Honing ring and method for producing the honing ring

The polyurethane-based honing ring with embedded abrasives addresses the limitations of ceramic honing rings by achieving superior surface quality and reduced weight, effectively meeting the demands of electric vehicle transmission parts.

WO2024246310A1PCT designated stage expired Publication Date: 2024-12-05KREBS & RIEDEL SCHLEIFSCHEIBENFABRIK GMBH & CO KG
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2024/065071
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-01
Filing Date
2024-05-31
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing honing rings, particularly those made of ceramic, fail to achieve high surface quality and are heavy, making them unsuitable for meeting the stringent requirements of transmission parts in electric vehicles and other applications.

Method used

A honing ring with an annular body composed of a polyurethane bonding matrix embedded with abrasives like corundum, zirconium corundum, silicon carbide, or diamond, which has a toothing on its inner surface for surface processing, offering improved damping behavior and reduced weight compared to ceramic systems.

Benefits of technology

The polyurethane-based honing ring achieves higher surface quality and lower weight, meeting the high requirements for electric vehicle transmission parts while avoiding the limitations of ceramic and multi-layer composite systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2024065071_05122024_PF_FP_ABST
    Figure EP2024065071_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a honing ring (100) for the surface treatment of toothing contours of workpieces, with an annular body (20) consisting substantially of a polyurethane bonding matrix (10) in which at least one abrasive (14), in the form of corundum, zirconium corundum, silicon carbide, cubic boron nitride or diamond or a combination of at least two of the aforementioned, is embedded, wherein the annular body (20) has a toothing (22) on an inner casing surface for the surface treatment of toothing contours of workpieces and has an outer casing surface (24) that can be brought into contact with a honing ring holder of a machine tool; and a method for producing a honing ring (100), comprising: mixing (200) raw materials of the polyurethane bonding matrix (10) with the at least one abrasive (14); casting (300) a honing ring blank (30) from the resulting mixture; curing (400); and mechanically conditioning (500) the honing ring blank (30) to obtain the honing ring (100) in the form of the annular body (20).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Honing ring and method for producing the honing ring

[0002] The invention relates to a honing ring and a method for producing the honing ring.

[0003] background

[0004] Gear honing is a hard finishing process for the surface treatment of gear components, especially gears, which is used, for example, in the manufacture of transmissions.

[0005] EP 3 760 369 A1 describes a honing ring for surface treatment of toothed workpieces, comprising an annular body made of ceramic in which abrasive is embedded and which has a toothing on an inner circumferential surface which can be brought into contact with the toothed workpiece, wherein the annular body made of ceramic is surrounded in a radial direction by at least one outer ring which consists essentially of at least one synthetic resin and has an outer ring thickness of more than 15 mm.

[0006] Disclosure of the invention

[0007] The object of the invention is to create a novel homing that enables a high surface quality when machining a workpiece.

[0008] The object is achieved by a homing according to claim 1. Advantageous embodiments are mentioned in the subclaims.

[0009] According to one aspect of the invention, a homing device is provided for surface machining of gear contours on workpieces, comprising: an annular body which consists essentially of a polyurethane bond matrix into which at least one abrasive in the form of corundum, zirconium corundum, silicon carbide, cubic boron nitride or diamond or a combination of at least two of the above is embedded, wherein the annular body has a toothing on an inner circumferential surface for surface machining of gear contours on workpieces, and wherein the annular body has an outer circumferential surface which can be brought into contact with a honing ring holder of a machine tool. The abrasive can be referred to as abrasive grain. The workpiece can in particular be a metallic workpiece and / or the gear contours can be metallic gear contours.

[0010] The invention provides a homing device for surface machining of workpieces, which comprises an annular body or, in particular, can consist of the annular body. The annular body consists essentially of a polyurethane bond matrix. At least one abrasive in the form of corundum, zirconium corundum, silicon carbide, cubic boron nitride, or diamond is embedded in the polyurethane bond matrix. A combination of at least two of the aforementioned abrasives can also be embedded in the polyurethane bond matrix. A toothing is formed on an inner circumferential surface of the annular body. The toothing is designed for surface machining of tooth contours of the workpieces. The annular body has an outer circumferential surface designed for contact with a honing ring holder of a machine tool.In particular, the annular body can comprise or consist of a pure polyurethane bond matrix and the at least one abrasive. The homing can, in particular, be a homing in the form of the annular body. That is, the homing can consist of the bond matrix and the abrasive / abrasive grain.

[0011] Homing is characterized by the fact that, due to the annular body comprising the inner surface with toothing and the outer surface and comprising at least one abrasive embedded in the polyurethane bond matrix, multi-layer composite systems, in particular a ceramic-ceramic composite or a ceramic-polymer composite, can be avoided.

[0012] At the same time, the polyurethane bonding matrix of the annular body provides favorable damping properties for the honing ring. Advantageous damping properties can also be provided by the grinding or polishing coating (the abrasive).

[0013] Due to the slightly elastic polyurethane bond matrix, higher surface qualities of the workpieces (components) to be machined can be achieved compared to ceramic tools or conventional multilayer composite systems with a ring-shaped ceramic body. This makes it possible, for example, to meet the high surface quality requirements of transmission parts for electric vehicles. Compared to ceramic honing rings, the polyurethane bond matrix also enables advantageous, particularly lower, weight.

[0014] For example, the polyurethane binding matrix can be obtained from a polyurethane composition comprising at least one polyol component and at least one isocyanate component, and at least one additive. The polyurethane binding matrix or polyurethane composition can thus comprise common polyurethane systems consisting of at least one polyol component and at least one isocyanate component.

[0015] In embodiments, the proportion of the polyurethane binding matrix in the total mass of the annular body or the honing ring is in a range of 20 to 95 mass percent (mass%).

[0016] In addition to the abrasive, the polyurethane bond matrix can also contain other additives, depending on the application conditions. These additives can consist of typical polymer additives (e.g., processing and temperature stabilizers) and can also contain reinforcing fiber materials.

[0017] The polyurethane binding matrix can be colored, e.g., using commercial color pastes for polyurethane materials. This means that the polyurethane binding matrix or the polyurethane composition can comprise at least one color additive or coloring additive.

[0018] In embodiments, the polyurethane binding matrix is ​​obtained from a polyurethane composition comprising at least one polyol component, at least one isocyanate component, and at least one additive. In embodiments, the additive content of the polyurethane composition is in a range from 2 to 75 percent by mass. The at least one additive can, for example, comprise at least one filler, in particular one or more common fillers for polyurethane systems, such as calcium silicates, aluminosilicates, aluminum oxides, aluminum hydroxides, or other ceramic oxides, or combinations of at least two thereof.

[0019] In embodiments, the polyurethane binding matrix contains at least one fiber material. The at least one fiber material can comprise at least one of glass fibers, carbon fibers, ceramic fibers, metal fibers, polymer fibers (e.g., aramids), and / or natural fibers (e.g., cellulose).

[0020] In embodiments, the at least one fiber material comprises at least one fiber material in the form of fibers with a length (or an average length) of more than 10 mm and / or fibers with a length (or an average length) of 10 mm or less. The at least one fiber material can comprise a fiber material in the form of short fibers with a length of more than 10 mm. Short fibers are fibers, in particular natural fibers, that have an average length approximately in the range of 40 mm to 100 mm, but have a length of more than 10 mm. The at least one fiber material can comprise a fiber material in the form of ultrashort fibers with a length of 10 mm or less. Ultrashort fibers are referred to here as fibers that have a length of 10 mm or less.In embodiments, the at least one fiber material comprises at least one fiber material in the form of fibers that are arranged or incorporated in a random or random manner in the polyurethane binding matrix. This can, in particular, comprise fibers with a length (or an average length) of more than 10 mm and / or fibers with a length (or an average length) of 10 mm or less, in particular made of the above-mentioned materials such as glass fibers, carbon fibers, ceramic fibers, metal fibers, polymer fibers (e.g., aramids), and / or natural fibers (e.g., cellulose).

[0021] In embodiments, the at least one fiber material comprises at least one fiber material in the form of a fiber composite, for example, a continuous composite and / or a long-fiber composite and / or a continuous and long-fiber composite. The fiber composite can, for example, comprise a woven fabric, a non-crimp fabric, a braided fabric, a knitted fabric, etc., and / or combinations thereof. A fiber material in the form of a fiber composite can, for example, be incorporated in a load-adapted manner.

[0022] In embodiments, the proportion of the at least one fiber material of the polyurethane binding matrix to the volume of the polyurethane binding matrix is ​​in the range of 0.5 to 60 volume percent (vol.%).

[0023] In embodiments, the annular body or honing ring has a porosity, in particular a porosity in the range of 0.5 to 60 volume percent, particularly preferably in the range of 1.0 to 20 volume percent. The porosity can, for example, be individually adapted to the requirements of a workpiece to be machined. By creating a porous tool structure (structure of the annular body), increased machining space can be achieved and material removal rates can be increased. The reduced weight compared to ceramic systems is a further advantage.

[0024] In embodiments, the annular body or homing has a density in the range of 1.0 to 9.0 g / cm 3 preferably in the range of 1.2 to 4.0 g / cm 3The density can, for example, be individually adapted to the requirements of a workpiece to be processed. When determining the density as mass per volume, any pore volume due to porosity is included in the volume, i.e., if porosity is present, the density differs from the true density of the annular body.

[0025] In embodiments, the polyurethane binding matrix has a modulus of elasticity in a range of 1.0 to 15 GPa, preferably between 4.0 and 12 GPa. The modulus of elasticity can, for example, be individually adapted to the requirements of a workpiece to be processed.

[0026] The polyurethane bonding matrix can be individually adapted to the requirements of a workpiece to be processed, particularly with regard to porosity, elasticity, and density, by adding additives. The honing ring can be manufactured using the process described below.

[0027] According to a further aspect of the invention, a method for producing a honing ring is provided, comprising: mixing raw materials of the polyurethane bond matrix with the at least one abrasive in the form of corundum, zirconium corundum, silicon carbide, cubic boron nitride, or diamond, or a combination of at least two of the above; casting a honing ring blank from the mixture obtained by mixing; curing (or allowing to cure) the honing ring blank; mechanically conditioning the honing ring blank to obtain the homing in the form of the annular body. The method can be a method for producing a honing ring of the type described above. The raw materials of the polyurethane bond matrix can, in particular, comprise a polyurethane composition.

[0028] In embodiments, the raw materials of the polyurethane binding matrix or the polyurethane composition can comprise at least one polyol component and at least one isocyanate component. For example, the raw materials of the polyurethane binding matrix or the polyurethane composition can comprise at least one polyol component and at least one isocyanate component and at least one additive. The raw materials of the polyurethane binding matrix or the polyurethane composition can comprise hollow spheres or the like as an additive for adjusting the porosity of the resulting annular body. The raw materials of the polyurethane binding matrix or the polyurethane composition can comprise at least one color additive or coloring additive. The raw materials of the polyurethane binding matrix or the polyurethane composition can comprise at least one filler, in particular of the types described above.

[0029] Mixing can take place in a mixing chamber, and / or pouring can take place in a mold. The raw materials are fed into the mixing chamber. Mixing can be performed, for example, using an extruder screw. Other common methods (mixing techniques) can also be used to bond and / or process the abrasive with the polyurethane bond matrix. Mixing can include homogenizing the mixture. The mixture can flow or be poured into the mold via at least one casting tube.

[0030] When raw materials of the polyurethane bond matrix are mixed with the at least one abrasive, a mixture is created, in particular a bond-abrasive mixture. A semi-finished product (blank) is then cast from the (bond-abrasive) mixture. The semi-finished product / blank can be made from highly dense to highly porous. For this purpose, known casting processes for the production of fine grinding and polishing tools from polyurethane or epoxy resins can be used, for example. Preferably, a vacuum-assisted casting process is used, which allows both highly dense and defined homogeneous and defined porosity semi-finished products to be produced. The final production step involves mechanical conditioning (adjustment of the final dimensions or profiling) of the semi-finished product.

[0031] The mixing of raw materials of the polyurethane bond matrix with the at least one abrasive can be carried out in a one-stage mixing process or in a two-stage mixing process in which, for example, only a part of the at least one polyol component is mixed with the at least one isocyanate component in a first stage.

[0032] In some embodiments, the honing ring blank is cured at room temperature. The honing ring blank can be cured at room temperature without subsequent tempering. After casting and during the curing process of the compound, a shrinkage process occurs. This process is caused by the onset of material crosslinking and can be accounted for by appropriate mold design.

[0033] In embodiments, the mechanical conditioning comprises adjusting the final dimensions of the honing ring and / or introducing or reworking the toothing on the inner circumferential surface of the annular body of the honing ring.

[0034] The mechanical conditioning of the honing ring blank can include adjusting the outer diameter and / or the inner diameter and / or a thickness dimension (in the radial direction) and / or a width dimension (in the direction transverse to the diameter). The mechanical conditioning of the honing ring blank can include the introduction or reworking of the toothing on the inner circumferential surface of the honing ring blank. The toothing type can be selected arbitrarily. The shape of the toothing can be adapted to the toothing depth of the workpiece. The thickness dimension and / or the width dimension can be adapted to a honing tool, in particular to a honing ring holder of a machine tool.

[0035] The raw materials of the polyurethane binding matrix or the polyurethane composition may comprise at least one fiber material. In embodiments, the raw materials of the polyurethane binding matrix that are mixed in the mixing step comprise at least one fiber material in the form of fibers with a length of more than 10 mm and / or fibers with a length of 10 mm or less, and / or the method comprises: introducing at least one fiber material in the form of a fiber composite into a casting mold for the honing ring blank prior to casting the honing ring blank.

[0036] In embodiments, in the mixing step, at least one fiber material is mixed with other raw materials of the polyurethane bond matrix and with the at least one abrasive. In embodiments, this at least one fiber material comprises at least one fiber material in the form of fibers with a length (or an average length) of more than 10 mm and / or fibers with a length (or an average length) of 10 mm or less. The at least one fiber material can comprise a fiber material in the form of short fibers with a length of more than 10 mm. The at least one fiber material can comprise a fiber material in the form of ultrashort fibers with a length of 10 mm or less. As a result of the mixing, the fibers in the resulting honing ring are arranged or incorporated in a disordered or random manner in the polyurethane bond matrix.This can particularly include fibers with a length (or an average length) of more than 10 mm and / or fibers with a length (or an average length) of 10 mm or less, in particular made of the above-mentioned materials such as glass fibers, carbon fibers, ceramic fibers, metal fibers, polymer fibers (e.g. aramids) and / or natural fibers (e.g. cellulose). In embodiments, the method comprises: placing (introducing) at least one fiber material in the form of a fiber composite in a casting mold, prior to the step of casting the honing ring blank. Casting then takes place in the casting mold. The fiber composite can, for example, be a continuous composite and / or long-fiber composite and / or a continuous and long-fiber composite. The fiber composite can, for example, comprise a woven fabric, a non-crimp fabric, a braided fabric, a knitted fabric, etc., and / or combinations of the above.One or more fiber composites can be placed in the mold in layers or tiers, for example. A fiber material in the form of a fiber composite can be placed in the mold in a load-bearing manner.

[0037] In embodiments, the proportion of the at least one fiber material of the polyurethane bond matrix to the volume of the polyurethane bond matrix of the honing ring is in the range of 0.5 to 60 volume percent (vol.%).

[0038] In embodiments, the casting is carried out using a negative pressure-assisted casting process. A negative pressure-assisted casting process can also be referred to as a vacuum-assisted casting process, where vacuum here can be a rough vacuum. Mixing can take place in a mixing chamber under negative pressure, and / or casting can take place in a / the casting mold under negative pressure. Negative pressure here refers to the (absolute) pressure (i.e. the air pressure) in the mixing chamber or in the casting mold. In embodiments, the negative pressure is at least 100 mbar. The negative pressure can in particular be in a range between 100 mbar and ambient pressure. Preferably, the negative pressure is in a range between 200 and 400 mbar. The raw materials are fed to the mixing chamber. Mixing can take place, for example, by means of an extruder screw.Other common methods (mixing techniques) can also be used to bond and / or process the abrasive with the polyurethane bond matrix. Mixing can involve homogenizing the mixture. The mixture can flow or be poured into the mold via at least one casting tube. The vacuum-assisted casting process, with mixing and pouring under reduced pressure, can produce an extremely high degree of homogeneity of the overall mass, and thus an extremely high degree of homogeneity of the annular body of the honing ring. The process can include: producing or adjusting the porosity of the resulting honing ring by adjusting the vacuum.

[0039] In embodiments, the annular body or honing ring has a porosity, in particular a porosity in the range of 0.5 to 60 volume percent, particularly preferably in the range of 1.0 to 20 volume percent. In embodiments, the annular body or homing has a density in the range of 1.0 to 9.0 g / cm 3 preferably in the range of 1.2 to 4.0 g / cm 3 The density can be adjusted and defined by the selected raw material combination. The abrasive grain and the polyurethane bond matrix used are crucial factors. The porosity can be adjusted by the mixing chamber conditions (negative pressure areas, for example, adjusted using a vacuum unit or gas supply) and / or the additives used (hollow spheres or similar).

[0040] Brief description of the drawings

[0041] Embodiments of the invention are explained in more detail below with reference to the drawings. They show:

[0042] Fig. 1 is a schematic perspective view of a honing ring according to an embodiment;

[0043] Fig. 2 is a schematic representation of a method for producing a honing ring according to an embodiment.

[0044] Detailed description of embodiments

[0045] The honing ring shown in Fig. 1 for surface finishing of workpieces consists of an annular body 20 made of a polyurethane bond matrix 10 with embedded abrasive 14 and can be manufactured by the method according to Fig. 2. At least one abrasive 14 in the form of corundum, zirconium corundum, silicon carbide, cubic boron nitride or diamond or a combination of at least two of the above is embedded in the polyurethane bond matrix 10. The polyurethane bond matrix 10 is obtained from a polyurethane composition comprising at least one polyol component 11 and at least one isocyanate component 12. The polyurethane composition of the polyurethane bond matrix 10 comprises at least one additive 16. The additive content is in a range from 2 to 75 mass percent.The polyurethane bonding matrix 10 comprises at least one fiber material 18, in particular glass fibers, carbon fibers, ceramic fibers, metal fibers, polymer fibers (e.g., aramids), and / or natural fibers (e.g., cellulose). The annular body 20 has a toothing 22 on an inner circumferential surface for surface machining of tooth contours of the workpieces. The annular body 20 has an outer circumferential surface 24 that can be brought into contact with a honing ring holder of a machine tool. The outer shape of the honing ring 100 corresponds to a cylindrical disk with a concentric, continuous opening, on whose circumferential surface the toothing 22 is formed. The opening can, for example, be substantially cylindrical or substantially conical. The honing ring 100 has a porosity in the range of 1.0 to 20 percent by volume. The homing 100 has a density in the range of 1.2 to 4.0 g / cm³. 3The Homing 100 exhibits elasticity, in particular a modulus of elasticity in a range of 4.0 to 12 GPa.

[0046] As schematically shown in Fig. 2, the method for producing the honing ring 100 comprises mixing 200 raw materials of the polyurethane bond matrix 10 with at least one abrasive 14. During mixing 200, the raw materials are mixed in a mixing chamber by means of an extruder screw. Mixing takes place under a vacuum, wherein the mixing chamber can be evacuated to adjust the vacuum in order to increase the homogeneity of the mixture and the resulting annular body 20. The raw materials of the polyurethane bond matrix 10 comprise at least one polyol 11 and at least one isocyanate 12. The polyurethane bond matrix content is in a range from 20 to 95 mass percent of the total mass of the honing ring 100. The at least one abrasive 14 is corundum, zirconium corundum, silicon carbide, cubic boron nitride, or diamond, or a combination of at least two of the above. The polyurethane binding matrix 10 comprises at least one additive 16, orThe raw materials of the polyurethane bond matrix 10 comprise at least one additive 16. The additive content 16 ranges from 2 to 75 percent by mass. The polyurethane bond matrix 10 can contain at least one fiber material 18. The density of the honing ring is determined by the at least one abrasive 14 and the polyurethane bond matrix 10. The density is, for example, in the range of 1.2 to 4.0 g / cm³. 3 The porosity of the honing ring 100 is adjusted by the negative pressure in the mixing chamber and at least one additive 16. The porosity of the honing ring, for example, is in a range of 1.0 to 20 percent by volume.

[0047] Mixing can take place in a casting system, which may include various support guides (hoses and / or channels), a pump unit (for generating the vacuum or negative pressure), a mixing chamber, and an output unit (casting pipe) to the casting mold. The raw materials are fed into the mixing chamber via the support guides. An extruder screw rotates in the mixing chamber, mixing all the components together.

[0048] In the next step of the method, a honing ring blank 30 is cast 300 from the mixture obtained by mixing 200. Before casting 300, in one variant of the method, continuous and / or long-fiber composites can be arranged as fiber material 18' in the casting mold, in particular introduced in layers and / or layers, in addition to or instead of the at least one fiber material 18. The homogenized, mixed raw materials are fed to the casting mold via a casting pipe. Casting 300 takes place under a vacuum. The vacuum lies in a range between 100 mbar and ambient pressure, in particular in a range between 200 and 400 mbar.

[0049] In the next step of the process, the honing ring blank 30 is hardened 400. The hardening 400 of the honing ring blank 30 takes place at room temperature without tempering the honing ring blank 30 after completion of the hardening 400.

[0050] In the final step, mechanical conditioning 500 of the honing ring blank 30 is performed to obtain the homing 100. The mechanical conditioning 500 includes adjusting the final dimensions of the honing ring 100. The mechanical conditioning 500 includes introducing and / or reworking a toothing 22 on an inner circumferential surface of the annular body 20 of the honing ring 100.

Claims

Patent claims 1. Honing ring (100) for surface machining of gear contours of workpieces, comprising: an annular body (20) which consists essentially of a polyurethane bond matrix (10) into which at least one abrasive (14) in the form of corundum, zirconium corundum, silicon carbide, cubic boron nitride or diamond or a combination of at least two of the above is embedded, wherein the annular body (20) has a toothing (22) on an inner circumferential surface for surface machining of gear contours of workpieces, and wherein the annular body (20) has an outer circumferential surface (24) which can be brought into contact with a honing ring holder of a machine tool.

2. Honing ring (100) according to claim 1, wherein the proportion of the polyurethane binding matrix (10) in the total mass of the annular body (20) is in a range of 20 to 95 mass percent.

3. Honing ring (100) according to claim 1 or 2, wherein the polyurethane bonding matrix (10) is obtained from a polyurethane composition comprising at least one polyol component (11) and at least one isocyanate component (12) and at least one additive (16), wherein the additive content of the polyurethane composition is in a range of 2 to 75 mass percent.

4. Honing ring (100) according to claim 1 to 3, wherein the polyurethane binding matrix (10) contains at least one fiber material (18).

5. Honing ring (100) according to claim 4, wherein the at least one fiber material (18) comprises at least one of glass fibers, carbon fibers, ceramic fibers, metal fibers, polymer fibers and / or natural fibers.

6. Honing ring (100) according to claim 4 or 5, wherein the at least one fiber material (18) comprises at least one fiber material in the form of fibers with a length of more than 10 mm and / or fibers with a length of 10 mm or less.

7. Honing ring (100) according to one of claims 4 to 6, wherein the at least one fiber material (18) comprises at least one fiber material in the form of a fiber composite.

8. Honing ring (100) according to one of claims 4 to 7, wherein the proportion of the at least one fiber material (18) of the polyurethane binding matrix (10) to the volume of the polyurethane binding matrix (10) is in the range of 0.5 to 60 volume percent.

9. Honing ring (100) according to one of the preceding claims, wherein the annular body (20) has a porosity in the range of 0.5 to 60 volume percent.

10. Honing ring (100) according to one of the preceding claims, wherein the annular body (20) has a density in the range of 1.0 to 9.0 g / cm 3 has.

11. Honing ring (100) according to one of the preceding claims, wherein the polyurethane bond matrix (10) has a modulus of elasticity in a range of 1.0 to 15 GPa.

12. A method for producing a honing ring (100), in particular a honing ring (100) according to one of claims 1 to 11, the method comprising: Mixing (200) raw materials of the polyurethane bond matrix (10) with the at least one abrasive (14) in the form of corundum, zirconium corundum, silicon carbide, cubic boron nitride or diamond or a combination of at least two of the above; Casting (300) a honing ring blank (30) from the mixture obtained by mixing (200); Hardening (400) of the honing ring blank (30); mechanically conditioning (500) of the honing ring blank (30) to obtain the honing ring (100) in the form of the annular body (20).

13. The method according to claim 12, wherein the mechanical conditioning (500) comprises adjusting the final dimensions of the honing ring (100) and / or introducing or reworking the toothing (22) on the inner circumferential surface of the annular body (20) of the honing ring (100).

14. The method according to claim 12 or 13, wherein the raw materials of the polyurethane binding matrix (10) which are mixed in the mixing step comprise at least one fiber material (18) in the form of fibers with a length of more than 10 mm and / or fibers with a length of 10 mm or less, and / or wherein the method comprises: introducing at least one fiber material (18) in the form of a fiber composite into a casting mold for the homing blank (30) before casting (300) the honing ring blank (30).

15. The method according to any one of claims 12 to 14, wherein the casting (300) is carried out by a vacuum-assisted casting process (310).

Citation Information

Patent Citations

  • Honing ring for surface machining of toothed workpieces and method if manufacturing the ring

    EP3760369A1

  • Composite honing ring, useful for machining cog wheels, has honing part, containing polishing particles and polishing particle agglomerates in binder, and elastic supporting part

    AT414104B

  • Helical honing tool for gear wheel - has abrasive particles embedded in polymer esp. mixt. of polyurethane and epoxy resin

    DE2304398A1

  • Composite honing ring

    EP1030757B1

  • Grindstone having resinoid abrasive structure including abrasive agglomerates each provided by vitrified abrasive structure

    US20040176019A1