Adhesive composition
The adhesive composition, with a solvent blend of aromatic, ketone or alcohol, and aliphatic solvents, addresses the issue of solidification at low temperatures, ensuring the adhesive remains usable and effective by inhibiting hydrogen bond formation, thus maintaining its fluidity and applicability.
Patent Information
- Application Number
- PCT/JP2024/019097
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2024-05-23
- Publication Date
- 2024-11-28
AI Technical Summary
Conventional adhesive compositions containing acid-modified olefins and solvents tend to solidify when stored at low temperatures, making them unusable without proper temperature control, especially during winter storage.
The adhesive composition includes acid-modified polyolefin and a solvent blend with specific ratios of aromatic, ketone or alcohol, and aliphatic solvents, which inhibits solidification by preventing hydrogen bond formation, ensuring the composition remains fluid at low temperatures.
The composition effectively prevents solidification at low temperatures, maintaining its applicability and usability, and suppressing deterioration during storage.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
adhesive composition
[0001] The present disclosure pertains to adhesive compositions.
[0002] BACKGROUND ART Adhesive compositions using acid-modified olefins have been known due to their high adhesive properties.
[0003] For example, Patent Document 1 discloses "an adhesive resin composition comprising an acid-modified polyolefin resin component (A) having a melting point of more than 80°C and not more than 140°C, a crosslinker component (B), and a solvent component (S), wherein the solvent component (S) contains an aromatic solvent (S1), an aliphatic solvent (S2), and a ketone solvent (S3), the aromatic solvent (S1) having the highest boiling point, and wherein the adhesive resin composition contains 50 parts by mass or more and 80 parts by mass or less of the aromatic solvent (S1), 10 parts by mass or more and 30 parts by mass or less of the aliphatic solvent (S2), and 5 parts by mass or more and 20 parts by mass or less of the ketone solvent (S3), when the total amount of the solvent component (S) is 100 parts by mass."
[0004] Furthermore, Patent Document 2 discloses "an adhesive resin composition comprising an acid-modified polyolefin resin component (A) having a weight-average molecular weight of 30,000 or more and 150,000 or less, a resin component (B) having an epoxy group in the molecule, a resin component (C) having an amino group at the molecular terminal, and a solvent (S), wherein the content of the resin component (B) is 1 part by mass or more and 30 parts by mass or less per 100 parts by mass of the modified polyolefin resin component (A), and the content of the resin component (C) is 0.5 parts by mass or more and 15 parts by mass or less per 100 parts by mass of the modified polyolefin resin component (A)."
[0005] Furthermore, Patent Document 3 discloses "an adhesive resin composition comprising an acid-modified polyolefin resin component (A) having a weight-average molecular weight of 30,000 or more and 150,000 or less, a resin component (B) having an epoxy group in the molecule, a resin component (C) having an amino group at the molecular terminal, and a solvent (S), wherein the content of the resin component (B) is 1 part by mass or more and 30 parts by mass or less per 100 parts by mass of the acid-modified polyolefin resin component (A), the content of the resin component (C) is 0.5 parts by mass or more and 15 parts by mass or less per 100 parts by mass of the acid-modified polyolefin resin component (A), and the melting point of the acid-modified polyolefin resin component (A) is 50°C or more and 85°C or less."
[0006] Patent No. 6914145 Patent No. 7094671 JP 2022-118154 A
[0007] However, conventional adhesive compositions containing an acid-modified olefin and a solvent may solidify (e.g., turn into pudding or gel) when stored at low temperatures. Therefore, if proper temperature control is not performed, particularly during storage in winter, the adhesive composition may become unusable as a product due to solidification.
[0008] Therefore, an object of the present disclosure is to provide an adhesive composition that is less likely to solidify when stored at low temperatures.
[0009] Means for solving the above problems include the following aspects. <1> An adhesive composition comprising an acid-modified polyolefin and a solvent, wherein the solvent contains, relative to 100 parts by mass of the total amount of the solvents, 10 to 45 parts by mass of an aromatic solvent, 5 to 19 parts by mass of at least one solvent A selected from ketone solvents and alcohol solvents, and 45 to 70 parts by mass of an aliphatic solvent. <2> The adhesive composition according to <1>, wherein a ratio of the aromatic solvent to the aliphatic solvent is 15 to 25% by mass. <3> The adhesive composition according to <1> or <2>, wherein a ratio of the solvent A to the aliphatic solvent is 5 to 35% by mass.
[0010] According to the present disclosure, an adhesive composition that is less likely to solidify even when stored at low temperatures can be provided.
[0011] An embodiment of the present disclosure will be described below. These descriptions and examples are illustrative of the embodiments and do not limit the scope of the embodiments. In this disclosure, a numerical range indicated using "to" indicates a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively. In numerical ranges described in stages in this disclosure, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In numerical ranges described in this disclosure, the upper or lower limit value of that numerical range may be replaced with a value shown in the examples. In this disclosure, the term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the purpose of that process is achieved. When embodiments are described in this disclosure with reference to drawings, the configuration of the embodiment is not limited to the configuration shown in the drawings. Furthermore, the sizes of components in each drawing are conceptual, and the relative size relationships between components are not limited thereto. In this disclosure, each component may contain multiple corresponding substances. In this disclosure, when referring to the amount of each component in a composition, if the composition contains multiple substances corresponding to each component, the total amount of the multiple substances present in the composition is meant unless otherwise specified. In this disclosure, "(meth)acrylic" is an expression that includes both acrylic and methacrylic, and "(meth)acrylate" is an expression that includes both acrylate and methacrylate.
[0012] <Adhesive Composition> The adhesive composition of the present disclosure contains an acid-modified polyolefin and a solvent. The solvent contains, relative to 100 parts by mass of the total amount of the solvents, 15 to 45 parts by mass of an aromatic solvent, 5 to 15 parts by mass of at least one solvent A selected from ketone solvents and alcohol solvents, and 45 to 70 parts by mass of an aliphatic solvent.
[0013] Due to the above-described composition, the adhesive composition of the present disclosure is less likely to solidify even when stored at low temperatures. Solidification is promoted by the association of the acid-modified polyolefin through hydrogen bonding of the acid groups in the acid-modified polyolefin. However, by blending the aromatic solvent, solvent A, and aliphatic solvent in the above amounts as solvents into the adhesive composition, it is presumed that the ketone-based solvent or alcohol-based solvent as solvent A inhibits the formation of hydrogen bonds. Therefore, solidification is less likely to occur even when stored at low temperatures. Furthermore, since the adhesive composition of the present disclosure is less likely to solidify even when stored at low temperatures, deterioration of coatability is also suppressed.
[0014] The adhesive composition of the present disclosure will be described in detail below.
[0015] (Acid-modified polyolefin) An acid-modified polyolefin is an acid-modified polyolefin obtained by modifying a polyolefin (hereinafter also referred to as an "unmodified polyolefin") to impart an acid group. Specifically, the acid-modified polyolefin is obtained by modifying an unmodified polyolefin with an acid group-containing monomer.
[0016] Specific examples of unmodified polyolefins include polyethylene, polypropylene, random copolymers of propylene and ethylene, block copolymers of propylene and ethylene, random copolymers of ethylene and α-olefins, block copolymers of ethylene and α-olefins, random copolymers of propylene and α-olefins, block copolymers of propylene and α-olefins, etc. Here, examples of α-olefins include 1-butene, isobutylene, 1-hexene, and 1-octene.
[0017] Among these, from the viewpoint of improving adhesiveness, polypropylene-based polymers such as polypropylene, propylene-ethylene block copolymers, propylene-ethylene random copolymers, propylene and α-olefin random copolymers, and propylene and α-olefin block copolymers are preferred as unmodified polyolefins.
[0018] In the acid group-containing monomer for modifying the unmodified polyolefin, examples of the acid group include a carboxylic acid group, a carboxylic acid anhydride group, a sulfonic acid group, and a phosphoric acid group. Among these, a carboxylic acid group (or a carboxylic acid anhydride group) is preferred because it is easy to modify.
[0019] The carboxylic acid group (or carboxylic anhydride group)-containing monomer is a compound having an ethylenic double bond and a carboxylic acid group in the same molecule, and examples thereof include various unsaturated monocarboxylic acid compounds, unsaturated dicarboxylic acid compounds, and unsaturated tricarboxylic acid compounds. Specific examples of unsaturated monocarboxylic acid compounds include acrylic acid, methacrylic acid, crotonic acid, and isocrotonic acid. Examples of unsaturated dicarboxylic acid compounds include maleic acid, itaconic acid, citraconic acid, tetrahydrophthalic acid, nadic acid, and endic acid. Examples of unsaturated tricarboxylic acid compounds include aconitic acid. As the acid group-containing monomer, unsaturated dicarboxylic acid compounds and unsaturated tricarboxylic acid compounds are preferred, with itaconic acid, maleic acid, and aconitic acid being particularly preferred, due to their ease of modification and excellent adhesive properties. The acid group-containing monomer may be used alone or in combination of two or more types.
[0020] The acid-modified polyolefin may be modified (e.g., graft-modified) with a (meth)acrylic acid alkyl ester. The (meth)acrylic acid alkyl ester is preferably an ester of an alkyl alcohol having 8 to 18 carbon atoms with (meth)acrylic acid.
[0021] The acid value can be used as a measure of the amount of functional groups introduced into the acid-modified polyolefin. From the viewpoint of improving adhesiveness, the acid value is preferably 1.0 to 30.0 mgKOH / g, more preferably 5.0 to 25.0 mgKOH / g, and even more preferably 8.0 to 20.0 mgKOH / g. The acid value of the acid-modified polyolefin is measured as follows: Approximately 10 g of acid-modified polyolefin is accurately weighed and placed in a 200 mL tall beaker. 150 mL of a mixed solvent consisting of xylene and dimethylformamide mixed in a 1:1 (volume ratio) ratio is added as the titration solvent. Titration is performed using a 1 w / v % phenolphthalein ethanol solution (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as an indicator, and the acid value is determined from the titration amount. Specifically, the acid value can be calculated using the following formula. The acid value is the average value of three repeated titrations. Acid value (mgKOH / g)=(EP1-BL1)×FA1×C1 / SIZE In the formula, "EP1" represents the titration amount (mL), "BL1" represents the blank value (mL), "FA1" represents the factor of the titrant (1.00), "C1" represents the concentration equivalent value (5.611 mg / m), and "SIZE" represents the amount of acid-modified polyolefin collected (g).
[0022] From the viewpoint of improving heat resistance, the melting point of the acid-modified polyolefin is preferably 50 to 120° C., more preferably 60 to 110° C., and even more preferably 70 to 95° C. The melting point of the acid-modified polyolefin is measured as follows: Using a differential scanning calorimeter (hereinafter referred to as DSC, manufactured by TA Instruments Japan, Q-2000), the polyolefin is heated and melted at a rate of 20° C. / min, cooled to form a resin, and then heated and melted again, and the melting point is measured from the top temperature of the melting peak.
[0023] The weight average molecular weight Mw of the acid-modified polyolefin is preferably 3,000 to 500,000, more preferably 25,000 to 250,000, from the viewpoint of improving adhesiveness and solubility in solvents. The weight average molecular weight Mw of the acid-modified polyolefin is a value obtained by converting the molecular weight measured by gel permeation chromatography into polystyrene equivalent.
[0024] In terms of improving adhesiveness, the propylene unit content in the acid-modified polyolefin is preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more.
[0025] The acid-modified polyolefins may be used alone or in combination of two or more.
[0026] The content of the acid-modified polyolefin is preferably 80 to 100% by mass, more preferably 90 to 100% by mass, based on all components of the adhesive composition other than the solvent.
[0027] (Solvent) The solvent contains an aromatic solvent, at least one solvent A selected from a ketone solvent and an alcohol solvent, and an aliphatic solvent.
[0028] Aromatic Solvents Aromatic solvents are solvents having an aromatic ring in one molecule. Examples of aromatic solvents include toluene, o-xylene, m-xylene, p-xylene, anisole, ethyl benzyl ether, cresyl methyl ether, diphenyl ether, dibenzyl ether, phenetole, butyl phenyl ether, ethyl benzene, diethyl benzene, pentyl benzene, isopropyl benzene, cymene, and mesitylene. Among these, aromatic solvents having 6 to 8 carbon atoms and a low number of substituents (particularly toluene) are preferred in terms of suppressing solidification.
[0029] -Solvent A- Ketone solvents are solvents having a ketone group in one molecule. Examples of ketone solvents include methyl ethyl ketone, acetone, diethyl ketone, methyl isobutyl ketone, methyl-n-pentyl ketone, methyl isopentyl ketone, and 2-heptanone.
[0030] An alcohol-based solvent is a solvent having an alcoholic hydroxyl group in one molecule. Examples of alcohol-based solvents include methanol, ethanol, isopropyl alcohol, normal propyl alcohol, ethylene glycol, diethylene glycol, propylene glycol, and dipropylene glycol.
[0031] Among these, from the viewpoint of inhibiting solidification, preferred ketone solvents are lower alkyl ketones having 3 to 5 carbon atoms (particularly methyl ethyl ketone), and preferred alcohol solvents are lower alcohols having 1 to 4 carbon atoms (particularly isopropyl alcohol). Also, from the viewpoint of inhibiting solidification, preferred solvents A are ketone solvents.
[0032] Aliphatic Solvents Aliphatic solvents are solvents having an aliphatic group in one molecule. Examples of aliphatic solvents include n-heptane, n-hexane, octane, nonane, decane, undecane, dodecane, cyclohexane, methylcyclohexane, ethylcyclohexane, dimethylcyclohexane, paraffin solvents, and isododecane. Among these, alicyclic hydrocarbons (particularly methylcyclohexane) are preferred as aliphatic solvents in terms of preventing solidification.
[0033] -Solvent Component Ratio- From the viewpoint of inhibiting solidification, when the total amount of solvents is taken as 100 parts by mass, the amount of each solvent is as follows: The amount of aromatic solvent is 10 to 45 parts by mass, preferably 10 to 30 parts by mass, and more preferably 10 to 20 parts by mass. The amount of at least one solvent A selected from ketone solvents and alcohols is 5 to 19 parts by mass, preferably 8 to 19 parts by mass, and more preferably 10 to 19 parts by mass. The amount of aliphatic solvent is 45 to 70 parts by mass, preferably 55 to 70 parts by mass, and more preferably 60 to 70 parts by mass.
[0034] From the viewpoint of suppressing solidification, the ratio of the aromatic solvent to the aliphatic solvent is preferably 15 to 25 mass%, more preferably 15 to 23 mass%, and even more preferably 15 to 20 mass%. From the viewpoint of suppressing solidification, the ratio of solvent A to the aliphatic solvent is preferably 5 to 35 mass%, more preferably 10 to 35 mass%, and even more preferably 15 to 35 mass%.
[0035] The solvent may contain a solvent other than an aromatic solvent, solvent A (at least one selected from a ketone solvent and an alcohol solvent), and an aliphatic solvent. However, the proportion of the aromatic solvent, solvent A, and aliphatic solvent in the solvent is preferably 90% by mass or more (preferably 95% by mass or more). The proportion of the aromatic solvent, solvent A, and aliphatic solvent in the solvent is preferably 100% by mass.
[0036] The content of the solvent is preferably 75 to 95% by mass, more preferably 80 to 90% by mass, based on the adhesive composition.
[0037] (Other Components) The adhesive composition of the present disclosure may be either a one-component adhesive composition or the first part of a two-component adhesive composition. Depending on the embodiment, the adhesive composition of the present disclosure may also contain a curing agent and / or a curing accelerator.
[0038] Examples of the curing agent include well-known compounds capable of curing (e.g., crosslinking) by reacting with at least the acid groups of the acid-modified polyolefin, such as polyfunctional isocyanate compounds, polyfunctional epoxy compounds, polyfunctional carbodiimide compounds, polyfunctional oxazoline compounds, and polyfunctional aziridine compounds. For purposes such as adjusting the viscosity of the solution and adjusting the properties of the cured product of the adhesive composition of the present disclosure, the curing agent may be used in combination with a monofunctional compound such as a monofunctional isocyanate compound, monofunctional epoxy compound, monofunctional carbodiimide compound, monofunctional oxazoline compound, or monofunctional aziridine compound. Examples of the curing accelerator include well-known curing accelerators such as imidazole compounds, amine compounds, and phosphorus compounds. When a curing agent is included, the content of the curing agent is preferably 1 to 30 parts by mass, more preferably 1 to 15 parts by mass, per 100 parts by mass of the acid group-containing resin, in terms of improving adhesion and heat resistance. When a curing accelerator is contained, the content of the curing accelerator is preferably 1 to 10 parts by mass, more preferably 2 to 5 parts by mass, per 100 parts by mass of the curing agent. When the content of the curing accelerator is within the above range, excellent adhesiveness and heat resistance are improved.
[0039] Depending on the above-described embodiment, the adhesive composition of the present disclosure may also contain well-known components such as thermoplastic resins other than the acid group-containing resin, tackifiers, flame retardants, coupling agents, heat aging inhibitors, leveling agents, antifoaming agents, inorganic fillers, and pigments.
[0040] (Applications) The adhesive composition of the present disclosure is suitable for bonding metals, glass, plastics, resin films, and the like.
[0041] The adhesive composition of the present disclosure will be described in more detail below with reference to examples. The materials, amounts used, ratios, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present disclosure. Therefore, the scope of the resin composition of the present disclosure should not be interpreted as being limited by the specific examples shown below.
[0042] Example 1 16.0 g of maleic anhydride-modified polyolefin-1 (propylene-butene-1 copolymer, melting point 80°C, weight average molecular weight Mw 90,000, acid value 10 mgKOH / g) was dissolved in a mixed solvent of 27.0 g of toluene, 6.0 g of methyl ethyl ketone, and 67.0 g of methylcyclohexane at 60°C, and then 2.0 g of an epoxy resin (EPICLON HP-7200, manufactured by DIC Corporation) as a curing agent was dissolved therein to obtain an adhesive composition.
[0043] Examples 2 to 6, Comparative Examples 1 to 6 The adhesive compositions of each example were prepared in the same manner as in Example 1, except that the components used and their blending amounts were changed as shown in Table 1.
[0044] The details of the components used are as follows: Maleic anhydride-modified polyolefin-1 (referred to as "acid-modified PO-1" in Table 1): propylene-butene-1 copolymer, melting point 80°C, weight average molecular weight Mw 90,000, acid value 10 mgKOH / g Maleic anhydride-modified polyolefin-2 (referred to as "acid-modified PO-2" in Table 1): propylene-butene-1 copolymer, melting point 85°C, weight average molecular weight Mw 147,000, acid value 15 mgKOH / g Maleic anhydride-modified polyolefin-3 (referred to as "acid-modified PO-3" in Table 1): propylene-butene-1 copolymer, melting point 80°C, weight average molecular weight Mw 60,000, acid value 20 mgKOH / g Epoxy resin: EPICLON HP-7200 (manufactured by DIC Corporation), a dicyclopentadiene skeleton-containing epoxy resin
[0045] <Evaluation> The adhesive compositions of the Examples and Comparative Examples were evaluated as follows, and the results are summarized in Table 1.
[0046] (Low temperature storage properties) The adhesive composition obtained in each example was stored in an atmosphere of 5°C for 7 days. After storage for 7 days, the adhesive composition was visually inspected for solidification. The state of the adhesive was evaluated as follows: [Evaluation criteria] A: No solidification, no turbidity. A-: No solidification, but turbidity present. B: Liquid has fluidity, but fine solid matter can be seen. C: Completely solidified, no fluidity.
[0047] (Coatability) The adhesive obtained in each example was stored in a 5°C atmosphere for 7 days. After storage for 7 days, the adhesive was applied to a 100 μm thick PET film at room temperature using a bar coater so that the resulting resin thickness after drying would be 5 μm, and the solvent was evaporated in a dryer at 100°C for 1 minute to obtain a coated film. The film was then visually inspected for the presence or absence of coating unevenness. The condition of the coated film was evaluated as follows: [Evaluation criteria] A: No coating unevenness at all. B: Coating unevenness present. C: Unable to coat.
[0048] The above examples and evaluation results are shown in Tables 1 to 3. The unit of the numerical values in the column for each component in Table 1 is "g." "*1" is the ratio (% by mass) of aromatic solvent to aliphatic solvent. "*2" is the ratio (% by mass) of solvent A (at least one selected from ketone solvents and alcohol solvents) to aliphatic solvent.
[0049] From the above results, the adhesive composition of this example did not solidify and had good applicability even when stored for 7 days in an atmosphere of 5° C. On the other hand, solidification was confirmed in the adhesive composition of the comparative example.
[0050] The disclosure of Japanese Patent Application No. 2023-085809 is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. An adhesive composition comprising an acid-modified polyolefin and a solvent, the solvent containing, relative to a total amount of the solvent being 100 parts by mass, 10 to 45 parts by mass of an aromatic solvent, 5 to 19 parts by mass of at least one solvent A selected from ketone solvents and alcohol solvents, and 45 to 70 parts by mass of an aliphatic solvent.
2. The adhesive composition according to claim 1, wherein the ratio of said aromatic solvent to said aliphatic solvent is 15 to 25% by mass.
3. The adhesive composition according to claim 1 or 2, wherein the ratio of said solvent A to said aliphatic solvent is 5 to 35 mass %.
Citation Information
Patent Citations
Binder resin solution composition having good solution properties
JP2002080666A
Curable resin composition, polarizing film and production method of the same, optical film and image display device
JP2017160313A
Adhesive resin composition and laminate
JP2019038902A
Adhesive composition, and adhesive layer-equipped layered product using same