Hot melt adhesive for edge protection of electrode sheets, preparation method therefor, and protection method thereof

Through hot melt adhesive component combination and functional filler treatment, the viscosity reduction and wave edge problems of electrode edge protection glue in high temperature and electrolyte environment are solved, and high adhesion, rapid surface drying and electrolyte resistance are achieved. Performance improves battery quality and finished product quality, and is simple and environmentally friendly.

WO2024244385A1PCT designated stage expired Publication Date: 2024-12-05STEADYCHEM (SHANGHAI) CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/138235
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2023-12-12
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The existing electrode sheet edge protection glue reduces viscosity, is prone to misalignment or falls off in high temperature and electrolyte environments, and the solvent dispersion method leads to high cost and high environmental risks, and the formation of wave edges after rolling and affects the advantage of the finished product.

Method used

Using hot melt adhesive components, including polyolefin resin, tackifying resin, wax and mineral oil, the adhesive strength and fluidity are improved through the polyolefin group and the second polyolefin group, combined with functional fillers and silane coupling The agent is treated to prepare hot melt adhesive with high adhesion and electrolyte resistance, and edge protection is carried out through laser die cutting or knife die cutting.

Benefits of technology

It realizes high adhesion, fast surface drying, and electrolyte-resistant electrode edge protection, avoids burrs and wavy edge problems, improves battery quality and finished product advantages, and is simple in process, low in cost, solvent-free, and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023138235_05122024_PF_FP_ABST
    Figure CN2023138235_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A hot melt adhesive for edge protection of electrode sheets, a preparation method therefor, and a protection method thereof. The hot melt adhesive comprises: 30-60% of a polyolefin resin, 20-40% of a tackifying resin, 5%-25% of wax, 2-10% of mineral oil and 0-20% of a functional filler. The polyolefin resin is prepared by compounding a first polyolefin group and a second polyolefin group in a mass ratio of (2-8):1, wherein the first polyolefin group comprises modified polypropylene, the density thereof being less than 0.9 g / cm3, and the melt flow rate being 4-10 g / 10 min, and the second polyolefin group comprises at least one of polyethylene, a copolymer of ethylene and a C4-C10 α-olefin, an amorphous poly(α-olefin), a polyolefin modified with an acid or anhydride and a polyolefin elastomer. The hot melt adhesive has a softening point of 100℃ or above, a melt viscosity of 5000 cps or below, and a surface drying time of within 5 min. The hot melt adhesive has good infiltration, adhesive force and solvent resistance, and can lock metal particles during edge cutting processes of electrode sheets.
Need to check novelty before this filing date? Find Prior Art

Description

Hot melt adhesive for electrode edge protection and its preparation method and protection method Technical Field

[0001] The present invention belongs to the field of adhesive technology, in particular to the field of adhesive technology for protecting pole pieces of new energy batteries, and particularly relates to a hot melt adhesive for protecting the edge of a pole piece, and a preparation method and a protection method thereof. Background Art

[0002] With the increasing popularity of new energy vehicles in recent years, electric vehicle safety has become a key concern for the public, leading to increased demands on power batteries. While the current cell manufacturing process for power batteries is relatively mature, the electrode slitting and roll-pressing processes still have limitations. Pole slitting inevitably produces burrs and metal particles, which can pierce the separator and cause internal short circuits, posing a potential safety hazard during battery operation. Furthermore, due to the differing ductility between the current collector and the active layer, the electrode develops wavy edges after roll-pressing, creating fine wrinkles along the substrate edge. This affects the precision of subsequent processes and, in turn, the quality of the finished product.

[0003] Currently, adhesives based on resins such as polyvinylidene fluoride (PVDF) are primarily used as protective layers for the edges of battery electrodes to reduce burrs, powder loss, and deformation. Patent CN 115000345A discloses a battery electrode comprising a body and a tab extending from the edge of the body. The tab comprises a base connected to the body and a main body connected to the base. At least one side of the base is provided with a tab adhesive layer, and the main body is provided with a reinforcement structure. The adhesive layer at the base of the tab comprises 5-15% adhesive, 20-30% inorganic insulating filler, and 65-75% solvent. The adhesive is one or more of polyvinylidene fluoride (PVDF) powder, styrene-butadiene rubber, polyacrylic acid, polyacrylonitrile, and polyurethane. The inorganic insulating filler is one or more of aluminum oxide, aluminum hydroxide, and boehmite. The solvent is N-methylpyrrolidone (NMP). The adhesive layer of the invention has two urgent problems to be solved during use: (1) To control costs, a large amount of inorganic fillers are added to the adhesive, which greatly reduces its adhesive strength. When the battery cell is used, it needs to be in an electrolyte (ester solvent) environment at 30-40°C for a long time. Under the erosion of the solvent, the viscosity gradually loses, and it is very easy to dislocate or fall off when experiencing severe vibration; (2) The adhesive layer swells severely in the ester solvent. As time goes by, the volume of the adhesive layer expands, causing the battery edge to bulge. In addition, the adhesive liquid adopts a solvent dispersion method, which has a low adhesive active ingredient, high cost, and a high environmental risk of the solvent.

[0004] Therefore, how to provide a pole edge protection glue that has high adhesion, high softening point, rapid surface drying and electrolyte resistance, and effectively apply it to pole edge protection, has become a technical problem that needs to be solved urgently in this field. Summary of the Invention

[0005] In response to the aforementioned shortcomings of the prior art, the present invention aims to provide a hot melt adhesive for electrode edge protection, as well as its preparation and protection methods. By rationally combining the hot melt adhesive components, a electrode edge protection adhesive is provided with excellent overall properties, including high adhesion, a high softening point, rapid surface drying, and electrolyte resistance. This adhesive is designed to effectively avoid potential safety hazards caused by metal particles generated during the slitting process, as well as the appearance defects caused by wavy edges, thereby comprehensively improving battery quality and process efficiency.

[0006] In a first aspect, the present invention provides a hot melt adhesive for protecting an edge of a pole piece, wherein the hot melt adhesive comprises the following components in percentage by weight:

[0007] Polyolefin resin 30-60%

[0008] Tackifying resin 20-40%

[0009] Wax 5%-25%

[0010] Mineral oil 2-10%

[0011] Functional filler 0-20%

[0012] The polyolefin resin is compounded by a first polyolefin group and a second polyolefin group at a mass ratio of (2-8):1; the first polyolefin group includes modified polypropylene, and the density of the modified polypropylene is less than 0.9g / cm 3 , the melt flow rate at 230℃ / 2.16kg is 4-10g / 10min; the second polyolefin group includes polyethylene, ethylene and C4-C 10 At least one of α-olefin copolymers, amorphous polyα-olefins, acid- or acid anhydride-modified polyolefins, and polyolefin elastomers; the hot melt adhesive has a softening point above 100° C., a melt viscosity below 5000 cps, and a surface drying time within 5 minutes.

[0013] There are many types of polyolefin resins with great differences. Generally speaking, the polyolefin resin of the present invention can be selected from one or more combinations of the following: polypropylene (PP), polyethylene (PE), ethylene and C4-C 10 α-olefin copolymers, amorphous polyα-olefin resins (APAO), maleic anhydride modified polyolefins (MA-APAO), ethylene-octene / butene polymers (POE), acrylic acid modified polyolefins, polyolefin elastomers, etc.

[0014] Specifically, the present invention uses two polyolefin groups for compounding, and the resin compositions of the two groups are different. Among them, the modified polypropylene included in the first polyolefin group can be mixed with modified polypropylenes having different modification methods, different molecular weights, different melt flow rates and / or different crystallinity, so that the final density thereof is less than 0.9 g / cm 3 The melt flow rate at 230℃ / 2.16kg is 4-10g / 10min, which facilitates the subsequent improvement of the overall fluidity through the mixing of the second polyolefin group, and can also provide the hot melt adhesive with sufficient comprehensive properties such as bonding strength and solvent resistance.

[0015] Furthermore, the tackifying resin is selected from at least one of dicyclopentadiene resin (DCPD), coumarone-indene resin, styrene resin, C5 petroleum resin, C9 petroleum resin, and C5-C9 copolymer resin.

[0016] The mineral oil is selected from at least one of white oil, naphthenic oil and paraffin oil.

[0017] The wax is selected from petroleum wax, synthetic wax and mixtures thereof. Preferably, the wax can be specifically selected from at least one of PP wax, PE wax, maleic anhydride modified polypropylene wax (PP-MA) and maleic anhydride modified polyethylene wax (PE-MA).

[0018] Among them, high-melting-point PP wax (≥130°C) is preferred, accounting for more than 10% of all raw materials. PE wax can be selected from low-molecular-weight polyethylene wax with a number-average molecular weight of 400 to 6000 g / mol. In addition, by selecting different proportions of PP wax and PE wax, preferably with a mass ratio of (5-15): (3-10), the surface-free time of the hot melt adhesive can be reduced to less than 5 minutes, preferably less than 3 minutes. By compounding the wax with other raw materials, the softening point of the hot melt adhesive can be increased to above 100°C, preferably between 120°C and 150°C.

[0019] The viscosity of the finished adhesive can be effectively adjusted by adjusting the content of mineral oil and tackifying resin, so that the viscosity of the hot melt adhesive at the melting temperature is below 5000 cps, preferably between 2000 cps and 4000 cps.

[0020] Furthermore, the modified polypropylene of the first polyolefin group includes acrylic acid modified polypropylene with a viscosity of less than 6000 cps at 30°C, and / or the modified polypropylene of the first polyolefin group includes maleic anhydride modified polypropylene with a density of 0.89±0.005 g / cm 3 , the melt flow rate at 230℃ / 2.16kg is 4-6g / 10min, and the maleic anhydride grafting rate is 1-5%.

[0021] There are many options for the specific composition and ratio of the second olefin group, including polyethylene, ethylene and C4-C 10 Based on at least one of α-olefin copolymers, amorphous polyα-olefins, acid or anhydride modified polyolefins, and polyolefin elastomers, it is further preferably a metallocene-catalyzed maleic anhydride grafted polyolefin elastomer with a density of 0.85-0.88 g / cm 3 The melt flow rate at 190°C / 2.16kg is greater than 600g / 10min. The compounding of the first polyolefin group and the second polyolefin group is beneficial to improving the adhesive strength of the hot melt adhesive, and preferably the adhesive strength of the hot melt adhesive is greater than or equal to 0.02N / mm.

[0022] Furthermore, the weight percentage of the functional filler is 0.5-20%, including:

[0023] (1) Colored fillers, which have light absorption effect at 1000-1100nm;

[0024] (2) Optional, white filler.

[0025] The present invention does not need to use functional fillers, and can use thermoplastic resin materials as the main body to meet the basic needs of hot melt adhesives, and can be used in conjunction with a slitting process of knife die cutting. However, preferably, the hot melt adhesive is colored by using colored fillers of various colors such as black, blue and / or yellow, so that the blank or finished product to be processed has an identifiable function, which meets the distinction between different links / positions / processing parameters in the processing process, and can be used through advanced color / image recognition and other technologies to intelligently monitor and control the production process, which is conducive to large-scale automated production. Particularly preferably, a colored filler with light absorption at 1000-1100nm is used, and the addition amount is 0.5%-20%, preferably 10-15%, and the processing method of cutting the pole ear at the edge of the pole piece is used in conjunction with laser die cutting, which effectively realizes the light absorption of the colloid at a specific laser wavelength (for example, 1064nm), thereby meeting the dual requirements of being able to laser cut at a specific power without shrinking the edge, and demonstrating the high efficiency and precision advantages of laser cutting. In addition, by controlling the total content of functional fillers and adjusting the ratio of colored fillers to white fillers, the light absorption efficiency and color of the colloid can be changed at multiple levels, thereby expanding the application range of the product.

[0026] Furthermore, the colored filler and white filler are compounded in a mass ratio of (3-5):(3-8); the colored filler includes a black filler selected from at least one of insulating carbon black, copper manganese black, copper chromium black, black talc, and graphene; and the white filler includes at least one of boehmite, alumina, and aluminum hydroxide. While the colored filler provides multiple functionalities such as identification and light absorption, the white filler provides the hot melt adhesive with positive benefits such as improved insulation, thermal conductivity, and reinforcement.

[0027] In order to improve the compatibility and dispersibility of the functional filler with the resin phase, the functional filler is preferably prepared / treated by the following method:

[0028] (1) dissolving dicumyl peroxide (DCP) in silane, and premixing the silane with a colored filler and an optional white filler to obtain a filler premix;

[0029] (2) Adding filler premix and polypropylene to the granulation equipment;

[0030] (3) Stir and heat to 120-150°C for 5-10 minutes, then continue to heat to 170-185°C and extrude into granules after 5-10 minutes.

[0031] During the preparation of the functional filler, the present invention not only uses a silane coupling agent to surface-activate the aforementioned colored and white fillers, but more importantly, the silane, filler, and polypropylene are subjected to a high-temperature treatment. Under the action of the high temperature and initiator, the silane modifies the polypropylene, thereby forming a functional filler containing silane-modified polypropylene as a carrier. Molecular structures of maleic anhydride, acrylic acid / acrylate, and silane coupling agents contain a large number of polar groups, such as aldehydes and hydroxyls. Introducing these polar groups into polyolefins can improve compatibility with other inorganic and organic components and contribute to increased bonding strength. The present invention utilizes an in-situ polymerization deposition method, simultaneously grafting and modifying polypropylene with a silane coupling agent and uniformly mixing the functional filler with the resin carrier. Particularly advantageously, in the method for preparing a hot-melt adhesive, when the functional filler is added to the resin phase in batches, each addition of the functional filler with the carrier is more easily miscible with the surrounding resin phase, improving dispersion uniformity within the resin phase. Specifically, the polypropylene can be selected from standard commercially available polypropylene, with its usage amount representing 5-15% of the total weight of the modified polypropylene in the first polyolefin group. Preferably, the silane usage amount is 2-6 phr, and the DCP usage amount is 0.15-0.25 phr. An antioxidant (e.g., Antioxidant 1010) of 0.1-0.3 phr may also be added. The silane can be selected from at least one of vinyltrimethoxysilane (VTMS), vinyltriethoxysilane (VTEO), and vinyltris(2-methoxyethoxy)silane (VTMES). Since grafting activity is determined by both the electronic and steric effects on the vinylsilane double bond, and the methoxy group has a smaller hyperconjugation effect than the ethoxy group, and the ethoxy group is larger than the methoxy group, VTMS exhibits higher grafting activity than VTEO under these conditions, making it more preferred. DCP generates free radicals upon heating; using too little of it will result in fewer free radicals and a lower grafting yield. If the dosage is too much, the free radicals generated will be excessive, which may easily cause side reactions such as macromolecular chain branching and self-crosslinking, resulting in excessive viscosity of the grafting system, decreased fluidity, and deterioration of processing performance.

[0032] In a second aspect, the present invention provides a method for preparing the above-mentioned hot melt adhesive, comprising the following steps:

[0033] S1: Under the protection of nitrogen or argon, in a reaction vessel, completely melt the polyolefin resin, tackifying resin, and wax at 170-200° C. to obtain a resin phase; stir at a speed of 30-50 rpm for 40-60 min;

[0034] S2: Premix the functional filler with mineral oil by high-speed centrifugation at a dispersion speed of 1800-2500 rpm for 2-3 times for a total of 5-15 minutes to obtain premix B;

[0035] S3: Add premix B to the completely molten resin phase in 3-5 times, disperse at high speed for 15 to 30 minutes at a dispersion speed of 1000 rpm-1500 rpm, cool and solidify to obtain a hot melt adhesive product.

[0036] In a third aspect, a method for protecting the edge of a pole piece using the aforementioned hot melt adhesive is provided, comprising the following steps:

[0037] Step 1: coating the active slurry on the electrode and curing it to form an active material layer, and the uncoated area between the active material layer and at least one edge of the electrode forms the tab forming area;

[0038] Step 2: Applying molten hot melt adhesive to the tab forming area at 170°C-220°C, covering at least a portion of the active material layer, and cooling and solidifying to form a hot melt adhesive layer;

[0039] Step 3: Cut the stacked hot melt adhesive layer and the pole piece to form a pole ear, so that the edge hot melt adhesive melts and encapsulates at least a portion of the pole piece cross section.

[0040] Furthermore, in step three, laser die-cutting is used to melt the edge hot melt adhesive to encapsulate the electrode section while die-cutting the hot melt adhesive; or knife die cutting is used, and after die-cutting, a hot pressing roller is used to melt the edge hot melt adhesive to encapsulate the electrode section.

[0041] For the laser die-cutting method, by adjusting parameters such as the glue layer thickness, glue surface drying time and viscosity, the effect of complete coverage of the cut end face can basically be achieved. Among them, the aluminum foil pole piece is selected with a thickness of 8-15μm, the active material layer thickness is 80-150μm, the hot melt adhesive layer thickness is 15-60μm, and the width is 5-15mm. The width of the hot melt adhesive layer covering the active material layer is about 0.3-1mm. The laser die-cutting power is 1000-3000W, and the die-cutting speed is 10-25m / s.

[0042] For die cutting, hot pressing roller wrapping parameters are optional: temperature 140-170℃, pressure 0.1-0.5Mpa, time 0.05-0.5s.

[0043] In addition, not limited to after laser die-cutting, a hot pressing roller is added to quickly roll the edge of the electrode to ensure that the cross section of the electrode is completely encapsulated, further improving the safety of use.

[0044] The present invention has the advantages that:

[0045] 1. Through the selection of the types and proportions of the various components, the hot melt adhesive of the present invention has low viscosity, is solid at room temperature, and is liquid above 140°C. It can be used with different gluing equipment and has good wettability to the substrate, providing high adhesion, and can better lock metal particles during use. The hot melt adhesive has a high Tg point, a high softening point, and a fast surface drying ability, which can meet the requirements of the double-sided gluing process. It does not stick to the process roller and ensures that the adhesive layers do not adhere to each other after the electrode is rolled up, allowing for smooth unwinding. The hot melt adhesive of the present invention has moderate flexibility and can be applied to the edge of the current collector near the active material layer area, which can balance the difference in ductility between the two and reduce the generation of wavy edges and wrinkles.

[0046] 2. During use, the hot melt adhesive of the present invention has excellent solvent resistance, can maintain stable physical and chemical properties in the electrolyte, has small dissolution and swelling, and enhances the reliability of the product for long-term use; and the inorganic functional fillers in the hot melt adhesive give the product a recognizable function, while meeting the requirements of laser cutting in the process.

[0047] 3. The preparation process of the hot melt adhesive of the present invention is simple, low-cost, does not require solvents throughout the process, has no by-products, and is environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] The above and other objects, features and advantages of the exemplary embodiments of the present disclosure will become readily understood by reading the following detailed description with reference to the accompanying drawings. In the accompanying drawings, several embodiments of the present disclosure are shown in an illustrative and non-limiting manner, and the same or corresponding reference numerals represent the same or corresponding parts, wherein:

[0049] FIG1 is a schematic flow chart showing a method for protecting an edge of a pole piece according to the present invention.

[0050] Explanation of the reference numerals: 1. Pole piece, 2. Active material layer, 3. Tab forming area, 4. Hot melt adhesive layer, 5. Tab. DETAILED DESCRIPTION

[0051] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in further detail below.

[0052] The present invention provides a hot melt adhesive for protecting the edge of a pole piece. The hot melt adhesive comprises the following components in weight percentage:

[0053] (1) 30-60% polyolefin resin, compounded by a first polyolefin group and a second polyolefin group at a mass ratio of (2-8):1, and the components of the first polyolefin group and the second polyolefin group are different; wherein:

[0054] (1.1) The first polyolefin group includes at least one of the following:

[0055] (a) Acrylic acid modified polypropylene, viscosity at 30°C below 6000 cps;

[0056] (b) Maleic anhydride modified polypropylene, density 0.89 ± 0.005 g / cm 3 , at 230℃ / 2.16kg, the melt flow rate is 4-6g / 10min, and the maleic anhydride grafting rate is 1-5%;

[0057] (1.2) The second polyolefin group includes polyethylene, ethylene and C4-C 10 At least one of α-olefin copolymers, amorphous polyα-olefins, acid or anhydride modified polyolefins, and polyolefin elastomers; preferably, a metallocene-catalyzed maleic anhydride grafted polyolefin elastomer having a density of 0.85-0.88 g / cm 3 , the melt flow rate is greater than 600g / 10min at 190℃ / 2.16kg.

[0058] (2) 20-40% of a tackifying resin, selected from at least one of dicyclopentadiene resin, coumarone-indene resin, styrene resin, C5 petroleum resin, C9 petroleum resin, and C5-C9 copolymer resin;

[0059] (3) 5%-25% wax, wherein the wax is selected from petroleum wax, synthetic wax and mixtures thereof, and specifically at least one of PP wax, PE wax, maleic anhydride modified polypropylene wax (PP-MA), and maleic anhydride modified polyethylene wax (PE-MA); preferably, high melting point PP wax (≥130°C), which accounts for more than 10% of all raw materials. PE wax can be selected from low molecular weight polyethylene wax with a number average molecular weight of 400 to 6000 g / mol. More preferably, PP wax and PE wax are compounded in a mass ratio of (5-15): (3-10);

[0060] (4) 2-10% mineral oil, at least one selected from white oil, naphthenic oil, and paraffin oil;

[0061] (5) Functional fillers 0-20%, preferably 0.5-20%, including:

[0062] (5.1) Colored fillers, which have light absorption in the range of 1000-1100 nm;

[0063] (5.2) Optional, white filler;

[0064] Preferably, the colored filler and the white filler are compounded in a mass ratio of (3-5):(3-8); the colored filler includes a black filler selected from at least one of insulating carbon black, copper manganese black, copper chromium black, black talc, and graphene; and the white filler includes at least one of boehmite, alumina, and aluminum hydroxide. More preferably, the functional filler is prepared by the following method:

[0065] (a) dissolving dicumyl peroxide (DCP) in silane, and premixing the silane with a colored filler and an optional white filler to obtain a filler premix; the silane is used in an amount of 2-6 phr, the DCP is used in an amount of 0.15-0.25 phr, and an antioxidant (e.g., antioxidant 1010) is optionally added in an amount of 0.1-0.3 phr;

[0066] (b) adding a filler premix and polypropylene to a pelletizing device; the amount of polypropylene used is 5-15% of the total mass of the modified polypropylene in the first polyolefin group;

[0067] (c) Stirring and heating to 120-150°C for 5-10 minutes, then continuing to heat to 170-185°C for 5-10 minutes, and extruding and granulating.

[0068] The method for preparing the hot melt adhesive for electrode edge protection comprises the following steps:

[0069] S1: Under the protection of nitrogen or argon, in a reaction vessel, the polyolefin resin, tackifying resin, and wax are completely melted at 170° C.-200° C. to obtain a resin phase;

[0070] S2: premixing the functional filler with mineral oil by high-speed centrifugation to obtain premix A;

[0071] S3: Add premix A to the completely molten resin phase in 3-5 portions, disperse at high speed, and cool and solidify to obtain a finished hot melt adhesive. The finished hot melt adhesive includes, but is not limited to, the following properties: a softening point above 100°C, a melt viscosity below 5000 cps, and a tack-free time of less than 5 minutes.

[0072] The specific application scenarios and application methods of the hot melt adhesive for electrode edge protection will be described in conjunction with Figure 1.

[0073] The method for protecting the edge of the electrode using the hot melt adhesive comprises the following steps:

[0074] Step 1: coating the active slurry on the electrode 1 and curing it to form an active material layer 2, and the uncoated area between the active material layer 2 and at least one edge of the electrode 1 forms a tab forming area 3;

[0075] Step 2: Apply the melted hot melt adhesive to the tab forming area 3 and cover at least a portion of the active material layer 2, and cool and solidify to form a hot melt adhesive layer 4;

[0076] Step 3: Cut the stacked hot melt adhesive layer 4 and the electrode 1 to form the electrode tab 5, so that the edge hot melt adhesive melts and encapsulates at least a portion of the electrode cross section. The cutting method can be laser die-cutting, where the hot melt adhesive melts and encapsulates at least a portion of the electrode cross section simultaneously with die-cutting; or knife die-cutting, where a hot press roller is used to melt and encapsulate the electrode cross section after die-cutting. Optionally, after laser die-cutting, the hot press roller is used to press the electrode cross section again to ensure that the edge of the electrode cross section is completely encapsulated.

[0077] Example 1

[0078] Under nitrogen protection, the temperature was set to 200°C, and maleic anhydride-modified polypropylene (APAO) from the first polyolefin group, maleic anhydride-grafted polyolefin elastomer (MA-APAO) from the second polyolefin group, tackifying resin, and wax were added. After heating and stirring until completely melted, premix A of functional filler and mineral oil was added. The mixture was vacuumed and dispersed at a speed of 1000 rpm for 20 minutes. After uniform dispersion, it was filtered and cooled to obtain finished hot melt adhesive samples A1-A6. The specific material composition is shown in Table 1.

[0079] Table 1 Material composition of samples A1-A6 of Example 1 (wt%)

[0080]

[0081] Example 2

[0082] Under nitrogen protection, the temperature was set to 200°C, and maleic anhydride-modified polypropylene (APAO) from the first polyolefin group, maleic anhydride-grafted polyolefin elastomer (MA-APAO) from the second polyolefin group, tackifying resin, and wax were added. After heating and stirring until completely melted, premix A of functional filler and mineral oil was added. The mixture was vacuumed and dispersed at a speed of 1000 rpm for 20 minutes. After uniform dispersion, it was filtered and cooled to obtain finished hot melt adhesive samples B1-B6. The specific material composition is shown in Table 2.

[0083] Table 2 Material composition of samples B1-B6 of Example 2 (wt%)

[0084]

[0085] Example 3

[0086] The finished hot melt adhesive sample C1 was obtained by referring to the preparation method and material composition of sample A2 in Example 1; the finished hot melt adhesive sample C2 was obtained by referring to the preparation method and material composition of sample B1 in Example 2. The main difference between C1 and A2, and C2 and B1, is that the functional fillers in C1 and C2 are prepared / treated by the following method:

[0087] (1) 0.2 phr of dicumyl peroxide (DCP) and 0.1 hpr of antioxidant (antioxidant 1010) were dissolved in 5 phr of silane (VTMS), and the silane was premixed with the functional filler raw material to obtain a filler premix;

[0088] (2) Adding filler premix and polypropylene to the granulation equipment;

[0089] (3) Stir and heat to 130°C for 10 minutes, then continue to heat to 175°C, and extrude and granulate after 8 minutes to obtain optimized functional fillers.

[0090] Performance Testing

[0091] The following performance tests were performed on the hot melt adhesive samples A1-A6 and B1-B6 of the above examples. The specific test methods are as follows. The test results are shown in Table 3:

[0092] (1) Viscosity test

[0093] Test Method: Set the temperature of a Brookfield DV2T hot melt adhesive viscometer to 180°C. Cut 10.5g of hot melt adhesive and melt it in the heating sleeve. Select a No. 27 spindle. After the temperature stabilizes for 30 minutes, set the speed to maintain a torque between 20% and 80%. Read the viscosity reading when the viscosity fluctuation is less than 1% within 1 minute.

[0094] (2) Softening point test

[0095] Test method: Melt the hot melt adhesive into a ring-shaped mold, let it stand for 24 hours, and then use a softening point tester to test the softening point of the material.

[0096] (3) Aluminum / copper foil adhesion test

[0097] Test method: Using aluminum foil and copper foil as substrates, respectively, prepare sample films with a thickness of 20um-30um on a film scraper at 170℃, cut into 20mm×100mm strips, fix the strips to the backing plate, fit the adhesive layer to the double-sided adhesive layer, and peel the samples 180° at a peeling speed of 50mm / min. Test 5 samples for each formulation and take the average value.

[0098] (4) Adhesion after soaking

[0099] Test Method: Using aluminum foil and copper foil as substrates, a film sample with a thickness of 20-30 μm was prepared on a film scraper at 170°C. The film was cut into 20 mm x 100 mm strips, placed in 30 ml of electrolyte, sealed, and placed in an 85°C oven for 24 hours. The film was then removed and tested for 180° peel strength. The peel speed was 50 mm / min. Five samples were tested for each formulation, and the average value was calculated.

[0100] (5) Dissolution rate

[0101] Test method: 0.5g of glue is soaked in 25g of electrolyte. The mixture is then aged in a 70°C oven for 48 hours. A weighing pan, M2, is weighed. The electrolyte solution, which has been used to soak the glue, is then poured into the weighing pan. The pan is then placed in a 180°C oven and baked for 2 hours. The weighing pan, M3, is weighed again. The dissolution rate is calculated as (M3 - M2) / 0.5.

[0102] (6) Surface drying time

[0103] Test method: Take 8g of glue, place it in an aluminum foil box, and place it in a 170℃ oven for 30 minutes. After taking it out, record the time it takes for the surface glue to be completely cured.

[0104] (7) Surface adhesion test

[0105] Test method: Prepare a scraped film sample with an aluminum foil substrate with a 20um adhesive layer thickness, cut the sample into 40×10mm strips, put the two strips adhesive surface together, and place them between two steel plates. Keep the steel plate and strip combination horizontal and place it between the flat vulcanizers. Maintain a certain pressure and holding time. After taking it out, perform a T peel test at a peel speed of 50mm / min. Test 5 samples for each formula and take the average value.

[0106] Table 3 Test results of samples from Examples 1 to 3

[0107]

[0108] The above introduces the preferred embodiments of the present invention, which is intended to make the spirit of the present invention clearer and easier to understand, and is not intended to limit the present invention. Any modifications, replacements, and improvements made within the spirit and principles of the present invention should be included in the scope of protection outlined by the claims attached to the present invention.

Claims

1. A hot melt adhesive for protecting the edge of a pole piece, characterized in that: The hot melt adhesive comprises the following components by weight percentage: Polyolefin resin 30-60% Tackifying resin 20-40% Wax 5%-25% Mineral oil 2-10% Functional filler 0-20% The polyolefin resin is compounded by a first polyolefin group and a second polyolefin group in a mass ratio of (2-8):1; The first polyolefin group includes modified polypropylene, wherein the density of the modified polypropylene is less than 0.9 g / cm 3 , the melt flow rate is 4-10g / 10min at 230℃ / 2.16kg; The second polyolefin group includes polyethylene, ethylene and C4-C 10 At least one of α-olefin copolymers, amorphous polyα-olefins, acid- or acid anhydride-modified polyolefins, and polyolefin elastomers; The hot melt adhesive has a softening point of above 100° C., a melt viscosity of below 5000 cps, and a surface drying time of within 5 minutes.

2. The hot melt adhesive according to claim 1, characterized in that: The tackifying resin is selected from at least one of dicyclopentadiene resin, coumarone-indene resin, styrene resin, C5 petroleum resin, C9 petroleum resin, and C5-C9 copolymer resin; the mineral oil is selected from at least one of white oil, cyclohexane oil, and paraffin oil; the wax is selected from petroleum wax, synthetic wax, and a mixture thereof.

3. The hot melt adhesive according to claim 2, characterized in that: The modified polypropylene of the first polyolefin group includes acrylic acid modified polypropylene, and the viscosity at 30° C. is below 6000 cps.

4. The hot melt adhesive according to claim 2, characterized in that: The modified polypropylene of the first polyolefin group includes maleic anhydride modified polypropylene having a density of 0.89±0.005 g / cm 3 , the melt flow rate at 230℃ / 2.16kg is 4-6g / 10min, and the maleic anhydride grafting rate is 1-5%.

5. The hot melt adhesive according to claim 3 or 4, characterized in that: The second polyolefin group includes a metallocene-catalyzed maleic anhydride grafted polyolefin elastomer having a density of 0.85-0.88 g / cm 3 , the melt flow rate at 190℃ / 2.16kg is greater than 600g / 10min.

6. The hot melt adhesive according to claim 5, characterized in that: The weight percentage of the functional filler is 0.5-20%, including: (1) Colored fillers, which have light absorption at 1000-1100nm; (2) Optional, white filler.

7. The hot melt adhesive according to claim 6, characterized in that: The colored filler and the white filler are compounded in a mass ratio of (3-5):(3-8); the colored filler includes a black filler selected from at least one of insulating carbon black, copper manganese black, copper chrome black, black talc, and graphene; the white filler includes at least one of boehmite, alumina, and aluminum hydroxide.

8. A method for preparing the hot melt adhesive for electrode edge protection according to any one of claims 1 to 7, characterized in that: The steps include: S1: Under the protection of nitrogen or argon, in a reaction container, the polyolefin resin, tackifying resin and wax are completely melted at 170° C.-200° C. to obtain a resin phase; S2: premixing the functional filler and mineral oil by high-speed centrifugation to obtain a premix A; S3: Add premix A to the completely molten resin phase in 3-5 times, disperse at high speed, cool and solidify to obtain a hot melt adhesive product.

9. A method for protecting the edge of a pole piece using the hot melt adhesive according to any one of claims 1 to 7, characterized in that: The steps include: Step 1: coating the active slurry on the pole piece and curing it to form an active material layer, wherein the uncoated area between the active material layer and at least one edge of the pole piece forms a pole ear forming area; Step 2: applying the melted hot melt adhesive to the tab forming area and covering at least a portion of the active material layer, and cooling and solidifying to form a hot melt adhesive layer; Step 3: Cut the stacked hot melt adhesive layers and pole pieces to form pole ears, so that the edge hot melt adhesive melts and encapsulates at least a portion of the pole piece cross section.

10. The pole piece edge protection method according to claim 9, characterized in that: In step three, laser die-cutting is used to melt the edge hot melt adhesive to encapsulate the electrode section while die-cutting the hot melt adhesive; or knife die cutting is used, and after die-cutting, a hot pressing roller is used to melt the edge hot melt adhesive to encapsulate the electrode section.

Citation Information

Patent Citations

  • Battery pole piece, production method thereof, battery core package comprising pole piece and battery

    CN115000345A

  • Glue, preparation method thereof and application of glue to battery cell

    CN109913161A

  • Hot melt adhesive and application thereof

    CN110511703A

  • Hot melt adhesive for bonding metal and plastic, and preparation method of hot melt adhesive

    CN110699013A

  • Hot melt adhesive for high-performance polypropylene barrier film as well as preparation method and application of hot melt adhesive

    CN114032049A