Positive electrode sheet slurry, and positive electrode sheet and preparation method therefor and use thereof
By introducing lithium manganese iron phosphate, high-voltage positive electrode materials and solid electrolytes into the positive electrode sheet slurry, the problem of low thermal stability of high-voltage positive electrode materials is solved, and the thermal stability and electrical power of the lithium battery cell are significantly improved. Chemical properties.
Patent Information
- Application Number
- PCT/CN2024/088795
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2024-04-19
- Publication Date
- 2024-12-05
AI Technical Summary
High voltage positive electrode materials have low thermal stability at high temperatures, resulting in thermal stability problems of lithium battery cells. The existing methods have limited improvements in thermal stability of the battery cells and affect electrochemical performance.
Using positive electrode sheet slurry, including lithium manganese iron phosphate and high voltage positive electrode materials, solid electrolytes such as titanium aluminum lithium phosphate and lithium lanthanum zirconium oxygen, the solid electrolyte is evenly distributed through the slurry coating method to increase the heat of the battery cell stability.
It significantly improves the high-temperature thermal stability of the battery cell, reduces thermal runaway and thermal abuse performance, and maintains the excellent electrochemical performance.
Smart Images

Figure PCTCN2024088795-FTAPPB-I100001
Abstract
Description
Positive electrode sheet slurry, positive electrode sheet, and preparation method and application thereof
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This disclosure claims priority to application number 202310625480X filed with the Patent Office of China on May 30, 2023, entitled “A positive electrode sheet slurry, a positive electrode sheet, a preparation method and application thereof,” the entire contents of which are incorporated by reference into this disclosure. Technical Field
[0003] The present disclosure relates to the technical field of lithium batteries, and in particular to a positive electrode sheet slurry, a positive electrode sheet, and a preparation method and application thereof. Background Art
[0004] High-voltage cathode materials are a type of commonly used cathode material for lithium-ion batteries. They typically offer advantages such as high energy density and high specific capacity, but they often suffer from poor thermal stability. There are several main types of high-voltage cathode materials: the first type is primarily based on layered materials; the second type is primarily represented by spinel; the third type is primarily based on lithium-rich manganese-based materials; and the fourth type is based on polyanion salts. Currently, in order to combine the excellent properties of various high-voltage cathode materials, mixed systems of different high-voltage materials have emerged. These systems not only offer the high energy density of high-voltage systems but also improve low-temperature, cycling, and electrical conductivity performance. However, high-voltage materials are relatively more active at high temperatures, resulting in lower thermal stability, a phenomenon that poses significant operational risks for battery cells.
[0005] Battery cell thermal stability is one of the most challenging issues to address in lithium-ion batteries, and this issue is particularly prominent. Lithium iron phosphate batteries, due to their crystal structure, have very high thermal stability, resulting in good thermal stability. However, high-voltage system materials may have less than ideal high-temperature stability. High-voltage system cells exhibit excellent low-temperature capacity, but relatively poor high-temperature stability.
[0006] At present, there are mainly the following methods to improve the thermal stability of high voltage system cells:
[0007] (1) Improving the thermal stability of the battery cell by adding high-temperature additives to the electrolyte to improve the thermal stability of the battery cell during the electrochemical reaction;
[0008] (2) Improving the thermal stability of the battery cell by replacing the diaphragm or coating the diaphragm surface with a material with higher thermal stability;
[0009] (3) From a technological perspective, materials with better thermal stability are introduced during the production of positive and negative electrode sheets to improve the overall thermal stability of the battery cell.
[0010] However, these conventional methods have limited effectiveness in improving the intrinsic thermal stability of high-voltage battery cells, and they can also negatively impact the electrochemical performance of the cells. Therefore, improving the intrinsic stability of high-voltage battery cells while maintaining their excellent electrochemical performance has become a pressing technical challenge.
[0011] In view of this, the present disclosure is proposed.
[0012] Summary of the Invention
[0013] The purpose of the present disclosure is to provide a positive electrode sheet slurry, a positive electrode sheet, and a preparation method and application thereof, aiming to improve the stability of high-voltage system batteries while maintaining the excellent electrochemical performance of the batteries.
[0014] The present disclosure is achieved as follows:
[0015] In a first aspect, the present disclosure provides a positive electrode sheet slurry, which comprises, by mass percentage, 87%-92% of a positive electrode active material, 3%-5% of a binder, 3%-5% of a conductive agent, and 2%-5% of a solid electrolyte;
[0016] The solid electrolyte is an oxide solid electrolyte, and the oxide solid electrolyte is selected from at least one of lithium aluminum titanium phosphate, lithium aluminum germanium phosphate, lithium lanthanum zirconium oxide, and lithium lanthanum zirconium titanium oxide;
[0017] The positive electrode active materials include lithium manganese iron phosphate and high voltage positive electrode materials.
[0018] In an optional embodiment, the oxide solid electrolyte is selected from at least one of lithium titanium aluminum phosphate and lithium lanthanum zirconium oxide.
[0019] In an optional embodiment, in the positive electrode active material, the mass ratio of lithium manganese iron phosphate to the high voltage positive electrode material is (50-70): (30-50).
[0020] In an optional embodiment, the high-voltage positive electrode material is selected from at least one of nickel-cobalt-manganese positive electrode material, lithium cobalt oxide positive electrode material and lithium vanadium phosphate.
[0021] In an optional embodiment, the composition includes, by mass percentage, 88%-90% of positive electrode active material, 3.5%-4.5% of binder, 3.5%-4.5% of conductive agent, and 2.5%-3.5% of solid electrolyte.
[0022] In an optional embodiment, the binder is selected from at least one of polyvinylidene fluoride, polytetrafluoroethylene and styrene-butadiene rubber.
[0023] In an optional embodiment, the conductive agent is selected from at least one of carbon nanotubes, Ketjen black, acetylene black, furnace black, carbon fiber and nanographite.
[0024] In a second aspect, the present disclosure provides a method for preparing a positive electrode sheet, comprising: providing a positive electrode sheet slurry according to any of the above embodiments, and forming a positive electrode active coating on a positive electrode current collector using the positive electrode sheet slurry.
[0025] In an optional embodiment, the process includes coating the positive electrode sheet slurry on both the front and back sides of the positive electrode current collector, followed by drying and roll pressing.
[0026] In an optional embodiment, when the positive electrode sheet slurry is coated on the positive electrode current collector, the coating surface density is controlled to be 20 mg / cm 2 -30mg / cm 2 , ear areas are reserved on both sides.
[0027] In an optional embodiment, the positive electrode current collector is aluminum foil.
[0028] In an optional embodiment, the drying process includes: passing the coated electrode through an oven with a length of 18m-30m and a temperature of 100°C-120°C at a speed of 1m / s-5m / s.
[0029] In an optional embodiment, during the roller pressing process, the compaction density is controlled to be 2.8 g / cm 3 -2.9g / cm 3 .
[0030] In a third aspect, the present disclosure provides a positive electrode sheet prepared by the preparation method in the aforementioned embodiment.
[0031] In a fourth aspect, the present disclosure provides a lithium battery comprising the positive electrode sheet of the aforementioned embodiment.
[0032] In an optional embodiment, a negative electrode sheet is also included, and the preparation process of the lithium battery includes: assembling the positive electrode sheet and the negative electrode sheet, and injecting liquid into them.
[0033] In a fifth aspect, the present disclosure provides a battery module, comprising the lithium battery of any one of the aforementioned embodiments or a lithium battery prepared by the preparation method of the aforementioned embodiments.
[0034] In a sixth aspect, the present disclosure provides a battery pack comprising the lithium battery of any one of the aforementioned embodiments, or the battery module of the aforementioned embodiments.
[0035] In a seventh aspect, the present disclosure provides an electrical device, comprising the lithium battery of the aforementioned embodiment, the battery module of the aforementioned embodiment, or the battery pack of the aforementioned embodiment. The present disclosure has the following beneficial effects: by using lithium manganese iron phosphate and high-voltage positive electrode materials as composite positive electrode active materials, introducing a solid electrolyte into the positive electrode plate slurry, and using the slurry coating method, the solid electrolyte is evenly distributed in the positive electrode material. The electrode plate prepared by the positive electrode plate slurry provided by the present disclosure can effectively improve the thermal stability of the battery cell, and greatly improve the performance in terms of thermal runaway and thermal abuse. DETAILED DESCRIPTION
[0036] To make the purpose, technical solutions, and advantages of the embodiments of the present disclosure more clear, the technical solutions in the embodiments of the present disclosure are described clearly and completely below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer were followed. Reagents or instruments used where the manufacturer is not specified are conventional products that can be purchased commercially.
[0037] An embodiment of the present disclosure provides a positive electrode plate slurry, which includes, by mass percentage, 87%-92% of positive electrode active material, 3%-5% of binder, 3%-5% of conductive agent and 2%-5% of solid electrolyte.
[0038] Specifically, the mass fraction of the positive electrode active material can be 87%, 88%, 89%, 90%, 91%, 92%, etc., the mass fraction of the binder can be 3%, 4%, 5%, etc., the mass fraction of the conductive agent can be 3%, 4%, 5%, etc., and the mass fraction of the solid electrolyte can be 2%, 3%, 4%, 5%, etc. The positive electrode active material, binder, conductive agent and solid electrolyte can also be any value among the above adjacent values.
[0039] In an optional embodiment, the composition, calculated by mass, includes 88%-90% positive electrode active material, 3.5%-4.5% binder, 3.5%-4.5% conductive agent, and 2.5%-3.5% solid electrolyte. The amount of each component in the positive electrode slurry is optimized to further improve the thermal stability of the battery cell.
[0040] The positive electrode active material includes lithium manganese iron phosphate and a high-voltage positive electrode material. The specific type of the high-voltage positive electrode material is not limited. This type of positive electrode material has the advantages of high energy density and high specific capacity, but has poor thermal stability. The specific ratio of lithium manganese iron phosphate to the high-voltage positive electrode material is also not limited, and can be (50-70): (30-50), specifically 50:50, 60:40, 70:30, etc., or any adjacent value.
[0041] In some embodiments, the high-voltage positive electrode material is selected from at least one of nickel-cobalt-manganese positive electrode material, lithium cobalt oxide positive electrode material and lithium vanadium phosphate, and can be any one or more of the above.
[0042] In some embodiments, the binder is selected from at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene, and styrene-butadiene rubber, and may be any one or more of the above.
[0043] In some embodiments, the conductive agent is selected from at least one of carbon nanotubes (CNTs), Ketjen black, acetylene black, furnace black, carbon fiber, and nanographite, and may be any one or more of the above. The solvents used for the positive electrode are primarily NMP / DMF / DMSO / THF; the solvent for the negative electrode is primarily H2O.
[0044] Furthermore, the solid electrolyte is an oxide solid electrolyte, and the oxide solid electrolyte is selected from at least one of lithium aluminum titanium phosphate (LATP), lithium aluminum germanium phosphate (LAGP), lithium lanthanum zirconium oxide (LLZO) and lithium lanthanum zirconium titanium oxide (LLZTO), and can be any one or more of the above; optionally, the oxide solid electrolyte is selected from at least one of lithium aluminum titanium phosphate and lithium lanthanum zirconium oxide. By optimizing the type of oxide solid electrolyte, since the oxide solid electrolyte has good ionic conductivity and very excellent thermal stability, it can not only significantly improve the thermal stability of the high voltage system battery cell, but also maintain the original electrochemical properties of the battery cell.
[0045] The embodiment of the present disclosure provides a method for preparing a positive electrode plate, comprising: using the above-mentioned positive electrode plate slurry to form a positive electrode active coating on a positive electrode current collector. The specific preparation method can refer to the existing technology.
[0046] In some embodiments, the positive electrode sheet slurry is coated on both sides of the positive electrode current collector, and then dried to remove the binder, and then rolled to obtain a sheet with a compaction density that meets the requirements. The sheet roll is then divided into two equal rolls, upper and lower, by laser cutting, and finally cut with a mold to obtain a positive electrode sheet with a size that meets the requirements.
[0047] Furthermore, in the process of coating the positive electrode slurry on the positive electrode current collector, the coating surface density is controlled to be 20 mg / cm 2 -30mg / cm 2 , the tab area is reserved on both sides, and the size of the tab area can be set according to needs, such as 18mm-23mm. Specifically, the surface density of the coating can be 20mg / cm 2 , 22mg / cm 2 , 24mg / cm 2 , 26mg / cm 2 , 28mg / cm 2、30mg / cm 2 etc. It can also be any value among the above adjacent values.
[0048] Furthermore, the positive electrode current collector may be aluminum foil.
[0049] Furthermore, the drying process includes: passing the coated electrode through an oven with a length of 18m-30m and a temperature of 100℃-120℃ at a speed of 1m / s-5m / s to remove the solvent. Specifically, the speed of passing through the oven can be 1m / s, 2m / s, 3m / s, 4m / s, 5m / s, etc., or any value among the above adjacent values; the length of the oven can be 18m, 20m, 22m, 25m, 28m, 30m, etc., or any value among the above adjacent values; the temperature of the oven can be 100℃, 105℃, 110℃, 115℃, 120℃, etc., or any value among the above adjacent values.
[0050] Furthermore, during the roller pressing process, a roller press was used to control the compaction density to 2.8 g / cm 3 -2.9g / cm 3 , such as 2.80g / cm 3 , 2.85g / cm 3 , 2.90g / cm 3 etc. It can also be any value among the above adjacent values.
[0051] The embodiment of the present disclosure provides a positive electrode plate, which is prepared by the above-mentioned positive electrode plate preparation method, and the positive electrode plate can be used to further prepare a lithium battery.
[0052] Generally speaking, lithium batteries also include negative electrode sheets. The preparation process of lithium batteries includes: assembling positive electrode sheets and negative electrode sheets, and injecting liquid into them. The specific assembly and injection processes can refer to the existing technology.
[0053] It should be noted that the disclosed embodiments effectively improve the thermal stability of high-voltage battery cells from the perspective of battery cell manufacturing and production. Experimental verification has demonstrated effective improvement in the high-temperature thermal stability of the fabricated high-voltage battery cells. Hot box stability performance has increased from 30 minutes at 130°C to 30 minutes at 150°C, resulting in significant reductions in voltage drop and temperature rise rate.
[0054] The present disclosure provides a battery module comprising the aforementioned lithium battery, which is assembled into a battery module. The number of lithium batteries contained in the battery module can be multiple, and the specific number can be adjusted according to the application and capacity of the battery module.
[0055] An embodiment of the present disclosure provides a battery pack, including the above-mentioned lithium battery or the above-mentioned battery module. The battery modules can be further assembled into a battery pack. The number of battery modules included in the battery pack is not limited and can be adjusted according to the application environment and capacity requirements of the battery pack.
[0056] It should be noted that the structure of the battery module and battery pack is not limited, and reference may be made to the existing battery module and battery pack structures. Any existing battery module or battery pack structure is within the scope of protection of the present disclosure.
[0057] The present disclosure provides an electrical device comprising the aforementioned lithium battery, battery module, or battery pack. The lithium battery, battery module, or battery pack can be used as a power source for the electrical device or as a power storage unit for the electrical device. The electrical device can also include other structures such as electrical appliances, and the types of electrical appliances are not limited.
[0058] Specifically, the power-consuming device may be a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle, an electric train, a ship, a satellite, etc.
[0059] The features and performance of the present disclosure are further described in detail below with reference to the embodiments.
[0060] Example 1
[0061] This embodiment provides a method for preparing a lithium battery, comprising the following steps:
[0062] (1) Preparation of positive electrode sheet
[0063] The positive electrode active material, PVDF, CNT and LATP are mixed, and the amounts of the positive electrode active material, PVDF, CNT and LATP are 89%, 4%, 4% and 3% respectively. The positive electrode active material includes lithium manganese iron phosphate (LMFP-LiMn6Fe4PO4) and NCM (LiNi 0.6 Co 0.2 Mn 0.2 ) with a mass ratio of 1:1, and an appropriate amount of solvent (methyl pyrrolidone, NMP) was added to homogenize to obtain a positive electrode sheet slurry.
[0064] Take an aluminum foil with a thickness of 13 μm and a length and width of 100 μm and 50 μm respectively, and evenly coat the positive electrode slurry on both sides of the copper foil. The surface density of the coating process is controlled at 24 mg / cm 2 , while leaving 20mm of tab area on both sides. The coated electrode was passed through a 20-meter-long 110℃ oven at a speed of 3m / s to remove the solvent NMP, thus obtaining the positive electrode. The electrode was rolled using a roller press to achieve a compaction density of 2.85g / cm 3Then use laser cutting to divide the electrode roll into two equal rolls; finally use a mold to cut it into 60cm long and 30cm wide positive electrode sheets.
[0065] Positive electrode thermal stability test: Perform thermal DSC-TG test on the composite electrode to check the thermal decomposition temperature of the electrode.
[0066] (2) Preparation of negative electrode sheet
[0067] Take a copper foil with a thickness of 8 μm and a length and width of 100 μm and 50 μm respectively, and evenly coat the negative electrode slurry (graphite slurry) on both sides of the copper foil with a thickness of 8 μm. The surface density of the coating process is controlled at 17 mg / cm 2 , while leaving 20mm of tab area on both sides; the coated electrode is passed through a 20m long 110℃ oven at a speed of 3m / s, and the negative electrode is obtained after baking.
[0068] (3) Preparation of soft pack batteries
[0069] The negative electrode sheets are rolled and cut, and the positive electrode sheets are assembled, injected and formed into batteries.
[0070] Example 2
[0071] This embodiment provides a method for preparing a lithium battery, comprising the following steps:
[0072] (1) Preparation of positive electrode sheet
[0073] The positive electrode active material, PVDF, CNT and LATP are mixed, and the amounts of the positive electrode active material, PVDF, CNT and LATP are 89%, 4%, 4% and 3% respectively. The positive electrode active material includes lithium manganese iron phosphate and lithium cobalt oxide (LiCoO2, LCO) in a mass ratio of 1:1. An appropriate amount of solvent (methyl pyrrolidone, NMP) is added to homogenize to obtain a positive electrode sheet slurry.
[0074] Take a copper foil with a thickness of 13μm and a length and width of 100mm and 50mm respectively, and evenly coat the positive electrode slurry on both sides of the copper foil. The coating process controls the surface density at 24mg / cm 2 , while leaving 20mm of tab area on both sides; the coated electrode was passed through a 20m long 110℃ oven at a speed of 3m / s to remove the solvent NMP to obtain the positive electrode; the electrode was rolled using a roller press to achieve a compaction density of 2.85g / cm 3 Then use laser cutting to divide the electrode roll into two equal rolls; finally use a mold to cut it into 60cm long and 30cm wide positive electrode sheets.
[0075] Positive electrode thermal stability test: Perform thermal DSC-TG test on the composite electrode to check the thermal decomposition temperature of the electrode.
[0076] (2) Preparation of negative electrode sheet
[0077] Please refer to Example 1 for the specific steps.
[0078] (3) Preparation of soft pack batteries
[0079] Please refer to Example 1 for the specific steps.
[0080] Example 3
[0081] This embodiment provides a method for preparing a lithium battery, comprising the following steps:
[0082] (1) Preparation of positive electrode sheet
[0083] The positive electrode active material, PVDF, CNT and LATP are mixed, and the amounts of the positive electrode active material, PVDF, CNT and LATP are 89%, 4%, 4% and 3% respectively. The positive electrode active material includes lithium manganese iron phosphate and Li2VPO4 (LVP) in a mass ratio of 1:1. An appropriate amount of solvent (methyl pyrrolidone, NMP) is added to homogenize to obtain a positive electrode sheet slurry.
[0084] Take a copper foil with a thickness of 13μm and a length and width of 100mm and 50mm respectively, and evenly coat the positive electrode slurry on both sides of the copper foil. The coating process controls the surface density at 24mg / cm 2 , while leaving 20mm of tab area on both sides; the coated electrode was passed through a 20m long 110℃ oven at a speed of 3m / s to remove the solvent NMP to obtain the positive electrode; the electrode was rolled using a roller press to achieve a compaction density of 2.85g / cm 3 Then use laser cutting to divide the electrode roll into two equal rolls; finally use a mold to cut it into 60cm long and 30cm wide positive electrode sheets.
[0085] Positive electrode thermal stability test: Perform thermal DSC-TG test on the composite electrode to check the thermal decomposition temperature of the electrode.
[0086] (2) Preparation of negative electrode sheet
[0087] Please refer to Example 1 for the specific steps.
[0088] (3) Preparation of soft pack batteries
[0089] Please refer to Example 1 for the specific steps.
[0090] Example 4
[0091] The only difference from Example 1 is that LATP is replaced by an equal amount of LLZO in the positive electrode slurry.
[0092] Comparative Example 1
[0093] The only difference from Example 1 is that no solid electrolyte LATP is added when preparing the positive electrode slurry. The specific steps are as follows:
[0094] (1) Preparation of positive electrode sheet
[0095] The positive electrode active material, PVDF and CNT are mixed to obtain the positive electrode sheet slurry. The amount of positive electrode active material, PVDF and CNT is 90%, 5% and 5% respectively. The positive electrode active material includes lithium iron manganese phosphate and NCM (LiNi 0.6 Co 0.2 Mn 0.2 ) with a mass ratio of 1:1, and an appropriate amount of solvent (methyl pyrrolidone, NMP) was added to homogenize to obtain a positive electrode sheet slurry.
[0096] Take a copper foil with a thickness of 13 μm and a length and width of 100 mm and 50 mm respectively, and evenly coat the positive electrode slurry on both sides of the copper foil. The surface density of the coating process is controlled at 24 mg / cm 2 , while leaving 20mm of tab area on both sides. The coated electrode was passed through a 20-meter-long 110℃ oven at a speed of 3m / s to remove the solvent NMP, thus obtaining the positive electrode. The electrode was rolled using a roller press to achieve a compaction density of 2.85g / cm 3 Then use laser cutting to divide the electrode roll into two equal rolls; finally use a mold to cut it into 60cm long and 30cm wide positive electrode sheets.
[0097] Positive electrode thermal stability test: Perform thermal DSC-TG test on the composite electrode to check the thermal decomposition temperature of the electrode.
[0098] (2) Preparation of negative electrode sheet
[0099] Please refer to Example 1 for the specific steps.
[0100] (3) Preparation of soft pack batteries
[0101] Please refer to Example 1 for the specific steps.
[0102] Test Example 1
[0103] The thermal stability of the positive electrode sheets prepared in the examples and comparative examples was tested, and the performance of the prepared soft-pack batteries was tested. The results are shown in Table 1.
[0104] Test method: Perform thermal DSC-TG test on the composite electrode to check the thermal decomposition temperature of the electrode; after the soft-pack battery is completed, install the corresponding size fixture and perform thermal runaway and thermal stability test on the battery cell. The test conditions are: place the battery cell in a hot box to heat the hot box and monitor the surface temperature of the battery cell.
[0105] Table 1 Tests on the performance of the electrodes and cells prepared in the examples and comparative examples Note: 150°-30min means that after heating to 150°C and keeping warm for 30 minutes, there is no risk of fire or explosion.
[0106] As can be seen from Table 1, the DSC trigger temperature of the positive electrode prepared in the embodiment of the present disclosure is significantly lower, indicating that the thermal stability of the battery cell is improved and the temperature cannot rise. The electrode without LATP addition has poor thermal stability, and the temperature rises quickly, and soon reaches the DSC trigger temperature.
[0107] The above are merely optional embodiments of the present disclosure and are not intended to limit the present disclosure. Those skilled in the art will readily appreciate that the present disclosure may be modified and varied in various ways. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present disclosure shall be within the scope of protection of the present disclosure. Industrial Applicability
[0108] This disclosure utilizes lithium manganese iron phosphate and a high-voltage cathode material as composite cathode active materials, introduces a solid electrolyte into the cathode plate slurry, and uniformly distributes the solid electrolyte throughout the cathode material through a slurry coating method. The electrode plates prepared using the cathode plate slurry provided in this disclosure can effectively improve the thermal stability of battery cells, significantly enhancing performance in areas such as thermal runaway and thermal abuse, and possesses high industrial applicability.
Claims
1. A positive electrode sheet slurry, characterized in that: Calculated by mass percentage, it includes 87%-92% of positive electrode active material, 3%-5% of binder, 3%-5% of conductive agent and 2%-5% of solid electrolyte; Wherein, the solid electrolyte is an oxide solid electrolyte, and the oxide solid electrolyte is selected from at least one of lithium aluminum titanium phosphate, lithium aluminum germanium phosphate, lithium lanthanum zirconium oxide and lithium lanthanum zirconium titanium oxide; The positive electrode active material includes lithium manganese iron phosphate and a high voltage positive electrode material.
2. The positive electrode sheet slurry according to claim 1, characterized in that: The oxide solid electrolyte is selected from at least one of lithium aluminum titanium phosphate and lithium lanthanum zirconium oxide.
3. The positive electrode sheet slurry according to claim 1 or 2, characterized in that: In the positive electrode active material, the mass ratio of the lithium manganese iron phosphate to the high voltage positive electrode material is (50-70): (30-50).
4. The positive electrode sheet slurry according to any one of claims 1 to 3, characterized in that: The high voltage positive electrode material is selected from at least one of nickel cobalt manganese positive electrode material, lithium cobalt oxide positive electrode material and lithium vanadium phosphate.
5. The positive electrode sheet slurry according to any one of claims 1 to 4, characterized in that: Calculated by mass percentage, it includes 88%-90% positive electrode active material, 3.5%-4.5% binder, 3.5%-4.5% conductive agent and 2.5%-3.5% solid electrolyte.
6. The positive electrode sheet slurry according to any one of claims 1 to 5, characterized in that: The binder is selected from at least one of polyvinylidene fluoride, polytetrafluoroethylene and styrene-butadiene rubber.
7. The positive electrode sheet slurry according to any one of claims 1 to 6, characterized in that: The conductive agent is selected from at least one of carbon nanotubes, Ketjen black, acetylene black, furnace black, carbon fiber and nanographite.
8. A method for preparing a positive electrode sheet, characterized in that: include: A positive electrode sheet slurry as described in any one of claims 1 to 7 is provided, and a positive electrode active coating is formed on a positive electrode current collector using the positive electrode sheet slurry.
9. The preparation method according to claim 8, characterized in that: include: The positive electrode sheet slurry is coated on the positive electrode current collector, and then dried and roll-pressed.
10. The preparation method according to claim 8 or 9, characterized in that: In the process of coating the positive electrode sheet slurry on the positive electrode current collector, the coating surface density is controlled to be 20 mg / cm 2 -30mg / cm 2 , ear areas are reserved on both sides.
11. The preparation method according to any one of claims 8 to 10, characterized in that: The positive electrode current collector is aluminum foil.
12. The preparation method according to any one of claims 9 to 11, characterized in that: The drying process includes: passing the coated electrode through an oven with a length of 18m-30m and a temperature of 100°C-120°C at a speed of 1m / s-5m / s.
13. The preparation method according to claim 9, characterized in that: During the rolling process, the compaction density was controlled to be 2.8 g / cm 3 -2.9g / cm 3 .
14. A positive electrode sheet, characterized in that: It is prepared by the preparation method described in any one of claims 8 to 13.
15. A lithium battery, characterized in that: Including the positive electrode sheet as described in claim 14.
16. The lithium battery according to claim 15, characterized in that: It also includes a negative electrode sheet, and the preparation process of the lithium battery includes: assembling the positive electrode sheet and the negative electrode sheet, and injecting liquid into them.
17. A battery module, characterized in that: Including the lithium battery of claim 15 or 16.
18. A battery pack, characterized in that: Comprising the lithium battery according to any one of claims 15-16 or the battery module according to claim 17.
19. An electrical device, characterized in that: It includes the lithium battery described in any one of claims 15-16, the battery module described in claim 17 or the battery pack described in claim 18.
Citation Information
Patent Citations
Positive electrode of lithium metal battery, lithium metal battery and preparation method of lithium metal battery
CN111834620A
Dual-composite modified spinel lithium manganate positive plate, preparation method thereof and lithium ion battery
CN113054157A
Positive pole piece containing solid electrolyte, and preparation method and application thereof
CN113707880A
Positive pole piece, secondary battery and electronic device
CN116111041A
Positive pole piece slurry, positive pole piece as well as preparation method and application of positive pole piece
CN117334833A
Cited By
Solid-state battery and preparation method thereof
CN120049005A