimethylformamide mixed in a 1:1 (volume ratio) ratio is added as the titration solvent. Titration is performed using a 1 w / v % phenolphthalein ethanol solution (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as an indicator, and the acid value is determined from the titration amount. Specifically, the acid value can be calculated using the following formula. The acid value is the average value of three repeated titrations. Formula: Acid value (mgKOH / g) = (EP1 - BL1) × FA1 × C1 / SIZE In the formula, "EP1" represents the titration amount (mL), "BL1" represents the blank value (mL), "FA1" represents the factor of the titrant (1.00), "C1" represents the concentration equivalent value (5.611 mg / m), and "SIZE" represents the amount of acid-modified polyolefin collected (g).

[0024] From the viewpoint of improving heat resistance, the melting point of the acid-modified polyolefin is preferably 50 to 120° C., more preferably 60 to 110° C., and even more preferably 70 to 95° C. The melting point of the acid-modified polyolefin is measured as follows: Using a differential scanning calorimeter (hereinafter referred to as DSC, manufactured by TA Instruments Japan, Q-2000), the polyolefin is heated and melted at a rate of 20° C. / min, cooled to form a resin, and then heated and melted again, and the melting point is measured from the top temperature of the melting peak.

[0025] The weight average molecular weight Mw of the acid-modified polyolefin is preferably 3,000 to 500,000, more preferably 25,000 to 250,000, from the viewpoint of improving adhesiveness and solubility in solvents. The weight average molecular weight Mw of the acid-modified polyolefin is a value obtained by converting the molecular weight measured by gel permeation chromatography into polystyrene equivalent.

[0026] In terms of improving adhesiveness, the propylene unit content in the acid-modified polyolefin is preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more.

[0027] The acid-modified polyolefins may be used alone or in combination of two or more.

[0028] - Content of Acid Group-Containing Resin - The content of the acid group-containing resin is preferably 70 to 99 mass %, and more preferably 75 to 99 mass %, based on all components of the adhesive composition other than the solvent.

[0029] (Epoxy Resin) An epoxy resin is a compound that can at least react with the acid groups in an acid group-containing resin to cure (for example, crosslink).

[0030] Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, and hydrogenated versions thereof; glycidyl ester-based epoxy resins such as orthophthalic acid diglycidyl ester, isophthalic acid diglycidyl ester, terephthalic acid diglycidyl ester, p-hydroxybenzoic acid glycidyl ester, tetrahydrophthalic acid diglycidyl ester, succinic acid diglycidyl ester, adipic acid diglycidyl ester, sebacic acid diglycidyl ester, and trimellitic acid triglycidyl ester; ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, 1,4 Examples of epoxy resins include glycidyl ether-based epoxy resins such as 1,6-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, pentaerythritol tetraglycidyl ether, tetraphenylglycidyl ether ethane, triphenylglycidyl ether ethane, sorbitol polyglycidyl ether, and polyglycerol polyglycidyl ether; glycidylamine-based epoxy resins such as triglycidyl isocyanurate and tetraglycidyldiaminodiphenylmethane; and linear aliphatic epoxy resins such as epoxidized polybutadiene and epoxidized soybean oil. Examples of epoxy resins also include novolac-type epoxy resins such as phenol novolac epoxy resin, o-cresol novolac epoxy resin, and bisphenol A novolac epoxy resin. Further examples of the epoxy resin include brominated bisphenol A type epoxy resins, phosphorus-containing epoxy resins, dicyclopentadiene skeleton-containing epoxy resins, naphthalene skeleton-containing epoxy resins, anthracene type epoxy resins, tertiary butylcatechol type epoxy resins, triphenylmethane type epoxy resins, tetraphenylethane type epoxy resins, biphenyl type epoxy resins, bisphenol S type epoxy resins, etc. Only one type of epoxy resin may be used, or two or more types may be used in combination.

[0031] As the epoxy resin, a compound having two or more epoxy groups in one molecule is preferred. This is because a crosslinked structure can be formed by reaction with the acid group-containing resin, thereby exhibiting high heat resistance. Furthermore, when an epoxy resin having two or more epoxy groups is used, the degree of crosslinking with the acid group-containing resin is sufficient, resulting in sufficient heat resistance.

[0032] The content of the epoxy resin is preferably 1 to 30 parts by mass, more preferably 1 to 15 parts by mass, per 100 parts by mass of the acid group-containing resin, from the viewpoint of improving adhesiveness and heat resistance.

[0033] (Solvent) Examples of the solvent used in the first agent include well-known solvents. In particular, from the viewpoint of inhibiting solidification, the solvent preferably contains an aromatic solvent, at least one solvent A selected from a ketone solvent and an alcohol solvent, and an aliphatic solvent.

[0034] Aromatic Solvents Aromatic solvents are solvents having an aromatic ring in one molecule. Examples of aromatic solvents include toluene, o-xylene, m-xylene, p-xylene, anisole, ethyl benzyl ether, cresyl methyl ether, diphenyl ether, dibenzyl ether, phenetole, butyl phenyl ether, ethyl benzene, diethyl benzene, pentyl benzene, isopropyl benzene, cymene, and mesitylene. Among these, aromatic solvents having 6 to 8 carbon atoms and a low number of substituents (particularly toluene) are preferred in terms of suppressing solidification.

[0035] -Solvent A- Ketone solvents are solvents having a ketone group in one molecule. Examples of ketone solvents include methyl ethyl ketone, acetone, diethyl ketone, methyl isobutyl ketone, methyl-n-pentyl ketone, methyl isopentyl ketone, and 2-heptanone.

[0036] An alcohol-based solvent is a solvent having an alcoholic hydroxyl group in one molecule. Examples of alcohol-based solvents include methanol, ethanol, isopropyl alcohol, normal propyl alcohol, ethylene glycol, diethylene glycol, propylene glycol, and dipropylene glycol.

[0037] Among these, from the viewpoint of inhibiting solidification, preferred ketone solvents are lower alkyl ketones having 3 to 5 carbon atoms (particularly methyl ethyl ketone), and preferred alcohol solvents are lower alcohols having 1 to 4 carbon atoms (particularly isopropyl alcohol). Also, from the viewpoint of inhibiting solidification, preferred solvents A are ketone solvents.

[0038] Aliphatic Solvents Aliphatic solvents are solvents having an aliphatic group in one molecule. Examples of aliphatic solvents include n-heptane, n-hexane, octane, nonane, decane, undecane, dodecane, cyclohexane, methylcyclohexane, ethylcyclohexane, dimethylcyclohexane, paraffin solvents, and isododecane. Among these, alicyclic hydrocarbons (particularly methylcyclohexane) are preferred as aliphatic solvents in terms of preventing solidification.

[0039] -Solvent Component Ratio- From the viewpoint of inhibiting solidification, when the total amount of solvents is taken as 100 parts by mass, the amount of each solvent is as follows. The amount of aromatic solvent is preferably 10 to 45 parts by mass, more preferably 10 to 30 parts by mass, and particularly preferably 10 to 20 parts by mass. The amount of at least one solvent A selected from ketone solvents and alcohols is preferably 5 to 19 parts by mass, more preferably 8 to 19 parts by mass, and even more preferably 10 to 19 parts by mass. The amount of aliphatic solvent is preferably 45 to 70 parts by mass, more preferably 55 to 70 parts by mass, and even more preferably 60 to 70 parts by mass.

[0040] From the viewpoint of suppressing solidification, the ratio of the aromatic solvent to the aliphatic solvent is preferably 15 to 25 mass%, more preferably 15 to 23 mass%, and even more preferably 15 to 20 mass%. From the viewpoint of suppressing solidification, the ratio of solvent A to the aliphatic solvent is preferably 5 to 35 mass%, more preferably 10 to 35 mass%, and even more preferably 15 to 35 mass%.

[0041] The solvent may contain a solvent other than an aromatic solvent, solvent A (at least one selected from a ketone solvent and an alcohol solvent), and an aliphatic solvent. However, the proportion of the aromatic solvent, solvent A, and aliphatic solvent in the solvent is preferably 90% by mass or more (preferably 95% by mass or more). The proportion of the aromatic solvent, solvent A, and aliphatic solvent in the solvent is preferably 100% by mass.

[0042] The content of the solvent is preferably 75 to 95% by mass, more preferably 80 to 90% by mass, based on the adhesive composition.

[0043] (Other Components) Examples of other components that can be applied to the first agent include well-known components such as thermoplastic resins other than acid group-containing resins, tackifiers, flame retardants, coupling agents, heat aging inhibitors, leveling agents, antifoaming agents, inorganic fillers, and pigments.

[0044] <Second agent> The second agent contains a curing accelerator. The second agent may contain a solvent and other components. The second agent preferably does not contain at least one of an acid group-containing resin and an epoxy resin, and more preferably does not contain both.

[0045] (Curing Accelerator) The curing accelerator is a compound that accelerates the reaction between the acid group-containing resin and the epoxy resin. Examples of the curing accelerator include well-known curing accelerators such as imidazole compounds, amine compounds, and phosphorus compounds.

[0046] Examples of the imidazole compound include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-methyl-4-ethylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 2,4-diamino-6-[2'-methylimidazolyl-(1')]ethyl-s-triazine, 2,4-diamino-6-[2'- undecylimidazolyl-(1')]ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and the like.

[0047] Examples of the amine compound include tertiary amines such as benzyldimethylamine, 2-(dimethylaminomethyl)phenol, 2,4,6-tris(dimethylaminomethyl)phenol, tetramethylguanidine, triethanolamine, N,N'-dimethylpiperazine, triethylenediamine, and 1,8-diazabicyclo[5.4.0]undecene. Examples of the amine compound also include tertiary amine salts such as the formate, octylate, p-toluenesulfonate, o-phthalate, phenol salt, and phenol novolac resin salt of 1,8-diazabicyclo[5.4.0]undecene; and the formate, octylate, p-toluenesulfonate, o-phthalate, phenol salt, and phenol novolac resin salt of 1,5-diazabicyclo[4.3.0]nonene.

[0048] Examples of the phosphorus compound include triphenylphosphine, tributylphosphine, methyldiphenylphosphine, tris(4-methylphenyl)phosphine, tris(4-butylphenyl)phosphine, diphenylphosphine, and phenylphosphine.

[0049] These curing accelerators may be used alone or in combination of two or more.

[0050] The content of the curing accelerator is preferably 1 to 10 parts by mass, more preferably 2 to 5 parts by mass, relative to 100 parts by mass of the epoxy resin when the first and second agents are mixed. When the content of the curing accelerator is within the above range, excellent adhesion and heat resistance are improved.

[0051] (Solvent) Examples of the solvent used in the first agent include well-known solvents. Specific examples of the solvent include aromatic solvents such as toluene and xylene; aliphatic solvents such as n-hexane; alicyclic solvents such as cyclohexane, methylcyclohexane, and ethylcyclohexane; ketone solvents such as acetone and methyl ethyl ketone; alcohol solvents such as methanol and ethanol; ester solvents such as ethyl acetate and butyl acetate; and propylene glycol ether solvents such as propylene glycol methyl ether, propylene glycol ethyl ether, and propylene glycol t-butyl ether. These solvents may be used alone or in combination of two or more.

[0052] (Other Components) Examples of other components that may be added to the second agent include well-known components such as tackifiers, flame retardants, coupling agents, heat aging inhibitors, leveling agents, antifoaming agents, inorganic fillers, and pigments.

[0053] (Applications) The adhesive composition of the present disclosure is suitable for bonding metals, glass, plastics, resin films, and the like.

[0054] The adhesive composition of the present disclosure will be described in more detail below with reference to examples. The materials, amounts used, ratios, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present disclosure. Therefore, the scope of the resin composition of the present disclosure should not be interpreted as being limited by the specific examples shown below.

[0055] <Materials used> 1. Maleic anhydride modified polyolefins Maleic anhydride modified polyolefin-1 (PO-1): propylene-butene-1 copolymer, melting point 80°C, weight average molecular weight Mw 90,000, acid value 10 mg KOH / g Maleic anhydride modified polyolefin-2 (PO-2): propylene-butene-1 copolymer, melting point 80°C, weight average molecular weight Mw 60,000, acid value 20 mg KOH / g

[0056] 2. Epoxy resin EPICLON HP-7200 (DIC Corporation) Dicyclopentadiene skeleton-containing epoxy resin

[0057] 3. Curing accelerators: Curesol SIZ (Shikoku Chemical Industry Co., Ltd.) imidazole compound; N,N-diisopropylethylamine (DIPEA, Fujifilm Wako Pure Chemical Industries, Ltd.) amine compound; Diazabicycloundecene (DBU, Fujifilm Wako Pure Chemical Industries, Ltd.) amine compound; Triphenylphosphine (TPP, Fujifilm Wako Pure Chemical Industries, Ltd.) phosphorus compound

[0058] <Preparation of First Agent> (Preparation of First Agent 1 (A-1)) 13.5 g of maleic acid-modified polyolefin (PO-1) was dissolved in a mixed solvent of 38.3 g of toluene, 4.3 g of methyl ethyl ketone, 38.3 g of methylcyclohexane, and 4.3 g of isopropyl alcohol at 60°C, and then 1.35 g of epoxy resin (EPICLON HP-7200, manufactured by DIC Corporation) was dissolved therein to obtain First Agent 1 (A-1).

[0059] (Preparation of First Agent 2 (A-2)) An adhesive (A-2) was prepared in the same manner as (A-1), except that the components and blending amounts used were changed as shown in Table 1.

[0060] (Preparation of First Agent 3 (A-3)) 14.4 g of maleic anhydride-modified polyolefin (PO-2) was dissolved in a mixed solvent of 38.5 g of toluene, 4.3 g of methyl ethyl ketone, 38.5 g of methylcyclohexane, and 4.2 g of isopropyl alcohol at 60°C, and then 0.1 g of Curesol SIZ (manufactured by Shikoku Chemicals Corporation) was dissolved therein to obtain First Agent 3 (A-3).

[0061] (Preparation of First Agents 4 to 7 (A-4 to A-7)) Adhesives (A-4 to A-7) were prepared in the same manner as (A-3), except that the components and blending amounts used were changed as shown in Table 1.

[0062] <Preparation of Second Agent> (Preparation of Second Agent 1 (B-1)) 10.0 g of Curesol SIZ (manufactured by Shikoku Chemicals Corporation) was dissolved in a mixed solvent of 36.0 g of methyl ethyl ketone and 54.0 g of isopropyl alcohol to obtain Second Agent 1 (B-1).

[0063] (Preparation of Second Agents 2 to 5 (B-2 to B-5)) Adhesives (B-2 to B-5) were prepared in the same manner as (B-1), except that the components and blending amounts used were changed as shown in Table 2.

[0064] (Preparation of Second Agent 6 (B-6)) 14.3 g of epoxy resin (EPICLON HP-7200, manufactured by DIC Corporation) was dissolved in 85.7 g of methyl ethyl ketone to obtain Second Agent 6 (B-6).

[0065] (Preparation of Second Agent 7 (B-7)) An adhesive (B-7) was prepared in the same manner as (B-6), except that the components and blending amounts used were changed as shown in Table 2.

[0066] <Evaluation of the state of the first and second agents> The solution state of First Agents 1 to 7 and Second Agents 1 to 7 immediately after preparation was evaluated by measuring the initial solution viscosity (I) at 25°C using a RE-85U type viscometer (hereinafter referred to as E type viscometer) manufactured by Toki Sangyo Co., Ltd.

[0067] <Evaluation of Solution Stability of First and Second Agents> Solution stability refers to the stability of the first and second agents immediately after preparation when they are stored at a specified temperature for a certain period of time. Good solution stability means that the solution viscosity increases little and can be stored for a long period of time. Poor solution stability means that the solution viscosity increases (thickens), and in severe cases, gelation occurs, making application to a substrate difficult and making long-term storage impossible. These factors are affected by storage temperature, and in particular in high-temperature environments such as summer, the solutions are exposed to relatively high temperatures and are prone to thickening. After storing the prepared solutions of First Agents 1 to 7 and Second Agents 1 to 7 at 40°C for 14 days, the solution viscosity (II) after storage at 25°C was measured using an E-type viscometer. The viscosity increase rate over time compared to the solution viscosity at 25°C immediately after preparation was calculated and evaluated using the method shown below.

[0068] [Temporal Viscosity Increase Rate] The temporal viscosity increase rate was calculated using the following formula: Temporal Viscosity Increase Rate = (Solution viscosity after storage (II) - Initial solution viscosity (I)) / Initial solution viscosity (I) x 100

[0069] [Evaluation Criteria] A: The rate of increase over time is 100% or less. B: The rate of increase over time is 101% or more and 200% or less. C: The rate of increase over time is 201% or more.

[0070] <Preparation of Adhesive> Example 1 The adhesive of Example 1 was prepared by thoroughly mixing 100 parts of the first part 1 (A-1) and 1 part of the second part 1 (B-1).

[0071] Examples 2 to 5 The adhesives of Examples 2 to 5 were prepared in the same manner as in Example 1, except that the types and mixing amounts of the first and second agents used were changed as shown in Table 3.

[0072] Comparative Example 1 An adhesive of Comparative Example 1 was prepared by thoroughly mixing 100 parts of the first part 3 (A-3) and 10 parts of the second part 6 (B-6).

[0073] Comparative Examples 2 to 5 The adhesives of Comparative Examples 2 to 5 were prepared in the same manner as in Example 1, except that the types and mixing amounts of the first and second agents used were changed as shown in Table 3.

[0074] <Evaluation> (Preparation of Laminate) The adhesive of each example was applied to a 100 μm thick aluminum foil (Al foil, surface untreated) with a bar coater to a coating thickness of 5 μm (dry), and the solvent was evaporated for 1 minute at 100° C. to obtain a coated foil. Thereafter, the coating surface of the obtained coated foil and a 100 μm thick aluminum foil (same as above) were bonded together at 100° C., and the coating was cured by aging at 80° C. for 1 day, thereby obtaining a laminate in which the Al foil, adhesive layer, and Al foil were laminated in this order.

[0075] (Coatability) When preparing the laminate, the adhesive was applied and dried, and the presence or absence of coating unevenness on the resulting coated foil was confirmed. The state of the coated foil was evaluated as follows: [Evaluation criteria] A: No coating unevenness at all. B: Coating unevenness present. C: The adhesive gelled, making it impossible to coat.

[0076] (Measurement of adhesive strength) Using Shimadzu Corporation's "Autograph AG-X," the adhesive strength at the interface between the aluminum foils of the laminate was evaluated under the conditions of a peel speed of 100 mm / min, a peel width of 10 mm, an ambient temperature of 23°C, and a T-type peeling form. The unit is N / 10 mm. [Evaluation criteria] A: 10 N / 10 mm or more. A-: 9 N / 10 mm or more, less than 10 N / 10 mm. B: 7 N / 10 mm or more, less than 9 N / 10 mm. C: Less than 7 N / 10 mm, or coating was not possible and a peel test could not be performed.

[0077] The above examples and evaluation results are shown in Tables 1 to 3. The numerical values ​​in the columns for each component in Tables 1 and 2 are in units of "g."

[0078]

[0079]

[0080] The above results show that the adhesive compositions of the first and second agents used in the Examples showed little increase in viscosity of the first agent over time, suppressing deterioration in adhesive performance and coatability. On the other hand, the adhesive compositions of the first and second agents used in the Comparative Examples showed an increase in viscosity of the first agent over time, resulting in deterioration in adhesive performance and coatability.

[0081] The disclosure of Japanese Patent Application No. 2023-085808 is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.

Claims

1. A two-component adhesive composition comprising: a first part containing an acid group-containing resin and an epoxy resin as a curing agent; and a second part containing a curing accelerator.

2. The two-component adhesive composition according to claim 1, wherein the acid group-containing resin is an acid-modified polyolefin.

3. A two-component adhesive composition according to claim 1 or 2, wherein the content of the epoxy resin is 1 to 30 parts by mass per 100 parts by mass of the acid group-containing resin.

Citation Information

Patent Citations

  • Rubber-based curable type hot melt adhesive composition

    JP2007051195A

  • Two-component reaction type hot melt resin composition and method of application thereof

    JP2010116530A

  • Adhesive, laminate, battery packaging material, and battery

    JP2020169250A

  • Packaging material for lithium-ion battery

    WO2017030024A1

  • Composition, laminate, packaging material, packaging material for battery cases, and battery

    WO2017126520A1