Composition of Anti-corrosion coating

A multilayer anticorrosive coating with an electrolytic or organometallic base, nanoceramic intermediate, and epoxy or polyester-polyurethane outer layer addresses the limitations of zinc-based coatings by offering exceptional acid resistance and durability, effectively extending the lifespan of metal parts in corrosive environments.

WO2024243666A1PCT designated stage expired Publication Date: 2024-12-05CIA IND H CARLOS SCHNEIDER
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/BR2024/050221
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-05-29
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional zinc-based coatings exhibit low resistance to acid attacks and corrosion in aggressive environments, leading to reduced useful life and increased maintenance costs, particularly in applications like agricultural and civil construction.

Method used

A multilayer anticorrosive coating composition comprising an electrolytic or organometallic base layer, a nanoceramic sealant intermediate layer, and an outer layer of epoxy resin or polyester-polyurethane resin, providing enhanced chemical resistance and durability against acid corrosion.

Benefits of technology

The multilayer coating demonstrates superior resistance to acid attacks, withstanding at least 40 Kesternich AHT 2.0 S test cycles, significantly outperforming traditional zinc-based coatings and extending the lifespan of metal parts in aggressive environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BR2024050221_05122024_PF_FP_ABST
    Figure BR2024050221_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention pertains to the field of coating compositions and, more specifically, it involves a multi-layered anti-corrosion coating (R) composition comprising at least three layers: the base layer (1) an electrolytic or organometallic base layer, a nanoceramic sealant as the intermediate layer (2), and an outer layer (3) of epoxy or polyester-polyurethane resin. The base layer (1) consists of an organometallic dispersion based on zinc and aluminium alloys or a zinc or zinc alloy base applied electrolytically to a metallic surface (not illustrated). Thus, in addition to being cost-effective, the coating (R) of the present invention demonstrates significantly higher efficiency against acid-induced corrosion than coatings in the state of the art, offering resistance to at least 40 cycles of Kesternich AHT 2.0 S testing.
Need to check novelty before this filing date? Find Prior Art

Description

ANTI-CORROSIVE COATING COMPOSITION [1] The present invention belongs to the field of coating compositions, more specifically, it relates to a multilayer anticorrosive coating composition having at least three layers, the base layer being electrolytic or organometallic, a nanoceramic sealant as an intermediate layer, and an outer layer containing epoxy resin or polyester-polyurethane resin. [2] Advantageously, the proposed coating composition exhibits superior chemical resistance to zinc-based coatings, which are widely used worldwide as excellent protective agents. In addition, it enhances resistance to chemical corrosion caused by contact with acidic substances, or even by the presence of moisture, which helps dissolve the metal and transport corrosion products away from the metal surface. History of the invention [3] Corrosion is a natural process of material deterioration that occurs due to the interaction between the material and its surrounding environment. It is a common phenomenon that affects a wide range of materials, from metals to concrete and plastics. [4] Corrosion occurs when there is a chemical reaction between the material and corrosive agents, such as oxygen, water, acids or salts. These agents corrode the surface of the material, resulting in mass loss, structural weakening and, eventually, component failure. In addition, corrosion can cause aesthetic damage, compromising the appearance of the material. [5] There are several types of corrosion, each with its own distinct characteristics. In particular, there is corrosion caused by chemical attack, which is a process of material deterioration caused Corrosion occurs through the interaction of chemical substances with the surface of the material. This form of corrosion can occur due to exposure to acids, bases, salts, or other corrosive chemicals. [6] Corrosive processes generate many problems related to the financial costs of replacing equipment and accessories, as well as reducing their useful life. An example is the storage and / or transport of acidic chemicals, where the damage is even greater due to the high reactivity and potential for corrosive attack. [7] Acid attack corrosion of metal parts occurs when the metal reacts with acidic substances, causing the metal to lose its continuity and deteriorate over time. The corrosion rate is influenced by several factors, including the type of metal, the acid concentration, the temperature, and the presence of other corrosion inhibitors or accelerators, such as moisture. [8] Thus, it is important to emphasize that selecting the appropriate material, protective coatings, controlling acidic conditions and applying monitoring techniques are essential strategies to prevent corrosion of metal parts by acid attack. [9] In this context, in order to prevent corrosion, metal parts are commonly coated with protective coatings and / or treated with corrosion inhibitors, with zinc-based coatings being commonly used. Zinc is widely used as a sacrificial coating, known as galvanizing, where it is applied as a layer over the metal surface. Zinc acts as an anode, sacrificing itself in relation to the base metal in case of exposure to corrosion. In this way, the zinc is preferentially corroded, protecting the underlying metal.

[0010] However, it is important to consider the environment and exposure conditions when choosing the most suitable protective coating for a specific application, given that although zinc is widely recognized worldwide as an excellent protective agent, when protection against acid attacks is verified, it becomes clear that it is not sufficient.

[0011] This is because acid attack on zinc-based coatings occurs when acidic substances react with zinc, causing zinc corrosion. Zinc is a reactive metal and corrodes relatively easily in acidic environments, forming hydrogen gas, which generally causes blistering and / or flaking of the metal. Consequently, this can result in the formation of cavities that penetrate the zinc coating and expose the underlying metal to further corrosion.

[0012] In addition to the concentration and type of acid, the corrosion rate can also be influenced by factors such as the presence of other metals in the coating, the presence of moisture, and temperature. To prevent acid attack, zinc-based coatings can be treated with corrosion inhibitors and / or coated with additional protective layers, such as paint or a transparent protective coating.

[0013] One way to assess the corrosion resistance of metallic surfaces is through the Kesternich test, also known as the acid salt spray test. This is a standardized laboratory test performed by exposing the metallic surface to a controlled environment containing sulfur dioxide gas and high humidity, simulating corrosive atmospheric conditions. The exposure duration is typically between 24 and 72 hours.

[0014] The Kesternich test works by simulating, in a standardized way, the conditions that can lead to corrosion in real-world environments, such as industrial or coastal environments where these elements are present. Sulfur dioxide and high humidity levels. The test results can be used to evaluate the effectiveness of corrosion inhibitors or to compare the corrosion resistance of different metal surfaces or coatings.

[0015] After the exposure period, the metal surface is inspected for signs of corrosion, such as rust or pitting. The severity of the corrosion is then assessed using standardized methods, such as weight loss or visual inspection, to quantify the level of corrosion resistance. The results of the Kesternich test can provide valuable information for the selection and design of metal components and coatings needed to function in corrosive environments.

[0016] The sulfur dioxide exposure corrosion test (Kesternich test) is standardized by several international and national standardization organizations, including: ASTM G87: This American Society for Testing and Materials (ASTM) standard covers the standard test method for evaluating the resistance of metals and metal alloys to sulfide stress corrosion cracking in corrosive environments. The Kesternich test is one of the methods specified in this standard. - DIN 50018: This German standard specifies test methods for evaluating the resistance of metallic surfaces to corrosion caused by sulfur dioxide. The Kesternich test is one of the methods specified in this standard. - ABNT NBR 8096 - Coated and uncoated metallic material - Corrosion by exposure to sulfur dioxide. This Standard prescribes the method (Kesternich) for carrying out sulfur dioxide exposure tests.

[0017] An example, shown in Figure 1, corresponds to a 2-liter Kesternich test cycle, called 2.0, which involves exposing a sample of the material to a volume of 2 liters of SO2 for a period of 24 hours. Each 24-hour period counts as one cycle. The test is performed for n cycles until the sample shows corrosion in the base metal. The number The number of cycles supported by the test specimen indicates the degree of corrosion resistance of the material for the test.

[0018] It is known that conventional zinc-based coatings have low resistance to the Kesternich test; that is, when exposed to acidic salt spray, which simulates more severe conditions, these coatings may perform worse. Therefore, if the application requires high resistance to the Kesternich test, the use of more advanced coatings specifically designed for this purpose is recommended.

[0019] Aiming for a technically sound and cost-effective solution, the present invention aims to provide a highly efficient coating against acid corrosion, resistant to at least 40 cycles of the Kesternich AHT 2.0 S test, with the objective of offering the market an alternative solution to stainless steel with efficiency far superior to conventional coatings such as zinc flakes, electrolytic zinc and zinc alloys.

[0020] Furthermore, it is an objective of the present invention to provide a coating, consisting of three distinct layers applied to the same metal piece, that allows it to be used in applications in more aggressive environments, such as the agricultural, livestock, and civil construction markets. Brief description of the figures

[0021] Figure 1 illustrates the result of a test on screws with organometallic coating (Zinc Flake) after 2 cycles of the Kesternich AHT 2.0 S test.

[0022] Figure 2 illustrates fixatives after 21 cycles of Kesternich AHT 2.0 S, using epoxy resin in the outer layer (3).

[0023] Figure 3 illustrates fixatives after 21 cycles of Kesternich AHT 2.0 S, using polyester-polyurethane resin in the outer layer (3).

[0024] Figure 4 illustrates fixatives after 30 cycles of Kesternich AHT 2.0 S, using epoxy resin in the outer layer (3).

[0025] Figure 5 illustrates fixatives after 30 cycles of Kesternich AHT 2.0 S, using polyester-polyurethane resin in the outer layer (3).

[0026] Figure 6 illustrates fixatives after 40 cycles of Kesternich AHT 2.0 S, using epoxy resin in the outer layer (3).

[0027] Figure 7 illustrates fixatives after 40 cycles of Kesternich AHT 2.0 S, using polyester-polyurethane resin in the outer layer (3). Detailed description

[0028] The present invention discloses a multilayer coating (R) configured by at least three distinct types of layers applied to the same metal part, with at least one electrolytic or organometallic base layer (1), at least one nanoceramic sealant as an intermediate layer (2), and at least one outer layer (3) of epoxy resin or polyester-polyurethane.

[0029] In addition to being affordable, the coating (R) of the present invention exhibits significantly higher efficiency against acid attack corrosion, i.e., resistance to at least 40 cycles of the Kesternich AHT 2.0 S test, aiming to offer the market an alternative solution to stainless steel with far superior efficiency to conventional coatings such as zinc flakes, electrolytic zinc and zinc alloys.

[0030] Thus, the triple-layer coating composition (R) causes the top coating, or outer layer (3), which will be in direct contact with the aggressive environment, to withstand the aggressions related to acid attacks for longer, improving the performance of traditional coated carbon steel fasteners, where zinc is easily attacked and the service life of the fastener or metal part is drastically reduced, thus having a poor cost-benefit ratio.

[0031] At the same time, the triplex coating (R) of the present invention has a very high resistance to natural corrosion (weathering). superior to traditional coatings, due to the combination of the intermediate layer (2) of a nanotechnology sealant with the outer layer (3).

[0032] It should be noted that the base layer (1) and the intermediate layer (2) are the subject of patent application BR102022011647-4, by the same applicant, the base layer (1) being a zinc or zinc alloy base applied electrolytically or a base coating of an organometallic dispersion (zinc flake) based on zinc and aluminum alloys in an aqueous or organic solvent base, containing binding elements, organic solvents, or water, alcohols and ethers.

[0033] Thus, in one embodiment of the invention, the base layer (1) is made of electrolytic zinc.

[0034] For the purposes of defining the application of the base layer (1), the cathode is the electrode where reduction occurs, the deposition of the metal - the object to be coated, and the anode is the electrode where oxidation occurs, which may be soluble - in which case the metal from the anode goes into solution - or insoluble.

[0035] Electrolytes are all solutions that conduct electric current. Ions are the charged particles that move within the solution.

[0036] Galvanization is the process of coating one metal with another in order to protect it against corrosion or improve its appearance. Thus, galvanization is a surface coating process using electrolysis where the metal to be coated acts as the cathode and the metal that will coat the piece acts as the anode; an inert material can also be used as the anode.

[0037] The electrolytic solution must contain a salt composed of cations of the metal that the part is to be coated with.

[0038] In general, different metals can be used to coat a part. The zinc coating process is called zinc plating. Zinc plating is a surface treatment that provides great resistance to corrosion, with a uniform and adherent protective layer.

[0039] The galvanizing time determines the thickness of the deposited layer. In the present invention, the thickness of the electrolytic zinc or zinc alloy layer is between 5 and 25 micrometers, and the following galvanizing variants can be used: Alkaline zinc plating without cyanide, rotary and still bath; - Acid Zinc Plating; - Zinc plating (Zinc / Iron); Zinc plating (Zinc Nickel).

[0040] In the present invention, electrolytic zinc or zinc alloys from 5 to 25 micrometers can be used, with acid zinc being used up to 12 micrometers and alkaline zinc being used from 12 micrometers onwards. Acid Zinc

[0041] Zinc plating processes using an acid solution were developed over 200 years ago. The first processes were based on zinc sulfate. This type of process is still used today for applications requiring high current densities, such as continuous sheet or wire lines. In zinc plating processes operating on rotary drums or racks, suitable acid processes are those using chloride-based solutions.

[0042] The concentrations and operating conditions for three processes are described in Table 1. Table 1 - Acid-base zinc process

[0043] The following describes considerations regarding the operating parameters of zinc metal and chloride.

[0044] Zinc is replenished in the bath through the use of high-purity zinc anodes in the form of balls, bars, or ingots. Because the process has good anodic corrosion efficiency, it is very easy to maintain the zinc concentration in the bath with good control of the anodic area.

[0045] Bar anodes are hung from the anode busbar with titanium hooks, but it is much more common to use anode baskets made of titanium.

[0046] Chloride is responsible for the solution's conductivity and for anodic corrosion. High chloride concentrations lower the solution's cloud point. Higher chloride concentrations lead to a greater tendency for burning at high current density, resulting in greater anode dissolution.

[0047] During electrolysis, hydrogen is produced, as shown in the reaction previously. This causes the pH to rise and must be corrected with hydrochloric acid.

[0048] Ammonium chloride, in addition to its other functions, also serves as a pH buffer. When ammonia is not used, boric acid is necessary for this purpose. For the complete elimination of chloride With the development of ammonium compounds, it was necessary to develop new additive systems to achieve the same results as those obtained with ammonia.

[0049] The additives were composed of water-insoluble organic products that required solvents to remain soluble in the bath. These components were intolerant to temperature, with solution cloud points below 50°C, initiating decomposition at temperatures of 30°C, causing stains and haze in the tank, and increasing organic contamination in the bath. Alkaline Zinc Plating

[0050] Cyanide-free alkaline electrolytic zinc plating is an environmentally friendly process (completely cyanide-free) that significantly reduces the amount of contaminated effluents generated. This process is suitable for iron, steel, or zamak materials.

[0051] The use of this process provides the following advantages: excellent penetration; layer uniformity; absence of white corrosion in weld areas; clear and bright deposits; can be applied in a still bath process (larger items) or automatic rotary bath process (smaller items).

[0052] After the zinc coating is applied, the process is finalized with passivation, which should be chosen according to the application characteristics of the items. For high-strength items, the application of sealants is also recommended. Table 2 - Alkaline Zinc Process

[0053] In one embodiment of the invention, the base layer (1) is organometallic (zinc flakes). Non-electrolytic organometallic coatings consist of lamellar zinc, which provide good protection against corrosion. These coatings comprise a mixture of zinc and aluminum, which are bonded together by an inorganic matrix.

[0054] The specifications for organometallic coatings are defined in the international standard ISO 10683 and also in the European standard DIN EN 13858.

[0055] DIN EN ISO 10683 defines the requirements for organometallic coatings for threaded elements, and DIN EN 13858 describes the requirements for zinc flake coatings for non-threaded elements and other parts as well.

[0056] There are three groups of organometallic coatings: - Containing Cr(VI) (hexavalent chromium): Surface treatments containing Cr(VI) provide greater corrosion protection with a thinner layer, but Cr(VI) is carcinogenic and poses a potential environmental risk. New European regulations prohibit the use of surface treatments containing Cr(VI). These include end-of-life vehicles and in Electrical and electronic equipment. For applications outside the automotive and electrical industries, these coatings are still valid; - Cr (VI) free - solvent-based coatings free of hexavalent chromium; - Cr (VI) free - water-based coatings free of hexavalent chromium; Cr(VI)-free coatings are more environmentally friendly than surface treatments containing Cr(VI). No organometallic coatings used in the automotive industry today contain this substance.

[0057] In a preferred embodiment of the invention, the composition of the organometallic coating (zinc flakes) based on organic solvent comprises the following composition in weight percent: - 20 to 60% zinc; - 1 to 5% aluminum - 10 to 20% 2-Ethylhexanol; - 5 to 10% hydrodesulfurized heavy naphtha (mineral oil); - 0 to 3% n-butyl alcohol 71-36-3 1; - from 1 to 3% naptha solvent, petroleum, light aromatic; - from 1 to 3% stearic acid; - 0 to 0.2% Ethylbenzene; - 0 to 0.2% standard solvent.

[0058] In another preferred embodiment of the invention, the composition of the water-based organometallic coating (zinc flakes) is configured by mixing compounds A, B, and C, which comprise the following composition in weight percentage: Compound A - 20 to 40% zinc; - 2 to 10% aluminum; - 20 to 30% dipropylene glycol; - 1 to 2.5% of non-ionic surfactant; - 15 to 20% deionized water. Compound B - Silane (A-187); - 70 to 90% deionized water; - 0.1 to 0.2% boric acid; - 2 to 3% sodium silicate. Compound C - Hydroxyethylcellulose: 0.5 to 2g per kg of mixture of compounds A + B.

[0059] Various manufacturers, such as automotive companies and their suppliers, have produced their own specifications and supply rules in order to define the requirements for these coating systems.

[0060] Organometallic coating (zinc flakes) is a generic term for coating technology.

[0061] Organometallic coatings are supplied in liquid form and can be applied using the following application techniques: - Before coating, the surface of the parts must be pre-treated. This process does not use pickling with acids (e.g., sulfuric acid or hydrochloric acid) which can produce atomic hydrogen and penetrate the steel structure, making it brittle. In order to avoid pickling processes, other pre-treatment processes are necessary. Typical cleaning processes are degreasing with an alkaline aqueous solution followed by abrasive cleaning using blasting with steel microspheres. Degreasing removes grease, oil, and dirt from the metal surface; - Sandblasting removes surface oxidation through the mechanical action of steel microspheres, which are fired against the parts inside a chamber using a turbine. Neither pre-treatment process produces any hydrogen, therefore there is no risk of hydrogen embrittlement of high-strength steels.

[0062] After the pre-treatment, the coating process is then carried out: - Spray: The coating is applied to the surface of the parts using a spray gun. This can be done manually or in a fully automated spraying installation (this process is used for larger or heavier parts). The parts are then placed on supports or hung on hangers or jigs. - Dip-spin (immersion and centrifugation): The parts are placed in a centrifuge basket. The coating is applied by immersion in a container filled with the coating, and after immersion, the basket begins centrifugation in order to remove excess coating material (this process is used for small, high-volume parts, also called batch processing). - Immersion-drain: Submerging the parts into the coating material and pulling it out so that the assembly drains off the excess coating, for example, in pipes. The parts must, however, have sufficient openings for the material to drain off; otherwise, the coating may have defects such as coating build-up and air bubbles.

[0063] The coating forms a uniform, liquid layer over the surface of the parts. In order to develop excellent Due to the properties of zinc flake coatings, a curing process is necessary.

[0064] The coated parts are cured in an oven at a controlled temperature for a set period. Typical curing temperatures are 200 to 340 °C, as they depend on the technology applied, whether solvent-based or water-based. After curing, a uniform, thin, and adherent protective film is produced.

[0065] The average thickness of the base layer (1) is between 5 pm and 12 microns, and it is possible to apply thicker layers.

[0066] The intermediate layer (2) is a nanoceramic sealant, more specifically an aqueous coating containing silicon oxide nanoparticles up to 50 nanometers dispersed in water, binders, alcohols and ethers.

[0067] In summary, the sealant is applied as an intermediate layer (2), its function being to significantly increase corrosion resistance.

[0068] The intermediate layer (2) is a liquid, free of heavy metals, applied in a manner similar to organometallic coatings, by immersion and centrifugation, spray or immersion and dripping, followed by curing in an oven between 170°C and 200°C for a minimum of 25 minutes and a maximum of 240 minutes.

[0069] The nanoceramic sealant, i.e., the intermediate layer (2) comprises the following components by weight: - 15% to 32% Colloidal Silica; - from 2.4% to 8% 2-Butoxyethanol; - 0% to 10% Methanol; - 50% to 70% Water; - from 0% to 6% Tetraethoxysilane; - from 0% to 2% polyvinyl alcohol.

[0070] Preferably, the intermediate layer (2) comprises the following components in the following proportions by weight: - 15% to 32% Colloidal Silica; - from 2.4% to 8% 2-Butoxyethanol; - 10% Methanol; - 50% Water.

[0071] The intermediate layer (2) promotes the sealing of the surface of the base layer (1), preventing or hindering contact between the base layer (1) and the atmosphere and, in this way, increasing the life of the coated metal part.

[0072] Regarding the outer layer (3), in a preferred embodiment of the invention, the base is epoxy resin and aluminum, i.e., a coating rich in epoxy resin dispersed in water or organic solvents, aluminum and binding elements, being a viscous liquid, silvery in color and containing as a base the following compounds in weight percentage: - 53 to 63% epoxy resin; - 11 to 13% titanium oxide; - 7 to 9% metallic aluminum; and - 6 to 8% silicates.

[0073] In another embodiment of the invention, the outer layer (3) is provided with solvent-based polyester-polyurethane resin, being a viscous, silvery-colored liquid, which contains the following compounds as a base in percentage: - 20 to < 30% propylene glycol methyl ether acetate (PMA); - from 10 to < 20% of 1-methoxy-2-propanol; - 1 to < 3% Isopropanol; - from 1 to < 3% n-butyl acetate; - < 1% 1-ethyl-2-pyrrolidinone; - < 1% methyl isobutyl ketone (MIBK); - < 1% Naphthalene; - < 1% Toluene; - 60 to <70% of other compounds below reported levels.

[0074] Furthermore, the outer layer (3) may contain some compound for lubricity, promoting adjustment of the coefficient of friction in the coated fasteners, this being, but not limited to, 6 to 8% polytetrafluoroethylene (PTFE).

[0075] The application of the outer layer (3) is carried out by immersion and centrifugation, spraying or immersion and draining, and 1 to 3 layers can be applied, each layer having to be cured in an oven between 170°C and 220°C for 10 to 20 minutes.

[0076] The examples presented below illustrate the scope of the invention proposed herein. For all examples described below, the Kesternich AHT 2.0 S test was used in accordance with the DIN 50018 standard. Example 1

[0077] The coating (R) consisting of at least one base layer (1), an intermediate layer (2) and an outer layer (3), applied to the same metal part, wherein the outer layer (3) comprises epoxy resin and aluminum, i.e., a coating rich in epoxy resin dispersed in water or organic solvents, aluminum and binders, was applied to fasteners to evaluate resistance to acid attack, the area considered for evaluation being the fastener head.

[0078] Figure 2 shows the fasteners after 21 Kesternich cycles; note that no corrosion occurred. Example 2

[0079] The coating (R) consisting of at least one base layer (1), one intermediate layer (2) and one outer layer (3), applied to the same metal part, wherein the outer layer (3) comprises solvent-based polyester-polyurethane resin, was applied to fasteners to evaluate resistance to acid attack, the area considered for evaluation being the fastener head.

[0080] Figure 3 shows the fasteners after 21 Kesternich cycles; note that no corrosion occurred. Example 3

[0081] The coating (R) consisting of at least one base layer (1), an intermediate layer (2) and an outer layer (3), applied to the same metal part, wherein the outer layer (3) comprises epoxy resin and aluminum, i.e., a coating rich in epoxy resin dispersed in water or organic solvents, aluminum and binders, was applied to fasteners to evaluate resistance to acid attack, the area considered for evaluation being the fastener head.

[0082] Figure 4 shows the fasteners after 30 Kesternich cycles; note that no corrosion occurred. Example 4

[0083] The coating (R) consisting of at least one base layer (1), an intermediate layer (2) and an outer layer (3), applied to the same metal part, wherein the outer layer (3) comprises solvent-based polyester-polyurethane resin, was applied to fixatives are used to evaluate resistance to acid attack, with the area considered for evaluation being the head of the fixative.

[0084] Figure 5 shows the fasteners after 30 Kesternich cycles; note that no corrosion occurred. Example 5

[0085] The coating (R) consisting of at least one base layer (1), an intermediate layer (2) and an outer layer (3), applied to the same metal part, wherein the outer layer (3) comprises epoxy resin and aluminum, i.e., a coating rich in epoxy resin dispersed in water or organic solvents, aluminum and binders, was applied to fasteners to evaluate resistance to acid attack, the area considered for evaluation being the fastener head.

[0086] Figure 6 shows the fasteners after 40 Kesternich cycles; it can be seen that no corrosion occurred, thus meeting the objective proposed by the invention. Example 6

[0087] The coating (R) consisting of at least one base layer (1), one intermediate layer (2) and one outer layer (3), applied to the same metal part, wherein the outer layer (3) comprises solvent-based polyester-polyurethane resin, was applied to fasteners to evaluate resistance to acid attack, the area considered for evaluation being the fastener head.

[0088] Figure 7 shows the fasteners after 40 Kesternich cycles; it can be seen that no corrosion occurred, thus fulfilling the objective proposed by the invention.

Claims

CLAIMS 1- “Composition of a coating”, wherein said coating (R) is configured by at least one base layer (1), one intermediate layer (2) and one external layer (3), applied to the same metal part, wherein the base layer (1) comprises: - an organometallic dispersion based on zinc and aluminum alloys or - a zinc or zinc alloy base applied electrolytically to the metal surface, the aqueous intermediate layer (2) comprising nanoparticles of silicon oxide of up to 50 nanometers and further comprising the following compounds in percentage by weight: - 15% to 32% Colloidal Silica; - from 2.4% to 8% 2-Butoxyethanol; - from 0% to 10% Methanol; - 50% to 70% water; - from 0% to 6% Tetraethoxysilane; - from 0% to 2% polyvinyl alcohol; characterized in that the outer layer (3) comprises the following compounds in percentage by weight: - 53 to 63% epoxy resin; - 11 to 13% titanium oxide; - 7 to 9% metallic aluminum; - from 6 to 8% silicates; or an outer layer (3) comprising a solvent-based polyester-polyurethane resin containing the following compounds in percentage by weight: - 20 to <30% propylene glycol methyl ether acetate (PMA); - from 10 to < 20% of 1-methoxy 2-propanol; - from 1 to <3% Isopropanol; - from 1 to < 3% n-butyl acetate; - < 1% 1-ethyl-2-pyrrolidinone; - < 1% methyl isobutyl ketone (MIBK); - < 1% Naphthalene; - <1% Toluene; and - 60 to <70% of other compounds below reported levels. 2- “Composition of a coating” according to claim 1, characterized in that the outer layer (3) preferably comprises the following compounds in percentage by weight: - 58% epoxy resin; - 12% titanium oxide; - 8% metallic aluminum; and - 7% silicates, preferably mica-type mineral. 3- “Composition of a coating” according to claim 1, characterized in that the outer layer (3) comprises 6 to 8% polytetrafluoroethylene (PTFE). 4- “Composition of a coating”, according to claim 1, characterized in that the base layer (1) is an organic solvent-based organometallic coating that comprises the following composition in percentage by weight: - 20 to 60% zinc; - 1 to 5% aluminum - 10 to 20% 2-Ethylhexanol; - 5 to 10% naphtha (mineral oil), heavy hydro desulfurized; - from 0 to 3% n-butyl alcohol 71-36-3 1; - from 1 to 3% naptha solvent, petroleum, light aromatic; - from 1 to 3% stearic acid; - 0 to 0.2% Ethylbenzene; - from 0 to 0.2% standard solvent. 5- “Composition of a coating”, according to claim 1, characterized in that the base layer (1) is an aqueous-based organometallic layer configured by the mixture of a compound A, a compound B and a compound C, in which the compounds comprise the following composition in percentage by weight: Compound A - 20 to 40% zinc; - 2 to 10% aluminum; - 20 to 30% dipropylene glycol; - 1 to 2.5% non-ionic surfactant; - 15 to 20% deionized water; Compound B - Silane (A-187); - 70 to 90% deionized water; - from 0.1 to 0.2% boric acid; - 2 to 3% sodium silicate; Compound C - hydroxyethylcellulose from 0.5 to 2g per kg of mixture of compounds A + B.

Citation Information

Patent Citations

  • COMPOSITION OF A COATING AND ITS APPLICATION PROCESS ON METALLIC SUBSTRATES

    BR102022011647A2

  • Anticorrosion paint for chimney of electric plant and its uses

    CN101007921A

  • Polyester polyurethane coating for rotor wings of helicopter and preparation method thereof

    CN102408824A

  • Coating material with characteristics of efficiency, energy saving, heat shield, cooling and corrosion resistance

    CN104985891A

  • Super-hydrophobic anticorrosive coating used for power transmission and transformation devices, and preparation method thereof

    CN106519955A