Method for producing regenerated fiber
The method of using superheated steam and an oxidizing agent within a cartridge system to recycle fiber composite materials addresses the inefficiencies and environmental concerns of existing methods, resulting in high-quality, economically viable, and eco-friendly recycled fibers.
Patent Information
- Application Number
- PCT/KR2024/006037
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-19
- Filing Date
- 2024-05-03
- Publication Date
- 2024-11-28
AI Technical Summary
Current methods for recycling carbon and glass fibers from composite materials face challenges such as energy-intensive processes, air pollution, complex procedures, and deterioration of physical properties, particularly with thermal decomposition, and environmental concerns with solvent methods.
A method involving pretreated fiber composite materials exposed to superheated steam and an oxidizing agent within a cartridge system, where the gaseous matrix resin is condensed using cooling water and recycled, minimizing physical property deterioration and simplifying the process.
This approach reduces energy consumption, shortens processing time, minimizes environmental impact, and enhances the quality and recyclability of regenerated fibers, making the process more economically feasible and productive compared to conventional methods.
Smart Images

Figure KR2024006037_28112024_PF_FP_ABST
Abstract
Description
Regenerated fiber manufacturing method
[0001] The present invention relates to a method for manufacturing regenerated fiber.
[0002]
[0003] Fiber composites, typically composed of carbon or glass fibers mixed with a thermosetting or thermoplastic resin (matrix resin), are high-strength, high-elasticity, lightweight, heat-resistant, and chemical-resistant materials widely used in industrial applications such as aerospace, wind power generation, and automobiles. However, fiber composites are difficult to separate due to the strong bond between the carbon and glass fibers and the resin. Furthermore, fiber composites, especially those manufactured with thermosetting resins, are undeniably non-recyclable, resulting in most waste being incinerated or landfilled. Recently, regulations on waste disposal of fiber composites, including carbon composites, have been strengthening. In Europe, incineration is prohibited, and while landfilling is restricted in some countries, landfilling is gradually becoming more widespread. Therefore, technologies for recovering carbon or glass fibers from fiber composites can reduce environmentally problematic waste generation and offer economic value from the perspective of recycling and reusing expensive carbon or glass fibers.
[0004] Currently, the two main technologies for recovering carbon fiber from carbon fiber composites are pyrolysis and solvent methods. Pyrolysis, due to its simple process, is the most widely used. However, it suffers from the generation of resin residue (char) on the surface of the regenerated fiber after decomposition and the deterioration of the physical properties of the recovered carbon fiber (regenerated fiber). Furthermore, large-capacity furnaces consume significant energy, and the decomposed resin is converted into gaseous substances and discharged, which can cause air pollution. The solvent method is considered a more environmentally friendly technology, as it produces stable physical properties of recovered carbon fiber (regenerated fiber) and produces no exhaust gases. However, it faces challenges in the treatment and recovery of decomposition products, including solvents discharged into wastewater. Furthermore, the solvent method has relatively long decomposition reaction times, and the degradation conditions (solvent, time, temperature, etc.) must be adjusted depending on the type and composition of the target resin. Furthermore, the solvent method requires pretreatment, decomposition, washing, and drying, resulting in a complex and lengthy process.
[0005] Therefore, the direction of recent research and development requires a combined decomposition technology that reduces the energy consumption, which is a disadvantage of thermal decomposition, and minimizes the complex process and long decomposition time, which are disadvantages of solvent decomposition, as well as an eco-friendly technology that can recycle decomposition substances generated from resins in addition to carbon fibers.
[0006]
[0007] Accordingly, the inventors of the present invention conducted research from various angles to solve the above problem, and as a result, they completed a method for manufacturing regenerated fibers that can prevent deterioration of the physical properties of regenerated fibers such as carbon fibers recovered from fiber composite materials, while simultaneously cooling and condensing superheated steam to convert it into water for recovery, and then recycling the resin, which is a decomposed substance, through separation and purification.
[0008] Accordingly, the purpose of the present invention is to provide an eco-friendly method for producing regenerated fibers capable of obtaining regenerated fibers with suppressed deterioration of physical properties.
[0009]
[0010] In order to achieve the above object, the present invention provides a method for producing regenerated fiber, comprising the steps of: loading a pretreated fiber composite material into a cartridge; moving the cartridge into which the pretreated fiber composite material is loaded, exposing the cartridge to superheated steam and an oxidizing agent to remove matrix resin and char from the pretreated fiber composite material, thereby producing regenerated fiber; and moving the cartridge containing the regenerated fiber and collecting the regenerated fiber from the cartridge.
[0011] The step of exposing the above cartridge to superheated steam and an oxidizing agent may be a step of first exposing the cartridge containing the pretreated fiber composite material to superheated steam, and then moving the cartridge and exposing it to an oxidizing agent.
[0012] The present invention may further include a step of first exposing the cartridge containing the pretreated fiber composite material to superheated steam and then, before exposing it to an oxidizer, condensing the gaseous matrix resin decomposed from the pretreated fiber composite material into a liquid state using cooling water and removing it.
[0013] The step of condensing the gaseous matrix resin decomposed from the pretreated fiber composite material into a liquid state and removing it may be a step in which the gaseous matrix resin decomposed from the pretreated fiber composite material escapes from the cartridge by exposure to the superheated steam, reacts with cooling water that is separated from the cartridge and exists separately, and becomes a liquid condensate and is removed.
[0014] The oxidizing agent may include air.
[0015] The above fiber composite material may be a matrix resin mixed with ‘carbon fiber, glass fiber or a mixture thereof.’
[0016] The above matrix resin may include an aromatic hydrocarbon compound.
[0017] The above aromatic hydrocarbon compound may include a phenol compound.
[0018] The above aromatic hydrocarbon compound includes bisphenol A, and the bisphenol A may be included in an amount of 30 wt% or more based on the total amount of the aromatic hydrocarbon compound.
[0019] The above pretreated fiber composite material may be a shredded or cut fiber composite material.
[0020] The above superheated steam may have a temperature range of 400°C to 900°C.
[0021] The cartridge containing the above-mentioned pretreated fiber composite material can be exposed to the above-mentioned superheated steam for 30 to 120 minutes.
[0022] The step of exposing to the superheated steam includes a step of spraying the superheated steam into a cartridge into which the pretreated fiber composite material is introduced, and the superheated steam can be sprayed into the cartridge at a flow rate of 10 kg / h to 30 kg / h.
[0023] The step of exposing to the oxidizing agent includes a step of spraying the superheated steam into a cartridge into which the pretreated fiber composite material is introduced, and then spraying the oxidizing agent into the cartridge, wherein the oxidizing agent can be sprayed into the cartridge at a flow rate of 5 L / min or more.
[0024] The present invention may further include a step of first exposing the cartridge to nitrogen before exposing the cartridge to the superheated steam after the step of introducing the pretreated fiber composite material into the cartridge.
[0025] The present invention may further include a step of first exposing the cartridge containing the regenerated fiber to nitrogen before moving the cartridge after the step of manufacturing the regenerated fiber.
[0026] The above-mentioned difference may be present on the surface of the regenerated fiber from which the matrix resin has been removed.
[0027]
[0028] The method for manufacturing regenerated fibers according to the present invention uses a pretreated fiber composite material, exposes the pretreated fiber composite material to superheated steam, and controls the temperature, exposure time, flow rate, etc. of the superheated steam when exposed to the superheated steam, and further, additionally injects an oxidizing agent such as air with a controlled flow rate separately from the superheated steam, thereby minimizing the deterioration of the physical properties of the recovered regenerated fibers, and further, since a cartridge method is used instead of a roller method, the process defect rate is significantly low and the process is simple, so that the process time can be greatly shortened, and since cooling water instead of outside air is used to convert the matrix resin, which is one of the decomposition products, into condensate, the matrix resin can be easily recycled, and further, since rapid condensate generation is possible, the energy consumption can be greatly reduced, so that the economic feasibility and productivity of the regenerated fiber manufacturing process can be dramatically improved compared to conventional pyrolysis methods, etc.
[0029]
[0030] Figure 1 is a flow chart sequentially illustrating a method for manufacturing regenerated fiber according to the present invention.
[0031]
[0032] Hereinafter, the present invention will be described in more detail.
[0033] The advantages and features of the technology described below, as well as the methods for achieving them, will become clearer with reference to the detailed implementation examples described below. However, the form of implementation may not be limited to the implementation examples disclosed below. Unless otherwise defined, all terms (including technical and scientific terms) used herein may be used in a meaning that can be commonly understood by those of ordinary skill in the relevant technical field. In addition, terms defined in commonly used dictionaries are not to be interpreted ideally or excessively unless explicitly and specifically defined.
[0034] The terms used in this invention are used solely to describe specific embodiments and are not intended to limit the invention. Singular expressions include plural expressions unless the context clearly dictates otherwise.
[0035] In the present invention, terms such as 'include' or 'have' are intended to specify the presence of a feature, number, step, operation, component, part or combination thereof described in the specification, but should be understood as not excluding in advance the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts or combinations thereof.
[0036]
[0037] Superheated steam refers to a high-temperature dry steam state that is obtained by heating water vapor above its saturation temperature, and it is a heat medium that contains more heat than heated air. Superheated steam has a high heat transfer rate at the same pressure and a high heat density, so it can shorten the heating time of the object to be heated through rapid heating. In addition, superheated steam is a gaseous substance composed only of water molecules and can maintain an inert state due to the absence of oxygen, and its heat efficiency is very high due to heat transfer through combined heat transfer (convection, radiation, and condensation). Therefore, the technology to recover regenerated fibers such as carbon fiber using superheated steam has the advantage of removing the resin more quickly by directly spraying superheated steam on the object to be decomposed.
[0038] However, the deterioration of the physical properties of regenerated fibers such as carbon fibers that are recovered is inevitable, and if the deterioration of the physical properties of the regenerated fibers is severe, they cannot be recycled. In addition, there is a high possibility that the resin decomposed together with the regenerated fibers may itself become an environmental pollution issue. Therefore, there has been a continuous need for more advanced technological improvements in decomposition technology using superheated steam.
[0039] After accurately identifying the needs in the market as described above, the inventors of the present invention conducted repeated research and found that, in a method for manufacturing regenerated fibers by spraying superheated steam, if a method of moving a fiber composite material through a roller was used in the past, by moving the fiber composite material in the form of a cartridge instead of the roller, and by condensing the gaseous matrix resin decomposed by the superheated steam spray using cooling water instead of the outside air, the eco-friendliness, economic efficiency, and productivity of the regenerated fiber manufacturing process were dramatically improved (in particular, eco-friendliness issues such as fine dust scattering have always been an issue when using rollers in the past, but there is no room for such issues when using cartridges. In addition, while cartridges can be continuously reused through washing, rollers need to be replaced periodically, making the use of cartridges much more advantageous in terms of eco-friendliness). Furthermore, by pretreating the fiber composite material, exposing it to superheated steam, and controlling the temperature, exposure time, flow rate, etc. of the superheated steam, it is possible to manufacture regenerated fibers having properties far superior to those of existing recovered regenerated fibers by minimizing the deterioration of the properties of the recovered regenerated fibers, such as carbon fibers.
[0040] Referring to FIG. 1, a method for manufacturing regenerated fibers according to the present invention will be described, including a step of loading a pretreated fiber composite material into a cartridge (S100); a step of moving the cartridge into which the pretreated fiber composite material is loaded (S200); a step of exposing the cartridge to superheated steam and an oxidizing agent (S300); a step of removing matrix resin and char from the pretreated fiber composite material to manufacture regenerated fibers (S400); and a step of moving the cartridge containing the regenerated fibers and collecting the regenerated fibers (S500).
[0041] That is, the pretreated fiber composite material is decomposed by superheated steam into regenerated fibers and matrix resin, and the regenerated fibers are sequentially moved through the cartridge and recovered, and the matrix resin is changed from a gaseous state to a liquid condensate by cooling water as described below and moved to a condensate tank, and thereafter, it can be recycled through a separation and purification process. The recovered regenerated fibers can be reused through chopping and milling.
[0042] In other words, according to the method for manufacturing regenerated fibers according to the present invention, regenerated fibers with minimized property degradation and recyclable matrix resins can be easily obtained simultaneously from a fiber composite material through a series of continuous processes.
[0043] Specifically, the step of exposing the cartridge to the superheated steam and the oxidizing agent may be a step of first exposing the cartridge containing the pretreated fiber composite material to the superheated steam, and then moving the cartridge and exposing it to the oxidizing agent. Exposing the cartridge to the superheated steam first may be more advantageous for removing the matrix resin and char than exposing it to the oxidizing agent first.
[0044] For example, the method for manufacturing regenerated fiber according to the present invention may further include a step of first exposing a cartridge containing the pretreated fiber composite material to superheated steam and then, before exposing it to an oxidizing agent, condensing the gaseous matrix resin decomposed from the pretreated fiber composite material into a liquid state using cooling water and removing it. By condensing the matrix resin decomposed from the pretreated fiber composite material using cooling water rather than the outside air, the matrix resin can be removed much more easily and completely. Specifically, the gaseous matrix resin decomposed from the pretreated fiber composite material by the exposure to superheated steam escapes from the cartridge, reacts with cooling water present separately from the cartridge, and becomes a liquid condensate, which can be transferred to a separate condensate tank and ultimately removed.
[0045] Fiber composite materials that can be used for superheated steam decomposition are largely divided into carbon fiber composite materials (CFRP) and glass fiber composite materials (GFRP), and can be used for decomposition regardless of the structure, shape, or type of material, and are usually a mixture of reinforcing materials and matrix resin. Fibrous materials used as the reinforcing materials include carbon fibers, glass fibers, etc., and the matrix resins include thermosetting resins such as epoxy, phenol, unsaturated polyester, polyurethane, melamine, urea, etc., and thermoplastic resins such as polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyamide, polycarbonate, polyimide, etc. Generally, the fiber composite materials used are in the form of a mixture of the reinforcing materials listed above and the matrix resin at a certain ratio, and the ratio of the reinforcing material and the resin may vary depending on the application.
[0046] For example, the matrix resin may include an aromatic hydrocarbon compound, and the aromatic hydrocarbon compound may include a phenol compound, and the phenol compound may include, but is not necessarily limited to, phenol, o-cresol, p-cresol, p-ethylphenol, p-isopropylphenol, p-isopropenylphenol, p-hydroxy-2,2-diphenylpropane, p-hydroxy-3-methyl-2,2-diphenylpropane, 2-(4-hydroxyphenyl)-2-(4'-methoxyphenyl)propane, bisphenol A, 2-(4-hydroxy-3-methylphenyl)-2-(4'-hydroxyphenyl)propane, 2-(benzofu-5-yl)-2-(p-hydroxyphenyl)propane, or a combination thereof.
[0047] However, the aromatic hydrocarbon compound, specifically the phenol compound, may include the bisphenol A.
[0048] For example, the bisphenol A may be included in the largest amount among the aromatic hydrocarbon compounds (specifically, phenol compounds), for example, 30 wt% or more, for example, 50 wt% or more, based on the total amount of the phenol compounds. When the composition of the matrix resin including the aromatic hydrocarbon compound (specifically, phenol compounds) containing the bisphenol A in the above content range is as described above, it may be very easy to separately recover it and recycle it through separation, filtration, and purification.
[0049] For example, the pretreated fiber composite material may be a shredded or cut fiber composite material. It may be advantageous to use the fiber composite material for decomposition using superheated steam by crushing or cutting it into a certain size and shape for use in the process, in terms of preventing deterioration of the physical properties of the ultimately obtained regenerated fiber. For example, the crushing method includes a shredder, a chopper, a cracker mill, a hammer mill, etc., and the fiber composite material can be crushed into a certain size range. However, the crushed composite material has an uneven size and generates a lot of dust and powder, which may reduce the effect of preventing a decline in the quality and yield of the recovered carbon fiber and may worsen the working environment. However, in the case of a fiber composite material manufactured using a cutter, the dust and powder generated as described above are small, which increases the yield and allows cutting to a certain size, so that the fiber length of the recovered carbon fiber and other regenerated fibers is relatively uniform and the deterioration in quality is minimized. That is, the above pretreatment may be more advantageous in preventing deterioration of the properties of regenerated fibers through cutting rather than shredding.
[0050] The above pretreated fiber composite material is placed in a cartridge, and then automatically moved and exposed to superheated steam and an oxidizer (specifically, the superheated steam and oxidizer are sequentially sprayed onto the automatically moved cartridge), thereby causing decomposition of the pretreated fiber composite material.
[0051] For example, according to the method for manufacturing regenerated fibers according to the present invention, the decomposition rate of the fiber composite material is very excellent. Here, the decomposition rate refers to a value according to the following mathematical formula 1.
[0052] [Mathematical Formula 1]
[0053] Decomposition rate (wt%) = {(A - B) / (A x C)} x 100
[0054] In the above mathematical formula 1,
[0055] A is the weight of the fiber composite material before decomposition (g),
[0056] B is the weight of the fiber composite material after decomposition (g),
[0057] C is the matrix resin content (wt%) in the fiber composite material based on the total amount of fiber composite material before decomposition.
[0058] The superheated steam injected into the cartridge containing the above-mentioned pretreated fiber composite material is injected using a superheated steam generator, and superheated steam heated to a temperature of, for example, 400°C to 900°C, for example, 400°C to 800°C, for example, 500°C to 900°C, for example, 500°C to 800°C can be used. If the temperature of the superheated steam is less than 400°C, a problem of a rapid decrease in the decomposition rate may occur, and if the temperature of the superheated steam exceeds 900°C, the tensile strength of the recovered (manufactured) regenerated fiber may be lowered, which may be undesirable.
[0059] For example, superheated steam having the above temperature range can be sprayed onto the cartridge for 30 to 120 minutes, for example, 30 to 110 minutes, for example, 30 to 100 minutes, for example, 30 to 90 minutes. If superheated steam in the above temperature range is sprayed onto the cartridge for less than 30 minutes, a problem of a rapid decrease in the decomposition rate may occur, and if superheated steam in the above temperature range is sprayed onto the cartridge for more than 120 minutes, the degree of increase in the decomposition rate and decrease in tensile strength is not large, and thus it may be uneconomical to expose the pretreated fiber composite material to superheated steam in the above temperature range for a time exceeding 120 minutes.
[0060] For example, superheated steam within the above temperature range can be injected into the cartridge at a flow rate of 10 kg / h to 30 kg / h, for example, 10 kg / h to 25 kg / h, for example, 10 kg / h to 20 kg / h, within the above time range. If the superheated steam flow rate is less than 10 kg / h or more than 30 kg / h, the tensile strength of the produced regenerated fiber may be lowered, which may be undesirable.
[0061] Char, which is composed of a small amount of carbon derived from the matrix resin decomposed from the fiber composite material by exposure to the superheated steam, may remain on the surface of the reinforcing material (carbon fiber and / or glass fiber). Char is generated at a ratio of about 5 to 10 wt% of the resin contained in the fiber composite material, and the reinforcing material is manufactured in a form in which it is not separated alone but is clumped together due to the char. Reinforcing material containing char has low flexibility and acts as an impurity in the subsequent process, so it needs to be removed. Char is a carbonaceous substance and is difficult to remove with only superheated steam in an inert atmosphere, but can be removed by introducing an oxidizer. Here, the oxidizer may be an active gas such as air or oxygen.
[0062] Specifically, the reinforcing material containing the Char is moved while being contained in a cartridge, and thereafter, air is automatically sprayed onto the cartridge containing the reinforcing material containing the Char. Through this continuous process, that is, by additionally introducing air, the Char can be removed. At this time, in order to remove the Char, high temperature heat and an appropriate amount of air flow are required. If the temperature is low or the air flow rate is small, the Char cannot be removed, and if the temperature is too high or the air flow rate is large, the Char can be completely removed, but the reinforcing material may be damaged and its physical properties may deteriorate. Therefore, an appropriate temperature, time, and air flow rate are important, and in order to remove the Char, the treatment can be performed within the range of a temperature of 400°C to 900°C, a time of 10 to 90 minutes, and an air flow rate of 5 L / min or more, and preferably, the treatment can be performed within the range of a temperature of 500°C to 800°C, a time of 30 to 60 minutes, and an air flow rate of 5 L / min. In particular, even if the temperature and time range of the injected air are controlled within the above range, the effect of improving the decomposition rate may be minimal when the air flow rate is less than 5 L / min.
[0063] If the above char is not removed, it acts as an impurity and lowers the decomposition rate, so it is better to remove it. However, as mentioned above, if the char is removed by injecting air, the decomposition rate increases, but there is a problem that the tensile strength retention rate and elasticity retention rate of the regenerated fiber ultimately recovered may slightly decrease. In order to solve this problem, in the method for manufacturing regenerated fiber according to the present invention, the flow rate of the injected air was controlled.
[0064] Furthermore, the method for manufacturing regenerated fibers according to the present invention may further include a step of first exposing the cartridge to nitrogen before exposing the cartridge to the superheated steam after the step of introducing the pretreated fiber composite material into the cartridge, or a step of first exposing the cartridge containing the regenerated fibers to nitrogen before moving the cartridge after the step of manufacturing the regenerated fibers. In this case, it may be more advantageous to prevent the phenomenon of a decrease in the tensile strength retention rate and elasticity retention rate of the recovered regenerated fibers.
[0065] In this way, the reinforcing material from which the char has been removed is automatically transported in a cartridge, and by collecting the reinforcing material (regenerated fiber) from the cartridge, regenerated fiber can be manufactured. The weight of the recovered regenerated fiber is confirmed, and the final decomposition rate and yield are calculated to confirm the physical properties of the regenerated fiber.
[0066] The tensile strength of the above-mentioned regenerated fiber (reinforcement) can be measured using the Single Fiber method (ASTM C1557-03). The Single Fiber method can be used to isolate a single strand of reinforcement longer than 25 mm, and measure it more than 30 times using a Universal Testing Machine (UTM) at a test speed of 1 mm / min, a grip spacing of 25 mm, and an initial load of 1 cN / tex, and then take the average value.
[0067]
[0068] According to the method for manufacturing regenerated fiber of the present invention, i) it is clearly distinguished from the conventional roller process in that it uses a pre-treated fiber composite material, ii) it is based on a series of automatic processes using a cartridge push method, iii) it is also distinguished from the conventional process using outside air in that it condenses and removes the gaseous matrix resin into a liquid state using cooling water, iv) it controls the temperature, time, and flow rate of the superheated steam in the superheated steam exposure section, and v) it controls the temperature, time, and flow rate of the air in the resin removal section, thereby not only being able to recover regenerated fibers with minimized deterioration in physical properties but also being able to easily obtain the matrix resin in the form of condensate at the same time, it is environmentally friendly and has excellent processability and economic feasibility compared to the conventional method for recovering regenerated fibers.
[0069]
[0070] Hereinafter, preferred examples are presented to help understand the present invention, but the following examples are only illustrative of the present invention, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope and technical idea of the present invention, and it is natural that such changes and modifications fall within the scope of the appended claims.
[0071]
[0072] Exam example
[0073] 1. Effect according to superheated steam temperature
[0074] 130 g of hydrogen tank cuttings (50 x 100 mm) were placed in a cartridge within the inlet of an automatic regenerated fiber manufacturing device of a cartridge push type, and the cartridge was moved to expose it to superheated steam. At this time, the discharge temperature of the superheated steam being sprayed was varied as shown in Table 1 below, and the decomposition rate and the properties of the ultimately recovered carbon fibers were evaluated, and the results are shown in Table 1 below. After the superheated steam was sprayed, the cartridge was moved again and air was sprayed to expose the cartridge to air, and the air flow rate at this time was controlled to 5 L / min. After the superheated steam was sprayed and before the air was sprayed, cooling water was used to condense and remove the decomposed matrix resin from the hydrogen tank cuttings in the cartridge into which the superheated steam was sprayed. After the air spraying, the cartridge was moved, and the carbon fibers were recovered from the cartridge.
[0075]
[0076] Temperature (℃) Time (min) Steam flow rate (kg / h) Air flow rate (L / min) Weight (g) Decomposition rate (wt%) Physical property (GPa) Tensile strength 3009020513040.064.6640085.784.6650088.374.6660090.134.6270090.944.6380095.644.4090097.004.111,00097.903.94
[0077] From the above Table 1, it can be confirmed that when the discharge temperature of the superheated steam is controlled to 400°C to 900°C, both the decomposition rate and the tensile strength of the recovered regenerated fiber are excellent.
[0078] 2. Effect according to superheated steam flow rate
[0079] Except that the superheated steam flow rate was changed to 20 kg / h as shown in Table 2 below, the same procedure as Test Example 1 was performed, and the results are shown in Table 2 below.
[0080]
[0081] Temperature (℃) Time (min) Steam amount (kg / h) Weight (g) Decomposition rate (wt%) Physical property (GPa) Tensile strength 80090513089.544.431095.854.411597.364.402095.644.402596.514.113096.164.103596.173.93
[0082] From the above Table 2, it can be confirmed that when the superheated steam flow rate is controlled to 10 kg / h to 30 kg / h, both the decomposition rate and the tensile strength of the recovered regenerated fiber are excellent.
[0083] 3. Effects according to exposure time to superheated steam
[0084] Except that the superheated steam exposure time was changed to 90 minutes as shown in Table 3 below, the same procedure as Test Example 1 was followed, and the results are shown in Table 3 below.
[0085]
[0086] Temperature (℃) Time (min) Steam amount (kg / h) Weight (g) Decomposition rate (wt%) Physical property (GPa) Tensile strength 800 15 20 13 0 8 3.2 2 4.6 5 30 9 5.0 2 4.7 16 0 9 5.5 14.5 6 9 0 9 5.6 4 4.4 0 12 0 9 5.2 14.5 3 13 0 9 7.0 0 3.77
[0087] From the above Table 3, it can be confirmed that when the superheated steam exposure time is controlled to 30 to 120 minutes, both the decomposition rate and the tensile strength of the recovered regenerated fiber are excellent.
[0088] 4. Effect according to air flow rate
[0089] Except that the air flow rate during air exposure was changed to 5 L / min as shown in Table 4 below, the same procedure as Test Example 1 was performed, and the results are shown in Table 4 below.
[0090]
[0091] Air flow rate (L / min) (Decomposition rate (wt%) Physical property (GPa) Tensile strength 090.124.55595.644.401097.784.381599.154.12201004.07251004.03301004.01
[0092] From the above Table 4, it can be confirmed that when the temperature, time, and flow rate of the superheated steam in the superheated steam exposure section as well as the air flow rate in the air injection section are controlled within a certain range, the decomposition rate and the tensile strength of the recovered regenerated fiber are both improved.
[0093] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the following claims also fall within the scope of the present invention.
Claims
1. Step of putting pretreated fiber composite material into a cartridge; A step of moving a cartridge into which the above-mentioned pretreated fiber composite material is injected; A step of exposing the above cartridge to superheated steam and an oxidizer; A step of manufacturing regenerated fiber by removing matrix resin and char from the above pretreated fiber composite material; and A step of moving a cartridge containing the above regenerated fibers and collecting the above regenerated fibers from the cartridge. A method for manufacturing regenerated fibers comprising:
2. In paragraph 1, A method for manufacturing regenerated fibers, wherein the step of exposing the cartridge to superheated steam and an oxidizing agent is a step of first exposing the cartridge containing the pretreated fiber composite material to superheated steam, and then moving the cartridge and exposing it to an oxidizing agent.
3. In paragraph 2, A method for manufacturing regenerated fibers, further comprising a step of first exposing a cartridge containing the pretreated fiber composite material to superheated steam and then, before exposing it to an oxidizer, condensing the gaseous matrix resin decomposed from the pretreated fiber composite material into a liquid state using cooling water and removing it.
4. In paragraph 3, The step of condensing the gaseous matrix resin decomposed from the above-mentioned pretreated fiber composite material into a liquid state and removing it is as follows: A method for manufacturing regenerated fibers, wherein the gaseous matrix resin decomposed from the pretreated fiber composite material is released from the cartridge by the above-mentioned superheated steam exposure, reacts with cooling water that is separated from the cartridge and exists separately, and becomes a liquid condensate and is removed.
5. In paragraph 1, A method for manufacturing regenerated fibers, wherein the oxidizing agent comprises air.
6. In paragraph 1, The above fiber composite material is a method for manufacturing regenerated fibers in which a matrix resin is mixed with 'carbon fibers, glass fibers or a mixture thereof'.
7. In paragraph 6, A method for manufacturing regenerated fibers, wherein the matrix resin comprises an aromatic hydrocarbon compound.
8. In paragraph 7, A method for producing regenerated fibers, wherein the aromatic hydrocarbon compound comprises a phenol compound.
9. In paragraph 7, A method for producing regenerated fiber, wherein the aromatic hydrocarbon compound comprises bisphenol A, and the bisphenol A is contained in an amount of 30 wt% or more based on the total amount of the aromatic hydrocarbon compound.
10. In paragraph 1, The above pretreated fiber composite material is a method for manufacturing regenerated fibers which are shredded or cut fiber composite materials.
11. In paragraph 1, A method for manufacturing regenerated fibers in which the above superheated steam has a temperature range of 400°C to 900°C.
12. In paragraph 1, A method for manufacturing regenerated fibers, wherein a cartridge containing the above-mentioned pretreated fiber composite material is exposed to the above-mentioned superheated steam for 30 to 120 minutes.
13. In paragraph 1, A method for manufacturing regenerated fibers, wherein the step of exposing to the superheated steam includes a step of spraying the superheated steam into a cartridge into which the pretreated fiber composite material is introduced, and the superheated steam is sprayed into the cartridge at a flow rate of 10 kg / h to 30 kg / h.
14. In paragraph 1, A method for manufacturing regenerated fibers, wherein the step of exposing to the oxidizing agent includes the step of spraying the superheated steam into a cartridge into which the pretreated fiber composite material is introduced, and then spraying the oxidizing agent into the cartridge, wherein the oxidizing agent is sprayed into the cartridge at a flow rate of 5 L / min or more.
15. In paragraph 1, A method for manufacturing regenerated fibers, further comprising a step of first exposing the cartridge to nitrogen before exposing the cartridge to the superheated steam after the step of introducing the pretreated fiber composite material into the cartridge.
16. In paragraph 1, A method for manufacturing regenerated fibers, further comprising a step of first exposing the cartridge containing the regenerated fibers to nitrogen before moving the cartridge after the step of manufacturing the regenerated fibers.
17. In paragraph 1, The above method for manufacturing regenerated fibers is a method for manufacturing regenerated fibers in which the matrix resin is present on the surface of the regenerated fibers from which the above matrix resin has been removed.
Citation Information
Patent Citations
Apparatus for producing regenerated carbon fibers and method for producing regenerated carbon fibers
CN114990733A
Method of regenerating carbon fiber
JP2013237716A
Manufacturing apparatus and manufacturing method of recycled carbon fiber
JP2017082036A
Recycled carbon fiber bundle, recycled carbon fiber, milled recycled carbon fiber manufacturing method and recycled carbon fiber bundle manufacturing device, carbon fiber reinforced resin manufacturing method, and carbon fiber reinforced resin pellet manufacturing method
JP6630991B2