Photoelectric device and display apparatus

By using high reflectivity metal microspheres and high transmittance silicon microspheres in the packaging layer of the optoelectronic device, the disorder of scattered light paths and optical paths is solved, and the problem of limited viewing angle range of traditional optoelectronic devices is achieved. Wide viewing angle and more stable luminous performance.

WO2024245385A1PCT designated stage expired Publication Date: 2024-12-05TCL TECHNOLOGY GROUP CORPORATION
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/096572
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-05-31
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Traditional OLED and QLED optoelectronic devices have great limitations in the viewing angle range, resulting in a decrease in luminous efficiency and a large difference in chromatic aberration when the observation angle increases.

Method used

The first microsphere with a reflectivity greater than or equal to 90% and a second microsphere with a light transmittance greater than or equal to 90% are introduced into the encapsulation layer of the optoelectronic device, and the viewing angle is improved by increasing the scattered light path and the optical path disorder.

Benefits of technology

It effectively improves the viewing angle of optoelectronic devices, while maintaining good luminous efficiency and stability, and reducing the chromatic difference at different observation angles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024096572_05122024_PF_FP_ABST
    Figure CN2024096572_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present application are a photoelectric device and a display apparatus. The photoelectric device in the present application comprises a device main body and a packaging layer arranged on the device main body, wherein the packaging layer comprises a first microsphere and / or a second microsphere, the material reflectivity of the first microsphere is greater than or equal to 90%, and the material transmittance of the second microsphere is greater than or equal to 90%. A first microsphere and / or a second microsphere are / is doped in a packaging layer, such that the number of scattered light paths is increased, and the disorder of the light paths is improved, thereby improving a visual angle.
Need to check novelty before this filing date? Find Prior Art

Description

Photoelectric device and display device

[0001] This application claims the patent application number filed on June 2, 2023 with the China Patent Office

[0002] 202310653166.2, the priority of the Chinese patent application entitled “A Photoelectric Device and Display Device”, the entire content of which is incorporated into this application by reference. Technical Field

[0003] The present application relates to the field of display technology, and in particular to an optoelectronic device and a display apparatus. Background Art

[0004] Currently, widely used optoelectronic devices include organic light-emitting diodes (OLEDs) and quantum dot light-emitting diodes (QLEDs). The traditional OLED and QLED device structure primarily consists of an anode, a hole-functional layer, a light-emitting layer, an electron-functional layer, and a cathode. Under the influence of an electric field, holes generated by the anode and electrons generated by the cathode of the optoelectronic device migrate, injecting into the hole transport layer and electron transport layer, respectively, before ultimately migrating to the light-emitting layer. When the two interact in the light-emitting layer, they generate energy excitons, which in turn excite the light-emitting molecules, ultimately producing visible light.

[0005] Optoelectronic devices often employ strong microcavity structures, which can produce a microcavity effect, significantly improving their optical performance. Specifically, when the light-emitting region of an optoelectronic device is located within a resonant cavity formed by a total reflective membrane and a semi-reflective membrane, and the cavity length is on the same order of magnitude as the wavelength of the light, light of specific wavelengths is selected and enhanced, narrowing the spectrum. This is known as the microcavity effect.

[0006] However, while the microcavity effect brought about by the strong microcavity structure significantly improves the optical performance of optoelectronic devices, it also leads to a poor viewing angle range. Therefore, how to improve the viewing angle range is an important research and development direction. Technical Solutions

[0007] In view of this, the present application provides an optoelectronic device and a display apparatus, aiming to improve the viewing angle range.

[0008] An embodiment of the present application is implemented by providing an optoelectronic device, comprising a device body; and an encapsulation layer disposed on the device body; wherein the material of the encapsulation layer comprises first microspheres and / or second microspheres, the first microspheres having a reflectivity greater than or equal to 90% for visible light, and the second microspheres having a transmittance greater than or equal to 90% for visible light.

[0009] Optionally, in some embodiments of the present application, the first microspheres are microspheres made of metal reflective material.

[0010] Optionally, in some embodiments of the present application, the average particle size of the first microspheres is 0.03 to 500 μm; and / or the material of the metal reflective material microspheres is selected from one or more of silver, aluminum, gold, copper, and chromium; and / or the first microspheres are selected from elemental silver microspheres.

[0011] Optionally, in some embodiments of the present application, the volume percentage of the first microspheres in the encapsulation layer is greater than 0 and less than or equal to 3%. Preferably, the volume percentage of the first microspheres in the encapsulation layer is greater than 0 and less than or equal to 1%.

[0012] Optionally, in some embodiments of the present application, the volume percentage of the second microspheres in the encapsulation layer is greater than 0 and less than or equal to 30%. Preferably, the volume percentage of the second microspheres in the encapsulation layer is greater than 0 and less than or equal to 20%.

[0013] Optionally, in some embodiments of the present application, the second microspheres are selected from one or more of silicone microspheres, polystyrene microspheres, and polymethyl methacrylate microspheres; and / or the average particle size of the second microspheres is 1 to 3 μm.

[0014] Optionally, in some embodiments of the present application, the encapsulation layer further includes a mesoporous material.

[0015] Optionally, in some embodiments of the present application, the mesoporous material is selected from one or more of mesoporous silica, mesoporous zeolite, mesoporous carbon, nano-iron oxide, and mesoporous bioactive glass-polyurethane nanocomposite materials; and / or, the pore size of the mesopores in the mesoporous material can be 2 to 50 nm; and / or, the average particle size of the mesoporous material is 0.1 to 5 μm.

[0016] Optionally, in some embodiments of the present application, the volume percentage of the mesoporous material in the encapsulation layer is 5% to 10%. Preferably, the volume percentage of the mesoporous material in the encapsulation layer is 7% to 10%.

[0017] Optionally, in some embodiments of the present application, the encapsulation layer includes a main material, and the main material is selected from one or more of epoxy resin, polyimide, benzocyclobutene resin, and bismaleimide triazine resin.

[0018] Optionally, in some embodiments of the present application, the encapsulation layer includes a first surface and a second surface arranged opposite to each other, the first surface is close to the device body, the second surface is far away from the device body, and the second surface is a convex surface.

[0019] Optionally, in some embodiments of the present application, the encapsulation layer is composed of the main material, the first microspheres, and the second microspheres.

[0020] Optionally, in some embodiments of the present application, the encapsulation layer is composed of the main material, the first microspheres, the second microspheres and a mesoporous material.

[0021] Optionally, in some embodiments of the present application, the optoelectronic device further includes a protective layer, and the protective layer is disposed on a side of the encapsulation layer away from the device body.

[0022] Optionally, in some embodiments of the present application, the material of the protective layer includes one or more of epoxy resin, polyimide, benzocyclobutene resin, and bismaleimide triazine resin.

[0023] Optionally, in some embodiments of the present application, the device body includes: a first electrode and a second electrode arranged opposite to each other, the first electrode or the second electrode is arranged close to the packaging layer; and an electronic functional layer is arranged between the first electrode and the second electrode.

[0024] Optionally, in some embodiments of the present application, the electronic functional layer includes at least two stacked sub-electronic functional layers; and / or, the material of the electronic functional layer includes inorganic particles, and the shape of the inorganic particles includes one or more of spherical and polyhedral shapes.

[0025] Optionally, in some embodiments of the present application, the average particle size of the inorganic particles is 3 to 6 nm; and / or the inorganic particles are selected from doped or undoped inorganic nanocrystals; wherein the undoped inorganic nanocrystals are selected from one or more of ZnO, TiO2, SnO2, Ta2O3, ZrO2, NiO, Al2O3, GaO, Ga2O3, ZnS, ZnSe, CdS, InP, GaP, BaTiO3, Cs2CO3, Rb2CO3, RbBr, LiF, LiF / Yb, MgP, and MgF2; the doped inorganic nanocrystals include the undoped inorganic nanocrystals and doping elements, and the doping elements are selected from one or more of Mg, Ca, Li, Ga, Al, Co, Mn, Zr, W, Ti, and Y.

[0026] Optionally, in some embodiments of the present application, the device body further includes a light-emitting layer, and the light-emitting layer is disposed between the first electrode and the electronic functional layer, or between the second electrode and the electronic functional layer; wherein the material of the light-emitting layer is selected from one or more of an organic light-emitting material and a quantum dot, wherein the organic light-emitting material is selected from one or more of a diarylanthracene derivative, a distyryl aromatic derivative, a pyrene derivative or a fluorene derivative, a blue-emitting TBPe fluorescent material, a green-emitting TTPA fluorescent material, an orange-emitting TBRb fluorescent material, and a red-emitting DBP fluorescent material;The quantum dots are selected from one or more of single-structure quantum dots, core-shell structure quantum dots and perovskite semiconductor materials. The single-structure quantum dots are selected from one or more of II-VI compounds, IV-VI compounds, III-V compounds and I-III-VI compounds. The II-VI compounds are selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHg One or more of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, SnPbSTe, and the II Group I-V compounds are selected from GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, In NP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAl One or more of NSb, InAlPAs and InAlPSb, the I-III-VI group compound is selected from one or more of CuInS, CuInSe and AgInS; the core of the core-shell structured quantum dots is selected from any one of the above-mentioned single-structure quantum dots, and the shell material of the core-shell structured quantum dots is selected from one or more of CdS, CdTe, CdSeTe, CdZnSe, CdZnS, CdSeS, ZnSe, ZnSeS and ZnS; the perovskite semiconductor material is selected from doped or undoped inorganic perovskite semiconductors, or organic-inorganic hybrid perovskite semiconductors; the general structural formula of the inorganic perovskite semiconductor is AMX3, wherein A is Cs; +ion, M is a divalent metal cation selected from Pb 2+ 、Sn 2+ 、Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ 、Mn 2+ 、Co 2+ 、Fe 2+ 、Ge 2+ 、Yb 2+ 、Eu 2+ One or more of, X is a halogen anion selected from Cl - Br - , I - One or more of the following; the general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX3, wherein B is an organic amine cation selected from CH3(CH2) n-2 NH3 + or [NH3(CH2) n NH3] 2+ , where n≥2, M is a divalent metal cation selected from Pb 2+ 、Sn 2+ 、Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ 、Mn 2+ 、Co 2+ 、Fe 2+ 、Ge 2+ 、Yb 2+ 、Eu 2+ One or more of, X is a halogen anion selected from Cl - Br - , I - One or more of; and / or

[0027] The first electrode and the second electrode are independently selected from metal electrodes, carbon electrodes, doped or undoped metal oxide electrodes and composite electrodes; wherein the material of the metal electrode is selected from one or more of Al, Ag, Cu, Mo, Au, Ba, Ca and Mg; the material of the carbon electrode is selected from one or more of graphite, carbon nanotubes, graphene and carbon fiber; the material of the doped or undoped metal oxide electrode is selected from one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO and AMO; the material of the composite electrode is selected from one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS and ZnS / Al / ZnS.

[0028] Correspondingly, an embodiment of the present application further provides a display device, which includes the above-mentioned optoelectronic device.

[0029] The optoelectronic device of the present application includes a device body and an encapsulation layer arranged on the device body, the encapsulation layer includes first microspheres and / or second microspheres, the material reflectivity of the first microspheres is greater than or equal to 90%, and the material transmittance of the second microspheres is greater than or equal to 90%. By adding first microspheres with a reflectivity greater than or equal to 90% and / or second microspheres with a transmittance greater than or equal to 90% into the encapsulation layer, the number of scattered light paths is increased and the disorder of the light paths is increased, thereby improving the viewing angle. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0031] FIG1 is a schematic structural diagram of an embodiment of a photoelectric device provided by the present application;

[0032] FIG2 is a schematic structural diagram of another embodiment of a photoelectric device provided by the present application;

[0033] FIG3 is a schematic diagram of an optoelectronic device at various viewing angles.

[0034] Implementation Methods of the Application

[0035] The following will clearly and completely describe the technical solutions in the embodiments of the present application in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application and are not used to limit the present application. In the present application, unless otherwise specified, the directional words used, such as "upper" and "lower", specifically refer to the directions of the drawings in the accompanying drawings. In addition, in the description of the present application, the term "including" means "including but not limited to". Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a rigid limitation on the scope of the present invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, description of a range from 1 to 6 should be considered to have specifically disclosed subranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as individual numbers within that range, such as 1, 2, 3, 4, 5, and 6. Furthermore, whenever a numerical range is indicated herein, it is meant to include any cited numeral (fractional or integral) within the indicated range.

[0036] In this application, "and / or" describes the association relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0037] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.

[0038] In the field of display technology, the viewing angle is also called the viewing angle range. It is based on the vertical normal of the display screen. When the vertical normal is deflected to the left or right by a certain angle, the displayed image can still be seen normally. This angle range is the horizontal viewing angle of the display panel. Generally speaking, the measurement of the viewing angle is based on the contrast change. When the observation angle increases, the contrast of the displayed image seen at this position will decrease. In optoelectronic devices such as QLED and OLED, this manifests as a large change in luminous efficiency. Furthermore, in display devices including optoelectronic devices, such as display panels, there will also be large differences in color difference at different observation angles.

[0039] Based on this, the present application provides an optoelectronic device and a display apparatus to improve the viewing angle range, as described below.

[0040] This application provides an optoelectronic device. Refer to Figure 1, which is a schematic structural diagram of one embodiment of the optoelectronic device provided herein. The optoelectronic device 100 includes a device body 10 and an encapsulation layer 20 disposed on the device body 10. The encapsulation layer 20 includes first microspheres 21 and / or second microspheres 22. The first microspheres 21 are made of a reflective material with a reflectivity greater than or equal to 90% for visible light, and the second microspheres 22 have a transmittance greater than or equal to 90% for visible light. Specifically, visible light refers to light with a wavelength range of 390 to 760 nanometers.

[0041] In this embodiment, the encapsulation layer 20 is doped with first microspheres 21 and / or second microspheres 22, which increases the number of scattered light paths and the disorder of the light paths, thereby improving the viewing angle. On the one hand, the presence of the microsphere structure in the encapsulation layer 20 creates more contact interfaces, increasing the number of scattered light paths and improving the disorder of the light paths. On the other hand, the first microspheres 21 and second microspheres 22 can respectively reflect and transmit light, and the different refractive indices of different materials can scatter light paths, which also increases the number of scattered light paths and improves the disorder of the light paths.

[0042] In this embodiment, the reflective material may also be referred to as a retro-reflective material or a reverse-reflective material.

[0043] In one embodiment, the material of the first microspheres 21 is selected from metal reflective materials, specifically one or more of silver, aluminum, gold, copper, and chromium.

[0044] Furthermore, the average particle size of the first microspheres 21 can be 0.03-500 μm, such as 0.03-0.1 μm, 0.1-1 μm, 1-20 μm, 20-50 μm, 50-100 μm, 100-200 μm, 200-500 μm, etc.

[0045] In a specific embodiment, the first microspheres 21 are selected from elemental silver microspheres, which have good stability.

[0046] In one embodiment, the volume percentage of the first microspheres 21 in the encapsulation layer is denoted by A1, where A1 is greater than 0 and less than or equal to 3%, i.e., 0<A1≤3%. Specifically, A1 can be: 0<A1≤1%, 1≤A1≤2%, 2≤A1≤3%, etc. Further, in one embodiment, 0<A1≤1%, specifically, 0<A1≤0.01%, 0.01≤A1≤0.1%, 0.1≤A1≤0.5%, 0.5≤A1≤1%, etc. The incorporation ratio of the first microspheres 21 is within the above range, which improves the viewing angle of the optoelectronic device 100 while enabling the optoelectronic device 100 to have better luminous efficiency.

[0047] In one embodiment, the second microspheres 22 are selected from one or more of silicone microspheres, polystyrene microspheres, and polymethyl methacrylate microspheres. The second microspheres 22 made of the above materials have a high light transmittance. When incorporated into the encapsulation layer 20, the second microspheres 22 can scatter light paths through different materials with different refractive indices, thereby increasing the number and disorder of light paths.

[0048] In one embodiment, the volume percentage of the second microspheres 22 in the encapsulation layer is denoted by A2, where A2 is greater than 0 and less than or equal to 30%, i.e., 0 < A2 ≤ 30%. Specifically, 0 < A2 ≤ 20%, 10 ≤ A2 ≤ 30%, 10 ≤ A2 ≤ 20%, etc. Further, in one embodiment, 0 < A2 ≤ 20%, specifically, A2 can be: 0 < A2 ≤ 0.01%, 0.01 ≤ A2 ≤ 0.1%, 0.1 ≤ A2 ≤ 0.5%, 0.5 ≤ A2 ≤ 1%, 1 ≤ A2 ≤ 5%, 5 ≤ A2 ≤ 10%, 10 ≤ A2 ≤ 20%, etc. The incorporation ratio of the second microspheres 22 within the above range improves the viewing angle of the optoelectronic device 100 while enabling the optoelectronic device 100 to have better luminous efficiency.

[0049] In one embodiment, the average particle size of the second microspheres is 1-3 μm, specifically 1-2.8 μm, 1.3-2.8 μm, 1.3-2.5 μm, 1.5-2.5 μm, 1.5-2.3 μm, 1.8-2.3 μm, 1.8-2.0 μm, etc.

[0050] In one embodiment, the encapsulation layer includes a host material selected from one or more of epoxy resin, polyimide (PI), benzocyclobutene resin (BCB), and bismaleimide triazine resin (BT). In this embodiment, the encapsulation layer 20 has excellent water and oxygen barrier properties, preventing water and oxygen from penetrating the encapsulation layer 20 and corroding the device body 10, thereby improving the luminous stability and lifespan of the optoelectronic device 100.

[0051] In one embodiment, the encapsulation layer 20 is composed of the host material, the first microspheres 21 and the second microspheres 22. In other embodiments, the encapsulation layer may further include other materials, such as mesoporous materials.

[0052] In one embodiment, the encapsulation layer further comprises a mesoporous material, wherein the mesoporous material can be selected from one or more of mesoporous silica, mesoporous zeolite, mesoporous carbon, nano-iron oxide, and a mesoporous bioactive glass-polyurethane nanocomposite. The mesoporous bioactive glass-polyurethane nanocomposite is a composite material formed by mesoporous bioactive glass (MBG) and polyurethane (PU).

[0053] The mesoporous material has a porous structure and good strength, which can improve the mechanical properties and film stability of the encapsulation layer 20 and avoid the influence of the viewing angle improvement process on the film stability.

[0054] Specifically, in one embodiment, the pore diameter of the mesopores in the mesoporous material may be 2-50 nm, specifically 2-40 nm, 10-40 nm, 10-30 nm, 20-30 nm, etc.

[0055] In one embodiment, the average particle size of the mesoporous material may be 0.1-5 μm, specifically 0.1-4.5 μm, 1-4.5 μm, 1-4 μm, 1.5-4 μm, 1.5-3.5 μm, 2-3.5 μm, 2.0-3.0 μm, 2.5-3.5 μm, 2.5-3.0 μm, etc.

[0056] In one embodiment, the volume percentage of the mesoporous material in the encapsulation layer is 5% to 10%, specifically 5% to 9%, 6% to 9%, 6% to 8%, 7% to 8%, 5% to 7%, 7% to 10%, etc. The mesoporous material doping ratio described above can improve the strength and film stability of the encapsulation layer 20, and the encapsulation layer 20 can also have good water and oxygen isolation properties.

[0057] In one embodiment, referring to Figure 2, Figure 2 is a schematic structural diagram of another embodiment of a photovoltaic device provided herein. The encapsulation layer 20 in the photovoltaic device 100 includes a first surface 201 and a second surface 202 disposed opposite each other. The first surface 201 is adjacent to the device body 10, while the second surface 202 is distal from the device body 10. The second surface 202 is convex. That is, when a section is made at any point on the second surface 202, the second surface 202 is always below or partially overlaps with the section.

[0058] It can be understood that in this embodiment, the second surface 202 is a light emitting surface, which is a convex surface (non-planar), which will change the light path and increase the number of scattered light paths and the disorder of the light paths.

[0059] In this embodiment, the thickness of the encapsulation layer 20 decreases as it diffuses from the center outward, that is, it presents a convex lens-like structure with a thicker center area and a slightly thinner edge, thereby improving the scattering and refraction of the light path.

[0060] The point on the second surface 202 with the greatest vertical distance from the first surface 201 is denoted by B, and the point on the second surface 202 with the smallest vertical distance from the first surface 201 is denoted by C. The angle α formed by the line connecting the two, BC, and the first surface 201 is less than or equal to 2°. In other words, the angle formed by the line connecting the thickest and thinnest points of the encapsulation layer 20 and the first surface 201 is less than or equal to 2°. An angle α of less than or equal to 2° can change the optical path without causing significant light dispersion or focusing.

[0061] In one embodiment, the optoelectronic device 100 further includes a protective layer 30, which is disposed on a side of the encapsulation layer 20 away from the device body 10. The material of the protective layer 30 includes one or more of epoxy resin, polyimide, benzocyclobutene resin, and bismaleimide triazine resin. The protective layer 30 can further improve the encapsulation effect.

[0062] It is understandable that the material of the protection layer 30 may be the same as or different from the main material of the encapsulation layer 20 .

[0063] In one embodiment, the material of the protection layer 30 is different from the main material of the encapsulation layer 20 , which can further improve light scattering.

[0064] In one embodiment, referring to FIG1 , the device body 10 includes a first electrode 11, a second electrode 12, a light-emitting layer 13, and an electronic functional layer 14. The first electrode 11 and the second electrode 12 are disposed opposite each other, with the second electrode 12 or the first electrode 11 disposed near the encapsulation layer 20; the light-emitting layer 13 is disposed between the first electrode 11 and the second electrode 12; and the electronic functional layer 14 is disposed between the light-emitting layer 13 and the second electrode 12.

[0065] In one embodiment, the second electrode 12 is disposed adjacent to the encapsulation layer 20. In this embodiment, the electronic functional layer 14 is located on the light-emitting side of the light-emitting layer 13, that is, light emitted by the light-emitting layer 13 is emitted outside the optoelectronic device 100 through the electronic functional layer 14, the first electrode 11, and other film layers.

[0066] In one embodiment, the electronic functional layer 14 includes inorganic particles 141 , and the shape of the inorganic particles 141 includes one or more of spherical and polyhedral shapes, wherein the polyhedral shape includes one or more of tetrahedron, hexagonal, octahedron, etc.

[0067] In one embodiment, the shapes of the inorganic particles 141 include at least two of polyhedrons such as sphere, tetrahedron, hexagon, octahedron, etc., that is, the inorganic particles 141 include a mixture of at least two different shapes.

[0068] In the above two embodiments, since the inorganic particles 141 have multiple interfaces, they can change the refraction and transmission of light, that is, increase the disorder of the light path and the number of light paths in the electronic functional layer 14 .

[0069] In one embodiment, the inorganic particles 141 are in a lattice shape or a crystal shape.

[0070] In one embodiment, the inorganic particles 141 are selected from doped or undoped inorganic nanocrystals; wherein the undoped inorganic nanocrystals are selected from one or more of ZnO, TiO2, SnO2, Ta2O3, ZrO2, NiO, Al2O3, GaO, Ga2O3, ZnS, ZnSe, CdS, InP, GaP, BaTiO3, Cs2CO3, Rb2CO3, RbBr, LiF, LiF / Yb, MgP, and MgF2; the doped inorganic nanocrystals include the undoped inorganic nanocrystals and doping elements, and the doping elements are selected from one or more of Mg, Ca, Li, Ga, Al, Co, Mn, Zr, W, Ti, and Y.

[0071] In one embodiment, the inorganic particles 141 are selected from ZnO with different lattices, such as tetragonal ZnO and hexagonal ZnO.

[0072] In one embodiment, the average particle size of the inorganic particles 141 is 3 to 6 nm, specifically 3 to 5 nm, 4 to 5 nm, 3 to 4 nm, 5 to 6 nm, etc. The inorganic particles 141 having this average particle size can support the formation of the electronic functional layer 14 having a predetermined thickness, while improving the optical performance without affecting the electrical performance.

[0073] In one embodiment, the thickness of the electronic functional layer 14 may be 20-50 nm, specifically 20-45 nm, 25-45 nm, 25-40 nm, 30-40 nm, 30-35 nm, etc.

[0074] In one embodiment, the electronic functional layer 14 may include at least two stacked sub-electronic functional layers (not shown). The multi-layer sub-electronic functional layers increase the number of contact interfaces, and the multi-layer sub-electronic functional layers may have different degrees of mutual dissolution of the film layers during the preparation process, resulting in changes in the smoothness of the interfaces, which can further scatter the light path.

[0075] Specifically, the optoelectronic device 100 further includes a substrate (not shown), which is disposed on a side of the first electrode 11 away from the encapsulation layer 20. The substrate can be a rigid substrate or a flexible substrate. The rigid substrate can be made of a ceramic material or various glass materials. The flexible substrate can be formed of a material such as polyimide film (PI) and its derivatives, polyethylene naphthalate (PEN), phosphoenolpyruvic acid (PEP), or diphenylene ether resin.

[0076] In one embodiment, the material of the light-emitting layer 13 is selected from organic light-emitting materials or quantum dot light-emitting materials.

[0077] The organic light-emitting material is selected from one or more of diaromatic anthracene derivatives, distyryl aromatic derivatives, pyrene derivatives or fluorene derivatives, TBPe fluorescent materials that emit blue light, TTPA fluorescent materials that emit green light, TBRb fluorescent materials that emit orange light, and DBP fluorescent materials that emit red light.

[0078] The quantum dots are selected from one or more of single-structure quantum dots, core-shell structure quantum dots and perovskite semiconductor materials. The single-structure quantum dots are selected from one or more of II-VI compounds, IV-VI compounds, III-V compounds and I-III-VI compounds. The II-VI compounds are selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe , one or more of CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, and the IV-VI group compound is selected from SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, One or more of SnPbSSe, SnPbSeTe, and SnPbSTe, wherein the III-V compound is selected from GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaIn One or more of NP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPSb, the I-III-VI group compound is selected from one or more of CuInS2, CuInSe2 and AgInS2; the core of the quantum dots of the core-shell structure is selected from any one of the above-mentioned single-structure quantum dots, and the shell material of the quantum dots of the core-shell structure is selected from one or more of CdS, CdTe, CdSeTe, CdZnSe, CdZnS, CdSeS, ZnSe, ZnSeS and ZnS.

[0079] The perovskite semiconductor material is selected from doped or undoped inorganic perovskite semiconductors, or organic-inorganic hybrid perovskite semiconductors; the inorganic perovskite semiconductor has the general structural formula AMX3, wherein A is Cs + ion, M is a divalent metal cation selected from Pb 2+ 、Sn 2+ 、Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ 、Mn 2+ 、Co 2+ 、Fe 2+ 、Ge 2+ 、Yb 2+ 、Eu 2+ One or more of, X is a halogen anion selected from Cl - Br - , I - One or more of the following; the general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX3, wherein B is an organic amine cation selected from CH3(CH2) n-2 NH3 + or [NH3(CH2) n NH3] 2+ , where n≥2, M is a divalent metal cation selected from Pb 2+ 、Sn 2+ 、Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ 、Mn 2+ 、Co 2+ 、Fe 2+ 、Ge 2+ 、Yb 2+ 、Eu 2+ One or more of, X is a halogen anion selected from Cl - Br - , I - One or more of .

[0080] When n=2, the inorganic metal halide octahedron MX6 4- The metal cation M is located at the center of the halogen octahedron, and the organic amine cation B fills the gaps between the octahedrons to form an infinitely extended three-dimensional structure. When n>2, the inorganic metal halide octahedron MX6 connected in a top-sharing manner 4- It extends in two dimensions to form a layered structure, with an organic amine cation bilayer (protonated monoamine) or an organic amine cation monolayer (protonated diamine) inserted between the layers, and the organic layer and the inorganic layer overlap to form a stable two-dimensional layered structure.

[0081] In one embodiment, the thickness of the light emitting layer 13 may be 30-50 nm, specifically 30-40 nm, 40-50 nm, etc.

[0082] The device body 10 further includes a hole functional layer 15, which is disposed between the first electrode 11 and the light-emitting layer 13. The hole functional layer 15 includes at least one of a hole injection layer (not shown) and a hole transport layer (not shown). The hole injection layer is disposed near the first electrode 11.

[0083] The material of the hole transport layer can be selected from organic materials with hole transport ability, and the material of the hole transport layer includes arylamine, polyaniline, polypyrrole, polyphenylene vinylene and its derivatives, 4,4'-bis(p-carbazolyl)-1,1'-biphenyl compound, N,N,N',N'-tetraarylbenzidine, PEDOT:PSS and its derivatives, poly(N-vinylcarbazole) and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, doped or undoped NiO, M One or more of oO3, WO3, V2O5, CrO3, CuO, MoS2, MoSe2, WS3, WSe3, CuS, and CuSCN; wherein the arylamine is selected from 4,4'-bis(9-carbazole)biphenyl, poly(9,9-dioctylfluorene-CO-N-(4-butylphenyl)diphenylamine), poly(N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)benzidine), N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine, poly(9,9- dioctylfluorene-co-bis-N,N-phenyl-1,4-phenylenediamine), 4,4',4"-tris(carbazol-9-yl)triphenylamine, 4,4',4"-tris(N-carbazolyl)-triphenylamine, 4,4',4"-tris(N-3-methylphenyl-N-phenylamino)triphenylamine, N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4"-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-1,1'-biphenyl-4,4'-diamine, N,N'-diphenyl-N,N'- One or more of (1-naphthyl)-1,1'-biphenyl-4,4'-diamine, Spiro-NPB, Spiro-TPD, N,N'-bis(3-methylphenyl)-N,N'-bis(phenyl)-spiro, and Spiro-NPB; the polyphenylene vinylene and its derivatives are selected from one or more of poly(phenylene vinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylene vinylene] and poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylene vinylene].

[0084] In one embodiment, the thickness of the hole transport layer may be 50-100 nm, such as 50-60 nm, 60-80 nm, 80-100 nm, etc.

[0085] The hole injection layer can be made of a material having hole injection capability, including but not limited to one or more of PEDOT:PSS, MCC, CuPc, F4-TCNQ, HATCN, doped or undoped NiO, V2O5, CrO3, CuO, CuS, MoO3, MoS2, MoSe2, WO3, WS2, WSe2, and CuSCN. PEDOT:PSS is a high molecular weight polymer, also known as poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) in Chinese.

[0086] In one embodiment, the thickness of the hole injection layer may be 50-100 nm, such as 50-60 nm, 60-80 nm, 80-100 nm, etc.

[0087] In one embodiment, the first electrode 11 and the second electrode 12 are independently selected from metal electrodes, carbon electrodes, doped or undoped metal oxide electrodes and composite electrodes; wherein the material of the metal electrode is selected from one or more of Al, Ag, Cu, Mo, Au, Ba, Ca and Mg; the material of the carbon electrode is selected from one or more of graphite, carbon nanotubes, graphene and carbon fibers; the material of the doped or undoped metal oxide electrode is selected from one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO and AMO; the material of the composite electrode is selected from one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS and ZnS / Al / ZnS. Wherein, " / " indicates a stacked structure. For example, a composite electrode AZO / Ag / AZO represents an electrode having a three-layer stacked structure consisting of an AZO layer, an Ag layer, and an AZO layer. The thickness of the first electrode 11 and the second electrode 12 are each independently 50 to 110 nm, such as 50 to 80 nm, 80 to 100 nm, 100 to 110 nm, 30 to 60 nm, 30 to 40 nm, 40 to 50 nm, or 50 to 60 nm.

[0088] In one embodiment, the optoelectronic device is a top-emitting device, and the second electrode 12 is a top electrode having a visible light transmittance of greater than or equal to 90%. The top electrode is located on the light-emitting side of the optoelectronic device and has a visible light transmittance of greater than or equal to 90%, thereby improving the light transmittance of the optoelectronic device 100 and enhancing luminous properties such as brightness.

[0089] In a specific embodiment, when the top electrode is the metal electrode or the composite electrode, the thickness of the metal electrode should not exceed 35 nm. In the composite electrode, the thickness of the metal layer sandwiched between the two transparent metal oxide layers should not exceed 35 nm, thereby improving the transparency and light transmittance of the top electrode.

[0090] It is understood that, in addition to the above-mentioned functional layers, the optoelectronic device 100 may further include some functional layers conventionally used in optoelectronic devices that help improve the performance of the optoelectronic device, such as an electron blocking layer, a hole blocking layer, etc.

[0091] It can be understood that the material and thickness of each layer of the optoelectronic device 100 can be set and adjusted accordingly according to the light emitting requirements of the optoelectronic device 100 .

[0092] It is understood that the various film layers in the device body 10 of the optoelectronic device 100 provided in the present application, including the first electrode 11, the second electrode 12, the light-emitting layer 13, the electronic functional layer 14, the hole functional layer 15 and other film layers, can be prepared using conventional techniques in the art, such as chemical methods or physical methods. Among them, chemical methods include chemical vapor deposition, continuous ion layer adsorption and reaction, anodic oxidation, electrolytic deposition, and co-precipitation. Physical methods include physical plating and solution methods, among which physical plating methods include thermal evaporation, electron beam evaporation, magnetron sputtering, multi-arc ion plating, physical vapor deposition, atomic layer deposition, pulsed laser deposition, etc.; solution methods can be spin coating, printing, inkjet printing, doctor blade coating, printing, dip coating, immersion, spraying, roller coating, casting, slit coating, and strip coating, etc.

[0093] It is understood that the encapsulation layer 20 can be encapsulated by a method known in the art. The encapsulation can be machine encapsulation or manual encapsulation. The concentration of oxygen and water in the environment during the encapsulation step is less than 0.1 ppm to ensure the stability of the optoelectronic device.

[0094] The present application also relates to a display device, which includes the optoelectronic device provided by the present application. The optoelectronic device provided by the present application can improve the viewing angle. The display device including the optoelectronic device can improve the situation where the color difference of the display device is large at different viewing angles and reduce the color difference at different viewing angles. The display device can be any electronic product with a display function, and the electronic products include but are not limited to smart phones, tablet computers, laptops, digital cameras, digital video cameras, smart wearable devices, smart weighing electronic scales, car displays, televisions or e-book readers, wherein the smart wearable device can be, for example, a smart bracelet, a smart watch, a virtual reality (VR) helmet, etc.

[0095] The present application will be described in detail below through specific examples. The following examples are only some examples of the present application and are not limitations of the present application.

[0096] Example 1

[0097] This embodiment 1 provides a quantum dot light emitting diode and a preparation method thereof. The quantum dot light emitting diode has a positive top emission structure, and the preparation method specifically includes the following steps.

[0098] Step 1: Spin-coat PEDOT:PSS material onto an ITO substrate (the thickness of the ITO layer is 50 nm) at a spin-coating speed of 5000 rpm for 30 seconds, followed by heating at 150°C for 15 minutes to obtain a 50 nm thick hole injection layer.

[0099] Step 2: Spin-coat 8 mg / mL TFB material onto the hole injection layer at a spin speed of 3000 rpm for 30 seconds, followed by heating at 120°C for 10 minutes to obtain a hole transport layer with a thickness of 30 nm.

[0100] Step 3: Spin-coat the hole transport layer with a concentration of 20 mg / ml of CdZnSe quantum material at a spin-coating speed of 2000 rpm for 30 seconds, and then heat on an 80°C hot plate for 10 minutes to obtain a light-emitting layer with a thickness of 20 nm.

[0101] Step 4: Tetragonal ZnO (30 mg / mL) and hexagonal ZnO (30 mg / mL) were mixed in a ratio of 1:1 and then spin-coated onto the light-emitting layer at a speed of 2000 rpm for 30 s. -2 MPa environment for 15 min to obtain an electron transport layer with a thickness of 30 nm;

[0102] Step 5: By thermal evaporation, the vacuum degree is not higher than 3x10 -4Pa, evaporating Ag on the light-emitting layer at a rate of 1 angstrom / second for 200 seconds to obtain a cathode with a thickness of 20 nm;

[0103] Step 6: First and second microspheres are added to the epoxy resin. The first microspheres are elemental silver microspheres, and the second microspheres are organosilicon microspheres. The organosilicon microspheres have an average particle size of 2 microns and a volume percentage of 15%. The elemental silver microspheres have a porous, hollow structure with a diameter of 200 microns and a surface composed of 30-80 nm spherical silver nanoparticles. The volume percentage of the silver microspheres is 0.5%. The device is encapsulated with this epoxy resin.

[0104] Example 2

[0105] This embodiment is substantially the same as embodiment 1, with the only difference being that in step 6, the volume percentage of the organosilicon microspheres is 20%.

[0106] Example 3

[0107] This embodiment is substantially the same as embodiment 1, with the only difference being that in step 6, the volume percentage of the organosilicon microspheres is 30%.

[0108] Example 4

[0109] This embodiment is substantially the same as embodiment 1, with the only difference being that in step 6, the volume percentage of elemental silver microspheres is 1%.

[0110] Example 5

[0111] This embodiment is substantially the same as embodiment 1, with the only difference being that in step 6, the volume percentage of elemental silver microspheres is 3%.

[0112] Example 6

[0113] This embodiment is substantially the same as embodiment 1, with the only difference being that in step 6, the second microspheres are polystyrene microspheres instead of silicone microspheres.

[0114] Example 7

[0115] This embodiment is substantially the same as embodiment 1, with the only difference being that in step 6, in addition to the first microspheres and the second microspheres, mesoporous silica is also added to the epoxy resin, and the volume percentage of the mesoporous silica is 7%.

[0116] Example 8

[0117] This embodiment is substantially the same as the embodiment 1, with the only difference being that in step 6, in addition to the first microspheres and the second microspheres, mesoporous silica is also added to the epoxy resin, and the volume percentage of the mesoporous silica is 5%.

[0118] Example 9

[0119] This embodiment is substantially the same as embodiment 1, with the only difference being that in step 6, in addition to the first microspheres and the second microspheres, mesoporous silica is also added to the epoxy resin, and the volume percentage of the mesoporous silica is 10%.

[0120] Example 10

[0121] This embodiment is basically the same as the embodiment 1, with the only difference being that in step 6, a packaging layer with a convex structure is formed. Referring to FIG2 , the angle α between the thickest part and the thinnest part of the packaging layer is 2°, and then an epoxy resin is used to form a protective layer on the packaging layer.

[0122] Example 11

[0123] This embodiment is basically the same as embodiment 7, with the only difference being that in step 6, a packaging layer with a convex structure is formed. Referring to FIG2 , the angle α between the thickest part and the thinnest part of the packaging layer is 2°, and then an epoxy resin is used to form a protective layer on the packaging layer.

[0124] Example 12

[0125] This embodiment is substantially the same as embodiment 1, with the only difference being that only tetragonal ZnO is used in step 4.

[0126] Example 13

[0127] This embodiment is basically the same as embodiment 1, with the only difference being that only the first microspheres are incorporated in step 6.

[0128] Example 14

[0129] This embodiment is basically the same as embodiment 1, with the only difference being that only the second microspheres are incorporated in step 6.

[0130] Comparative Example 1

[0131] This embodiment is substantially the same as the embodiment 1, with the only difference being that in step 4, conventional ZnO is spin-coated to form an electron transport layer, and in step 6, an epoxy resin is used to form an encapsulation layer.

[0132] Test 1

[0133] The quantum dot light-emitting diodes of Examples 1-14 and Comparative Example 1 were subjected to CE tests at various viewing angles, as well as the yield rate of 200-300 samples corresponding to each Example and Comparative Example. The results are shown in Table 1. Referring to Figure 3, Figure 3 is a schematic diagram of the optoelectronic device at various viewing angles. With the normal to the light-emitting surface of the optoelectronic device 100 at 0°, the angles were varied leftward and rightward, corresponding to viewing angles of 60°, 30°, 0°, -30°, and -60°, respectively.

[0134] CE@1knit is the current efficiency of the quantum dot LED at a brightness of 1knit, reflecting the device's luminous efficiency. After driving the quantum dot LEDs of Examples 1-8 and Comparative Example 1, a large number of samples corresponding to each example and comparative example were driven at different currents (0.01mA to 2mA). Devices that illuminated normally were considered good, while devices exhibiting leakage, short circuits, or other abnormalities were considered abnormal. The yield rate was thus calculated.

[0135] Test 2

[0136] After the quantum dot LEDs of Examples 1-10 and Comparative Example 1 were stored for ten days, a lifetime T95@1knit test was performed. The results are shown in Table 1. T95@1knit is the time it takes for the device's brightness to decay from 100% to 95% at a brightness of 1000 nits, calculated from the measured lifetime.

[0137] Table 1

[0138] As shown in Table 1, the luminous efficiency of the optoelectronic device of Comparative Example 1 changes significantly with increasing viewing angle. For example, as the viewing angle increases from -60° to 0°, the luminous efficiency changes from 60.51 cd / A to 248.69 cd / A, an increase of approximately 3 times. In contrast, the optoelectronic devices of Examples 1-14 show a significantly reduced variation in luminous efficiency with increasing viewing angle, thus improving the viewing angle. This can also improve display devices including the optoelectronic devices provided herein, such as display panels, which exhibit significant color differences at different viewing angles.

[0139] The optoelectronic devices of Examples 1-14 not only improve the viewing angle but also have good luminous efficiency, yield rate and lifespan. It also shows that the optoelectronic devices provided in this application have an improved packaging layer, which not only improves the viewing angle but also has good packaging performance and can still provide a stable water-oxygen-isolated environment to give the optoelectronic devices a good lifespan.

[0140] The above is a detailed introduction to the optoelectronic devices and display devices provided in the embodiments of the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for those skilled in the art, based on the ideas of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A photoelectric device, wherein: include: Device body; A packaging layer, disposed on the device body; The material of the encapsulation layer includes first microspheres and / or second microspheres, the reflectivity of the first microspheres to visible light is greater than or equal to 90%, and the transmittance of the second microspheres to visible light is greater than or equal to 90%.

2. The optoelectronic device according to claim 1, wherein The first microspheres are microspheres made of metal reflective material.

3. The optoelectronic device according to claim 2, wherein: The material of the metal reflective material microspheres is selected from one or more of silver, aluminum, gold, copper, and chromium; and / or The first microsphere is selected from elemental silver microspheres; and / or The average particle size of the first microspheres is 0.03-500 μm.

4. The optoelectronic device according to claim 1, wherein The volume percentage of the first microspheres in the encapsulation layer is greater than 0 and less than or equal to 3%. Preferably, the volume percentage of the first microspheres in the encapsulation layer is greater than 0 and less than or equal to 1%.

5. The optoelectronic device according to claim 1, wherein The volume percentage of the second microspheres in the encapsulation layer is greater than 0 and less than or equal to 30%. Preferably, the volume percentage of the second microspheres in the encapsulation layer is greater than 0 and less than or equal to 20%.

6. The optoelectronic device according to claim 1, wherein: The second microspheres are selected from one or more of silicone microspheres, polystyrene microspheres, and polymethyl methacrylate microspheres; and / or, The average particle size of the second microspheres is 1 to 3 μm.

7. The optoelectronic device according to claim 1, wherein: The encapsulation layer also includes mesoporous material.

8. The optoelectronic device according to claim 7, wherein: The mesoporous material is selected from one or more of mesoporous silica, mesoporous zeolite, mesoporous carbon, nano-iron oxide, and mesoporous bioactive glass-polyurethane nanocomposite materials; and / or, The pore size of the mesopores in the mesoporous material may be 2 to 50 nm; and / or, The average particle size of the mesoporous material is 0.1-5 μm.

9. The optoelectronic device according to claim 7, wherein: The volume percentage of the mesoporous material in the encapsulation layer is 5% to 10%. Preferably, the volume percentage of the mesoporous material in the encapsulation layer is 7% to 10%.

10. The optoelectronic device according to any one of claims 1 to 9, wherein: The encapsulation layer includes a main material, and the main material is selected from one or more of epoxy resin, polyimide, benzocyclobutene resin, and bismaleimide triazine resin.

11. The optoelectronic device according to any one of claims 1 to 10, wherein: The packaging layer comprises a first surface and a second surface which are arranged opposite to each other, wherein the first surface is close to the device body, the second surface is far away from the device body, and the second surface is a convex surface.

12. The optoelectronic device according to any one of claims 1 to 10, wherein: The encapsulation layer consists of the main material, the first microspheres, and the second microspheres.

13. The optoelectronic device according to any one of claims 1 to 10, wherein: The encapsulation layer consists of the main material, the first microspheres, the second microspheres and a mesoporous material.

14. The optoelectronic device according to claim 1, wherein: The optoelectronic device further comprises a protective layer, which is arranged on a side of the packaging layer away from the device body.

15. The optoelectronic device according to claim 14, wherein: The material of the protective layer includes one or more of epoxy resin, polyimide, benzocyclobutene resin, and bismaleimide triazine resin.

16. The optoelectronic device according to any one of claims 1 to 15, wherein: The device body comprises: A first electrode and a second electrode are arranged opposite to each other, wherein the first electrode or the second electrode is arranged close to the encapsulation layer; The electronic functional layer is arranged between the first electrode and the second electrode.

17. The optoelectronic device according to claim 16, wherein: The electronic functional layer comprises at least two sub-electronic functional layers stacked in layers; and / or The material of the electronic functional layer includes inorganic particles, and the shape of the inorganic particles includes one or more of spherical and polyhedral shapes.

18. The optoelectronic device according to claim 17, wherein: The average particle size of the inorganic particles is 3 to 6 nm; and / or The inorganic particles are selected from doped or undoped inorganic nanocrystals; wherein the undoped inorganic nanocrystals are selected from one or more of ZnO, TiO2, SnO2, Ta2O3, ZrO2, NiO, Al2O3, GaO, Ga2O3, ZnS, ZnSe, CdS, InP, GaP, BaTiO3, Cs2CO3, Rb2CO3, RbBr, LiF, LiF / Yb, MgP, and MgF2; the doped inorganic nanocrystals include the undoped inorganic nanocrystals and doping elements, and the doping elements are selected from one or more of Mg, Ca, Li, Ga, Al, Co, Mn, Zr, W, Ti, and Y.

19. The optoelectronic device according to claim 18, wherein: The device body also includes a light-emitting layer, which is arranged between the first electrode and the electronic functional layer, or the light-emitting layer is arranged between the second electrode and the electronic functional layer; wherein the material of the light-emitting layer is selected from one or more of organic light-emitting materials and quantum dots, wherein the organic light-emitting material is selected from one or more of diaromatic anthracene derivatives, distilbene aromatic derivatives, pyrene derivatives or fluorene derivatives, TBPe fluorescent materials emitting blue light, TTPA fluorescent materials emitting green light, TBRb fluorescent materials emitting orange light and DBP fluorescent materials emitting red light; the quantum dots are selected from one or more of single-structure quantum dots, core-shell structure quantum dots and perovskite semiconductor materials, and the single The structural quantum dots are selected from one or more of II-VI compounds, IV-VI compounds, III-V compounds and I-III-VI compounds, wherein the II-VI compounds are selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZn The IV-VI group compound is selected from one or more of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, SnPbSTe, and the III-V group compound is selected from one or more of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, One or more of AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPSb, the I-III-VI group materials The compound is selected from one or more of CuInS, CuInSe and AgInS; the core of the quantum dot with core-shell structure is selected from any one of the above-mentioned single structure quantum dots, and the shell material of the quantum dot with core-shell structure is selected from one or more of CdS, CdTe, CdSeTe, CdZnSe, CdZnS, CdSeS, ZnSe, ZnSeS and ZnS; the perovskite semiconductor material is selected from doped or undoped inorganic perovskite semiconductor, or organic-inorganic hybrid perovskite semiconductor; the general structural formula of the inorganic perovskite semiconductor is AMX3, wherein A is Cs + ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ One or more of, X is a halogen anion selected from Cl - Br - ,I - One or more of; the general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX3, wherein B is an organic amine cation selected from CH3(CH2) n-2 NH3 + or [NH3(CH2) n NH3] 2+ , where n≥2, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ One or more of, X is a halogen anion selected from Cl - Br - ,I - One or more of; and / or The first electrode and the second electrode are independently selected from metal electrodes, carbon electrodes, doped or undoped metal oxide electrodes and composite electrodes; wherein the material of the metal electrode is selected from one or more of Al, Ag, Cu, Mo, Au, Ba, Ca and Mg; the material of the carbon electrode is selected from one or more of graphite, carbon nanotubes, graphene and carbon fiber; the material of the doped or undoped metal oxide electrode is selected from one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO and AMO; the material of the composite electrode is selected from one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS and ZnS / Al / ZnS.

20. A display device, wherein: The display device comprises the optoelectronic device according to any one of claims 1-19.

Citation Information

Patent Citations

  • Organic electroluminescent device and preparation method thereof

    CN104183742A

  • Waterproof anti-reflection flexible OLED device and preparation method thereof

    CN105226198A

  • Electroluminescent device, preparation method thereof and photoelectric device

    CN116171063A

  • Organic light emitting diode display

    KR1020170050847A

  • Light emitting device package

    US20130256728A1