Composite adsorbent and full-chain integrated application thereof in separation of nickel and thallium from slag
By using a composite adsorbent with an active silicate matrix loaded with Fe-Mn composite in the slag, the problem of difficult separation and recovery of thallium nickel slag in the prior art is solved, and efficient adsorption of thallium ions and regeneration of nickel is achieved. Improve resource recycling efficiency and environmental protection effect.
Patent Information
- Application Number
- PCT/CN2023/098173
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-06-02
- Publication Date
- 2024-12-05
AI Technical Summary
The prior art is difficult to efficiently separate and recover nickel and thallium in thallium nickel slag containing thallium, resulting in environmental pollution and waste of resources, and the existing adsorbents have poor adsorption effect on thallium ion.
Using a composite adsorbent, the adsorbent is loaded with an active silicate as a matrix, and the Fe-Mn complex is supported, and the high-efficiency thallium ion adsorption site is formed through physical and chemical dual combinations, and nickel is used in the form of nickel hydroxide through synchronous separation. Regeneration realizes the integrated application of the entire chain of slag.
It realizes efficient adsorption of thallium ions and effective separation and regeneration of nickel, improves resource recovery efficiency, reduces environmental pollution, and the adsorbent has excellent metal ion adsorption specificity and stability.
Smart Images

Figure PCTCN2023098173-FTAPPB-I100001 
Figure 00000016_0000 
Figure 00000016_0001
Abstract
Description
A composite adsorbent and its full-chain integrated application for separating nickel and thallium from slag Technical Field
[0001] The present application relates to the field of waste recycling, and in particular to a composite adsorbent and its application in separating nickel and thallium from slag. Background Art
[0002] In recent years, with the rapid development of the electric vehicle and large-scale energy storage markets, the production of ternary lithium-ion batteries, which currently hold the largest market share, has also grown rapidly, leading to a growing demand for nickel in lithium-ion batteries. Nickel is a key raw material for electric vehicle batteries, primarily providing high voltage and capacity, thereby enhancing battery performance. Furthermore, the addition of nickel improves the battery's cycle life and safety. Currently, nickel resources are primarily supplied from two sources: newly produced nickel concentrate and recycled nickel. Recycled nickel, due to its energy-saving and environmentally friendly advantages, is particularly valuable due to its scale and specialized production.
[0003] The mining, beneficiation, and smelting of nickel ore, as well as the rough processing of nickel salts, generate large amounts of waste slag containing both thallium and nickel. Thallium is a highly toxic rare element, and due to its high mobility, it easily enters the natural environment and poses serious health risks through soil, water, and the food chain. Therefore, the large amounts of thallium-containing nickel slag produced by the rough processing of nickel salts in most existing nickel salt plants cannot be directly scrapped. Furthermore, this type of slag generally contains a high nickel content. Separating the nickel and thallium from the slag and recovering the nickel for use in the production of nickel hydroxide would have positive implications for environmental protection and resource recycling.
[0004] Summary of the Invention
[0005] Based on the defects of the relevant technology, the purpose of this application is to provide a composite adsorbent and a preparation method thereof. This product uses active silicate as a matrix and a composite metal compound through a dual physical and chemical combination to produce efficient thallium ion adsorption sites, which can achieve efficient adsorption of thallium ions separated from slag; at the same time, this application also adopts a synchronous separation method to separate and regenerate the nickel in the slag in the form of nickel hydroxide, realizing the full-chain integrated application of thallium-containing nickel slag resources from recovery to the production of new products.
[0006] In order to achieve the above objectives, the technical solutions adopted in this application are:
[0007] A composite adsorbent comprising an active silicate and a composite metal compound loaded on the surface and in the pores of the active silicate; the metals comprising iron, manganese and sodium;
[0008] The specific surface area of the composite adsorbent is 60 to 80 m2 / g, average pore diameter of 1-10 nm, total pore volume of 0.05-0.15 cm 3 / g.
[0009] In one embodiment, the ratio of the total molar amount of active silicate to the total molar amount of iron atoms and manganese atoms in the composite metal compound is n(active silicate):n(Fe+Mn)=(1.5-3):1, calculated as SiO2 in the active silicate.
[0010] Another object of the present application is to provide a method for preparing the composite adsorbent:
[0011] The following steps are involved:
[0012] (1) dissolving a sodium-containing manganese source and an iron source in water to form a mixed solution;
[0013] (2) Adding active silicate to the mixed solution, dispersing and drying it, and then calcining it at 450-650° C. After calcination, grinding and sieving it to obtain the composite adsorbent.
[0014] In one embodiment, the dispersion in step (2) is ultrasonic dispersion.
[0015] Active silicate is a mineral containing dissolved silicon compounds in the form of orthosilicic acid and its dimers. In addition to silicon and oxygen, it also contains a complex of Al and Ca. Active silicates are mostly derived from rock weathering or river input, and are relatively stable and have a relatively large pore size. During the preparation process, the composite adsorbent described in the present application is pre-dispersed in the solution with a sodium-containing manganese source and a trivalent iron source, and then the active silicate is used as a matrix to perform a highly dispersed physical load of the iron source and manganese source under an ultrasonic environment. After high-temperature calcination, Si-O-Mn and Si-O-Fe groups can be formed in the composite product and a complex Fe-Mn chemical load network structure is formed. At the same time, due to its load modification method, a large number of hydroxyl groups are formed on the surface of the active silicate, and the sodium ions introduced by the sodium-containing iron source can realize ion exchange when in contact with thallium ions, so that the composite adsorbent has a large thallium ion binding site and adsorption capacity, which can realize rapid and efficient capture of thallium ions. At the same time, experimental verification shows that, compared to active silicates, Fe-Mn composites loaded onto some other common matrix materials do not have similar thallium ion adsorption effects as the products described in this application. On the other hand, the applicant discovered that only ultrasonic dispersion treatment can weaken the interaction between the iron and manganese source components during the early stage of compounding, avoiding precursor agglomeration. At the same time, it can also orderly transform the macroporous structure on the surface of the active silicate into a mesoporous structure with a large specific surface area and high charge variability, which has a significant performance improvement in both the adsorption of thallium ions and the filtration and regeneration after adsorption.
[0016] In one embodiment, the active silicate includes the following elements in percentage by mass: 65-70% O, 5-10% Al, 5-6% Si, 10-15% Ca, and a small amount of unavoidable impurity elements.
[0017] In one embodiment, the specific surface area of the active silicate is 0.15 to 2 m 2 / g, average pore diameter of 2000-2200 nm, total pore volume of 0.005-0.01 cm 3 / g.
[0018] The initial surface properties and addition amount of the active silicate will have a certain impact on the final product. If the addition amount is too small, the final product will have insufficient pore structure and cannot effectively capture thallium ions. However, if the active silicate is added too much, it may not only cause raw material agglomeration during ultrasonic dispersion, but also poor dispersion and binding of iron and manganese sites, and the relative content of Fe-Mn complexes will be reduced, and the overall adsorption effect will also be poor. Based on the results of multiple experiments, the product prepared under the conditions within the above range has the best thallium ion adsorption effect.
[0019] In one embodiment, the sodium-manganese source is an aqueous solution of NaMnO 4 , and the molar concentration of manganese element is 0.05-0.2 mol / L.
[0020] In one embodiment, the iron source is an aqueous solution of at least one of ferric nitrate, ferric sulfate, and ferric chloride, and the molar concentration of the iron element is 0.15 to 0.6 mol / L.
[0021] In one embodiment, the ultrasonic dispersion time in step (2) is 1 to 2 hours, the calcination time is 0.5 to 1 hour, and the particle size of the powder obtained after grinding and sieving is 80 to 100 meshes.
[0022] Another object of the present application is to provide an application of the composite adsorbent in adsorbing and removing metal ions in water.
[0023] Preferably, the metal ions include at least one of thallium ions, arsenic ions, and lead ions.
[0024] The composite adsorbent described in the present application has excellent metal ion adsorption specificity and high stability, and is very suitable for adsorbing and removing metal ions (especially heavy metal ions) contained in some water bodies.
[0025] Another object of the present application is a method for separating nickel and thallium from nickel and thallium-containing slag, comprising the following steps:
[0026] (1) crushing and screening the nickel-thallium-containing slag, and dispersing the obtained particles in water to prepare a slurry;
[0027] (2) adding a pH adjusting agent to adjust the slurry to a pH of 0.5 to 1.5 and reacting, followed by filtering to obtain a filtrate;
[0028] (3) heating and stirring the filtrate, and then adding an oxidant for oxidation reaction to obtain a reaction solution;
[0029] (4) adding thiocyanate to the reaction solution for complexation reaction, then adjusting the pH of the resulting mixed solution to 10-13 and reacting, filtering, and obtaining a complexation solution and a solid;
[0030] (5) washing and drying the solid to obtain nickel hydroxide;
[0031] (6) Adding a reducing agent to the complexing liquid for reduction reaction, then adjusting the pH of the resulting mixed solution to 5-9, adding the composite adsorbent described in the present application for adsorption, and filtering to complete the separation of thallium from the slag.
[0032] In the method for separating nickel and thallium from nickel and thallium-containing slag described in the present application, the impurities in the slag are firstly removed by preliminary acid washing and nickel and thallium ions are leached out, and then the thallium ions are oxidized by an oxidant to convert them into thallium ions, and thiocyanate is introduced to react with them to form a complex anion Tl(SCN)4 - At this point, an alkaline environment is introduced to convert the leached nickel into nickel hydroxide, which is free of thallium ions. Subsequently, the remaining solution containing complexed anions undergoes a complex breaking reaction to reduce the thallium ions. The composite adsorbent described herein is then introduced to chemically and physically adsorb the ions, ultimately achieving nickel-thallium separation from the slag and the production of new nickel products. This method has simple operating steps and high slag recovery efficiency.
[0033] In one embodiment, the particle size of the particles in step (1) is 40-100 mesh, and the solid-liquid ratio of the particles to water in the slurry is 1:(1-10).
[0034] In one embodiment, the pH adjusting agent in step (2) is concentrated sulfuric acid, and the reaction time is 2 to 4 hours.
[0035] In one embodiment, the molar ratio of thallium ions in the reaction solution to thiocyanate in the thiocyanate in step (4) is 1:(4-6).
[0036] In one embodiment, the amount of the composite adsorbent added to the complexing liquid in step (6) is 2-5 g / L.
[0037] The beneficial effect of the present application is that the present application provides a composite adsorbent and a preparation method thereof. The product uses active silicate as a matrix and an Fe-Mn complex to produce efficient thallium ion adsorption sites through a dual physical and chemical combination, thereby achieving efficient adsorption of thallium ions separated from slag. At the same time, the present application also adopts a synchronous separation method to separate and regenerate the nickel in the slag in the form of nickel hydroxide, thereby achieving a full-chain integrated application of thallium-containing nickel slag resources from recovery to the production of new products. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] FIG1 is a schematic flow diagram of the method for separating nickel and thallium from slag described in the present application.
[0039] FIG2 is a scanning electron microscope image of the active silicate (left) and the composite adsorbent (right) described in Example 1 of the present application.
[0040] FIG3 is an infrared spectrum of the active silicate and the composite adsorbent (labeled as Fe-Mn-Si composite material) described in Example 1 of the present application.
[0041] FIG4 is a scanning electron microscope (a) and an EDX element distribution diagram (right) of the active silicate described in Example 1 of the present application.
[0042] FIG5 is a scanning electron microscope (a) and an EDX element distribution diagram (right) of the composite adsorbent described in Example 1 of the present application.
[0043] FIG6 is a scanning electron microscope (a) and an EDX element distribution diagram (right) of the composite adsorbent described in Example 1 of the present application after use.
[0044] FIG7 is an XRD pattern of nickel hydroxide prepared by the method described in Example 1 of the present application.
[0045] FIG8 is a high-magnification transmission electron microscope image (left) and a low-magnification transmission electron microscope image (right) of the composite adsorbent described in Comparative Example 1 of the present application. DETAILED DESCRIPTION
[0046] In order to better illustrate the purpose, technical solutions and advantages of the present application, the present application will be further described below in conjunction with specific examples and comparative examples. The purpose is to understand the content of the present application in detail, rather than to limit the present application. The experimental reagents and instruments involved in the implementation of this application are all commonly used ordinary reagents and instruments unless otherwise specified. The active silicate used in this application is a commercially purchased product. Specifically, the element mass distribution of the active silicate is: O 69.43%, Al 8.42%, Si 5.56%, K 1.86%, Ca 12.55%, Na 2.18%. The specific surface area of the active silicate is 0.1851m 2 / g, the average pore diameter is 2109nm, and the total pore volume is 0.0097cm3 / g.
[0047] Example 1
[0048] The composite adsorption method described in this application and its application in separating nickel and thallium from slag is shown in the flow chart in FIG1 .
[0049] As shown, the following steps are included:
[0050] (1) After crushing and screening the massive nickel-thallium-containing slag using a small crusher, the resulting 40-100 mesh particles were dispersed in water at a solid-liquid ratio of 1:5 to prepare a slurry. The slurry was placed in a water bath at 80°C and stirred at a constant speed of 100 rpm;
[0051] (2) slowly adding concentrated sulfuric acid to adjust the slurry to a pH of 1 and reacting for 2 h, followed by filtering to obtain a filtrate;
[0052] (3) heating the filtrate to 50° C. and stirring at 100 rpm, and then adding hydrogen peroxide as an oxidant to oxidize the thallium ions to obtain a reaction solution;
[0053] (4) adding thiocyanate to the reaction solution for complexation reaction, then adding sodium hydroxide to adjust the pH of the resulting mixture to 12 and reacting, filtering to obtain a complex solution and a solid; the molar ratio of thallium ions in the reaction solution to thiocyanate in thiocyanate is 1:4;
[0054] (5) washing and drying the solid to obtain nickel hydroxide;
[0055] (6) adding sodium sulfite as a reducing agent to the complexing liquid for reduction reaction, then adjusting the pH of the resulting mixed solution to 7, adding a composite adsorbent in an amount of 2 g / L for adsorption, and filtering to complete the separation of thallium from the slag.
[0056] The preparation method of the composite adsorbent comprises the following steps:
[0057] (1) 60 mL of a 0.08 mol / L aqueous solution of NaMnO4 and 60 mL of a 0.24 mol / L aqueous solution of Fe(NO3)3·9H2O were mixed to form a mixed solution;
[0058] (2) 5 g of active silicate was added to the mixed solution and ultrasonically dispersed for 1 h, dried in a water bath at 75° C., and then calcined at 650° C. for 0.5 h. After calcination, the mixture was ground and sieved to 80 mesh to obtain the composite adsorbent.
[0059] Example 2
[0060] The composite adsorption method and its application in separating nickel and thallium from slag described in the present application include the following steps:
[0061] (1) After crushing and screening the massive nickel-thallium-containing slag using a small crusher, the resulting 40-100 mesh particles were dispersed in water at a solid-liquid ratio of 1:8 to prepare a slurry. The slurry was placed in a water bath at 80°C and stirred at a constant speed of 200 rpm;
[0062] (2) Slowly adding concentrated sulfuric acid to adjust the slurry to a pH of 1 and reacting for 2 h, followed by filtration to obtain filtrate B;
[0063] (3) heating the filtrate B to 40° C. and stirring at 100 rpm, and then adding hydrogen peroxide as an oxidant to oxidize the thallium ions to obtain a reaction solution;
[0064] (4) adding thiocyanate to the reaction solution C for complexation reaction, then adding sodium hydroxide to adjust the pH of the resulting mixture to 12 and reacting, filtering to obtain a complex solution and a solid; the molar ratio of thallium ions in the reaction solution to thiocyanate in thiocyanate is 1:6;
[0065] (5) washing and drying the solid to obtain nickel hydroxide;
[0066] (6) adding sodium sulfite as a reducing agent to the complexing liquid for reduction reaction, then adjusting the pH of the resulting mixed solution to 7, adding a composite adsorbent in an amount of 3 g / L for adsorption, and filtering to complete the separation of thallium from the slag.
[0067] The preparation method of the composite adsorbent comprises the following steps:
[0068] (1) Mix 60 mL of a 0.1 mol / L aqueous solution of NaMnO4 and 60 mL of a 0.3 mol / L aqueous solution of Fe(NO3)3·9H2O to form a mixed solution;
[0069] (2) 5 g of active silicate was added to the mixed solution and ultrasonically dispersed for 1 h, dried in a water bath at 80° C., and then calcined at 650° C. for 1 h. After calcination, the mixture was ground and sieved to 80 mesh to obtain the composite adsorbent.
[0070] Example 3
[0071] The composite adsorption method and its application in separating nickel and thallium from slag described in the present application include the following steps:
[0072] (1) After crushing and screening the massive nickel-thallium-containing slag using a small crusher, the resulting 40-100 mesh particles were dispersed in water at a solid-liquid ratio of 1:3 to prepare a slurry. The slurry was placed in a water bath at 80°C and stirred at a constant speed of 300 rpm;
[0073] (2) slowly adding concentrated sulfuric acid to adjust the slurry to a pH of 1 and reacting for 2 h, followed by filtering to obtain a filtrate;
[0074] (3) heating the filtrate to 40° C. and stirring at 300 rpm, and then adding hydrogen peroxide as an oxidant to oxidize the thallium ions to obtain a reaction solution;
[0075] (4) adding thiocyanate to the reaction solution for complexation reaction, then adding sodium hydroxide to adjust the pH of the resulting mixture to 12 and reacting, filtering to obtain a complex solution and a solid; the molar ratio of thallium ions in the reaction solution to thiocyanate in thiocyanate is 1:5;
[0076] (5) washing and drying the solid to obtain nickel hydroxide;
[0077] (6) adding sodium sulfite as a reducing agent to the complexing liquid for reduction reaction, then adjusting the pH of the resulting mixed solution to 7, adding a composite adsorbent in an amount of 4 g / L for adsorption, and filtering to complete the separation of thallium from the slag.
[0078] The preparation method of the composite adsorbent comprises the following steps:
[0079] (1) Mix 60 mL of a 0.1 mol / L aqueous solution of NaMnO4 and 60 mL of a 0.3 mol / L aqueous solution of Fe(NO3)3·9H2O to form a mixed solution;
[0080] (2) 6 g of active silicate was added to the mixed solution and ultrasonically dispersed for 2 h, dried in a water bath at 85° C., and then calcined at 650° C. for 1 h. After calcination, the mixture was ground and sieved to 80 mesh to obtain the composite adsorbent.
[0081] Example 4
[0082] The composite adsorbent and its application in separating nickel and thallium from slag described in this application differ from Example 1 only in that the preparation method of the composite adsorbent comprises the following steps:
[0083] (1) 60 mL of a 0.08 mol / L aqueous solution of NaMnO4 and 60 mL of a 0.24 mol / L aqueous solution of Fe(NO3)3·9H2O were mixed to form a mixed solution;
[0084] (2) 7.5 g of active silicate was added to the mixed solution and ultrasonically dispersed for 1 h, dried in a water bath at 75 ° C, and then calcined at 650 ° C for 0.5 h. After calcination, the mixture was ground and sieved to 80 mesh to obtain the composite adsorbent with a specific surface area of 72.75 m 2 / g, the average pore diameter is 6.11nm, and the total pore volume is 0.12cm 3 / g.
[0085] Example 5
[0086] The composite adsorbent and its application in separating nickel and thallium from slag described in this application differ from Example 1 only in that the preparation method of the composite adsorbent comprises the following steps:
[0087] (1) 60 mL of a 0.08 mol / L aqueous solution of NaMnO4 and 60 mL of a 0.24 mol / L aqueous solution of Fe(NO3)3·9H2O were mixed to form a mixed solution;
[0088] (2) 3.75 g of active silicate was added to the mixed solution and ultrasonically dispersed for 1 h, dried in a water bath at 75 ° C, and then calcined at 650 ° C for 0.5 h. After calcination, the mixture was ground and sieved to 80 mesh to obtain the composite adsorbent with a specific surface area of 61.42 m 2 / g, the average pore diameter is 8.31nm, and the total pore volume is 0.83cm 3 / g.
[0089] Comparative Example 1
[0090] A composite adsorbent and its application in separating nickel and thallium from slag, the difference from Example 1 is that the preparation method of the composite adsorbent comprises the following steps:
[0091] (1) 60 mL of a 0.08 mol / L aqueous solution of NaMnO4 and 60 mL of a 0.24 mol / L aqueous solution of Fe(NO3)3·9H2O were mixed to form a mixed solution;
[0092] (2) 1 g of active silicate was added to the mixed solution and ultrasonically dispersed for 1 h, dried in a water bath at 75 ° C, and then calcined at 650 ° C for 0.5 h. After calcination, the mixture was ground and sieved to 80 mesh to obtain the composite adsorbent with a specific surface area of 39.77 m 2 / g, the average pore diameter is 189nm, and the total pore volume is 0.365cm 3 / g.
[0093] Comparative Example 2
[0094] A composite adsorbent and its application in separating nickel and thallium from slag, the difference from Example 1 is that the preparation method of the composite adsorbent comprises the following steps:
[0095] (1) 60 mL of a 0.08 mol / L aqueous solution of NaMnO4 and 60 mL of a 0.24 mol / L aqueous solution of Fe(NO3)3·9H2O were mixed to form a mixed solution;
[0096] (2) 10 g of active silicate was added to the mixed solution and ultrasonically dispersed for 1 h, dried in a water bath at 75 ° C, and then calcined at 650 ° C for 0.5 h. After calcination, the mixture was ground and sieved to 80 mesh to obtain the composite adsorbent with a specific surface area of 41.11 m 2 / g, the average pore diameter is 141nm, and the total pore volume is 0.297cm 3 / g.
[0097] Comparative Example 3
[0098] A composite adsorbent and its application in separating nickel and thallium from slag, the difference from Example 1 is that the preparation method of the composite adsorbent comprises the following steps:
[0099] (1) 60 mL of a 0.08 mol / L aqueous solution of NaMnO4 and 60 mL of a 0.24 mol / L aqueous solution of Fe(NO3)3·9H2O were mixed to form a mixed solution;
[0100] (2) 5 g of active silicate was added to the mixed solution and stirred and dispersed at 400 rpm for 1 h, dried in a water bath at 75 ° C, and then calcined at 650 ° C for 0.5 h. After calcination, the mixture was ground and sieved to 80 mesh to obtain the composite adsorbent with a specific surface area of 47.83 m 2 / g, the average pore diameter is 202.5nm, and the total pore volume is 0.2861cm 3 / g.
[0101] Comparative Example 4
[0102] A composite adsorbent and its application in separating nickel and thallium from slag, the difference from Example 1 is that the preparation method of the composite adsorbent comprises the following steps:
[0103] (1) Mix 60 mL of a 0.08 mol / L KMnO4 aqueous solution and 60 mL of a 0.24 mol / L Fe(NO3)3·9H2O aqueous solution to form a mixed solution;
[0104] (2) 5 g of active silicate was added to the mixed solution and ultrasonically dispersed for 1 h, dried in a water bath at 75 ° C, and then calcined at 650 ° C for 0.5 h. After calcination, the mixture was ground and sieved to 80 mesh to obtain the composite adsorbent with a specific surface area of 63.75 m 2 / g, the average pore diameter is 8.14nm, and the total pore volume is 0.071cm 3 / g.
[0105] Comparative Example 5
[0106] A composite adsorbent and its application in separating nickel and thallium from slag, the difference from Example 1 is that the preparation method of the composite adsorbent comprises the following steps:
[0107] (1) 60 mL of a 0.08 mol / L aqueous solution of NaMnO4 and 60 mL of a 0.24 mol / L aqueous solution of Fe(NO3)3·9H2O were mixed to form a mixed solution;
[0108] (2) 5 g of active silicate was added to the mixed solution and ultrasonically dispersed for 1 h, dried in a water bath at 75°C, and then calcined at 650°C for 0.5 h. After calcination, the mixed solution was ground and sieved to 80 mesh to obtain the composite adsorbent. The active silicate was subjected to secondary pulverization treatment, and the specific surface area after treatment was 0.397 m 2 / g, the average pore diameter is 1124nm, and the total pore volume is 0.047cm 3 / g. The specific surface area of the final product is 89m 2 / g, the average pore diameter is 0.77nm, and the total pore volume is 0.34cm 3 / g.
[0109] Comparative Example 6
[0110] A composite adsorbent and its application in separating nickel and thallium from slag, the difference from Example 1 is that the preparation method of the composite adsorbent comprises the following steps:
[0111] (1) 60 mL of a 0.08 mol / L aqueous solution of NaMnO4 was added dropwise to 60 mL of a 0.24 mol / L aqueous solution of Fe(NO3)3·9H2O under magnetic stirring, and sodium hydroxide was added during mixing to maintain the pH at 8-10 to form a mixed solution;
[0112] (2) The mixed solution was adjusted to pH 10 and stirred for 1 hour. After standing at room temperature for 24 hours, it was filtered, washed and dried. After calcination, it was ground and sieved to 80 mesh to obtain the composite adsorbent with a specific surface area of 13.64 m 2 / g, the average pore diameter is 157nm, and the total pore volume is 0.5214cm 3 / g.
[0113] Comparative Example 7
[0114] A composite adsorption method and its application in separating nickel and thallium from slag, the difference from Example 1 is that the composite adsorbent in step (6) is replaced by an untreated active silicate with a specific surface area of 0.1851m 2 / g, the average pore diameter is 2109nm, and the total pore volume is 0.0097cm 3 / g.
[0115] Comparative Example 8
[0116] A composite adsorbent and its application in separating nickel and thallium from slag, the difference from Example 1 is that the preparation method of the composite adsorbent comprises the following steps:
[0117] (1) 60 mL of a 0.08 mol / L aqueous solution of NaMnO4 and 60 mL of a 0.24 mol / L aqueous solution of Fe(NO3)3·9H2O were mixed to form a mixed solution;
[0118] (2) 5 g of activated carbon was added to the mixed solution and ultrasonically dispersed for 1 h, dried in a water bath at 75 ° C, and then calcined at 650 ° C for 0.5 h. After calcination, the mixture was ground and sieved to 80 mesh to obtain the composite adsorbent with a specific surface area of 36.71 m 2 / g, the average pore diameter is 167nm, and the total pore volume is 0.382cm 3 / g.
[0119] Comparative Example 9
[0120] A composite adsorbent and its application in separating nickel and thallium from slag, the difference from Example 1 is that the preparation method of the composite adsorbent comprises the following steps:
[0121] (1) 60 mL of a 0.08 mol / L aqueous solution of NaMnO4 was added dropwise to 60 mL of a 0.24 mol / L aqueous solution of Fe(NO3)3·9H2O under magnetic stirring, and sodium hydroxide was added during mixing to maintain the pH at 8-10 to form a mixed solution;
[0122] (2) adjusting the pH of the mixture to 10 and stirring the mixture for 1 hour, allowing it to stand at room temperature for 24 hours, filtering it, washing it, drying it, and grinding it into powder to obtain an Fe-Mn composite material;
[0123] (3) The Fe-Mn composite material was mixed evenly with 5 g of active silicate and sieved to 80 mesh to obtain the composite adsorbent with a specific surface area of 3.74 m2 / g, an average pore diameter of 751 nm, and a total pore volume of 0.714 cm3 / g.
[0124] Effect Example 1
[0125] The active silicate used in Example 1 and the prepared composite adsorbent (labeled as Fe-Mn-Si composite material) were subjected to scanning electron microscopy and infrared spectroscopy tests. The results are shown in Figures 2 and 3. It can be seen that the surface morphology of the composite adsorbent described in this application has changed significantly compared with the active silicate matrix after loading preparation. Further testing found that the specific surface area of the composite adsorbent is 71.41m 2 / g, the average pore diameter is 5.69nm, and the total pore volume is 0.1051cm 3 / g, indicating that the loading of iron and manganese sources effectively contributed to the formation of the mesoporous structure of the product, increasing the contact sites with thallium ions; and the active silicate in Figure 3 at 516cm -1 The peak at 3432 cm-1 was significantly weakened after the composite adsorbent was prepared, indicating that Si-O-Mn and Si-O-Fe bonds appeared in the product. The iron and manganese sources can be effectively combined in the active silicate through chemical bonds. The active silicate was at 3432 cm-1 after processing. -1 The broadband intensity at the position is improved, indicating that the number of surface hydroxyl groups of the product increases after preparation, which is more conducive to the capture of thallium ions.
[0126] In addition, the specific surface area and pore-related test data of the products of Examples 2 to 5 are:
[0127] Example 2: Specific surface area is 74.44m 2 / g, the average pore diameter is 5.22nm, and the total pore volume is 0.127cm 3 / g;
[0128] Example 3: Specific surface area is 77.94m 2 / g, the average pore diameter is 3.77nm, and the total pore volume is 0.141cm 3 / g.
[0129] Effect Example 2
[0130] The filtrate, complexing liquid, waste liquid after composite adsorbent adsorption, and prepared nickel hydroxide from each method in each embodiment and comparative example were tested for nickel and thallium content, and the results are shown in Table 1. As can be seen from Table 1, after the steps of the methods described in each embodiment of the present application are completed, the thallium concentration of the waste liquid obtained can reach less than 10 μg / L, with high separation and removal efficiency, high nickel recovery rate for slag, and high purity of the obtained nickel hydroxide product. Taking Example 1 as an example, the active silicate used to prepare the composite adsorption material in Example 1, the composite adsorbent that was not subjected to adsorption treatment, and the composite adsorbent after adsorption treatment of the complex liquid were subjected to EDX detection. The results are shown in Figures 4 to 6. It can be seen that after the preparation of the composite adsorbent is completed, the iron and manganese content in the product is relatively high, indicating that they are effectively loaded on the active silicate. After the complex liquid is adsorbed, thallium element appears in the product, indicating that the composite adsorbent can effectively adsorb the reduced thallium ions in the complex liquid. At the same time, the nickel hydroxide obtained in Example 1 was subjected to XRD detection. The results are shown in Figure 7. It can be seen that the product corresponds to the standard spectrum and the crystal form, has no other obvious impurity peaks, and has a high purity. The adsorbent used in the method described in Comparative Example 6 is only a free iron-manganese complex, which is not compounded with active silicate. As shown in Figure 8, the product has high agglomeration and does not have a porous structure, so it cannot effectively adsorb thallium, and the difficulty of filtration after adsorption is much greater than that of the composite adsorbent described in this application; the adsorbent in Comparative Example 7 is pure active silicate. Although it has a certain adsorption effect on ions, it is far from meeting the standard for effective removal of thallium. In Comparative Example 8, the iron source and manganese source are loaded on activated carbon. Although activated carbon is also a material with a high porous adsorption effect, its combination effect with the iron source and manganese source is far inferior to that of active silicate. The composite material has poor stability and weak adsorption capacity. Even if the iron-manganese complex is directly mixed with the active silicate in the same ratio as shown in Comparative Example 9, the two cannot achieve the expected adsorption effect because they are not chemically combined. From the comparison of Example 1 with Examples 4 and 5 and Comparative Examples 1 and 2, it can be seen that when preparing the composite adsorbent, the ratio of active silicate to iron-manganese source needs to be maintained at a moderate level. If too little active silicate is added, it cannot completely bind to the iron-manganese complex, causing the complex to a certain extent to agglomerate during the loading process, affecting the adsorption performance of the product; and if too much active silicate is added, the physical adsorption effect of the active silicate itself is limited relative to the iron-manganese complex, and an excessive proportion will lead to a reduction in the overall product's ability to capture thallium. Compared with Comparative Example 3, Example 1 uses a conventional stirring dispersion method during the preparation of the composite adsorbent. Compared with the product prepared by ultrasonic dispersion, its thallium adsorption effect is weakened, indicating that in the preparation process of the composite adsorbent, the preparation in the form of ultrasonic dispersion has the best effect.
[0131] Table 1
[0132] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application and are not intended to limit the scope of protection of the present application.
Claims
1. A composite adsorbent, characterized in that: It includes active silicate and composite metal compound loaded on the surface and pores of active silicate; the metal includes iron, manganese and sodium; The specific surface area of the composite adsorbent is 60 to 80 m 2 / g, average pore diameter of 1-10nm, total pore volume of 0.05-0.15cm 3 / g.
2. The composite adsorbent according to claim 1, characterized in that: Calculated on the basis of SiO2 in the active silicate, the ratio of the total molar amount of the active silicate to the total molar amount of iron atoms and manganese atoms in the composite metal compound is n(active silicate):n(Fe+Mn)=(1.5-3):
1.
3. The method for preparing the composite adsorbent according to claim 1 or 2, characterized in that: The following steps are involved: dissolving a sodium-containing manganese source and an iron source in water to form a mixed solution; Active silicate is added into the mixed solution, dispersed and dried, and then calcined at 450-650° C. After calcination, the mixed solution is ground and sieved to obtain the composite adsorbent.
4. The method for preparing the composite adsorbent according to claim 3, characterized in that: The dispersion is ultrasonic dispersion.
5. The method for preparing the composite adsorbent according to claim 3, characterized in that: The specific surface area of the active silicate is 0.15 to 2 m 2 / g, average pore diameter is 2000-2200nm, total pore volume is 0.005-0.01cm 3 / g.
6. The method for preparing the composite adsorbent according to claim 3, characterized in that: The sodium-manganese source is an aqueous solution of NaMnO4, and the molar concentration of manganese element is 0.05-0.2 mol / L.
7. The method for preparing the composite adsorbent according to claim 3, characterized in that: The iron source is an aqueous solution of at least one of ferric nitrate, ferric sulfate and ferric chloride, and the molar concentration of the iron element is 0.15-0.6 mol / L.
8. The method for preparing the composite adsorbent according to claim 3, characterized in that: The ultrasonic dispersion time is 1 to 2 hours, the calcination time is 0.5 to 1 hour, and the particle size of the powder obtained after grinding and sieving is 80 to 100 meshes.
9. Use of the composite adsorbent as claimed in claim 1 or 2 in the adsorption and removal of metal ions in water.
10. The use according to claim 9, characterized in that The metal ions include at least one of thallium ions, arsenic ions and lead ions.
11. A method for separating nickel and thallium from nickel and thallium-containing slag, characterized in that: The following steps are involved: After crushing and screening the nickel-thallium-containing slag, the obtained particles are dispersed in water to prepare a slurry; Adding a pH adjusting agent to adjust the slurry to a pH of 0.5 to 1.5 and reacting, followed by filtering to obtain a filtrate; The filtrate is heated and stirred, and then an oxidant is added for oxidation reaction to obtain a reaction solution; Adding thiocyanate to the reaction solution for complex reaction, then adjusting the pH of the obtained mixed solution to 10-13 and reacting, filtering, and obtaining a complex solution and a solid; The solid is washed and dried to obtain nickel hydroxide; A reducing agent is added to the complexing liquid for reduction reaction, and then the pH of the resulting mixed solution is adjusted to 5-9, and the composite adsorbent according to claims 1-2 is added for adsorption and filtration to complete the separation of thallium from the slag.
12. The method according to claim 11, characterized in that The particle size of the particles is 40-100 meshes, and the solid-liquid ratio of the particles to water in the slurry is 1:(1-10).
13. The method according to claim 11, characterized in that The pH adjusting agent is concentrated sulfuric acid, and the reaction time is 2 to 4 hours.
14. The method according to claim 11, characterized in that The molar ratio of thallium ions in the reaction solution to thiocyanate in thiocyanate is 1:(4-6).
15. The method according to claim 11, characterized in that The addition amount of the composite adsorbent in the complexing liquid is 2-5 g / L.
Citation Information
Patent Citations
Iron-manganese composite pillared clay mineral material for treating thallium in wastewater and preparation method of iron-manganese composite pillared clay mineral material
CN106268623A
Thallium pollution deep solidification agent, and preparation method and application thereof
CN110203995A
Arsenic removal adsorption material, preparation method thereof and application of arsenic removal adsorption material in removal of As (III) in acid wastewater
CN113000012A